Manufacturing method of chip

By forming a crack inducing layer on the wafer surface and aligning internal cracks with the film cracks, the method addresses the issue of film peeling during chip manufacturing, ensuring stable film attachment during wafer division.

JP2024135678APending Publication Date: 2024-10-04DISCO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023046480
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

The formation of cracks in semiconductor wafers during chip manufacturing can cause films with low crystallinity, such as oxide or nitride films, to peel off obliquely from the wafer surface, leading to potential film detachment issues.

Method used

A chip manufacturing method that involves forming a crack inducing layer on the wafer surface using a focused laser beam, followed by altering a linear region inside the wafer to create aligned cracks, ensuring the film cracks in the same direction as the internal cracks, thereby reducing the likelihood of diagonal cracking and film peeling.

Benefits of technology

The method effectively aligns the direction of film cracks with internal wafer cracks, minimizing the risk of film detachment from the wafer during the division process, resulting in stable chip production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135678000001_ABST
    Figure 2024135678000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a chip, capable of suppressing a possibility of peeling a film from a wafer when manufacturing a chip by dividing the wafer in which the film is provided onto a front surface.SOLUTION: A manufacturing method of a chip, includes: a crack induction layer formation step of modifying a linear first region of a wafer containing a front surface by irradiation with a laser beam, and forming a crack induction layer in the first region; a crack formation step of forming a modification layer in a linear second region by modifying the second region in an inner part of the wafer separated from the front surface from the crack induction layer by irradiation with the laser beam, and forming a first crack extended from the modification layer toward the crack induction layer and a second crack extended toward the inner part of a film; and a division step of obtaining a plurality of chips by applying an external force to the wafer, and dividing the wafer along the division schedule line with the film.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a chip. [Background technology]

[0002] A semiconductor chip equipped with a semiconductor device is manufactured, for example, by forming a plurality of semiconductor devices on the surface of a wafer made of crystalline silicon or the like, and dividing the wafer into individual semiconductor devices along planned dividing lines. An example of a manufacturing method for such a semiconductor chip is described in Patent Document 1.

[0003] In the method described in Patent Document 1, a laser beam having a wavelength that transmits the wafer is irradiated along the planned dividing line so as to be focused inside the wafer, thereby forming a modified layer (degraded layer) along the planned dividing line and cracks extending from the modified layer inside the wafer. After the modified layer and cracks are formed, an external force is applied to the wafer, so that the wafer is divided along the planned dividing line. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-192370 A Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, the surface of a wafer that becomes a semiconductor chip may be provided with a film, such as an oxide film or a nitride film, that has low crystallinity and that constitutes a semiconductor device. When a modified layer is formed by a laser beam inside a wafer that has such a film on its surface, it is possible to extend cracks from the modified layer along the atomic arrangement direction inside a wafer with high crystallinity.

[0006] On the other hand, it is difficult to make cracks extend in a specific direction inside films with low crystallinity such as oxide films or nitride films, as in the case of wafers. Therefore, the directions of crack extension do not necessarily match between the wafer and the film provided on its surface, and the film may crack obliquely with respect to the wafer surface and peel off from the wafer.

[0007] Therefore, an object of the present invention is to provide a chip manufacturing method that can reduce the possibility of a film peeling off from a wafer when dividing a wafer having a film on its surface to manufacture chips. [Means for solving the problem]

[0008] According to one aspect of the present invention, there is provided a method for manufacturing chips by dividing a wafer having a film on its surface along a planned dividing line to produce a plurality of chips, the method including the steps of: forming a crack inducing layer in a crack inducing layer forming step of forming a crack inducing layer in a linear first region of the wafer including the surface by irradiating a laser beam having a wavelength that transmits through one or both of the wafer and the film along the planned dividing line while converging the laser beam; and forming a crack inducing layer in the first region after the crack inducing layer forming step of forming a crack inducing layer in the linear first region of the wafer including the surface by irradiating the laser beam having a wavelength that transmits through the wafer along the planned dividing line while converging the laser beam. The present invention provides a method for manufacturing chips, the method including: a crack formation step of irradiating a line to alter a linear second region inside the wafer that is farther from the surface than the crack induction layer, thereby forming an altered layer in the second region and forming a first crack extending from the altered layer toward the crack induction layer and a second crack extending toward the inside of the film; and a division step of applying an external force to the wafer after the crack formation step to divide the wafer together with the film along the planned division line to obtain a plurality of the chips.

[0009] Preferably, in the crack induction layer formation step, each of the two linear first regions spaced apart in the width direction of the planned division line is altered to form two crack induction layers, and in the crack formation step, the linear second region inside the wafer farther from the surface than the two crack induction layers is altered to form an altered layer in the second region, and the first crack extends from the altered layer toward the two crack induction layers and reaches the region between the two crack induction layers, and the second crack extends toward the inside of the film.

