Method for manufacturing solar cell and method for manufacturing circuit board
A manufacturing method for solar cells and circuit boards using a physical peeling resin and reduced pressure spraying forms metal electrode layers and wiring with a layered structure, addressing warpage and stress issues, enhancing reliability and simplifying production.
Patent Information
- Application Number
- JP2023046202
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Solar cells and circuit boards experience warpage due to internal stress generated by metal electrode layers and metal wiring, respectively, which reduces their reliability.
A manufacturing method involving a physical peeling step using a resin pattern and reduced pressure spraying to form metal electrode layers and metal wiring with a layered structure, where metal particles are deposited in rows, allowing for low Young's modulus and high flexibility, thereby reducing internal stress and warpage.
The method effectively reduces warpage and internal stress in solar cells and circuit boards, improving their reliability and simplifying manufacturing processes while maintaining adhesion, resistance, and bonding strength.
Smart Images

Figure 2024135493000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a solar cell and a method for manufacturing a circuit board. [Background technology]
[0002] Solar cells using a semiconductor substrate include a double-sided electrode type solar cell in which electrodes are formed on both the light-receiving surface side and the back surface side, and a back surface electrode type solar cell in which an electrode is formed only on the back surface side. Patent Document 1 discloses a double-sided electrode type solar cell, and Patent Document 2 discloses a back surface electrode type solar cell. As disclosed in Patent Documents 1 and 2, whether it is a double-sided electrode type or a back surface electrode type solar cell, the solar cell includes a semiconductor substrate, a conductive semiconductor layer disposed on the main surface of the semiconductor substrate, and a metal electrode layer corresponding to the conductive semiconductor layer.
[0003] It is also known that circuit boards include metal wiring. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-152620 A [Patent Document 2] JP 2019-121627 A Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, in solar cells, a metal electrode layer is formed on a semiconductor substrate, which causes the semiconductor substrate to warp and generates stress inside the semiconductor substrate. This tendency is more pronounced in back electrode type solar cells. When the internal stress of the semiconductor substrate increases, the reliability of the solar cell decreases.
[0006] Furthermore, since metal wiring is formed on a circuit board, warping also occurs in the circuit board.
[0007] An object of the present invention is to provide a method for manufacturing a solar cell and a method for manufacturing a circuit board that reduce (suppress or mitigate) warpage. [Means for solving the problem]
[0008] A method for manufacturing a solar cell according to the present invention is a method for manufacturing a solar cell comprising a semiconductor substrate, a conductive semiconductor layer disposed on a main surface of the semiconductor substrate, and a metal electrode layer corresponding to the conductive semiconductor layer, and includes the following steps: a semiconductor layer forming step of forming the conductive semiconductor layer on the main surface of the semiconductor substrate; a physical release resin forming step of forming a pattern of physically peelable physically peelable resin in an area of the main surface of the semiconductor substrate where the metal electrode layer is not formed; a metal electrode layer material film forming step of forming a material film of the metal electrode layer by using a reduced pressure spraying method to melt metal particles by discharge in a reduced pressure environment, spraying the melted metal particles with a carrier gas onto the semiconductor substrate, and depositing the metal particles on the conductive semiconductor layer of the semiconductor substrate and the physical release resin; and a metal electrode layer forming step of removing the material film of the metal electrode layer on the physical release resin by peeling off the physical release resin, thereby forming the metal electrode layer having a layer structure in which metal particles are stacked in a continuous manner.
[0009] The method for manufacturing a circuit board according to the present invention is a method for manufacturing a circuit board including a dielectric layer and metal wiring, and includes the following steps: a physical release resin formation step of forming a pattern of physically peelable physically peelable resin in an area of the dielectric layer where the metal wiring is not formed; a metal wiring material film formation step of forming a material film for the metal wiring by melting metal particles by discharge in a reduced pressure environment using a reduced pressure spraying method, spraying the molten metal particles with a carrier gas onto the dielectric layer, and depositing the metal particles on the dielectric layer and the physically release resin; and a metal wiring formation step of removing the material film for the metal wiring on the physically release resin by peeling off the physically release resin, and forming the metal wiring having a layer structure in which metal particles are accumulated in a continuous manner. Effect of the Invention
[0010] According to the present invention, it is possible to reduce (suppress, mitigate) warpage in solar cells and circuit boards. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram showing a solar cell (back electrode type) according to a first embodiment as viewed from the back surface side. [Diagram 2] 2 is a cross-sectional view taken along line II-II of the solar cell (back electrode type) of FIG. 1. [Figure 3A] 5 is a diagram showing a semiconductor layer formation step in the method for manufacturing the solar cell (back electrode type) according to the first embodiment. FIG. [Figure 3B] FIG. 4 is a diagram showing a physical release resin formation step in the method for manufacturing the solar cell (back electrode type) according to the first embodiment. [Figure 3C] FIG. 4 is a diagram showing a transparent electrode layer material film forming step in the method for manufacturing the solar cell (back electrode type) according to the first embodiment. [Figure 3D] FIG. 4 is a diagram showing a metal electrode layer material film forming step in the method for manufacturing the solar cell (back electrode type) according to the first embodiment. [Figure 3E] 3A to 3C are diagrams illustrating a transparent electrode layer and metal electrode layer forming step in the method for manufacturing the solar cell according to the first embodiment. [Figure 4] FIG. 4 is a cross-sectional view of a solar cell (double-sided electrode type) according to a modified example of the first embodiment. [Diagram 5] 2 is a cross-sectional view of a solar cell (back electrode type) according to a second embodiment, taken along line II-II in FIG. [Figure 6A] 10 is a diagram showing a semiconductor layer formation step in a method for manufacturing a solar cell (back electrode type) according to a second embodiment. FIG. [Figure 6B] FIG. 11 is a diagram showing a physical release resin formation step in the method for manufacturing a solar cell (back electrode type) according to the second embodiment. [Figure 6C] FIG. 11 is a diagram showing a transparent electrode layer material film forming step in a manufacturing method for a solar cell (back electrode type) according to a second embodiment. [Figure 6D]FIG. 11 is a diagram showing a step of forming an underlayer material film for a metal electrode layer in a manufacturing method for a solar cell (back electrode type) according to the second embodiment. [Figure 6E] 10A to 10C are diagrams illustrating a step of forming an underlayer for a transparent electrode layer and a metal electrode layer in a method for manufacturing a solar cell according to a second embodiment. [Figure 6F] 11A to 11C are diagrams showing a plating layer forming step of a metal electrode layer in a method for manufacturing a solar cell according to a second embodiment. [Figure 7] FIG. 11 is a cross-sectional view of a solar cell (double-sided electrode type) according to a modified example of the second embodiment. [Figure 8] FIG. 11 is a cross-sectional view of a circuit board according to a third embodiment. [Figure 9A] 13A to 13C are diagrams illustrating a physical release resin forming step in the method for manufacturing a circuit board according to the third embodiment. [Figure 9B] 13A to 13C are diagrams illustrating a metal wiring material film forming step in the method for manufacturing a circuit board according to the third embodiment. [Figure 9C] 13A to 13C are diagrams illustrating a metal wiring forming step in the method for manufacturing a circuit board according to the third embodiment. [Figure 10] FIG. 11 is a cross-sectional view of a circuit board according to a fourth embodiment. [Figure 11A] 13A to 13C are diagrams illustrating a physical release resin forming step in the method for manufacturing a circuit board according to the fourth embodiment. [Figure 11B] 13A to 13C are diagrams showing a step of forming an underlayer material film for metal wiring in the method for manufacturing a circuit board according to the fourth embodiment. [Figure 11C] 13A to 13C are diagrams illustrating a step of forming an underlayer for metal wiring in the method for manufacturing a circuit board according to the fourth embodiment. [Figure 11D] 13A to 13C are diagrams showing a step of forming a plating layer for metal wiring in the method for manufacturing a circuit board according to the fourth embodiment. [Figure 12A] 3 is an example of an SEM image of the surface of the metal electrode layer in the solar cell of FIG. 2. [Figure 12B] FIG. 12B is an example of an enlarged SEM image of part VB in FIG. 12A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals. For convenience, hatching and reference numerals may be omitted, in which case other drawings shall be referred to.
