Carbon nanotube dispersion, method of producing the same, and carbon nanotube composite
By using single-walled carbon nanotubes with a high G/D ratio and sulfate-esterified cellulose nanofibers, the carbon nanotube composite achieves enhanced dispersibility and conductivity, addressing inefficiencies in existing composite production methods.
Patent Information
- Application Number
- JP2023046569
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing carbon nanotube composites with high electrical conductivity are inefficient, as they often result in poor dispersibility and suboptimal conductivity due to the use of non-specific cellulose nanofibers and carbon nanotubes.
A carbon nanotube dispersion is created using single-walled carbon nanotubes with a peak intensity ratio G/D of 30 or more and cellulose nanofibers with sulfate ester groups within a specific sulfur content range (0.5 to 3.5 mmol/g), which enhances the dispersibility and conductivity of the composite.
The method produces a carbon nanotube composite with high electrical conductivity, achieving conductivity levels of 1×10^3 S/cm or more, suitable for applications in conductive films and inks.
Smart Images

Figure 2024135732000001 
Figure 2024135732000002 
Figure 2024135732000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon nanotube dispersion, a production method thereof, and a carbon nanotube composite. [Background technology]
[0002] Conventional methods for producing a film-like conductive composite include a method in which a dispersion containing a conductive material such as carbon nanotubes (hereinafter sometimes referred to as "CNTs") is cast onto a substrate, followed by drying and peeling, and a method in which carbon nanotubes and cellulose nanofibers are mixed to obtain a composite structure.
[0003] For example, Patent Document 1 discloses a technique for producing a conductive composite having stable conductivity, in which a dispersion liquid containing cellulose nanofibers modified with a carboxy group and carbon nanotubes modified with a carboxy group is cast onto a substrate, followed by drying and peeling to obtain a film-like conductive composite. In Patent Document 1, modified celluloses obtained by oxidizing celluloses with sodium hypochlorite as a co-oxidant in the presence of 2,2,6,6-tetramethylpiperidinooxy radical (TEMPO) are used as the cellulose nanofibers modified with a carboxy group.
[0004] Non-Patent Document 1 reports a technology in which a slurry containing cellulose nanofibers is mixed with an aqueous dispersion containing carbon nanotubes, and then a conductive paper containing 17% carbon nanotubes is produced through processes such as filtration and drying.Non-Patent Document 2 introduces a technology in which a mixed slurry containing cellulose nanofibers and carbon nanotubes is processed into a fibrous structure, which is then used as an electrode to create a fibrous capacitor.
[0005] Patent Document 2 discloses a method for producing a dispersion liquid obtained by mixing single-walled carbon nanotubes with metal-containing oxidized cellulose nanofibers that contain a specific metal in the form of a salt, as a method for producing a composite having high conductivity with a small content of single-walled carbon nanotubes.
[0006] Patent Document 3 describes that sulfated modified cellulose is used for applications such as medical materials and surfactants. A known method for producing sulfated cellulose is to add cellulose to a mixed solution of sulfuric anhydride and dimethylformamide, and modify the surface of cellulose particles by sulfate esterification while controlling the temperature in an ice bath. The sulfated cellulose prepared by this sulfate esterification method is not cellulose nanofiber, but a cellulose derivative in which the type I crystal structure and microfibrils inherent to natural cellulose are destroyed.
[0007] Patent Document 4 discloses a method for producing a dispersion of single-walled carbon nanotubes and oxidized cellulose nanofibers containing a metal other than sodium in the form of a salt in order to obtain a composite having high electrical conductivity. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2013-211108 A [Patent Document 2] Patent Publication No. 2021-57271 [Patent Document 3] JP 2007-92034 A [Patent Document 4] Patent Publication No. 2021-57271 [Non-patent literature]
[0009] [Non-Patent Document 1] Composites Science AND Technology, Volume 87, 18 October 2013, Pages 103-110 [Non-Patent Document 2] Electrochimica Acta, Volume 283, 1 September 2018, Pages 1578-1588 Summary of the Invention [Problem to be solved by the invention]
[0010] For example, carbon nanotube composites that exhibit high electrical conductivity are required for use in display components, electronics components, and the like.
[0011] The main object of the present invention is to provide a carbon nanotube dispersion that can suitably produce a carbon nanotube composite exhibiting high electrical conductivity. Another object of the present invention is to provide a method for producing the carbon nanotube dispersion, and a carbon nanotube composite using the carbon nanotube dispersion. [Means for solving the problem]
[0012] The present inventors have conducted extensive research to solve the above problems, and have found that a carbon nanotube composite exhibiting high electrical conductivity can be suitably obtained by using, in a carbon nanotube dispersion, single-walled carbon nanotubes having a peak intensity ratio G / D of a predetermined value or more and cellulose nanofibers having sulfate ester groups with an amount of sulfur introduced adjusted to a predetermined range.
[0013] The present invention was completed through further investigation based on the above findings.