[0010] Preferably, in the crack inducing layer forming step, a laser beam having a wavelength that is transmitted through the film and absorbed by the wafer is irradiated onto the intended dividing line from the film side while being focused. Effect of the Invention

[0011] A chip manufacturing method according to one aspect of the present invention includes a crack-inducing layer formation step in which a linear first region of a wafer, including its surface, is altered along a planned division line to form a crack-inducing layer in the first region.When an altered layer is formed inside the wafer in the crack formation step following the crack-inducing layer formation step, a first crack is formed extending from the altered layer toward the crack-inducing layer.

[0012] The first crack acts on the film provided on the surface of the wafer through the crack induction layer, and the second crack extends in the direction in which the first crack extends. In other words, the first crack formed inside the wafer and the second crack formed in the film provided on the surface of the wafer extend in roughly the same direction, making it difficult for the film to crack diagonally, and therefore reducing the possibility of the film peeling off from the wafer due to the film cracking diagonally. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a perspective view diagrammatically illustrating a wafer according to the first embodiment. [Diagram 2]FIG. 2 is a top view diagrammatically illustrating the wafer according to the first embodiment. [Diagram 3] FIG. 3 is a cross-sectional view illustrating a schematic view of the wafer according to the first embodiment. [Figure 4] FIG. 4 is a top view diagrammatically showing a chip obtained by the chip manufacturing method according to the first embodiment. [Diagram 5] FIG. 5 is a flow diagram showing a method for manufacturing a chip according to the first embodiment. [Figure 6] FIG. 6 is a diagram showing a schematic diagram of a laser irradiation device used in the chip manufacturing method according to the first embodiment. [Figure 7] FIG. 7 is a cross-sectional view illustrating a wafer and a film during the crack induction layer forming step in the chip manufacturing method of the first embodiment. [Figure 8] FIG. 8 is a cross-sectional view that illustrates a schematic view of the wafer and the film during the crack formation step according to the chip manufacturing method of the first embodiment. [Figure 9] FIG. 9 is a cross-sectional view that typically shows a wafer and a film in the case where cracks are formed without forming a crack induction layer. [Figure 10] FIG. 10 is a perspective view that illustrates a schematic diagram of an expansion device used in the chip manufacturing method according to the first embodiment. [Figure 11] FIG. 11 is a cross-sectional view that illustrates an expansion device, a wafer, and a membrane that are used in the chip manufacturing method according to the first embodiment. [Figure 12] FIG. 12 is a cross-sectional view that illustrates an expansion device, a wafer, and a membrane that are used in the chip manufacturing method according to the first embodiment. [Figure 13] FIG. 13 is a diagram showing a schematic diagram of a laser irradiation device used in the chip manufacturing method according to the second embodiment. [Figure 14] FIG. 14 is a cross-sectional view illustrating a wafer and a film during the crack inducing layer forming step according to the chip manufacturing method of the second embodiment. [Figure 15]FIG. 15 is a cross-sectional view illustrating a schematic view of the wafer and the film during the crack forming step according to the second embodiment. [Figure 16] FIG. 16 is a cross-sectional view illustrating a wafer and a film during the crack induction layer forming step according to the third embodiment. [Figure 17] FIG. 17 is a cross-sectional view illustrating a schematic view of the wafer and the film during the crack forming step according to the fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In Fig. 1 to Fig. 4, the directions of a wafer are conveniently represented using a first direction D1, a second direction D2, and a third direction D3 that are orthogonal to each other.

[0015] Fig. 1 is a perspective view showing a wafer 2 according to the present embodiment, Fig. 2 is a top view showing a wafer 2 according to the present embodiment, and Fig. 3 is a cross-sectional view showing a wafer 2 according to the present embodiment. As shown in Fig. 1 to Fig. 3, the wafer 2 according to the present embodiment is formed in a disk shape from a material such as crystalline silicon, and one or more films 4 are provided on the front surface 2a side.

[0016] For example, electrodes constituting a plurality of semiconductor devices 6 are provided above the film 4 (opposite side to the wafer 2). That is, the film 4 constitutes the semiconductor devices 6 together with the portion on the front surface 2a side of the wafer 2. The shape of the wafer 2 is not limited to a disk shape, and may be other shapes such as a rectangle.

[0017] 2, the region between two adjacent rows of the plurality of semiconductor devices 6 aligned along a first direction D1 parallel to the surface 2a of the wafer 2 constitutes a planned dividing line 8. Similarly, the region between two adjacent rows of the plurality of semiconductor devices 6 aligned along a second direction D2 parallel to the surface 2a of the wafer 2 and perpendicular to the first direction D1 constitutes a planned dividing line 8.