[0013] (Solar cell of the first embodiment) Fig. 1 is a view of the solar cell according to the first embodiment as seen from the back surface side, and Fig. 2 is a cross-sectional view of the solar cell along line II-II in Fig. 1. The solar cell 1 shown in Fig. 1 and Fig. 2 is a back electrode type (also called a back contact type or back junction type) heterojunction solar cell.
[0014] Solar cell 1 includes a semiconductor substrate 11 with two main surfaces, and the main surface of semiconductor substrate 11 has a first region 7 and a second region 8. In the following, the main surface of semiconductor substrate 11 that receives light is referred to as the light-receiving surface, and the main surface of semiconductor substrate 11 opposite the light-receiving surface is referred to as the back surface.
[0015] The first region 7 has a so-called comb shape and includes a plurality of finger portions 7f corresponding to the teeth of the comb and busbar portions 7b corresponding to supports for the teeth of the comb. The busbar portions 7b extend in a first direction (X direction) along one side of the semiconductor substrate 11, and the finger portions 7f extend from the busbar portions 7b in a second direction (Y direction) intersecting the first direction.
[0016] Similarly, the second region 8 has a so-called comb shape and has a plurality of finger portions 8f corresponding to the teeth of the comb and a busbar portion 8b corresponding to a support portion of the teeth of the comb. The busbar portion 8b extends in a first direction along one side portion of the semiconductor substrate 11 opposite the other side portion, and the finger portions 8f extend in a second direction from the busbar portion 8b.
[0017] The finger portions 7f and 8f are strip-shaped extending in the second direction and are alternately provided in the first direction. The first region 7 and the second region 8 may be formed in a stripe pattern.
[0018] 2, the solar cell 1 includes a passivation layer 13 and an optical adjustment layer 15, which are formed (deposited, laminated, formed) in that order on the light-receiving surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 23, a first conductivity type semiconductor layer 25, and a first electrode layer 27, which are formed (deposited, laminated, formed) in that order on a portion (mainly, the first region 7) of the back surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 33, a second conductivity type semiconductor layer 35, and a second electrode layer 37, which are formed (deposited, laminated, formed) in that order on another portion (mainly, the second region 8) of the back surface side of the semiconductor substrate 11.
[0019] The semiconductor substrate 11 is formed of a crystalline silicon material such as single crystal silicon or polycrystalline silicon. The semiconductor substrate 11 is, for example, an n-type semiconductor substrate in which a crystalline silicon material is doped with an n-type dopant. The semiconductor substrate 11 may be, for example, a p-type semiconductor substrate in which a crystalline silicon material is doped with a p-type dopant. An example of the n-type dopant is phosphorus (P). An example of the p-type dopant is boron (B). The semiconductor substrate 11 functions as a photoelectric conversion substrate that absorbs incident light from the light-receiving surface side and generates photocarriers (electrons and holes).
[0020] By using crystalline silicon as the material for the semiconductor substrate 11, the dark current is relatively small, and a relatively high output (stable output regardless of illuminance) can be obtained even when the intensity of incident light is low.
[0021] Semiconductor substrate 11 may have a pyramidal fine uneven structure called a texture structure on the light-receiving surface side, which reduces the reflection of incident light on the light-receiving surface and improves the light trapping effect in semiconductor substrate 11.
[0022] Furthermore, the semiconductor substrate 11 may have a pyramidal fine uneven structure, called a texture structure, on the back surface side thereof, which increases the efficiency of collection of light that is not absorbed by the semiconductor substrate 11 and passes through it.
[0023] The passivation layer 13 is formed on the light-receiving surface side of the semiconductor substrate 11. The passivation layer 23 is formed in a first region 7 on the back surface side of the semiconductor substrate 11. The passivation layer 33 is formed in a second region 8 on the back surface side of the semiconductor substrate 11. The passivation layers 13, 23, and 33 are formed of, for example, an intrinsic (i-type) amorphous silicon material. The passivation layers 13, 23, and 33 suppress recombination of carriers generated in the semiconductor substrate 11 and increase the carrier collection efficiency.
[0024] The optical adjustment layer 15 is formed on the passivation layer 13 on the light-receiving surface side of the semiconductor substrate 11. The optical adjustment layer 15 functions as an anti-reflection layer that prevents or suppresses reflection of incident light, and improves the efficiency of light incidence on the semiconductor substrate 11. The optical adjustment layer 15 also functions as a protective layer that protects the light-receiving surface side of the semiconductor substrate 11 and the passivation layer 13. The optical adjustment layer 15 is formed of an insulating material, for example, silicon oxide (SiO), silicon nitride (SiN), or a composite thereof such as silicon oxynitride (SiON).
[0025] The first conductive type semiconductor layer 25 is formed on the passivation layer 23, i.e., in the first region 7 on the back surface side of the semiconductor substrate 11. The first conductive type semiconductor layer 25 is formed of, for example, an amorphous silicon material. The first conductive type semiconductor layer 25 is, for example, a p-type semiconductor layer in which an amorphous silicon material is doped with a p-type dopant (for example, the above-mentioned boron (B)).
[0026] The second conductive type semiconductor layer 35 is formed on the passivation layer 33, i.e., in the second region 8 on the back surface side of the semiconductor substrate 11. The second conductive type semiconductor layer 35 is formed of, for example, an amorphous silicon material. The second conductive type semiconductor layer 35 is, for example, an n-type semiconductor layer in which an amorphous silicon material is doped with an n-type dopant (for example, the above-mentioned phosphorus (P)).
[0027] Alternatively, the first conductive type semiconductor layer 25 may be an n-type semiconductor layer, and the second conductive type semiconductor layer 35 may be a p-type semiconductor layer.
[0028] The first conductive type semiconductor layer 25 and the passivation layer 23, and the second conductive type semiconductor layer 35 and the passivation layer 33 form strips extending in the second direction (Y direction) and are arranged alternately in the first direction (X direction). Parts of the second conductive type semiconductor layer 35 and the passivation layer 33 may overlap parts of the adjacent first conductive type semiconductor layer 25 and passivation layer 23.
[0029] The first electrode layer 27 corresponds to the first conductive type semiconductor layer 25, specifically, is formed on the first conductive type semiconductor layer 25 in the first region 7 on the back surface side of the semiconductor substrate 11. The first electrode layer 27 may have a first transparent electrode layer 28 and a first metal electrode layer 29 formed in this order on the first conductive type semiconductor layer 25 (FIG. 2), or may have only the first metal electrode layer 29 formed on the first conductive type semiconductor layer 25 (not shown).
[0030] The second electrode layer 37 corresponds to the second conductive type semiconductor layer 35, specifically, is formed on the second conductive type semiconductor layer 35 in the second region 8 on the back surface side of the semiconductor substrate 11. The second electrode layer 37 may have a second transparent electrode layer 38 and a second metal electrode layer 39 formed in this order on the second conductive type semiconductor layer 35 (FIG. 2), or may have only the second metal electrode layer 39 formed on the second conductive type semiconductor layer 35 (not shown).
[0031] The first electrode layer 27 and the second electrode layer 37 are in the form of strips extending in the second direction (Y direction) and are alternately arranged in the first direction (X direction). The first electrode layer 27 and the second electrode layer 37 are separated from each other. That is, the first transparent electrode layer 28 and the second transparent electrode layer 38 are in the form of strips extending in the second direction and are alternately arranged in the first direction. The first transparent electrode layer 28 and the second transparent electrode layer 38 are separated from each other. Also, the first metal electrode layer 29 and the second metal electrode layer 39 are in the form of strips extending in the second direction and are alternately arranged in the first direction. The first metal electrode layer 29 and the second metal electrode layer 39 are separated from each other.
[0032] The first transparent electrode layer 28 and the second transparent electrode layer 38 are made of a transparent conductive material, such as ITO (Indium Tin Oxide: a composite oxide of indium oxide and tin oxide).