[0014] That is, the present invention provides the following aspects. Item 1. A carbon nanotube dispersion liquid comprising carbon nanotubes, cellulose nanofibers, and a dispersion medium, the carbon nanotube is a single-walled carbon nanotube, and has a peak intensity ratio G / D of G band to D band in a Raman spectrum at an excitation wavelength of 532 nm measured by a resonance Raman scattering method of 30 or more; The cellulose nanofiber has a sulfate ester group represented by the following formula (1), and the amount of sulfur introduced due to the sulfate ester group is 0.5 mmol / g or more and 3.5 mmol / g or less. [ka] [In the above formula (1), n is an integer of 1 to 3, and M n+1 is an n-valent cation, and the wavy lines are the sites of attachment to other atoms.] Item 2. The carbon nanotube dispersion according to Item 1, wherein the cellulose nanofibers have an average fiber diameter of 1 nm or more and 1000 nm or less and have a type I crystal structure. Item 3. The carbon nanotube dispersion according to Item 1 or 2, wherein the carbon nanotubes have an average fiber diameter of 0.8 nm or more and 5.0 nm or less. Item 4. The carbon nanotube dispersion liquid according to any one of Items 1 to 3, wherein the dispersion medium is water. Item 5. The carbon nanotube dispersion liquid according to any one of Items 1 to 4, wherein the carbon nanotube content is 0.05% by mass or more. Item 6. The carbon nanotube dispersion liquid according to any one of Items 1 to 5, wherein the content of the cellulose nanofibers is 0.005% by mass or more. Item 7. A method for producing a carbon nanotube dispersion liquid according to any one of items 1 to 6, A step of preparing a crude dispersion by mixing the carbon nanotubes, the cellulose nanofibers, and the dispersion medium; a step of dispersing the crude dispersion to obtain a carbon nanotube dispersion; The method for producing a carbon nanotube dispersion liquid includes the steps of: Item 8. A carbon nanotube composite obtained by removing the dispersion medium from the carbon nanotube dispersion liquid according to any one of Items 1 to 6. Item 9. The electrical conductivity of the carbon nanotube composite measured by the following method is 1×10 3 A carbon nanotube composite having a hardness of 1.0 S / cm or more. (Method of measuring electrical conductivity) In the carbon nanotube dispersion according to any one of items 1 to 6, a step of preparing a crude dispersion by mixing the carbon nanotubes, the cellulose nanofibers, and the dispersion medium using ion-exchanged water as the dispersion medium, and a step of dispersing the crude dispersion are performed. The mass ratio of the carbon nanotubes to the cellulose nanofibers in the carbon nanotube dispersion is 50:50, and the total concentration thereof is 0.4 mass%. The obtained carbon nanotube dispersion liquid is applied onto a polyethylene terephthalate film and dried in an oven at 40°C for 5 days to obtain a composite of carbon nanotubes and cellulose nanofibers with a thickness of 5 µm. The surface resistivity (Ω / sq) and electrical conductivity (S / cm) of the resulting composite are measured using a resistivity meter. Effect of the Invention
[0015] According to the present invention, it is possible to provide a carbon nanotube dispersion that can suitably produce a carbon nanotube composite exhibiting high electrical conductivity. Furthermore, according to the present invention, it is also possible to provide a method for producing the carbon nanotube dispersion and a carbon nanotube composite using the carbon nanotube dispersion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In this specification, a numerical value connected with "~" means a numerical range including the numerical values before and after "~" as the lower limit and upper limit. When multiple lower limit values and multiple upper limit values are listed separately, any lower limit value and upper limit value can be selected and connected with "~".
[0017] In addition, in this specification, carbon nanotubes may be abbreviated as "CNT". Therefore, in this specification, carbon nanotube dispersions may be abbreviated as "CNT dispersions", single-walled carbon nanotubes may be abbreviated as "single-walled CNTs", and carbon nanotube composites may be abbreviated as "CNT composites". Similarly, cellulose nanofibers may be abbreviated as "CNF", and cellulose nanofibers having sulfate ester groups in particular may be abbreviated as "S-CNF".
[0018] 1. Carbon nanotube dispersion The carbon nanotube dispersion of the present invention comprises carbon nanotubes, cellulose nanofibers, and a dispersion medium, wherein the carbon nanotubes are single-walled carbon nanotubes, and the peak intensity ratio G / D of the G band to the D band in a Raman spectrum at an excitation wavelength of 532 nm measured by a resonance Raman scattering method is 30 or more, and the cellulose nanofibers have sulfate ester groups represented by the following formula (1), and the amount of sulfur introduced due to the sulfate ester groups is 0.5 mmol / g or more and 3.5 mmol / g or less.
[0019] [ka] [In the above formula (1), n is an integer of 1 to 3, and M n+ is an n-valent cation, and the wavy lines are the sites of attachment to other atoms.]
[0020] The carbon nanotube dispersion of the present invention has the above-mentioned configuration, and thus can suitably produce a carbon nanotube composite exhibiting high electrical conductivity. The peak intensity ratio G / D of the single-walled carbon nanotubes contained in the carbon nanotube dispersion of the present invention is 30 or more, and has high crystallinity. Therefore, although the single-walled carbon nanotubes have high electrical conductivity, they are characterized in that they do not have high dispersibility in the dispersion medium. In contrast, in the present invention, the single-walled carbon nanotubes are used in combination with cellulose nanofibers having a specific range of sulfur introduction amount resulting from sulfate ester groups of 0.5 mmol / g or more and 3.5 mmol / g or less, so that the highly crystalline single-walled carbon nanotubes are suitably dispersed in the dispersion medium, and the resulting carbon nanotube composite exhibits high electrical conductivity. The carbon nanotube dispersion of the present invention will be described in detail below.
[0021] (Carbon Nanotubes (CNT)) The carbon nanotube dispersion of the present invention contains single-walled carbon nanotubes as carbon nanotubes.
[0022] Of the carbon nanotubes contained in the carbon nanotube dispersion of the present invention, the proportion of single-walled carbon nanotubes is preferably 95 mass % or more, more preferably 98 mass % or more, even more preferably 99 mass % or more, and particularly preferably 100 mass %.
[0023] The origin (manufacturing method) of the single-walled carbon nanotube is not limited, and the single-walled carbon nanotube may be manufactured by any manufacturing method as long as the effect of the present invention is exhibited. Examples of the manufacturing method of the single-walled carbon nanotube include an arc discharge method, a laser evaporation method, and a chemical vapor deposition method (CVD) method, and the chemical vapor deposition method (CVD) method is preferable. In particular, the single-walled carbon nanotube manufactured by the manufacturing method described in Japanese Patent No. 6479202, which is incorporated herein by reference, is preferable. The single-walled carbon nanotube contained in the CNT dispersion of the present invention may be one type or two or more types.
[0024] In the CNT dispersion of the present invention, the single-walled carbon nanotube has a G band (1590 cm ) in the Raman spectrum at an excitation wavelength of 532 nm measured by a resonance Raman scattering method. -1 around 1300 cm -1 The peak intensity ratio G / D (near the peak intensity ratio G / D of the carbon nanotube) is 30 or more. From the viewpoint of further enhancing the effects of the present invention, the peak intensity ratio G / D is preferably 35 or more, more preferably 50 or more, even more preferably 70 or more, and even more preferably 80 or more, and the upper limit can be, for example, 200 or less, 150 or less, or 120 or less. Note that "peak intensity ratio" means "height ratio." It can be said that the higher the peak intensity ratio G / D ratio of the carbon nanotube, the fewer the number of defects in the carbon nanotube structure and the higher the electrical conductivity of the carbon nanotube.
[0025] The average fiber diameter of the single-walled carbon nanotubes is preferably 0.8 nm or more, more preferably 1.0 nm or more, and even more preferably 1.5 nm or more, and is preferably 5.0 nm or less, more preferably 3.0 nm or less, and even more preferably 2.5 nm or less. When the average fiber diameter of the single-walled carbon nanotubes is 0.8 nm or more, the dispersibility tends to be good when mixed with cellulose nanofibers described later. When the average fiber diameter of the single-walled carbon nanotubes is 5.0 nm or less, the fiber diameter is not too large, and the performance of the carbon nanotubes tends to be easily exhibited. The average fiber diameter of the single-walled carbon nanotubes is a value obtained by randomly selecting 50 single-walled carbon nanotubes from the image of the SEM photograph and averaging them.