[0018] 2, in consideration of ease of viewing the drawing, only an area corresponding to one planned dividing line 8 along the first direction D1 is shown by a dashed line, but any area between any two adjacent rows of all the rows of semiconductor devices 6 constitutes a planned dividing line 8. The portion on the front surface 2a side of the wafer 2 is divided into individual semiconductor devices 6 by these planned dividing lines 8 provided along the first direction D1 and the second direction D2.

[0019] As shown in Fig. 3, for example, two films 4 are provided on the front surface 2a side of the wafer 2. In Fig. 3, an oxide film 4a is provided on the front surface 2a of the wafer 2, and a nitride film 4b is overlaid on the oxide film 4a. The oxide film 4a is, for example, a silicon oxide film, etc., and is formed by a CVD (Chemical Vapor Deposition) method or thermal oxidation. The nitride film 4b is, for example, a silicon nitride film, etc., and is formed by a CVD method.

[0020] The crystallinity of the oxide film 4a and the nitride film 4b formed by these film forming methods is lower than that of the wafer 2 formed of crystalline silicon or the like. The thickness of the wafer 2 is, for example, 80 μm, and the thickness of the oxide film 4a and the nitride film 4b is, for example, 2 μm. However, the configuration, composition, thickness, etc. of the wafer 2 and the configuration, composition, thickness, etc. of the film 4 can be appropriately changed according to the specifications of the chip.

[0021] Fig. 4 is a top view showing a schematic diagram of a chip obtained by the chip manufacturing method according to the first embodiment. As shown in Fig. 4, by dividing the wafer 2 shown in Fig. 1 to Fig. 3 together with the film 4 along the division lines 8, a plurality of chips 10 each including a semiconductor device 6 is obtained.

[0022] Fig. 5 is a flow diagram showing the method for manufacturing a chip according to the first embodiment. As shown in Fig. 5, the method for manufacturing a chip according to this embodiment includes a crack induction layer forming step S1, a crack forming step S2, and a division step S3. Each step of the crack induction layer forming step S1, the crack forming step S2, and the division step S3 will be described below with reference to the drawings.

[0023] In the chip manufacturing method according to this embodiment, first, a crack induction layer forming step S1 is performed. In this crack induction layer forming step S1, a laser beam is irradiated onto the wafer 2 to partially alter the wafer 2, thereby forming a linear crack induction layer 12 along the planned division lines 8 on the wafer 2. FIG. 6 is a schematic diagram showing a laser irradiation device 20 configured to be able to irradiate the wafer 2 with a laser beam 28.

[0024] 6, the laser irradiation device 20 includes a laser oscillator 22. The laser oscillator 22 includes a laser medium such as Nd:YAG that is suitable for laser oscillation, and can generate, for example, a pulsed laser beam 28 having a wavelength that is transmitted through the wafer 2.

[0025] A reflector 24 such as a mirror is disposed downstream of the laser oscillator 22 along the traveling direction of the laser beam 28. The laser beam 28 generated by the laser oscillator 22 is reflected by the reflector 24, and the traveling direction of the laser beam 28 is changed to a downward direction (along the Z-axis).

[0026] A condenser 26 such as a lens capable of condensing the laser beam 28 to a focusing point further below is disposed below the reflector 24. A holding table 62 capable of holding the wafer 2 is disposed below the condenser 26. The laser beam 28 reflected by the reflector 24 passes through the condenser 26 and is irradiated onto the wafer 2 held by the holding table 62.

[0027] The holding table 62 is supported by, for example, a rotation mechanism including a motor and a ball screw type movement mechanism, and rotates around the Z axis by the force generated by the rotation mechanism, and moves along the X and Y axes by the force generated by the movement mechanism. When the holding table 62 holding the wafer 2 is moved along the X and Y axes by the movement mechanism, the wafer 2 and the focal point of the collector 26 move relatively along the X and Y axes.

[0028] 7 is a cross-sectional view showing the wafer 2 and the film 4 during the crack induction layer formation step S1 in the chip manufacturing method of the first embodiment. In the crack induction layer formation step S1, first, the front surface 2a side of the wafer 2 is held by the holding table 62 so that the back surface 2b side of the wafer 2 is exposed upward. That is, the upper surface side of the film 4 shown in FIG. 7 is held by the holding table 62. Next, the rotation mechanism rotates the holding table 62 so that the planned division line 8 to be processed is parallel to the X-axis.