[0033] The first metal electrode layer 29 and the second metal electrode layer 39 are formed by a reduced pressure spraying method using particulate metal material such as silver, copper, aluminum, etc., as described later. Fig. 12A is an example of a SEM (Scanning Electron Microscope) image of the surface of the first metal electrode layer 29 and the second metal electrode layer 39, and Fig. 12B is an example of an SEM image in which the portion XIIB in Fig. 12A is enlarged. In the example of Fig. 12A and Fig. 12B, reduced pressure spraying was performed using copper powder with a particle diameter of 8 μm.
[0034] 12A and 12B, the first metal electrode layer 29 and the second metal electrode layer 39 have a layer structure in which metal particles are stacked in a continuous manner. When viewed from the back surface side, the size (particle diameter) of the metal particles in the first metal electrode layer 29 is 0.9 μm or more and 500 μm or less, and preferably 0.9 μm or more and 13 μm or less. When viewed from the back surface side, the size (particle diameter) of the metal particles in the second metal electrode layer 39 is 0.9 μm or more and 500 μm or less, and preferably 0.9 μm or more and 13 μm or less.
[0035] Also, in a cross section of the first metal electrode layer 29 along the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the first metal electrode layer 29 intersecting the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the back surface, there are gaps at the boundaries between the layer adjacent to the first metal electrode layer 29, i.e., the first transparent electrode layer 28, and the metal particles of the first metal electrode layer 29 (FIG. 2). Note that, if the first electrode layer 27 does not have the first transparent electrode layer 28, there are gaps at the boundaries between the layer adjacent to the first metal electrode layer 29, i.e., the first conductive type semiconductor layer 25, and the metal particles of the first metal electrode layer 29 in the cross section intersecting the back surface (not shown).
[0036] Also, in a cross section of the second metal electrode layer 39 along the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the second metal electrode layer 39 intersecting the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the back surface, there are gaps at the boundary between the layer adjacent to the second metal electrode layer 39, i.e., the second transparent electrode layer 38, and the metal particles of the second metal electrode layer 39 (FIG. 2). Note that, if the second electrode layer 37 does not have the second transparent electrode layer 38, there are gaps at the boundary between the layer adjacent to the second metal electrode layer 39, i.e., the second conductive type semiconductor layer 35, and the metal particles of the second metal electrode layer 39 in a cross section intersecting the light receiving surface (not shown).
[0037] (Method for manufacturing solar cell according to the first embodiment) Next, the method for manufacturing the solar cell according to the first embodiment will be described with reference to Figs. 3A to 3E. Fig. 3A is a diagram showing a semiconductor layer forming step in the method for manufacturing the solar cell according to the first embodiment, and Fig. 3B is a diagram showing a physical peeling resin forming step in the method for manufacturing the solar cell according to the first embodiment. Fig. 3C is a diagram showing a transparent electrode layer material film forming step in the method for manufacturing the solar cell according to the first embodiment, and Fig. 3D is a diagram showing a metal electrode layer material film forming step in the method for manufacturing the solar cell according to the first embodiment. Fig. 3E is a diagram showing a transparent electrode layer and metal electrode layer forming step in the method for manufacturing the solar cell according to the first embodiment.
[0038] 3A, a passivation layer 23 and a first conductive type semiconductor layer 25 are formed on a part of the back surface side of the semiconductor substrate 11, specifically, on the first region 7 (semiconductor layer formation step). An example of a method for forming the passivation layer 23 and the first conductive type semiconductor layer 25 will be described below, but the method for forming the passivation layer 23 and the first conductive type semiconductor layer 25 is not limited thereto.
[0039] For example, a passivation film and a first conductive type semiconductor film may be formed on the entire back surface of semiconductor substrate 11 by using a CVD method or a PVD method, and then passivation layer 23 and first conductive type semiconductor layer 25 may be patterned by using an etching method that uses a mask or a metal mask generated by a photolithography technique. Note that examples of etching solutions for p-type semiconductor films include acidic solutions such as hydrofluoric acid containing ozone and a mixture of nitric acid and hydrofluoric acid, and examples of etching solutions for n-type semiconductor films include alkaline solutions such as an aqueous solution of potassium hydroxide.
[0040] Alternatively, when a passivation layer and a first conductive type semiconductor layer are laminated on the back surface side of the semiconductor substrate 11 using a CVD method or a PVD method, the passivation layer 23 and the p-type semiconductor layer 25 may be deposited and patterned simultaneously using a mask.
[0041] Next, a passivation layer 33 and a second conductive type semiconductor layer 35 are formed on another part of the back surface side of the semiconductor substrate 11, specifically, on the second region 8 (semiconductor layer formation step). An example of a method for forming the passivation layer 33 and the second conductive type semiconductor layer 35 will be described below, but the method for forming the passivation layer 33 and the second conductive type semiconductor layer 35 is not limited thereto.
[0042] For example, as described above, a passivation film and a second conductive type semiconductor film may be formed on the entire back surface side of semiconductor substrate 11 using a CVD method or a PVD method, and then passivation layer 33 and second conductive type semiconductor layer 35 may be patterned using an etching method that uses a mask or a metal mask generated using a photolithography technique.
[0043] Alternatively, when a passivation layer and a second conductive type semiconductor layer are laminated on the back surface side of the semiconductor substrate 11 using a CVD method or a PVD method, the passivation layer 33 and the second conductive type semiconductor layer 35 may be deposited and patterned simultaneously using a mask.
[0044] In this semiconductor layer forming step, a passivation layer 13 may be formed on the entire light-receiving surface side of semiconductor substrate 11.
[0045] Next, as shown in FIG. 3B, a physically peelable physical release resin pattern 40 is formed in an area on the rear surface of the semiconductor substrate 11 where the first electrode layer 27 and the second electrode layer 37 are not formed, i.e., an area where the first metal electrode layer 29 and the second metal electrode layer 39 are not formed (physical release resin formation process).
[0046] Materials used for the physically releasing resin pattern 40 include acrylic, epoxy, polyimide, silicone, silsesquioxane, and oxetane. This allows the physically releasing resin pattern 40 to be mechanically peeled off, and the physically releasing resin pattern 40 is peeled off from the semiconductor substrate 11 when an external force is applied. The peel strength of the physically releasing resin pattern 40 against the semiconductor substrate 11 is preferably 1 N or less.
[0047] Next, as shown in FIG. 3C, for example, using a CVD method or a PVD method, a transparent electrode layer material film 28Z is formed on the entire back side of the semiconductor substrate 11, i.e., on and spanning the first conductive type semiconductor layer 25, the second conductive type semiconductor layer 35 and the physical peelable resin pattern 40 (transparent electrode layer material film formation process).
[0048] At this time, the optical adjustment layer 15 may be formed on the entire light-receiving surface side of the semiconductor substrate 11.
[0049] Next, as shown in FIG. 3D, a metal electrode layer material film 29Z is formed on the entire back surface side of the semiconductor substrate 11, i.e., on and spanning the first conductive type semiconductor layer 25, the second conductive type semiconductor layer 35 and the physical peel-off resin pattern 40 (metal electrode layer material film formation process).
[0050] For example, the material film 29Z of the metal electrode layer is formed by a reduced pressure spraying method using a particulate metal material. - By discharging plasma or other electrical discharge, the particulate metal material is melted, The molten particles are sprayed onto the target surface by the carrier gas. Depositing molten particles onto the surface of the object; This is a film-forming method in which the molten particles deposited on the surface of the object are instantly cooled to form a metal film.
[0051] As a result, as described above, the first metal electrode layer 29 and the second metal electrode layer 39 have a layer structure in which metal particles are stacked in a continuous manner. Furthermore, in the cross section of the first metal electrode layer 29 and the second metal electrode layer 39 along the back surface, there are gaps at the grain boundaries of the metal particles. Furthermore, in the cross section of the first metal electrode layer 29 and the second metal electrode layer 39 intersecting the back surface, there are gaps at the grain boundaries of the metal particles.