[0026] The length of the single-walled carbon nanotubes is not particularly limited, but from the viewpoint of more suitably achieving the effects of the present invention, the lower limit may be, for example, 0.001 mm or more, 0.03 mm or more, 0.06 mm or more, 0.1 mm or more, 0.5 mm or more, 1.0 mm or more, 2.0 mm or more, 5.0 mm or more, 10 mm or more, 50 mm or more, and the upper limit may be, for example, 100 mm or less. In the CNT dispersion of the present invention, the single-walled carbon nanotubes may be present in a bundled state (bundled state) by being aggregated together to have these lengths, or may be present alone to have these lengths.
[0027] The carbon purity of the single-walled carbon nanotubes is preferably 98.0% or more, more preferably 98.5% or more, and even more preferably 99.0% or more.
[0028] In the CNT dispersion of the present invention, the content of single-walled carbon nanotubes is not particularly limited as long as it does not inhibit the effects of the present invention, but from the viewpoint of more suitably exerting the effects of the present invention, the content is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, even more preferably 0.5 mass% or more, even more preferably 1.0 mass% or more, and also preferably 95.0 mass% or less, more preferably 92.0 mass% or less, even more preferably 90.0 mass% or less, 80.0 mass% or less, 60.0 mass% or less, 50.0 mass% or less, 40.0 mass% or less, 30.0 mass% or less, 20.0 mass% or less, 15.0 mass% or less, 10.0 mass% or less, etc., in terms of solid content. Here, the content of single-walled CNTs in the CNT dispersion of the present invention is the ratio of single-walled CNTs to the solid content in the dispersion. The content of single-walled CNTs can be determined by centrifuging the dispersion or the like and separating the cellulose nanofibers containing sulfate ester groups from the single-walled CNTs. When the solid content of the single-walled CNT in the CNT dispersion of the present invention satisfies the above value, the CNT composite formed using the CNT dispersion of the present invention can exhibit excellent electrical conductivity. In addition, by setting the solid content of the single-walled CNT in the CNT dispersion to the above value, the amount of expensive single-walled CNT used can be reduced, and raw material costs can be reduced. In addition, when the solid content of the single-walled CNT is 5% by mass or more, the effect of improving the electrical conductivity of the composite when cellulose nanofibers containing sulfate ester groups are added to the CNT dispersion is particularly excellent.
[0029] (Cellulose nanofiber) The cellulose nanofibers contained in the CNT dispersion of the present invention are characterized by having sulfate ester groups represented by the following formula (1), and by the amount of sulfur introduced due to the sulfate ester groups being 0.5 mmol / g or more and 3.5 mmol / g or less. The cellulose nanofibers having such characteristics can suitably disperse highly crystalline single-walled carbon nanotubes having a peak intensity ratio G / D of 30 or more in the dispersion medium.
[0030] [ka]
[0031] In the present invention, cellulose nanofibers containing sulfate ester groups can be produced by sulfurizing and defibrating raw pulp mainly composed of cellulose using a carboxylic anhydride and sulfuric acid, as shown in the examples. For sulfate esterification, known reactions such as a method using sulfamic acid and urea can be used. As the cellulose nanofibers contained in the CNT dispersion of the present invention, any cellulose nanofiber containing sulfate ester groups, for example, disclosed in Japanese Patent No. 6797215, Japanese Patent No. 7215553, Japanese Patent No. 7215554, etc., can be used as long as the amount of sulfur introduced due to sulfate ester groups is in the range of 0.5 mmol / g to 3.5 mmol / g. The amount of sulfur introduced due to sulfate ester groups in cellulose nanofibers can be expressed as the sulfur content (mmol) per 1 g of cellulose nanofibers.
[0032] In the formula (1), n is an integer of 1 to 3; M n+ is an n-valent cation, and the wavy lines are binding sites to other atoms. The cellulose nanofibers contained in the CNT dispersion of the present invention may be of only one type, or of two or more types.
[0033] In the formula (1), M n+ As for hydrogen ions (H + ), metal ions, ammonium ions, etc. When n is 2 or 3, M n+ forms ionic bonds with two or three -OSO3-.
[0034] Examples of the metal ion include an alkali metal ion, an alkaline earth metal ion, a transition metal ion, and other metal ions.
[0035] The alkali metal ion is lithium ion (Li + ), sodium ion (Na +), potassium ion (K + ), rubidium ion (Rb + ), Cesium ion (Cs + ) etc.
[0036] The alkaline earth metal ions include calcium ions (Ca 2+ ), strontium ion (Sr 2+ ) etc.
[0037] Examples of the transition metal ions include iron ions, nickel ions, palladium ions, copper ions, silver ions, etc. Examples of other metal ions include beryllium ions, magnesium ions, zinc ions, aluminum ions, etc.
[0038] The ammonium ion is NH 4+ Not only NH 4+ Ammonium ions derived from various amines in which one or more hydrogen atoms are replaced by organic groups are also included. Examples of ammonium ions include NH 4+ , quaternary ammonium cation, alkanolamine ion, pyridinium ion, etc.
[0039] M n+ is preferably a hydrogen ion, a sodium ion, a potassium ion, a calcium ion, or a quaternary ammonium cation, and more preferably a sodium ion (Na + It is particularly preferable that M of the sulfate ester group represented by the formula (1) is n+ may be only one type, or may be two or more types.
[0040] When sulfate ester groups have been introduced into cellulose nanofibers by substituting some of the OH groups in the cellulose that constitutes the fibers with sulfate ester groups represented by general formula (1), the wavy lines indicate the bonding sites to the carbon atoms previously bonded to the OH groups.
[0041] The cellulose nanofiber may have other substituents in addition to the sulfate ester group represented by formula (1). Here, when the cellulose nanofiber has a group other than the sulfate ester group represented by formula (1), i.e., other substituents, the other substituents are usually substituted with at least one of the OH groups in the cellulose constituting the cellulose nanofiber. Examples of the other substituents include, but are not limited to, anionic substituents and their salts, ester groups, ether groups, acyl groups, aldehyde groups, alkyl groups, alkylene groups, aryl groups, and combinations of two or more of these. When the other substituents are a combination of two or more types, the content ratio of each of the substituents is not limited. Among them, the other substituents are preferably anionic substituents and their salts, or acyl groups from the viewpoint of nano-dispersibility. As the anionic substituents and their salts, particularly preferred are carboxy groups, phosphate ester groups, phosphite ester groups, and xanthate groups. When the anionic substituent is in the form of a salt, sodium salts, potassium salts, and calcium salts are particularly preferred from the viewpoint of nano-dispersibility. In addition, as a particularly preferred acyl group, an acetyl group is preferred from the viewpoint of nano-dispersibility.