[0029] Furthermore, the movement mechanism moves the holding table 62 along the Y-axis so that the focal point of the collector 26 is positioned along an extension of the target planned dividing line 8. Thereafter, for example, the movement mechanism moves the holding table 62 along the X-axis while the laser oscillator 22 generates a laser beam 28 having a wavelength that transmits through the wafer 2. Note that the height of the focal point is adjusted in advance so that the laser beam 28 is focused on an area including the surface 2a of the wafer 2.

[0030] 7, the laser beam 28 is incident from the back surface 2b side of the wafer 2 so as to be focused on a region including the front surface 2a of the wafer 2, and is irradiated along a linear first region 50 parallel to the X-axis. The linear first region 50 of the wafer 2 is then altered by the laser beam 28, and a crack induction layer 12 is formed in this first region 50.

[0031] After the laser beam 28 has been irradiated along one of the target division lines 8, the movement mechanism moves the holding table 62 in the direction of the arrow along the Y axis. This moves the focusing point of the collector 26 to a position where it overlaps with an extension of the adjacent division line 8. Then, by repeating the same operation, the laser beam 28 is irradiated along the adjacent division line 8, and a similar crack induction layer 12 is formed on the adjacent division line 8 as well.

[0032] The above-mentioned operation is repeated, for example, until the crack guiding layer 12 is formed along all of the planned division lines 8. Note that Fig. 7 shows the state in which the crack guiding layer 12 is formed by the laser beam 28 depicted by the solid line, and the laser beam 28 irradiated at an earlier timing is depicted by the dashed line.

[0033] For example, the wavelength of the laser beam 28 is set to 1064 nm to 2000 nm, the pulse width is set to 10 ps to 40 ns, the output is set to 0.01 W to 1 W, the repetition frequency is set to 10 kHz to 500 kHz, the NA (Numerical Aperture) of the condenser lens is set to 0.3, and the feed speed of the wafer 2 is set to 10 mm / s to 2000 mm / s. The output is appropriately adjusted according to the wavelength band and pulse width of the laser beam 28, and the feed speed is appropriately adjusted according to the frequency, etc. For example, the wavelength is set to 1064 nm, the pulse width is set to 40 ns, the output is set to 0.1 W, the frequency is set to 80 kHz, and the feed speed is set to 500 mm / s. However, the conditions for irradiating the laser beam 28 may be changed within a range in which the crack guiding layer 12 is appropriately formed in the first region 50 of the wafer 2.

[0034] After the above-mentioned crack induction layer forming step S1, a crack forming step S2 is performed. In this crack forming step S2, a laser beam 56 is irradiated onto the wafer 2 to partially modify the wafer 2, thereby forming a linear modified layer (modified layer) along the planned division line 8 on the wafer 2. Fig. 8 is a cross-sectional view that shows the wafer 2 and the film 4 during the execution of the crack forming step S2 according to the chip manufacturing method of the first embodiment.

[0035] In this embodiment, the laser irradiation device 20 used in the crack guiding layer forming step S1 is also used in the crack forming step S2. However, a laser irradiation device other than the laser irradiation device 20 used in the crack guiding layer forming step S1 may be used in the crack forming step S2.

[0036] 8, in the crack forming step S2, first, the rotation mechanism rotates the holding table 62 so that the division line 8 to be processed is parallel to the X-axis. Note that, following the crack induction layer forming step S1, the front surface 2a side of the wafer 2 is held by the holding table 62, and the back surface 2b side of the wafer 2 is exposed upward.

[0037] Furthermore, the moving mechanism moves the holding table 62 along the Y-axis so that the focal point of the collector 26 is positioned along an extension of the target planned division line 8. Thereafter, for example, the moving mechanism moves the holding table 62 along the X-axis while the laser oscillator 22 generates a laser beam 56 having a wavelength that transmits through the wafer 2. Note that the height of the focal point is adjusted in advance so that the laser beam 56 is focused in an area farther from the front surface 2a than the crack induction layer 12 of the wafer 2.

[0038] 8, the laser beam 56 is incident from the back surface 2b side of the wafer 2 so as to be focused on a region farther from the front surface 2a than the crack inducing layer 12 of the wafer 2, and is irradiated along a linear second region 52 parallel to the X-axis. The linear second region 52 of the wafer 2 is then altered by the laser beam 56, and an altered layer 14 is formed in the second region 52.

[0039] After the laser beam 56 has been irradiated along one of the target division lines 8, the movement mechanism moves the holding table 62 in the direction of the arrow along the Y axis. This moves the focusing point of the collector 26 to a position where it overlaps with an extension of the adjacent division line 8. Then, by repeating the same operation, the laser beam 56 is irradiated along the adjacent division line 8, and a similar affected layer 14 is formed on the adjacent division line 8 as well.