[0052] Furthermore, in a cross section intersecting the rear surface, gaps exist at the boundary between the layer adjacent to the first metal electrode layer 29 (first transparent electrode layer 28 or first conductive type semiconductor layer 25) and the metal particles of the first metal electrode layer 29. Furthermore, in a cross section intersecting the rear surface, gaps exist at the boundary between the layer adjacent to the second metal electrode layer 39 (second transparent electrode layer 38 or second conductive type semiconductor layer 35) and the metal particles of the second metal electrode layer 39.
[0053] 3E, the physically peelable resin pattern 40 is physically peeled off to remove the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z on the physically peelable resin pattern 40. As a result, a first transparent electrode layer 28 and a first metal electrode layer 29 are formed on the first conductive type semiconductor layer 25, specifically in the first region 7, and a second transparent electrode layer 38 and a second metal electrode layer 39 are formed on the second conductive type semiconductor layer 35, specifically in the second region 8 (transparent electrode layer forming step and metal electrode layer forming step).
[0054] Through the above steps, the back electrode type solar cell 1 of the first embodiment shown in FIG. 2 is obtained.
[0055] As described above, according to the manufacturing method for the solar cell of the first embodiment, the first metal electrode layer 29 and the second metal electrode layer 39 are formed by a reduced pressure spraying method using a particulate metal material. As a result, according to the solar cell 1 of the first embodiment, the first metal electrode layer 29 and the second metal electrode layer 39 have a layer structure in which metal particles are accumulated in a continuous manner.
[0056] Therefore, first metal electrode layer 29 and second metal electrode layer 39 have a low Young's modulus and high flexibility. Therefore, according to solar cell 1 of the first embodiment, warping of semiconductor substrate 11 can be reduced, and internal stress of semiconductor substrate 11 can be reduced (suppressed, alleviated).
[0057] Furthermore, according to the manufacturing method of the solar cell of the first embodiment, the first metal electrode layer 29 and the second metal electrode layer 39 have a low Young's modulus and high flexibility, so that a mechanical lift-off method using a physically peelable resin pattern 40 that can be physically peeled off can be used in patterning the first metal electrode layer 29 and the second metal electrode layer 39, thereby simplifying the manufacturing of the solar cell.
[0058] Furthermore, it has been confirmed that the method for forming a metal electrode layer using the reduced pressure spraying method of this embodiment has equivalent adhesion, resistance, and bonding strength to the method for forming a metal electrode layer using a plating method, and furthermore, it is possible to reduce warping of the semiconductor substrate and reduce (suppress, mitigate) internal stress in the semiconductor substrate.
[0059] The adhesion of the metal electrode layer was evaluated by a cross-cut test conforming to the JIS-K5400 standard. The resistance of the metal electrode layer was evaluated by measuring the volume resistivity and surface resistivity conforming to JIS-C2139-3 and JIS K6911. The bonding strength of the metal electrode layer was evaluated by a tweezers peel strength test conforming to JIS-Z3198-8 and JIS-K6855. The warpage of the semiconductor substrate (internal stress of the semiconductor substrate) was evaluated by a test strip test conforming to JIS-H8626 (quality, item 12, electrodeposition stress).
[0060] (Modification of Solar Cell of First Embodiment) Although the first embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various changes and modifications are possible. For example, in the above-mentioned embodiment, a back electrode type solar cell 1 is exemplified (for example, FIG. 2). However, the features of the present invention are not limited to this, and can also be applied to a double-sided electrode type solar cell.
[0061] Fig. 4 is a cross-sectional view of a solar cell according to a modified example of the first embodiment. The solar cell 1 shown in Fig. 4 is a double-sided electrode type heterojunction solar cell. The solar cell 1 shown in Fig. 4 includes a passivation layer 23, a first conductivity type semiconductor layer 25, and a first electrode layer 27, which are formed (deposited, laminated, formed) in this order on the light-receiving surface side of a semiconductor substrate 11. The solar cell 1 also includes a passivation layer 33, a second conductivity type semiconductor layer 35, and a second electrode layer 37, which are formed (deposited, laminated, formed) in this order on the back surface side of the semiconductor substrate 11.
[0062] The passivation layer 23 and the first conductive type semiconductor layer 25 are formed in this order on the entire light-receiving surface side of the semiconductor substrate 11. The passivation layer 33 and the second conductive type semiconductor layer 35 are formed on the entire back surface side of the semiconductor substrate 11.
[0063] The first electrode layer 27 corresponds to the first conductive type semiconductor layer 25, and specifically, is formed on the first conductive type semiconductor layer 25. The first electrode layer 27 may have a first transparent electrode layer 28 and a first metal electrode layer 29 formed in this order on the first conductive type semiconductor layer 25 (FIG. 4), or may have only the first metal electrode layer 29 formed on the first conductive type semiconductor layer 25 (not shown).
[0064] The second electrode layer 37 corresponds to the second conductive type semiconductor layer 35, and specifically, is formed on the second conductive type semiconductor layer 35. The second electrode layer 37 may have a second transparent electrode layer 38 and a second metal electrode layer 39 formed in this order on the second conductive type semiconductor layer 35 (FIG. 4), or may have only the second metal electrode layer 39 formed on the second conductive type semiconductor layer 35 (not shown).
[0065] The first transparent electrode layer 28 is formed on the entire surface of the first conductive type semiconductor layer 25, and the second transparent electrode layer 38 is formed on the entire surface of the second conductive type semiconductor layer 35. Meanwhile, the first metal electrode layer 29 and the second metal electrode layer 39 are in the form of strips extending in the second direction, and are arranged alternately in the first direction. The second metal electrode layer 39 on the back surface side may be formed on the entire surface of the second conductive type semiconductor layer 35.
[0066] As described above, the first metal electrode layer 29 and the second metal electrode layer 39 have a layer structure in which metal particles are stacked in series.
[0067] Also, in a cross section of the first metal electrode layer 29 along the light receiving surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the first metal electrode layer 29 intersecting the light receiving surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the light receiving surface, there are gaps at the boundaries between the layer adjacent to the first metal electrode layer 29, i.e., the first transparent electrode layer 28, and the metal particles of the first metal electrode layer 29 (FIG. 2). Note that, if the first electrode layer 27 does not have the first transparent electrode layer 28, there are gaps at the boundaries between the layer adjacent to the first metal electrode layer 29, i.e., the first conductive type semiconductor layer 25, and the metal particles of the first metal electrode layer 29 in a cross section intersecting the back surface (not shown).
[0068] Also, in a cross section of the second metal electrode layer 39 along the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the second metal electrode layer 39 intersecting the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the back surface, there are gaps at the boundary between the layer adjacent to the second metal electrode layer 39, i.e., the second transparent electrode layer 38, and the metal particles of the second metal electrode layer 39 (FIG. 2). Note that, if the second electrode layer 37 does not have the second transparent electrode layer 38, there are gaps at the boundary between the layer adjacent to the second metal electrode layer 39, i.e., the second conductive type semiconductor layer 35, and the metal particles of the second metal electrode layer 39 in a cross section intersecting the light receiving surface (not shown).
[0069] (Method of manufacturing a solar cell according to a modification of the first embodiment) The above-described solar cell manufacturing method can also be applied to the solar cell 1 shown in Fig. 4. First, in the same manner as described above, for example, a CVD method or a PVD method is used to form a passivation layer 23 and a first conductive type semiconductor layer 25 on the light-receiving surface side of the semiconductor substrate 11, and a passivation layer 33 and a second conductive type semiconductor layer 35 on the back surface side of the semiconductor substrate 11 (semiconductor layer formation step).
[0070] Next, in the same manner as described above, for example, using a CVD method or a PVD method, a first transparent electrode layer 28 is formed on the light-receiving surface side of semiconductor substrate 11, and a second transparent electrode layer 38 is formed on the back surface side of semiconductor substrate 11 (transparent electrode layer formation process).
[0071] Next, as described above, a pattern of physically peelable resin is formed in the area on the light-receiving surface of the semiconductor substrate 11 where the first metal electrode layer 29 is not formed, and in the area on the back surface of the semiconductor substrate 11 where the second metal electrode layer 39 is not formed (physical peeling resin formation process).