[0042] In the present invention, the amount of sulfur introduced into the cellulose nanofiber due to sulfate ester groups is 0.5 mmol / g or more and 3.5 mmol / g or less. The amount of sulfate ester groups introduced can be set to any appropriate value within the above range depending on the application, etc. From the viewpoint of more suitably exerting the effects of the present invention, the amount of sulfur introduced into the cellulose nanofiber due to sulfate ester groups can be expressed as the sulfur content (mmol) per 1 g of cellulose nanofiber. The amount of sulfur introduced is preferably 0.7 mmol / g or more and 3.2 mmol / g or less, and more preferably 1.0 mmol / g or more and 3.0 mmol / g or less.
[0043] The amount of sulfur incorporated into the cellulose nanofibers can be determined, for example, using an organic elemental analyzer (EA-3100, manufactured by JASCO) described in the Examples. The amount of sulfur incorporated can be adjusted, for example, by controlling the concentration of a reagent such as sulfuric acid in the solution (defibration solution) used to defibrate the pulp, the amount of pulp relative to the defibration solution, the reaction time, the reaction temperature, etc.
[0044] The cellulose nanofibers preferably have a type I crystal structure inherent to natural cellulose. Cellulose nanofibers having a type I crystal structure are highly hydrophilic and have excellent water retention and moisture retention properties. In addition, the cellulose nanofibers have excellent adsorption properties for cations, metals, inorganic particles, and the like.
[0045] The average fiber diameter of the cellulose nanofibers is not particularly limited, but from the viewpoint of more suitably exerting the effects of the present invention, it is preferably 1 nm or more, more preferably 2 nm or more, even more preferably 3 nm or more, even more preferably 5 nm or more, and also preferably 1000 nm or less, more preferably 100 nm or less, even more preferably 50 nm or less, even more preferably 20 nm or less. When the average fiber diameter of the cellulose nanofibers is 1 nm or more, the dispersibility of the carbon nanotubes tends to be more favorable. On the other hand, when the average fiber diameter of the cellulose nanofibers is 1000 nm or less, the fiber diameter of the cellulose nanofibers is not too large, and the performance of the cellulose nanofibers tends to be easily exerted. In the present invention, the average fiber diameter of the cellulose nanofibers containing sulfate ester groups can be measured by measuring the fiber width (fiber diameter (circle equivalent diameter)) and fiber length of 50 arbitrarily selected fibers using an atomic force microscope (e.g., SPM-9700HT, manufactured by Shimadzu Corporation) and taking the arithmetic average value for each. The average fiber diameter can be set within a desired range by adjusting the concentration of the reagent such as sulfuric acid, the amount of pulp relative to the reaction solution, and the reaction time.
[0046] The content of the cellulose nanofibers containing sulfate ester groups in the CNT dispersion of the present invention is, in terms of solid content, preferably 0.005% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, even more preferably 5% by mass or more, even more preferably 10% by mass or more, and also preferably 99% by mass or less, more preferably 95% by mass or less, even more preferably 90% by mass or less. Here, the content of the cellulose nanofibers containing sulfate ester groups in the CNT dispersion of the present invention is the ratio of the cellulose nanofibers containing sulfate ester groups to the solid content in the dispersion. When the content of the cellulose nanofibers containing sulfate ester groups satisfies the above value, the solid content in the CNT dispersion is not too small, and the dispersion efficiency of the single-walled CNTs is high. Also, when the content of the cellulose nanofibers satisfies the above value, stirring is smooth and the dispersion of the single-walled CNTs proceeds efficiently. The content of cellulose nanofibers containing sulfate ester groups in a CNT dispersion can be determined by centrifuging the CNT dispersion and separating the cellulose nanofibers containing sulfate ester groups from single-walled CNTs, etc.
[0047] (dispersion medium) The dispersion medium contained in the CNT dispersion of the present invention is not particularly limited as long as it can disperse the single-walled carbon nanotubes and cellulose nanofibers in the dispersion and can be subsequently removed by drying or the like to obtain a cellulose nanofiber dispersion. The dispersion medium can be selected arbitrarily depending on the application, for example, but from the viewpoint of favorably dispersing the single-walled CNTs and S-CNFs, polar solvents such as alcohols such as methanol and ethanol, ketones such as acetone and methyl ethyl ketone, and water are preferred, and among these, water is particularly preferred.
[0048] (Other ingredients) The CNT dispersion of the present invention may further contain other components in addition to the carbon nanotubes, cellulose nanofibers, and dispersion medium, as long as the effects of the present invention are not impaired. Examples of other components include dispersants, binders, antioxidants, heat stabilizers, light stabilizers, UV absorbers, pigments, colorants, foaming agents, surfactants, antistatic agents, flame retardants, lubricants, softeners, tackifiers, plasticizers, release agents, deodorizers, and fragrances.
[0049] The dispersant used in the CNT dispersion of the present invention is not particularly limited, but specific examples include polymeric dispersants such as carboxymethyl cellulose, polyvinyl butyral, polyvinyl pyrrolidone, and polyvinyl acetal, and low molecular weight dispersants such as sodium fatty acid, potassium fatty acid, sodium alkylbenzene sulfonate, sodium alkylnaphthalene sulfonate, sodium alkyl sulfate, sodium alkyl sulfonate, sodium alkyl ether sulfate, monoalkyl phosphate, sodium polyoxyethylene alkyl ether phosphate, sodium fatty acid ester sulfonate, sodium fatty acid ester sulfate, sodium fatty acid alkylose amide sulfate, sodium fatty acid amide sulfonate, polyoxyethylene alkyl ether, polyoxyethylene alkylaryl ether, alkylmethyl ammonium chloride, alkyltrimethyl ammonium chloride, dialkyldimethyl ammonium chloride, alkyldimethylbenzyl ammonium chloride, and alkylpyridinium chloride. The content of the dispersant is not particularly limited as long as it does not impair the desired conductivity, but is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and particularly preferably 50 parts by mass or more, relative to 100 parts by mass of the carbon nanotubes (A), and is preferably 500 parts by mass or less, more preferably 300 parts by mass or less, and particularly preferably 100 parts by mass or less.
[0050] The solid content of the CNT dispersion of the present invention is not particularly limited, but from the viewpoint of suitably dispersing single-walled carbon nanotubes while suitably producing carbon nanotube composites, it is preferably about 0.01 to 10.0 mass %, more preferably about 0.05 to 8.0 mass %, and even more preferably about 0.1 to 5.0 mass %.