[0040] The above-mentioned operation is repeated, for example, until the affected layers 14 are formed along all of the planned division lines 8. Note that Fig. 8 shows the state in which the affected layers 14 are formed by the laser beam 56 depicted by the solid line, and the laser beam 56 irradiated at an earlier timing is depicted by the dashed line.

[0041] The laser beam 56 used in the crack formation step S2 is generated under different conditions from the laser beam 28 used in the crack induction layer formation step S1, for example. For this reason, in the crack formation step S2 of this embodiment, a laser irradiation device different from the laser irradiation device 20 used in the crack induction layer formation step S1 is used. However, the basic structure of the laser irradiation device used in the crack formation step S2 may be similar to the structure of the laser irradiation device 20 used in the crack induction layer formation step S1.

[0042] For example, the wavelength of the laser beam 56 is set to 1064 nm to 2000 nm, the pulse width is set to 10 ps to 40 ns, the output is set to 0.1 to 10 W, the repetition frequency is set to 10 kHz to 500 kHz, the NA (Numerical Aperture) of the condenser lens is set to 0.7, and the feed speed of the wafer 2 is set to 10 mm / s to 2000 mm / s. The output is appropriately adjusted according to the wavelength band and pulse width of the laser beam 28, and the feed speed is appropriately adjusted according to the frequency, etc. For example, the wavelength is set to 1064 nm, the pulse width is set to 40 ns, the output is set to 0.4 W, the frequency is set to 80 kHz, and the feed speed is set to 500 mm / s. However, the conditions for irradiating the laser beam 56 may be changed within a range in which the affected layer 14 is appropriately formed in the second region 52 of the wafer 2.

[0043] As described above, the wafer 2 is made of a crystalline material. Therefore, when the deteriorated layer 14 is formed on the wafer 2 in the crack forming step S2, cracks extend from the deteriorated layer 14 in accordance with the crystal structure. In this embodiment, a crack (first crack) 16 extending from the deteriorated layer 14 toward the crack guiding layer 12 and a crack (third crack) 54 extending from the deteriorated layer 14 toward the back surface 2b side of the wafer 2 (the surface opposite to the front surface 2a side of the wafer 2) are formed.

[0044] In this embodiment, a crack induction layer 12 is formed in a region including the surface 2a of the wafer 2, and this crack induction layer 12 is in contact with the film 4. Therefore, a crack (first crack) 16 acts on the film 4 provided on the surface 2a of the wafer 2 through the crack induction layer 12, and a crack (second crack) 18 extends in the direction in which this first crack 16 extends. Although the detailed mechanism is unclear, it is speculated that the formation of the crack induction layer 12 in a region including the surface 2a of the wafer 2 changes the state of bonding at the interface between this crack induction layer 12 and the film 4, and the extension direction of the second crack 18 becomes more susceptible to the influence of the first crack 16.

[0045] In this embodiment, by forming the crack guiding layer 12 in advance, the first crack 16 formed inside the wafer 2 and the second crack 18 formed in the film 4 provided on the surface of the wafer 2 extend in approximately the same direction. As a result, the film 4 is less likely to crack diagonally, and the possibility of the film peeling off from the wafer 2 due to the film cracking diagonally can be reduced. That is, the crack guiding layer 12 formed in the region including the surface 2a of the wafer 2 has the function of guiding the extension direction of the second crack 18 formed in the film 4 to approximately the same direction as the extension direction of the first crack 16 formed inside the wafer 2.

[0046] After the laser beam 56 has been applied along one of the division lines 8, the holding table 62 moves the wafer 2 in a direction perpendicular to the division lines 8 (the X-axis direction in FIG. 5, the direction of the arrow in FIG. 8). Then, the laser beam 56 is applied in the same manner along the adjacent division line 8, whereby the linear second region 52 of the wafer 2 is altered, and an altered layer 14 is formed in the second region 52.

[0047] 9 is a cross-sectional view showing a wafer 2 and a film 4 when cracks are formed without forming a crack induction layer 12. Inside the film 4, which has a lower crystallinity than the wafer 2, it is difficult to make the cracks extend in the same direction as the cracks formed in the wafer 2. For this reason, when the crack induction layer 12 is not formed on the wafer 2, as shown in FIG. 9, the directions in which the cracks extend do not necessarily match between the wafer 2 and the film 4 provided on its surface 2a, and the film 4 may crack obliquely with respect to the surface 2a of the wafer 2 and peel off from the wafer 2.

[0048] In contrast, in this embodiment, the crack leading layer 12 provided in the first region 50 including the surface 2a of the wafer 2 can cause the crack to extend in the film 4 along the extension direction of the first crack 16. This can reduce the possibility that the film 4 will crack obliquely with respect to the surface 2a of the wafer 2 and peel off from the wafer 2.