[0072] Next, in the same manner as described above, a material film for a metal electrode layer is formed over the entire light-receiving surface side of the semiconductor substrate 11, i.e., on and across the first conductive type semiconductor layer 25 and the physically peelable resin pattern (metal electrode layer material film forming process). Also, a material film for a metal electrode layer is formed over the entire back surface side of the semiconductor substrate 11, i.e., on and across the second conductive type semiconductor layer 35 and the physically peelable resin pattern 40 (metal electrode layer material film forming process).
[0073] Next, in the same manner as described above, the physically peelable resin pattern is physically peeled off to remove the metal electrode layer material film on the physically peelable resin pattern, thereby forming a first metal electrode layer 29 on the light-receiving surface side of the semiconductor substrate 11, and a second metal electrode layer 39 on the back surface side of the semiconductor substrate 11 (metal electrode layer forming process).
[0074] Through the above steps, a double-sided electrode type solar cell 1 according to a modification of the first embodiment shown in FIG. 4 is obtained.
[0075] (Solar Cell of Second Embodiment) In the first embodiment, a solar cell 1 having metal electrode layers 29, 39 formed by a reduced pressure spraying method is exemplified. In the second embodiment, a solar cell having a metal electrode layer having a laminated structure of a base layer and a plating layer formed by a reduced pressure spraying method is exemplified.
[0076] Fig. 5 is a cross-sectional view of a solar cell according to a second embodiment, taken along line II-II in Fig. 1. The solar cell 1 of the second embodiment shown in Fig. 5 differs from the solar cell 1 of the first embodiment shown in Fig. 1 in the configuration of metal electrode layers 29, 39. Other configurations of the solar cell 1 of the second embodiment are similar to the configuration of the solar cell 1 of the first embodiment.
[0077] The first metal electrode layer 29 has a first underlayer 29l and a first plating layer 29u, and the second metal electrode layer 39 has a second underlayer 39l and a second plating layer 39u.
[0078] The first underlayer 29l and the second underlayer 39l are formed by a reduced pressure spraying method using particulate metal materials such as silver, copper, and aluminum, as described later. As a result, similar to the examples of Figs. 12A and 12B described above, the first underlayer 29l and the second underlayer 39l have a layer structure in which metal particles are stacked in a continuous manner. When viewed from the back side, the size (particle diameter) of the metal particles in the first underlayer 29l is 0.9 μm or more and 500 μm or less, preferably 0.9 μm or more and 13 μm or less, and when viewed from the back side, the size (particle diameter) of the metal particles in the second underlayer 39l is 0.9 μm or more and 500 μm or less, preferably 0.9 μm or more and 13 μm or less.
[0079] Also, in a cross section of the first underlayer 29l along the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the first underlayer 29l intersecting the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the back surface, there are gaps at the boundaries between the layer adjacent to the first underlayer 29l, i.e., the first transparent electrode layer 28, and the metal particles of the first underlayer 29l (FIG. 2). Note that, if the first electrode layer 27 does not have the first transparent electrode layer 28, there are gaps at the boundaries between the layer adjacent to the first underlayer 29l, i.e., the first conductive type semiconductor layer 25, and the metal particles of the first underlayer 29l in the cross section intersecting the back surface (not shown).
[0080] In addition, in a cross section of the second underlayer 39l along the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section of the second underlayer 39l intersecting the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section intersecting the back surface, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second transparent electrode layer 38, and the metal particles of the second underlayer 39l (FIG. 2). Note that, if the second electrode layer 37 does not have the second transparent electrode layer 38, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second conductive type semiconductor layer 35, and the metal particles of the second underlayer 39l in a cross section intersecting the light receiving surface (not shown).
[0081] As described below, the first plating layer 29u and the second plating layer 39u are formed by a plating method (electrolytic plating method or electroless plating method) using a metal material such as silver, copper, aluminum, etc. As a result, a part of the first plating layer 29u is embedded in gaps between grain boundaries of some of the metal particles on the first plating layer 29u side of the first foundation layer 29l, and a part of the second plating layer 39u is embedded in gaps between grain boundaries of some of the metal particles on the second plating layer 39u side of the second foundation layer 39l.
[0082] (Solar Cell Manufacturing Method) Next, a method for manufacturing a solar cell according to this embodiment will be described with reference to Figs. 6A to 6F. Fig. 6A is a diagram showing a semiconductor layer forming step in the method for manufacturing a solar cell according to this embodiment, and Fig. 6B is a diagram showing a physical peeling resin forming step in the method for manufacturing a solar cell according to this embodiment. Fig. 6C is a diagram showing a transparent electrode layer material film forming step in the method for manufacturing a solar cell according to this embodiment, and Fig. 6D is a diagram showing an underlayer material film forming step for a metal electrode layer in the method for manufacturing a solar cell according to this embodiment. Fig. 6E is a diagram showing an underlayer forming step for a transparent electrode layer and a metal electrode layer in the method for manufacturing a solar cell according to this embodiment, and Fig. 6F is a diagram showing a plating layer forming step for a metal electrode layer in the method for manufacturing a solar cell according to this embodiment.
[0083] First, as in the above, as shown in FIG. 6A, a passivation layer 23 and a first conductivity type semiconductor layer 25 are formed on a part of the back surface side of the semiconductor substrate 11, specifically, on the first region 7 (semiconductor layer formation step).
[0084] Next, in the same manner as described above, a passivation layer 33 and a second conductive type semiconductor layer 35 are formed on another part of the back surface side of the semiconductor substrate 11, specifically, on the second region 8 (semiconductor layer forming step).
[0085] In this semiconductor layer forming step, a passivation layer 13 may be formed on the entire light-receiving surface side of semiconductor substrate 11.
[0086] Next, similarly to the above, as shown in FIG. 6B, a physically peelable physical release resin pattern 40 is formed in an area on the rear surface of the semiconductor substrate 11 where the first electrode layer 27 and the second electrode layer 37 are not formed, i.e., an area where the first metal electrode layer 29 and the second metal electrode layer 39 are not formed (physical release resin formation process).
[0087] Next, similarly to the above, as shown in FIG. 6C, a transparent electrode layer material film 28Z is formed over the entire back side of the semiconductor substrate 11, i.e., over and across the first conductive type semiconductor layer 25, the second conductive type semiconductor layer 35 and the physical peelable resin pattern 40, using, for example, a CVD method or a PVD method (transparent electrode layer material film formation process).
[0088] At this time, the optical adjustment layer 15 may be formed on the entire light-receiving surface side of the semiconductor substrate 11.
[0089] Next, similarly to the above, as shown in FIG. 6D, a material film 29lZ of an underlayer for a metal electrode layer is formed on the entire back surface side of the semiconductor substrate 11, i.e., on and across the first conductive type semiconductor layer 25, the second conductive type semiconductor layer 35 and the physical peel-off resin pattern 40 (underlayer material film formation process for a metal electrode layer).
[0090] For example, the material film 291Z of the underlayer is formed by a reduced pressure thermal spraying method using a particulate metal material. - By discharging plasma or other electrical discharge, the particulate metal material is melted, The molten particles are sprayed onto the target surface by the carrier gas. Depositing molten particles onto the surface of the object; This is a film-forming method in which the molten particles deposited on the surface of the object are instantly cooled to form a metal film.
[0091] As a result, as described above, the first underlayer 29l and the second underlayer 39l have a layer structure in which metal particles are stacked in a continuous manner. Also, in the cross section of the first underlayer 29l and the second underlayer 39l along the back surface, there are gaps at the grain boundaries of the metal particles. Also, in the cross section of the first underlayer 29l and the second underlayer 39l intersecting the back surface, there are gaps at the grain boundaries of the metal particles.
[0092] In addition, in a cross section intersecting the rear surface, there are gaps at the boundary between the layer adjacent to the first underlayer 29l (first transparent electrode layer 28 or first conductive type semiconductor layer 25) and the metal particles of the first underlayer 29l. In addition, in a cross section intersecting the rear surface, there are gaps at the boundary between the layer adjacent to the second underlayer 39l (second transparent electrode layer 38 or second conductive type semiconductor layer 35) and the metal particles of the second underlayer 39l.