[0051] For example, the CNT dispersion of the present invention has a binder content of preferably 50 mass % or less, more preferably 30 mass % or less, even more preferably 10 mass % or less, and particularly preferably 0 mass % (i.e., no binder is included), calculated as solid content. Examples of binders include polymers such as conductive polymers, carbodiimide-containing polymers, oxazoline group-containing polymers, and epoxy group-containing polymers. When the binder content in the CNT dispersion of the present invention satisfies the above value, the conductivity of the carbon nanotube composite can be further increased and the strength can be further strengthened.
[0052] The CNT dispersion of the present invention can be applied to a substrate such as a film and dried to form a carbon nanotube composite. That is, when the CNT dispersion of the present invention containing cellulose nanofibers having sulfate ester groups is applied (cast) to a substrate, the fibers self-organize and are regularly aligned, so that a dense free-standing film can be formed as a carbon nanotube composite without using a binder or the like.
[0053] The substrate is not particularly limited, and examples thereof include resin films such as polyethylene terephthalate film, polypropylene film, triacetyl cellulose film, nylon film, and polycarbonate film.
[0054] 2. Method for producing carbon nanotube dispersion The method for producing the carbon nanotube dispersion liquid of the present invention is not particularly limited as long as it is a method that can produce the CNT dispersion liquid described in the section "1. Carbon nanotube dispersion liquid" above. For example, the carbon nanotube dispersion liquid can be suitably produced by a method including the following steps. A process of preparing a crude dispersion by mixing carbon nanotubes, cellulose nanofibers, and a dispersion medium (crude dispersion process) A step of dispersing the crude dispersion to obtain a carbon nanotube dispersion (dispersion step)
[0055] The carbon nanotubes used in the method for producing a carbon nanotube dispersion of the present invention are single-walled carbon nanotubes, and have a peak intensity ratio G / D of G band to D band in a Raman spectrum at an excitation wavelength of 532 nm measured by a resonance Raman scattering method of 30 or more. The cellulose nanofibers have sulfate ester groups represented by the formula (1) above, and the amount of sulfur introduced due to the sulfate ester groups is 0.5 mmol / g or more and 3.5 mmol / g or less. Details of the single-walled carbon nanotubes and cellulose nanofibers, the solid content, other components, etc. are as explained in the section "1. Carbon nanotube dispersion" above.
[0056] In the method for producing a carbon nanotube dispersion of the present invention, first, in a coarse dispersion step, carbon nanotubes, cellulose nanofibers, and a dispersion medium are mixed and coarsely dispersed. The obtained coarse dispersion is then subjected to a dispersion treatment to obtain the carbon nanotube dispersion of the present invention.
[0057] In the crude dispersion step, the crude dispersion may be prepared by (1) adding S-CNF and single-walled CNT to a dispersion medium, (2) adding single-walled CNT to an S-CNF dispersion obtained by dispersing S-CNF in a dispersion medium, and optionally further adding an additional dispersion medium, (3) adding S-CNF to a single-walled CNT dispersion obtained by dispersing single-walled CNT in a dispersion medium, and optionally further adding an additional dispersion medium, or (4) mixing the S-CNF dispersion and the single-walled CNT dispersion, and optionally further adding an additional dispersion medium. Among these, from the viewpoint of dispersing S-CNF and single-walled CNT well, any of the above preparation methods (2) to (4) is preferable, and the preparation method (2) is more preferable.
[0058] The method for preparing the S-CNF dispersion liquid or the single-walled CNT dispersion liquid is not particularly limited, and they can be prepared by known methods such as a method of directly stirring the dispersion liquid using a stirrer, a dispersion method that produces a cavitation effect, or a dispersion method that produces a disintegration effect. Here, the "dispersion method that produces a cavitation effect" refers to a dispersion method that utilizes shock waves generated by the bursting of vacuum bubbles generated in a liquid due to a pressure difference that occurs in the liquid when high energy is applied to the liquid. Specific examples of dispersion treatments that produce a cavitation effect include dispersion treatments using ultrasonic waves, dispersion treatments using a jet mill, and dispersion treatments using high shear stirring.
[0059] The ultrasonic dispersion treatment of the crude dispersion liquid is not particularly limited, and can be performed using a known ultrasonic dispersion treatment device. During the ultrasonic treatment, it is preferable to cool the surroundings of the dispersion liquid to prevent damage to the S-CNF or single-walled CNT.
[0060] The dispersion treatment in the dispersion process is a process in which the bundles of carbon nanotubes in the crude dispersion are mechanically defibrated into nano-dispersions using a high-speed rotation type, colloid mill type, high-pressure type, roll mill type, ultrasonic type, or ultra-high pressure wet type micronization device (specifically, an ultrasonic dispersion treatment device, an ultra-high pressure wet type micronization device, etc.).
[0061] 3. Carbon nanotube composite The carbon nanotube composite of the present invention can be obtained by removing the dispersion medium from the carbon nanotube dispersion of the present invention.
[0062] The carbon nanotubes contained in the carbon nanotube composite of the present invention are single-walled carbon nanotubes, and have a peak intensity ratio G / D of G band to D band in a Raman spectrum at an excitation wavelength of 532 nm measured by a resonance Raman scattering method of 30 or more. The cellulose nanofibers have sulfate ester groups represented by the formula (1) above, and the amount of sulfur introduced due to the sulfate ester groups is 0.5 mmol / g or more and 3.5 mmol / g or less. Details of the single-walled carbon nanotubes and cellulose nanofibers, the solid content, other components, etc. are as explained in the section "1. Carbon nanotube dispersion liquid" above.
[0063] Methods for removing the dispersion medium from the carbon nanotube dispersion of the present invention include filtration, drying, and the like.
[0064] The shape of the carbon nanotube composite of the present invention is not particularly limited, and may be appropriately selected depending on the application. The shape of the carbon nanotube composite of the present invention may be, for example, a film. As described above, the CNT dispersion of the present invention can be applied to a substrate and dried to form a carbon nanotube composite in the form of a film. For example, a film-shaped CNT composite is preferably prepared by a method of drying the CNT dispersion directly in a container such as a petri dish, or a method of drying a coating of the CNT dispersion on a substrate. For example, a wrinkle-free film-shaped CNT composite can be obtained by drying in a thermo-hygrostat at 35 to 60°C and 40 to 60% RH, in which the dispersion medium such as water is evaporated gradually rather than suddenly.
[0065] When the carbon nanotube composite of the present invention is a film, the thickness is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 2.5 μm or more, and is preferably 10.0 μm or less, more preferably 8.0 μm or less, and even more preferably 7.5 μm or less.
[0066] The CNT composite of the present invention preferably has a conductivity of 1×103 S / cm or more, preferably 1.3×10 3 S / cm or more, and 1.5×10 3 S / cm or more, and the upper limit of the conductivity is, for example, 1×10 4 S / cm.