[0049] After the above-mentioned crack forming step S2, a dividing step S3 is performed. In the dividing step S3, an external force is applied to the wafer 2, so that the wafer 2 is divided into a plurality of chips 10 along the division lines 8. The dividing step S3 is performed, for example, by attaching the wafer 2 to an expandable tape 58 made of a tensile (expandable) resin and expanding the expandable tape 58.

[0050] To expand the expanding tape 58, for example, an actuator capable of applying a mechanical force to the expanding tape 58 to expand the expanding tape 58 is used. Fig. 10 is a perspective view showing an expansion device 30 used in the method for manufacturing the chip 10 according to the first embodiment. Figs. 11 and 12 are cross-sectional views showing the expansion device 30, the wafer 2, and the film 4 used in the method for manufacturing the chip 10 according to the first embodiment.

[0051] 11 shows the state of the wafer 2 before it is divided, and FIG. 12 shows the state of the wafer 2 after it is divided. The expansion device 30 pulls and expands the expanding tape 58, and divides the wafer 2 along the first crack 16, the second crack 18, and the third crack 54. In this embodiment, an annular frame 48 surrounding the wafer 2 is fixed to the peripheral portion of the expanding tape 58 so that the expansion device 30 can hold the wafer 2 and the expanding tape 58.

[0052] The expansion device 30 includes, for example, a disk-shaped base 32. On the upper surface of the base 32, there are arranged a cylindrical drum 34 having a diameter larger than that of the wafer 2, and four sets of air actuators (air cylinders) 36 surrounding the drum 34. Each air actuator 36 includes a cylinder 38 fixed to the upper surface of the base 32. The cylinders 38 are arranged, for example, at equal intervals (equal angular intervals) along the outer periphery of the drum 34.

[0053] A piston (not shown) is inserted into each cylinder 38 so that it can move up and down. The piston inserted in the cylinder 38 moves up and down by air supplied to the cylinder 38 through an air supply passage (not shown). The lower end of a rod 40 is connected to the upper end of each piston. An annular support base 42 capable of supporting the above-mentioned frame 48 is fixed to the upper end of the rod 40.

[0054] Therefore, when air is supplied to the cylinder 38 of each air actuator 36 and the piston and rod 40 are moved up and down, the support base 42 moves up and down. Specifically, the support base 42 can move up and down between a first position where the height of the upper end of the drum 34 and the height of the upper surface of the support base 42 are approximately the same, and a second position where the height of the upper surface of the support base 42 is lower than the height of the upper end of the drum 34.

[0055] A plurality of clamps 44 are fixed to the outer periphery of the support base 42. The multiple clamps 44 are arranged at approximately equal intervals (equal angular intervals) along the circumferential direction of the support base 42, and grip and fix a frame 48 arranged on the support base 42. The frame 48 is arranged on the support base 42 and fixed by the multiple clamps 44, whereby the frame 48 is held by the frame holding unit 46.

[0056] In the division step S3, first, the support table 42 is positioned at a first position. That is, the height of the support table 42 is adjusted so that the height of the upper end of the drum 34 and the height of the upper surface of the support table 42 are approximately equal. Next, the frame 48 supporting the wafer 2 via the expandable tape 58 is placed on the support table 42. At this time, the wafer 2 is placed inside the outer periphery of the drum 34 in a plan view.

[0057] Thereafter, the frame 48 placed on the support table 42 is fixed by the multiple clamps 44. As a result, the wafer 2 is held by the frame holding unit 46 via the expanding tape 58 and the frame 48.

[0058] Next, the support table 42 is lowered by the air actuator 36 and positioned at the second position. This causes the frame 48 to move downward, and the expanding tape 58 in contact with the upper end of the drum 34 is expanded so as to be pulled outward in the radial direction. As a result, an external force directed outward in the radial direction of the wafer 2 is applied to the wafer 2.

[0059] As shown in Figures 11 and 12, when an external force is applied to the wafer 2 by the expansion of the expandable tape 58, the wafer 2 is divided along the first crack 16 and the third crack 54, and the film 4 is divided along the second crack 18. As a result, a plurality of chips 10 are obtained. After the wafer 2 and the film 4 are divided, each chip 10 is picked up by, for example, a collet (not shown) and mounted on a predetermined substrate (such as a wiring substrate).

[0060] 13 is a schematic diagram showing a laser irradiation device 70 used in the manufacturing method of the chip 10 of the second embodiment. In this embodiment, in the crack guiding layer forming step S1, the crack guiding layer 12 is formed using a laser irradiation device 70 provided with a branching portion 60. The basic structure of the laser irradiation device 70 may be similar to the structure of the laser irradiation device 20 used in the manufacturing method of the chip 10 of the first embodiment.