[0093] 6E, the physically peelable resin pattern 40 is physically peeled off to remove the transparent electrode layer material film 28Z and the underlayer material film 29lZ of the metal electrode layer on the physically peelable resin pattern 40. As a result, the first transparent electrode layer 28 and the first underlayer 29l of the first metal electrode layer are formed on the first conductive type semiconductor layer 25, specifically in the first region 7, and the second transparent electrode layer 38 and the second underlayer 39l of the second metal electrode layer are formed on the second conductive type semiconductor layer 35, specifically in the second region 8 (transparent electrode layer forming step and underlayer forming step of the metal electrode layer).
[0094] Next, as shown in FIG. 6F, a plating method is used to form a first plating layer 29u of the first metal electrode layer on the first base layer 29l, specifically in the first region 7, and a second plating layer 39u of the second metal electrode layer is formed on the second base layer 39l, specifically in the second region 8 (plating layer formation process of metal electrode layer).
[0095] Through the above steps, a back electrode type solar cell 1 according to the second embodiment shown in FIG. 5 is obtained.
[0096] As described above, according to the method for manufacturing the solar cell of the second embodiment, the first underlayer 29l of the first metal electrode layer 29 and the second underlayer 39l of the second metal electrode layer 39 are formed by a reduced pressure spraying method using a particulate metal material. As a result, according to the solar cell 1 of the second embodiment, the first underlayer 29l of the first metal electrode layer 29 and the second underlayer 39l of the second metal electrode layer 39 have a layer structure in which metal particles are deposited in a continuous manner.
[0097] Therefore, the first and second base layers 29l and 39l have a low Young's modulus and high flexibility, and therefore, according to the solar cell 1 of the second embodiment, it is possible to reduce warping of the semiconductor substrate 11 and reduce (suppress, alleviate) the internal stress of the semiconductor substrate 11.
[0098] Furthermore, according to the second embodiment of the solar cell manufacturing method, the first base layer 29l and the second base layer 39l have a low Young's modulus and high flexibility, so that a mechanical lift-off method using a physically peelable resin pattern 40 that can be physically peeled off can be used in patterning the first base layer 29l and the second base layer 39l, thereby simplifying the manufacture of the solar cell.
[0099] Furthermore, it has been confirmed that the method for forming the underlayer of the metal electrode layer using the reduced pressure spraying method of this embodiment has equivalent adhesion, resistance, and bonding strength of the metal electrode layer compared to the method for forming the metal electrode layer using a plating method, and furthermore, it is possible to reduce warping of the semiconductor substrate and reduce (suppress, mitigate) the internal stress of the semiconductor substrate.
[0100] The adhesion of the metal electrode layer was evaluated by a cross-cut test conforming to the JIS-K5400 standard. The resistance of the metal electrode layer was evaluated by measuring the volume resistivity and surface resistivity conforming to JIS-C2139-3 and JIS K6911. The bonding strength of the metal electrode layer was evaluated by a tweezers peel strength test conforming to JIS-Z3198-8 and JIS-K6855. The warpage of the semiconductor substrate (internal stress of the semiconductor substrate) was evaluated by a test strip test conforming to JIS-H8626 (quality, item 12, electrodeposition stress).
[0101] Moreover, according to the manufacturing method of the solar cell of the second embodiment, the first plating layer 29u of the first metal electrode layer 29 and the second plating layer 39u of the second metal electrode layer 39 are formed by plating. As a result, according to the solar cell 1 of the second embodiment, the first metal electrode layer 29 has the first plating layer 29u, and the second metal electrode layer 39 has the second plating layer 39u. Therefore, the resistance of the first metal electrode layer 29 and the second metal electrode layer 39 can be reduced. In addition, the smoothness (surface roughness) of the surfaces of the first metal electrode layer 29 and the second metal electrode layer 39 can be increased, and the solder bondability can be improved.
[0102] (Modification of the second embodiment) Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various changes and modifications are possible. For example, in the above-mentioned embodiment, a back electrode type solar cell 1 is illustrated (for example, FIG. 5). However, the features of the present invention are not limited to this, and can also be applied to a double-sided electrode type solar cell.
[0103] Fig. 7 is a cross-sectional view of a solar cell according to a modified example of the second embodiment. The solar cell 1 shown in Fig. 7 is a double-sided electrode type heterojunction solar cell. The solar cell 1 shown in Fig. 7 includes a passivation layer 23, a first conductivity type semiconductor layer 25, and a first electrode layer 27, which are formed (deposited, laminated, formed) in this order on the light-receiving surface side of a semiconductor substrate 11. The solar cell 1 also includes a passivation layer 33, a second conductivity type semiconductor layer 35, and a second electrode layer 37, which are formed (deposited, laminated, formed) in this order on the back surface side of the semiconductor substrate 11.
[0104] The passivation layer 23 and the first conductive type semiconductor layer 25 are formed in this order on the entire light-receiving surface side of the semiconductor substrate 11. The passivation layer 33 and the second conductive type semiconductor layer 35 are formed on the entire back surface side of the semiconductor substrate 11.
[0105] The first electrode layer 27 corresponds to the first conductive type semiconductor layer 25, and specifically, is formed on the first conductive type semiconductor layer 25. The first electrode layer 27 may have a first transparent electrode layer 28 and a first metal electrode layer 29 formed in this order on the first conductive type semiconductor layer 25 (FIG. 7), or may have only the first metal electrode layer 29 formed on the first conductive type semiconductor layer 25 (not shown).
[0106] The second electrode layer 37 corresponds to the second conductive type semiconductor layer 35, and specifically, is formed on the second conductive type semiconductor layer 35. The second electrode layer 37 may have a second transparent electrode layer 38 and a second metal electrode layer 39 formed in this order on the second conductive type semiconductor layer 35 (FIG. 7), or may have only the second metal electrode layer 39 formed on the second conductive type semiconductor layer 35 (not shown).
[0107] The first transparent electrode layer 28 is formed on the entire surface of the first conductive type semiconductor layer 25, and the second transparent electrode layer 38 is formed on the entire surface of the second conductive type semiconductor layer 35. Meanwhile, the first metal electrode layer 29 and the second metal electrode layer 39 are in the form of strips extending in the second direction, and are arranged alternately in the first direction. The first metal electrode layer 29 has a first base layer 29l and a first plating layer 29u, and the second metal electrode layer 39 has a second base layer 39l and a second plating layer 39u. The second metal electrode layer 39 on the back side may be formed on the entire surface of the second conductive type semiconductor layer 35.
[0108] As described above, the first underlayer 29l and the second underlayer 39l have a layer structure in which metal particles are deposited in series.
[0109] Also, in a cross section of the first underlayer 29l along the light receiving surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the first underlayer 29l intersecting the light receiving surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the light receiving surface, there are gaps at the boundary between the layer adjacent to the first underlayer 29l, i.e., the first transparent electrode layer 28, and the metal particles of the first underlayer 29l (FIG. 2). Note that, if the first electrode layer 27 does not have the first transparent electrode layer 28, there are gaps at the boundary between the layer adjacent to the first underlayer 29l, i.e., the first conductive type semiconductor layer 25, and the metal particles of the first underlayer 29l in a cross section intersecting the back surface (not shown).
[0110] In addition, in a cross section of the second underlayer 39l along the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section of the second underlayer 39l intersecting the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section intersecting the back surface, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second transparent electrode layer 38, and the metal particles of the second underlayer 39l (FIG. 2). Note that, if the second electrode layer 37 does not have the second transparent electrode layer 38, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second conductive type semiconductor layer 35, and the metal particles of the second underlayer 39l in a cross section intersecting the light receiving surface (not shown).
[0111] (Modification of the second embodiment of the solar cell manufacturing method) The above-described solar cell manufacturing method can also be applied to the solar cell 1 shown in Fig. 7. First, in the same manner as described above, for example, a CVD method or a PVD method is used to form a passivation layer 23 and a first conductive type semiconductor layer 25 on the light-receiving surface side of the semiconductor substrate 11, and a passivation layer 33 and a second conductive type semiconductor layer 35 on the back surface side of the semiconductor substrate 11 (semiconductor layer formation step).