[0067] (Method of measuring electrical conductivity) The carbon nanotube dispersion includes a step of preparing a crude dispersion by mixing carbon nanotubes, cellulose nanofibers, and the dispersion medium using ion-exchanged water as the dispersion medium (the crude dispersion step) and a step of dispersing the crude dispersion (the dispersion treatment step). The mass ratio of carbon nanotubes to cellulose nanofibers in the carbon nanotube dispersion is 50:50, and the total concentration of these is 0.4 mass%. The obtained carbon nanotube dispersion liquid is applied onto a polyethylene terephthalate film and dried in an oven at 40°C for 5 days to obtain a composite of carbon nanotubes and cellulose nanofibers with a thickness of 5 µm. The surface resistivity (Ω / sq) and electrical conductivity (S / cm) of the resulting composite are measured using a resistivity meter.
[0068] Since the CNT composite of the present invention has high electrical conductivity, it can be suitably used, for example, as a conductive film, conductive ink, etc. For example, conductive ink is expected to be applied as wiring, transparent conductive materials, and sensors by coating or printing. EXAMPLES
[0069] The present invention will be described in more detail below with reference to examples, which are not intended to limit the scope of the present invention.
[0070] Details of the raw materials used in the examples and comparative examples are as follows.
[0071] (single-walled carbon nanotubes) Single-walled CNT-A: Single-walled carbon nanotube manufactured by Osaka Soda Co., Ltd. (product name: OStube) Outer diameter: 2.0-3.0 nm, carbon purity: 99.7%, peak intensity ratio G / D in the Raman spectrum at an excitation wavelength of 532 nm measured by resonance Raman scattering method: 80 Single-walled CNT-A': Single-walled carbon nanotube manufactured by Osaka Soda Co., Ltd. (product name: OStube) Outer diameter: 2.0-3.0 nm, carbon purity: 99.5%, peak intensity ratio G / D in the Raman spectrum at an excitation wavelength of 532 nm measured by resonance Raman scattering method: 50 Single-walled CNT-B: Single-walled carbon nanotube manufactured by Zeon Corporation (product name: ZEONANO SG101) Outer diameter: 4.0 nm, carbon purity: 99.2%, peak intensity ratio G / D in the Raman spectrum at an excitation wavelength of 532 nm measured by resonance Raman scattering method: 3
[0072] (Preparation of cellulose nanofibers) (S-CNF-1: sulfur content due to sulfate ester groups: 3.5 mmol / g) 180 g of dimethyl sulfoxide (DMSO), 20 g of acetic anhydride, and 5.6 g of sulfuric acid were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 25°C to prepare a defibration solution.
[0073] Next, 6.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 25°C to carry out a sulfate esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0074] An additional 1350 ml of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washes. After washing by centrifugation, distilled water was added and the total weight was diluted to 600 g.
[0075] Next, a uniform aqueous dispersion of cellulose nanofibers (sulfated CNF) with sulfate ester groups was obtained at a concentration of 1% by mass by mixing for 3 minutes using a mixer (G5200, manufactured by Biolomix). The aqueous dispersion of cellulose nanofibers with sulfate ester groups was evaluated using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation), and the average fiber diameter of the cellulose nanofibers with sulfate ester groups was found to be 2 nm.
[0076] The aqueous dispersion of sulfated CNF was dried for 24 hours at room temperature of 23°C to obtain solid sulfated CNF. The sulfate ester group was quantified using an organic elemental analyzer (EA-3100, manufactured by JASCO), and the degree of sulfate ester group substitution per glucose unit of cellulose was found to be 3.5 mmol / g. In addition, crystallinity was evaluated using an X-ray diffraction measurement device (LabX XRD-6000, manufactured by Shimadzu Corporation), and a cellulose type I structure was confirmed.
[0077] (S-CNF-2: sulfur content due to sulfate ester groups: 2.7 mmol / g) 180 g of dimethyl sulfoxide (DMSO), 20 g of acetic anhydride, and 4.0 g of sulfuric acid were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 25°C to prepare a defibration solution.
[0078] Next, 6.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 25°C to carry out a sulfate esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0079] An additional 1350 ml of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washes. After washing by centrifugation, distilled water was added and the total weight was diluted to 600 g.
[0080] Next, a uniform aqueous dispersion of cellulose nanofibers (sulfated CNF) with sulfate ester groups was obtained at a concentration of 1% by mass by mixing for 3 minutes using a mixer (G5200, manufactured by Biolomix). The aqueous dispersion of cellulose nanofibers with sulfate ester groups was evaluated using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation), and the average fiber diameter of the cellulose nanofibers with sulfate ester groups was found to be 6 nm.
[0081] The aqueous dispersion of sulfated CNF was dried for 24 hours at room temperature of 23°C to obtain solid sulfated CNF. The sulfate ester group was quantified using an organic elemental analyzer (EA-3100, manufactured by JASCO), and the degree of sulfate ester group substitution per glucose unit of cellulose was found to be 2.7 mmol / g. In addition, crystallinity was evaluated using an X-ray diffraction measurement device (LabX XRD-6000, manufactured by Shimadzu Corporation), and a cellulose type I structure was confirmed.
[0082] (S-CNF-3: sulfur content due to sulfate ester group 0.5mmol / g) 180 g of dimethyl sulfoxide (DMSO), 20 g of acetic anhydride, and 1.0 g of sulfuric acid were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 25°C to prepare a defibration solution.
[0083] Next, 6.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 25°C to carry out a sulfate esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0084] An additional 1350 ml of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washes. After washing by centrifugation, distilled water was added and the total weight was diluted to 600 g.
[0085] Next, a uniform aqueous dispersion of cellulose nanofibers (sulfated CNF) with sulfate ester groups was obtained at a concentration of 1% by mass by mixing for 3 minutes using a mixer (G5200, manufactured by Biolomix). The aqueous dispersion of cellulose nanofibers with sulfate ester groups was evaluated using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation), and the average fiber diameter of the cellulose nanofibers with sulfate ester groups was found to be 92 nm.
[0086] The aqueous dispersion of sulfated CNF was dried for 24 hours at room temperature of 23°C to obtain solid sulfated CNF. The sulfate ester group was quantified using an organic elemental analyzer (EA-3100, manufactured by JASCO), and the degree of sulfate ester group substitution per glucose unit of cellulose was found to be 0.5 mmol / g. In addition, crystallinity was evaluated using an X-ray diffraction measurement device (LabX XRD-6000, manufactured by Shimadzu Corporation), and a cellulose type I structure was confirmed.