[0061] The splitter 60 of the laser irradiation device 70 splits the laser beam 28 generated by the laser oscillator 22 into two laser beams 68 along the Y-axis. For example, a combination of a half-wave plate and a Wollaston prism is used as the splitter 60. The Wollaston prism splits the incident laser beam 28 into two linearly polarized laser beams 68 polarized in directions perpendicular to each other.

[0062] Fig. 14 is a cross-sectional view showing the wafer 2 and the film 4 during the crack induction layer formation step S1 in the manufacturing method of the chip 10 of the second embodiment, and Fig. 15 is a cross-sectional view showing the wafer 2 and the film 4 during the crack formation step in the manufacturing method of the chip 10 of the second embodiment. In the second embodiment, as shown in Fig. 14, in the crack induction layer formation step S1, a crack induction layer 12 is formed in each of two linear first regions 50 spaced apart in the width direction of one planned division line 8.

[0063] Then, in the crack formation step S2, when the affected layer 14 is formed, a first crack 16 is formed which extends from the affected layer 14 toward between the two crack guiding layers 12 and reaches the region between the two crack guiding layers 12. The first crack 16 formed in the wafer 2 acts on the film 4, and a second crack 18 extends from between the two crack guiding layers 12 toward the inside of the film 4 in approximately the same direction as the extension direction of the first crack 16. Therefore, in the second embodiment, the extension starting point of the second crack 18 in the film 4 is controlled to occur between the two crack guiding layers 12.

[0064] The crack forming step S2 and the dividing step S3 in the method for manufacturing the chip 10 according to the second embodiment are similar to the method for manufacturing the chip 10 according to the first embodiment.

[0065] Fig. 16 is a cross-sectional view showing the wafer 2 and the film 4 during the crack induction layer formation step S1 in the manufacturing method of the chip 10 of the third embodiment. As shown in Fig. 16, in the third embodiment, a laser beam 64 is incident on the front surface 2a side of the wafer 2. A wavelength that is transmitted through the film 4 and absorbed by the wafer 2 is selected as the wavelength of the laser beam 64.

[0066] For example, the wavelength of the laser beam 64 is set to 355 to 800 nm, the pulse width is set to 10 ps to 40 ns, the output is set to 0.01 W to 0.1 W, the frequency is set to 10 kHz to 500 kHz, and the feed speed is set to 10 mm / s to 2000 mm / s. The output is appropriately adjusted according to the wavelength band and pulse width of the laser beam 28, and the feed speed is appropriately adjusted according to the frequency, etc. For example, the wavelength is set to 355 nm, the pulse width is set to 10 ps, ​​the output is set to 0.01 W, the frequency is set to 500 kHz, and the feed speed is appropriately adjusted according to the frequency, etc. of the laser beam 64.

[0067] The basic structure of the laser irradiation device used in the manufacturing method of the chip 10 of the third embodiment may be similar to the structure of the laser irradiation device 20 used in the manufacturing method of the chip 10 of the first embodiment. However, the laser oscillator of the laser irradiation device needs to be configured so as to be able to generate a laser beam 64 having a wavelength that is transmitted through the film 4 and absorbed by the wafer 2.

[0068] In this embodiment, since the laser beam 64 is absorbed by the wafer 2, precise adjustment of the position of the focal point where the laser beam 64 is focused is not required, and the crack induction layer 12 is easily and appropriately formed in the crack induction layer formation step S1. The crack formation step S2 and the division step S3 in the method for manufacturing the chip 10 according to the third embodiment are the same as those in the method for manufacturing the chip 10 according to the first embodiment.

[0069] Fig. 17 is a cross-sectional view showing the wafer 2 and the film 4 during the crack formation step S2 in the manufacturing method of the chip 10 according to the fourth embodiment. As shown in Fig. 17, in the fourth embodiment, a laser beam 66 is incident on the front surface 2a side of the wafer 2. A wavelength that transmits the wafer 2 and the film 4 is selected as the wavelength of the laser beam 66.

[0070] For example, the wavelength of the laser beam 66 is set to 1064 nm to 2000 nm, the pulse width is set to 10 ps to 40 ns, the output is set to 0.1 to 10 W, the repetition frequency is set to 10 kHz to 500 kHz, the NA (Numerical Aperture) of the condenser lens is set to 0.7, and the feed speed of the wafer 2 is set to 10 mm / s to 2000 mm / s. The output is appropriately adjusted according to the wavelength band and pulse width of the laser beam 28, and the feed speed is appropriately adjusted according to the frequency, etc. For example, the wavelength is set to 1064 nm, the pulse width is set to 40 ns, the output is set to 0.4 W, the frequency is set to 80 kHz, and the feed speed is set to 500 mm / s. However, the conditions for irradiating the laser beam 56 may be changed within a range in which the affected layer 14 is appropriately formed in the second region 52 of the wafer 2.