[0112] Next, in the same manner as described above, for example, using a CVD method or a PVD method, a first transparent electrode layer 28 is formed on the light-receiving surface side of semiconductor substrate 11, and a second transparent electrode layer 38 is formed on the back surface side of semiconductor substrate 11 (transparent electrode layer formation process).
[0113] Next, as described above, a pattern of physically peelable resin is formed in the area on the light-receiving surface of the semiconductor substrate 11 where the first metal electrode layer 29 is not formed, and in the area on the back surface of the semiconductor substrate 11 where the second metal electrode layer 39 is not formed (physical peeling resin formation process).
[0114] Next, in the same manner as described above, a material film for the underlayer of the metal electrode layer is formed over the entire light-receiving surface side of the semiconductor substrate 11, i.e., on and across the first conductive type semiconductor layer 25 and the physically peelable resin pattern (underlayer material film forming process for metal electrode layer). Also, a material film for the underlayer of the metal electrode layer is formed over the entire back surface side of the semiconductor substrate 11, i.e., on and across the second conductive type semiconductor layer 35 and the physically peelable resin pattern 40 (underlayer material film forming process for metal electrode layer).
[0115] Next, in the same manner as described above, the physical release resin pattern is physically peeled off to remove the underlayer material film of the metal electrode layer on the physical release resin pattern, thereby forming an underlayer 29l of the first metal electrode layer 29 on the light-receiving surface side of the semiconductor substrate 11, and forming an underlayer of the second metal electrode layer 39 on the back surface side of the semiconductor substrate 11 (underlayer formation process for the metal electrode layer).
[0116] Next, similarly to the above, a plating method is used to form the first plating layer 29u of the first metal electrode layer 29 on the first base layer 29l, and the second plating layer 39u of the second metal electrode layer 39 on the second base layer 39l (plating layer formation process of the metal electrode layer).
[0117] Through the above steps, a double-sided electrode type solar cell 1 according to a modification of the second embodiment shown in FIG. 7 is obtained.
[0118] (Circuit board according to the third embodiment) Fig. 8 is a schematic diagram showing a side view of a circuit board according to a third embodiment. As shown in Fig. 8, the circuit board 100 includes a dielectric layer 110 and metal wiring 120 disposed on the dielectric layer 110.
[0119] The dielectric layer 110 is made of an insulating dielectric material, such as glass, silicone, epoxy, polyimide, polyethylene naphthalate, or polyethylene terephthalate.
[0120] Metal traces 120 are disposed on the dielectric layer 110 and are patterned into a desired pattern.
[0121] The metal wiring 120 is formed by a reduced pressure spraying method using a particulate metal material such as copper, aluminum, nickel, silver, tin, etc., as described below. As a result, similar to the examples of Figures 12A and 12B described above, the metal wiring 120 has a layer structure in which metal particles are stacked in a continuous manner. When viewed from the main surface side of the dielectric layer 110, the size (particle diameter) of the metal particles in the metal wiring 120 is 0.9 μm or more and 500 μm or less, and preferably 0.9 μm or more and 13 μm or less.
[0122] Furthermore, in a cross section of the metal wiring 120 along the main surface of the dielectric layer 110, there are gaps at the grain boundaries of the metal particles. Furthermore, in a cross section of the metal wiring 120 intersecting the main surface of the dielectric layer 110, there are gaps at the grain boundaries of the metal particles. Furthermore, in a cross section of the metal wiring 120 intersecting the main surface of the dielectric layer 110, there are gaps at the boundaries between the dielectric layer 110 and the metal particles of the metal wiring 120.
[0123] (Method for manufacturing the circuit board according to the third embodiment) Next, a method for manufacturing a circuit board according to the third embodiment will be described with reference to Figures 9A to 9C. Figure 9A is a diagram showing a physically peelable resin forming step in the method for manufacturing a circuit board according to the third embodiment, and Figure 9B is a diagram showing a metal wiring material film forming step in the method for manufacturing a circuit board according to the third embodiment. Figure 9C is a diagram showing a metal wiring forming step in the method for manufacturing a circuit board according to the third embodiment.
[0124] First, as shown in FIG. 9A, a physically peelable resin pattern 40 is formed on the main surface of the dielectric layer 110 in an area where the metal wiring 120 is not formed (physical peeling resin forming step).
[0125] Next, as shown in FIG. 9B, a metal wiring material film 120Z is formed over the entire main surface of the dielectric layer 110, that is, on and across the dielectric layer 110 and the physically peelable resin pattern 40 (metal wiring material film forming step). For example, the metal wiring material film 120Z is formed by using a reduced pressure spraying method using a particulate metal material. The reduced pressure spraying method is a method in which, under a reduced pressure environment, - By discharging plasma or other electrical discharge, the particulate metal material is melted, The molten particles are sprayed onto the target surface by the carrier gas. Depositing molten particles onto the surface of the object; This is a film-forming method in which the molten particles deposited on the surface of the object are instantly cooled to form a metal film.
[0126] As a result, as described above, the metal wiring 120 has a layer structure in which metal particles are deposited in a continuous manner. Furthermore, in a cross section of the metal wiring 120 along the main surface of the dielectric layer 110, gaps exist at the grain boundaries of the metal particles. Furthermore, in a cross section of the metal wiring 120 intersecting with the main surface of the dielectric layer 110, gaps exist at the grain boundaries of the metal particles. Furthermore, in a cross section intersecting with the main surface of the dielectric layer 110, gaps exist at the boundaries between the dielectric layer 110 and the metal particles of the metal wiring 20.
[0127] Next, as shown in FIG. 9C, the physically release resin pattern 40 is physically peeled off to remove the material film 120Z of the metal wiring on the physically release resin pattern 40, thereby forming the metal wiring 120 (metal wiring formation step).
[0128] Through the above steps, the circuit board 100 of the third embodiment shown in FIG. 8 is obtained.
[0129] As described above, according to the method for manufacturing a circuit board of the third embodiment, the metal wiring 120 is formed by using a reduced pressure spraying method using a particulate metal material. As a result, according to the circuit board 100 of the third embodiment, the metal wiring 120 has a layer structure in which metal particles are continuously deposited.
[0130] Therefore, the metal wiring 120 has a low Young's modulus and is highly flexible, and therefore, according to the circuit board 100 of the third embodiment, warping can be reduced.
[0131] Furthermore, according to the method for manufacturing a circuit board of the third embodiment, since the metal wiring 120 has a low Young's modulus and high flexibility, a mechanical lift-off method using a physically peelable resin pattern 40 that can be physically peeled off can be used in patterning the metal wiring 120, thereby simplifying the manufacture of the circuit board.
[0132] (Circuit board according to the fourth embodiment) In the third embodiment, a circuit board 100 including metal wiring 120 formed by a reduced pressure spraying method is exemplified. In the fourth embodiment, a solar cell including metal wiring having a laminated structure of a base layer and a plating layer formed by a reduced pressure spraying method is exemplified.
[0133] Fig. 10 is a schematic diagram showing a side surface of a circuit board according to a fourth embodiment. The circuit board 100 of the fourth embodiment shown in Fig. 10 is different from the circuit board 100 of the third embodiment shown in Fig. 8 in the configuration of the metal wiring 120. The other configurations of the circuit board 100 of the fourth embodiment are similar to the configurations of the circuit board 100 of the third embodiment.
[0134] The metal wiring 120 has a laminated structure of a base layer 121 and a plating layer 122 arranged in this order on the dielectric layer 110 .
[0135] As described below, the underlayer 121 is formed by a reduced pressure spraying method using a particulate metal material such as copper, aluminum, nickel, silver, tin, etc. As a result, similar to the examples of Figures 12A and 12B described above, the underlayer 121 has a layer structure in which metal particles are deposited in a continuous manner. When viewed from the main surface side of the dielectric layer 110, the size (particle diameter) of the metal particles in the underlayer 121 is 0.9 μm or more and 500 μm or less, and preferably 0.9 μm or more and 13 μm or less.