[0087] (S-CNF-4: sulfur content due to sulfate ester group 0.2mmol / g) 180 g of dimethyl sulfoxide (DMSO), 10 g of acetic anhydride, and 0.5 g of sulfuric acid were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 25°C to prepare a defibration solution.
[0088] Next, 6.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 25°C to carry out a sulfate esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0089] An additional 1350 ml of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washes. After washing by centrifugation, distilled water was added and the total weight was diluted to 600 g.
[0090] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of cellulose nanofibers having sulfate ester groups (sulfate-esterified CNF) with a concentration of 1% by mass.
[0091] The aqueous dispersion of sulfated CNF was dried for 24 hours at room temperature of 23°C to obtain solid sulfated CNF. The sulfate ester group was quantified using an organic elemental analyzer (EA-3100, manufactured by JASCO), and the degree of substitution of sulfate ester group per glucose unit of cellulose was 0.2 mmol / g. In addition, crystallinity was evaluated using an X-ray diffraction measurement device (LabX XRD-6000, manufactured by Shimadzu Corporation), and a cellulose type I structure was confirmed.
[0092] <Average fiber diameter of cellulose nanofiber> The dispersion of cellulose nanofiber (S-CNF) was diluted to prepare a dispersion with an S-CNF concentration of 0.0001% by mass. The obtained dispersion was then measured for the fiber diameters of 50 randomly selected fibers using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation), and the average fiber diameter of the S-CNF was calculated by taking the arithmetic mean value.
[0093] <Crystalline structure of cellulose nanofiber> The method for measuring the crystallinity of cellulose type I of chemically modified cellulose fibers is as follows: The sample is placed in a glass cell and measured using an X-ray diffraction measuring device (LabX XRD-6000, manufactured by Shimadzu Corporation). The degree of crystallinity is calculated using the method of Segal et al., and is calculated from the diffraction intensity of the 002 plane at 2θ = 22.6° and the diffraction intensity of the amorphous part at 2θ = 18.5° using the diffraction intensity of the X-ray diffraction pattern at 2θ = 10° to 30° as the baseline, according to the following formula. Xc = (I002c - Ia) / I002c × 100 Xc = Crystallinity of cellulose type I (%) I002c: 2θ=22.6°, diffraction intensity of 002 plane Ia: 2θ=18.5°, diffraction intensity of the amorphous part.
[0094] Example 1 <Production of Carbon Nanotube Dispersion> (1) Rough dispersion treatment A mixture was obtained by putting 1,480 g of ion-exchanged water, 2.96 g of S-CNF-2 (sulfur content 2.7 mmol / g), and 0.015 g of 5 cm square sheet-shaped single-walled CNT-A (G / D: 80) into a 2 L polyethylene container. Next, the mixture was stirred for a total of 5 sets using a TK Robomics manufactured by Primix Corporation under the conditions of 5,000 rpm forward rotation for 10 seconds and 5,000 rpm reverse rotation for 10 seconds to disperse the carbon nanotubes, thereby obtaining 1,480 g of a 0.001 mass% aqueous crude dispersion of carbon nanotubes.
[0095] (2) Mechanical Distributed Processing Next, the above-mentioned crude carbon nanotube aqueous dispersion was passed once through a unit equipped with a spray nozzle with a hole diameter of 3.5 mmφ at the hose outlet, and a dispersion process was carried out using a Starburst MINI manufactured by Sugino Machine Co., Ltd. (nozzle diameter: 0.5 mmφ, 245 MPa, 10 passes) to obtain a 0.001 mass % carbon nanotube dispersion (carbon nanotube dispersion).
[0096] <Production of carbon nanotube composite> The obtained carbon nanotube dispersion was coated on a PET film using a film applicator and dried for 5 days in an oven at 40° C. Next, the dried material on the PET film was peeled off from the PET film to obtain a carbon nanotube composite having a thickness of 5 μm (cast film: CNT-A / S-CNF-2 (mass ratio) = 0.5 / 99.5).
[0097] Example 2 A 5 μm-thick carbon nanotube composite (cast film: CNT-A / S-CNF-2 (mass ratio) = 1.0 / 99.0) was obtained in the same manner as in Example 1, except that the amount of single-walled CNT-A (G / D: 80) was 0.015 g and the amount of S-CNF-2 (sulfur introduction amount 2.7 mmol / g) was 1.485 g.
[0098] Example 3 A 5 μm-thick carbon nanotube composite (cast film: CNT-A / S-CNF-2 (mass ratio) = 5.0 / 95.0) was obtained in the same manner as in Example 1, except that the amount of single-walled CNT-A (G / D: 80) was 0.03 g and the amount of S-CNF-2 (sulfur introduction amount 2.7 mmol / g) was 0.57 g.
[0099] Example 4 A 5 μm-thick carbon nanotube composite (cast film: CNT-A / S-CNF-2 (mass ratio) = 10.0 / 90.0) was obtained in the same manner as in Example 1, except that the amount of single-walled CNT-A (G / D: 80) was 0.06 g and the amount of S-CNF-2 (sulfur introduction amount 2.7 mmol / g) was 0.54 g.
[0100] Example 5 A 5 μm-thick carbon nanotube composite (cast film: CNT-A / S-CNF-2 (mass ratio) = 30.0 / 70.0) was obtained in the same manner as in Example 1, except that the amount of single-walled CNT-A (G / D: 80) was 0.12 g and the amount of S-CNF-2 (sulfur introduction amount 2.7 mmol / g) was 0.28 g.
[0101] Example 6 A 5 μm-thick carbon nanotube composite (cast film: CNT-A / S-CNF-2 (mass ratio) = 50.0 / 50.0) was obtained in the same manner as in Example 1, except that the amount of single-walled CNT-A (G / D: 80) was 0.24 g and the amount of S-CNF-2 (sulfur introduction amount 2.7 mmol / g) was 0.24 g.
[0102] Example 7 A carbon nanotube composite having a thickness of 5 μm (cast film: CNT-A / S-CNF-1 (mass ratio) = 50.0 / 50.0) was obtained in the same manner as in Example 6, except that S-CNF-1 (sulfur introduction amount: 3.5 mmol / g) was used instead of S-CNF-2 (sulfur introduction amount: 2.7 mmol / g) in Example 6.
[0103] Example 8 A carbon nanotube composite having a thickness of 5 μm (cast film: CNT-A / S-CNF-3 (mass ratio) = 50.0 / 50.0) was obtained in the same manner as in Example 6, except that S-CNF-3 (sulfur introduction amount 0.5 mmol / g) was used instead of S-CNF-2 (sulfur introduction amount 2.7 mmol / g) in Example 6.