[0071] In cases where the intended dividing lines (streets) are narrow, or there is a layer in the area through which the laser beam passes that absorbs or reflects the laser beam 66, and if the laser beam is incident from the wafer, it is effective to have the laser beam 66 incident from the front surface 2a side of the wafer 2, as in this embodiment.

[0072] Therefore, the basic structure of the laser irradiation device used in the manufacturing method of the chip 10 of the fourth embodiment may be similar to the structure of the laser irradiation device 20 used in the manufacturing method of the chip 10 of the first embodiment. The crack induction layer forming step S1 and the division step S3 in the manufacturing method of the chip 10 of the fourth embodiment are similar to those of the first and third embodiments.

[0073] In addition, in the crack induction layer formation step S1 in the manufacturing method of chip 10 of the third embodiment, laser beam 64 is incident from the front surface 2a side of wafer 2, but in the crack formation step S2 in the manufacturing method of chip 10 of the third embodiment, the laser beam may be incident from the front surface 2a side of wafer 2 or from the back surface 2b side of wafer 2.

[0074] Similarly, in the crack formation step S2 in the manufacturing method of chip 10 of the fourth embodiment, laser beam 66 is incident from the front surface 2a side of wafer 2, but in the crack induction layer formation step S1 in the manufacturing method of chip 10 of the fourth embodiment, the laser beam may be incident from either the front surface 2a side of wafer 2 or the back surface 2b side of wafer 2.

[0075] In addition, the structures, methods, and the like according to the above-described embodiments may be modified as appropriate without departing from the scope of the present invention. [Explanation of symbols]

[0076] 2: Wafer 2a: surface 4: Membrane 4a: oxide film 4b: Nitride film 6: Semiconductor devices 8: Planned division line 10: Semiconductor chips 12: Crack induction layer 14: Deteriorated layer (modified layer) 16: First Crack 18: Second Crack 20: Laser irradiation device 22: Laser oscillator 24:Reflector 26: Concentrator 28: Laser beam 30: Expansion device (split device) 32: Bass 34: Drums 36: Air actuator 38: Cylinder 40: Rod 42: Support stand 44: Clamp 46: Frame holding unit 48: Frame 50: 1st area 52:Second area 54: Third Crack 56: Laser beam 58: Expandable tape 60: Branch 62: Holding table 64: Laser beam 66: Laser beam 68: Laser beam 70: Laser irradiation device

Claims

1. A method for manufacturing a chip, comprising the steps of: dividing a wafer having a film on a surface thereof along a division line to manufacture a plurality of chips, the method comprising the steps of: a crack inducing layer forming step of irradiating the dividing line with a focused laser beam having a wavelength that is transmitted through one or both of the wafer and the film, thereby modifying a linear first region of the wafer including the surface, and forming a crack inducing layer in the first region; a crack forming step in which, after the crack inducing layer forming step, a laser beam having a wavelength that is transmitted through the wafer is focused and irradiated onto the intended dividing line to alter a linear second region inside the wafer that is farther from the surface than the crack inducing layer, thereby forming an altered layer in the second region and forming a first crack extending from the altered layer toward the crack inducing layer and a second crack extending toward the inside of the film; A method for manufacturing a chip, comprising: after the crack formation step, a dividing step of applying an external force to the wafer to divide the wafer together with the film along the intended dividing lines to obtain a plurality of the chips.

2. In the crack induction layer forming step, two linear first regions separated in a width direction of the division line are each modified to form two crack induction layers; The method for manufacturing a chip as described in claim 1, wherein the crack formation step involves altering a linear second region inside the wafer, which is farther from the surface than the two crack induction layers, to form an altered layer in the second region, and forming a first crack extending from the altered layer toward the two crack induction layers and reaching the region between the two crack induction layers, and a second crack extending toward the inside of the film.

3. In the crack inducing layer forming step, 3. The method for manufacturing chips according to claim 1, wherein a laser beam having a wavelength that is transmitted through the film and absorbed by the wafer is irradiated onto the intended dividing lines from the film side while being focused.

Citation Information

Patent Citations

  • Method of dividing wafer

    JP2009290148A

  • Manufacturing method of device chip

    JP2016163016A

  • Method of cutting laminate including silicone layer

    JP2021089935A

  • Laser processing method and semiconductor chip

    WO2005098915A1

  • Laser beam machining method

    JP2002192370A