[0136] Furthermore, in a cross section of the underlayer 121 along the main surface of the dielectric layer 110, there are gaps at the grain boundaries of the metal particles. Furthermore, in a cross section of the underlayer 121 intersecting the main surface of the dielectric layer 110, there are gaps at the grain boundaries of the metal particles. Furthermore, in a cross section of the underlayer 121 intersecting the main surface of the dielectric layer 110, there are gaps at the boundaries between the dielectric layer 110 and the metal particles of the underlayer 21.
[0137] As described below, the plating layer 122 is formed by a plating method (electrolytic plating method or electroless plating method) using a metal material such as copper, aluminum, nickel, silver, tin, etc. As a result, part of the plating layer 122 is embedded in gaps between grain boundaries of some of the metal particles in the underlayer 121 on the plating layer 122 side.
[0138] (Method of manufacturing the circuit board according to the fourth embodiment) Next, a method for manufacturing a circuit board according to the fourth embodiment will be described with reference to Fig. 11A to Fig. 11D. Fig. 11A is a diagram showing a physically peelable resin forming step in the method for manufacturing a circuit board according to the fourth embodiment, and Fig. 11B is a diagram showing a base layer material film forming step for metal wiring in the method for manufacturing a circuit board according to the fourth embodiment. Fig. 11C is a diagram showing a base layer forming step for metal wiring in the method for manufacturing a circuit board according to the fourth embodiment, and Fig. 11D is a diagram showing a plating layer forming step for metal wiring in the method for manufacturing a circuit board according to the fourth embodiment.
[0139] First, as in the above, as shown in FIG. 11A, a physically peelable physically release resin pattern 40 is formed in an area of the main surface of the dielectric layer 110 where the metal wiring 120 is not formed (physical release resin forming step).
[0140] 11B, a material film 121Z for an underlayer of metal wiring is formed over the entire main surface of the dielectric layer 110, that is, on and across the dielectric layer 110 and the physically peelable resin pattern 40 (underlayer material film forming process for metal wiring). For example, the material film 121Z for an underlayer of metal wiring is formed by using a reduced pressure spraying method using a particulate metal material.
[0141] As a result, as described above, the underlayer 121 of the metal wiring 120 has a layer structure in which metal particles are deposited in a continuous manner. Furthermore, in a cross section of the underlayer 121 along the main surface of the dielectric layer 110, gaps exist at the grain boundaries of the metal particles. Furthermore, in a cross section of the underlayer 121 intersecting with the main surface of the dielectric layer 110, gaps exist at the grain boundaries of the metal particles. Furthermore, in a cross section intersecting with the main surface of the dielectric layer 110, gaps exist at the boundaries between the dielectric layer 110 and the metal particles of the underlayer 121.
[0142] Next, as described above, as shown in FIG. 11C, the physically peelable resin pattern 40 is physically peeled off to remove the material film 121Z of the base layer of the metal wiring on the physically peelable resin pattern 40, thereby forming the base layer 121 of the metal wiring (base layer formation process for the metal wiring).
[0143] 11D, a plating method (electrolytic plating method or electroless plating method) is used to form a plating layer 122 on the underlayer 121 (metal wiring plating layer forming step). As a result, part of the plating layer 122 is filled into gaps between grain boundaries of some of the metal particles in the underlayer 121 on the plating layer 122 side.
[0144] Through the above steps, the circuit board 100 of the fourth embodiment shown in FIG. 10 is obtained.
[0145] As described above, according to the manufacturing method for the circuit board of the fourth embodiment, the underlayer 121 of the metal wiring 120 is formed by a reduced pressure spraying method using a particulate metal material. As a result, according to the circuit board 100 of the fourth embodiment, the underlayer 121 of the metal wiring 120 has a layer structure in which metal particles are continuously deposited.
[0146] Therefore, the underlayer 121 of the metal wiring 120 has a low Young's modulus and is highly flexible, and therefore, according to the circuit board 100 of the fourth embodiment, warping can be reduced.
[0147] Furthermore, according to the method for manufacturing a circuit board of the fourth embodiment, the underlayer 121 of the metal wiring 120 has a low Young's modulus and high flexibility, so that in patterning the underlayer 121 of the metal wiring 120, a mechanical lift-off method using a physically peelable resin pattern 40 can be used, simplifying the manufacture of the circuit board.
[0148] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various changes and modifications are possible. [Explanation of symbols]
[0149] 1. Solar Cell 7 First area 8 Second area 7b, 8b Busbar section 7f,8f Finger section 11 Semiconductor substrate 13,23,33 Passivation layer 25 First conductive type semiconductor layer 27 1st electrode layer 28 First transparent electrode layer 28Z Transparent electrode layer material film 29 First metal electrode layer 29l 1st base layer 29lZ Underlayer material film 29u 1st plating layer 35 Second conductive type semiconductor layer 37 Second electrode layer 38 Second transparent electrode layer 39 Second metal electrode layer 39l 2nd base layer 39u Second plating layer 40 Physical peeling resin 100 Circuit Board 110 Dielectric layer 120 Metal wiring 120Z Metal Wiring Material Film 121 Base layer 121Z Undercoat layer material film 122 Plating layer
Claims
1. A method for manufacturing a solar cell comprising: a semiconductor substrate; a conductive semiconductor layer disposed on a main surface of the semiconductor substrate; and a metal electrode layer corresponding to the conductive semiconductor layer, the method comprising the steps of: a semiconductor layer forming step of forming the conductive semiconductor layer on a main surface of the semiconductor substrate; a physical release resin forming step of forming a pattern of a physically peelable physical release resin in an area of the main surface of the semiconductor substrate where the metal electrode layer is not formed; a metal electrode layer material film forming process in which metal particles are melted by discharge under a reduced pressure environment using a reduced pressure spraying method, the melted metal particles are sprayed onto the semiconductor substrate by a carrier gas, and the metal particles are deposited on the conductive semiconductor layer and the physical release resin of the semiconductor substrate, thereby forming a material film for the metal electrode layer; a metal electrode layer forming step of removing a material film of the metal electrode layer on the physical release resin by peeling off the physical release resin, thereby forming the metal electrode layer having a layer structure in which metal particles are continuously deposited; A method for manufacturing a solar cell, comprising:
2. The metal electrode layer has a laminated structure of a base layer and a plating layer, In the metal electrode layer material film forming step, a material film of the underlayer is formed as a material film of the metal electrode layer, In the metal electrode layer forming step, removing the material film of the underlayer on the physical release resin to form the underlayer having a layer structure in which metal particles are continuously deposited; forming a metal plating layer on the underlayer by a plating method to form the metal electrode layer; The method for producing the solar cell according to claim 1 .
3. A method for manufacturing a circuit board having a dielectric layer and metal wiring, comprising the steps of: a physical release resin forming step of forming a pattern of a physically peelable physical release resin in an area of the dielectric layer where the metal wiring is not formed; a metal wiring material film forming process in which metal particles are melted by discharge under a reduced pressure environment using a reduced pressure spraying method, the melted metal particles are sprayed onto the dielectric layer by a carrier gas, and the metal particles are deposited on the dielectric layer and the physical release resin, thereby forming a material film for the metal wiring; a metal wiring forming step of removing a material film of the metal wiring on the physical release resin by peeling off the physical release resin, thereby forming the metal wiring having a layer structure in which metal particles are continuously deposited; A method for manufacturing a circuit board, comprising:
4. The metal wiring has a laminated structure of a base layer and a plating layer, In the metal wiring material film forming step, a material film of the underlayer is formed as a material film of the metal wiring, In the metal wiring forming step, removing the material film of the underlayer on the physical release resin to form the underlayer having a layer structure in which metal particles are continuously deposited; forming a metal plating layer on the underlayer by a plating method to form the metal wiring; The method for manufacturing the circuit board according to claim 3 .
Citation Information
Patent Citations
Solar cell
JP2018152620A
Method for manufacturing solar cell and solar cell
JP2019121627A