[0104] Example 9 A carbon nanotube composite having a thickness of 5 μm (cast film: CNT-A′ / S-CNF-2 (mass ratio)=50.0 / 50.0) was obtained in the same manner as in Example 6, except that single-walled CNT-A' (G / D: 50) was used instead of single-walled CNT-A in Example 6.
[0105] Comparative Example 1 A carbon nanotube composite having a thickness of 5 μm (cast film: CNT-B / S-CNF-2 (mass ratio) = 50.0 / 50.0) was obtained in the same manner as in Example 6, except that single-walled CNT-B (G / D: 3) was used instead of single-walled CNT-A in Example 6.
[0106] Comparative Example 2 A carbon nanotube composite having a thickness of 5 μm (cast film: CNT-A / S-CNF-4 (mass ratio) = 10.0 / 90.0) was obtained in the same manner as in Example 4, except that S-CNF-4 (sulfur introduction amount: 0.2 mmol / g) was used instead of S-CNF-2 (sulfur introduction amount: 2.7 mmol / g).
[0107] Comparative Example 3 A carbon nanotube composite having a thickness of 5 μm (cast film: CNT-A / S-CNF-4 (mass ratio) = 30.0 / 70.0) was obtained in the same manner as in Example 5, except that S-CNF-4 (sulfur introduction amount 0.2 mmol / g) was used instead of S-CNF-2 (sulfur introduction amount 2.7 mmol / g) in Example 5.
[0108] [Evaluation of dispersibility of carbon nanotube dispersion liquid (carbon nanotube dispersion)] The carbon nanotube dispersions (carbon nanotube dispersions) obtained in Examples 1 to 9 and Comparative Examples 1 to 3 were visually evaluated for dispersibility according to the following evaluation criteria. [Evaluation Criteria] ○: No visible aggregates are present. x: Visible aggregates present.
[0109] [Evaluation of electrical conductivity of carbon nanotube composites] (Surface resistivity and conductivity measurements) The surface resistivity (Ω / sq) of the carbon nanotube composite was measured using Nitto Seiko Analytec's Hiresta UX (MCP-HT800) and Loresta AX (MCP-T370) under the conditions of applied voltage: 500V, measurement environment: 25℃±2℃, 45%±5%RH, and the conductivity (S / cm) was calculated. The results are shown in Table 1.
[0110] [Table 1]
[0111] From the results of the examples shown in Table 1, it can be seen that a carbon nanotube composite with high conductivity can be obtained by using cellulose nanofibers (S-CNF) having sulfate ester groups with a specific amount of sulfur introduced as a dispersant for highly crystalline carbon nanotubes with a G / D ratio of a predetermined value or more. This can be attributed to the fact that highly crystalline carbon nanotubes are well dispersed in the carbon nanotube dispersion liquid by using a specific cellulose nanofiber (S-CNF) as a dispersant.
[0112] In particular, when comparing Examples 6, 7, 8, and 9 with Comparative Example 1, it can be seen that even though the amount of single-walled CNTs in the carbon nanotube composite is a high concentration of 50 mass%, by using cellulose nanofiber (S-CNF) having sulfate ester groups with a specific range of sulfur introduction amount, highly crystalline single-walled CNTs are well dispersed, and a carbon nanotube composite (film) with extremely high electrical conductivity can be obtained. [Industrial Applicability]
[0113] The carbon nanotube composite using the carbon nanotube dispersion of the present invention can be suitably used as a conductive film and can also be used as a conductive ink. Furthermore, the conductive ink can be expected to be applied as wiring, transparent conductive materials, and sensors by coating or printing.
Claims
1. A carbon nanotube dispersion liquid comprising carbon nanotubes, cellulose nanofibers, and a dispersion medium, the carbon nanotube is a single-walled carbon nanotube, and has a peak intensity ratio G / D of a G band to a D band in a Raman spectrum at an excitation wavelength of 532 nm measured by a resonance Raman scattering method of 30 or more; The cellulose nanofiber has a sulfate ester group represented by the following formula (1), and the amount of sulfur introduced due to the sulfate ester group is 0.5 mmol / g or more and 3.5 mmol / g or less. 【Chemistry 1】 [In the formula (1), n is an integer of 1 to 3, and M n+1 is an n-valent cation, and the wavy lines are the sites of attachment to other atoms.
2. The carbon nanotube dispersion liquid according to claim 1 , wherein the cellulose nanofibers have an average fiber diameter of 1 nm or more and 1000 nm or less and have an I-type crystal structure.
3. The carbon nanotube dispersion according to claim 1 , wherein the carbon nanotubes have an average fiber diameter of 0.8 nm or more and 5.0 nm or less.
4. The carbon nanotube dispersion liquid according to claim 1 , wherein the dispersion medium is water.
5. The carbon nanotube dispersion according to claim 1 , wherein the carbon nanotube content is 0.05% by mass or more.
6. The carbon nanotube dispersion according to claim 1 , wherein the cellulose nanofiber content is 0.005% by mass or more.
7. A method for producing the carbon nanotube dispersion liquid according to claim 1 or 2, A step of preparing a crude dispersion by mixing the carbon nanotubes, the cellulose nanofibers, and the dispersion medium; a step of dispersing the crude dispersion to obtain a carbon nanotube dispersion; The method for producing a carbon nanotube dispersion liquid includes the steps of:
8. 3. A carbon nanotube composite obtained by removing the dispersion medium from the carbon nanotube dispersion liquid according to claim 1.
9. The electrical conductivity of the carbon nanotube composite obtained by the following measurement method is 1×10 3 The carbon nanotube composite has a specific surface area of 100 nm or more. (Method of measuring electrical conductivity) The carbon nanotube dispersion according to claim 1 or 2 includes a step of using ion-exchanged water as the dispersion medium, mixing the carbon nanotubes, the cellulose nanofibers, and the dispersion medium to prepare a crude dispersion, and a step of dispersing the crude dispersion. The mass ratio of the carbon nanotubes to the cellulose nanofibers in the carbon nanotube dispersion is 50:50, and the total concentration thereof is 0.4 mass%. The obtained carbon nanotube dispersion liquid is applied onto a polyethylene terephthalate film and dried in an oven at 40° C. for 5 days to obtain a composite of carbon nanotubes and cellulose nanofibers having a thickness of 5 μm. The surface resistivity (Ω / sq) and electrical conductivity (S / cm) of the resulting composite are measured using a resistivity meter.
Citation Information
Patent Citations
Spherical sulfated cellulose and production process for the same
JP2007092034A
Conductive complex
JP2013211108A
Dispersion and production method of the same, as well as composite body
JP2021057271A
Cited By
Method for preparing composite provided with catalyst material on support including carbon nanotube molded body
WO2026205248A1