Material set for producing fiber-reinforced composite material, and method for producing fiber-reinforced composite material

The material set with a 2.5 cm or more rise height of the base resin component, combined with sizing agents and fillers, addresses the impregnation challenges in fiber-reinforced composites, enhancing bending strength and reducing variations.

JP2024135939AInactive Publication Date: 2024-10-04SEKISUI CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023046857
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for impregnating interfiber portions of fiber-reinforced composite materials with matrix resin either reduce bending strength or fail to uniformly increase it, leading to variations in bending strength.

Method used

A material set comprising a base resin component and fiber bundle, where the combination ensures a rise height of the base resin component of 2.5 cm or more, achieved through specific measurement methods, including the use of sizing agents and fillers to enhance impregnation.

Benefits of technology

This configuration results in a fiber-reinforced composite material with increased bending strength and reduced variations, achieving a composite with fewer voids and improved mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135939000001_ABST
    Figure 2024135939000001_ABST
Patent Text Reader

Abstract

To provide a material set for producing a fiber-reinforced composite material which can enhance flexural strength and can suppress variation in the flexural strength, in an obtained fiber-reinforced composite material.SOLUTION: A material set for producing a fiber-reinforced composite material is a material set for producing a fiber-reinforced composite material, and is a material set of a base material resin component and a fiber bundle, wherein a combination of the base material resin component and the fiber bundle is such a combination that a rise height of the base material resin component measured by a specific measuring method is 2.5 cm or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a material set for producing a fiber-reinforced composite material. The present invention also relates to a method for producing a fiber-reinforced composite material using the material set. [Background technology]

[0002] Fiber-reinforced composites in which a matrix resin is reinforced with reinforcing fibers such as carbon fibers are known. Fiber-reinforced composites have the advantages of being lightweight yet excellent in strength, rigidity, and dimensional stability. For this reason, fiber-reinforced composites are used in a variety of applications, such as vehicles such as automobiles and aircraft, office equipment, IC trays, notebook computer housings, waterstops, and wind turbine blades, and the demand for them is increasing year by year.

[0003] Fiber-reinforced composite materials are manufactured by impregnating the spaces between fibers of a fiber bundle with a matrix resin (a base resin component). However, it is difficult to impregnate the spaces between fibers well with the base resin component. If there are spaces (voids) between the fibers that are not impregnated with the base resin component, the bending strength of the fiber-reinforced composite material decreases or the variation in bending strength increases due to these spaces.

[0004] Conventionally, methods for effectively impregnating the spaces between fibers with the matrix resin components have been known, such as using a matrix resin that has been modified to enhance its wettability with the fibers, and using an airflow to increase the spacing between the fibers, as described in Patent Document 1 below. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-172562 [Patent Document 2] JP 2016-056491 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the method of using a matrix resin that has been modified to enhance its wettability with the fibers, the impregnation of the matrix resin components into the interfiber portions can be enhanced to a certain extent, but the flexural strength of the fiber-reinforced composite material may decrease due to the modified matrix resin.

[0007] In the method of expanding the fiber spacing by using an air flow as described in Patent Document 1, it is difficult to uniformly open the entire fiber bundle, and therefore it is difficult to sufficiently increase the impregnation of the matrix resin component into the spaces between the fibers. As a result, it is not possible to sufficiently increase the bending strength of the fiber-reinforced composite material, or to sufficiently reduce the variation in bending strength.

[0008] An object of the present invention is to provide a material set for producing a fiber-reinforced composite material, which can increase the bending strength of the resulting fiber-reinforced composite material and suppress the variation in bending strength. Another object of the present invention is to provide a method for producing a fiber-reinforced composite material using the material set for producing a fiber-reinforced composite material. [Means for solving the problem]

[0009] This specification discloses the following material set for manufacturing a fiber-reinforced composite material and a method for manufacturing a fiber-reinforced composite material.

[0010] Item 1. A material set for producing a fiber-reinforced composite material, the material set being a base resin component and a fiber bundle, wherein the combination of the base resin component and the fiber bundle is such that the rise height of the base resin component measured by the following measurement method is 2.5 cm or more. A material set for producing a fiber-reinforced composite material.

[0011] Method for measuring the rise height of the base resin component: The fiber bundle is cut to obtain fiber bundle X having a length of 50 cm and 24,000 fibers. A weight of 25 g is hung from one end of the fiber bundle X, and the fiber bundle X together with the weight is immersed in the molten base resin component from the one end of the fiber bundle X to a position 5 cm toward the other end. After 24 hours or more have passed since the immersion, the distance between the top surface of the base resin component at a position away from the fiber bundle X and the top surface of the base resin component at a position in contact with the fiber bundle X is measured, and this distance is taken as the rise height of the base resin component.

[0012] Item 2. The fiber bundle includes fibers and a sizing agent attached to the outer surface of the fibers. The material set for manufacturing a fiber-reinforced composite material according to Item 1.

[0013] Item 3. The material set for producing a fiber-reinforced composite material according to Item 2, wherein the sizing agent is discretely attached to the outer surface of the fiber.

[0014] Item 4. The material set for producing a fiber-reinforced composite material according to any one of Items 1 to 3, wherein the fiber bundle includes fibers and a filler disposed between the fibers.

[0015] Item 5. The material set for producing a fiber-reinforced composite material according to any one of Items 1 to 4, wherein the fibers of the fiber bundles are carbon fibers.

[0016] Item 6. The material set for producing a fiber-reinforced composite material according to any one of Items 1 to 5, wherein the base resin component has a thermosetting resin and a curing agent.

[0017] Item 7. A method for producing a fiber-reinforced composite material using the material set for producing a fiber-reinforced composite material according to any one of items 1 to 6, comprising an impregnation step of impregnating the matrix resin component into inter-fiber portions of the fiber bundle. Effect of the Invention

[0018] The material set for producing a fiber-reinforced composite material according to the present invention is a material set for producing a fiber-reinforced composite material. The material set according to the present invention is a material set of a matrix resin component and fiber bundles. In the material set according to the present invention, the combination of the matrix resin component and the fiber bundles is such that the rise height of the matrix resin component measured by a specific measurement method is 2.5 cm or more. Since the material set according to the present invention is provided with the above configuration, the bending strength of the obtained fiber-reinforced composite material can be increased and the variation in bending strength can be suppressed. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a diagram for explaining a method for measuring the rise height of the base material resin component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described in detail below.

[0021] (Fiber-reinforced composite manufacturing material set) A material set for producing a fiber-reinforced composite material according to the present invention (hereinafter sometimes abbreviated as "material set") is a material set for producing a fiber-reinforced composite material.

[0022] The material set according to the present invention is a material set of a matrix resin component and a fiber bundle. The material set according to the present invention has a matrix resin component (first material) and a fiber bundle (second material). The material set according to the present invention is a combination of a matrix resin component and a fiber bundle.

[0023] In the material set according to the present invention, the combination of the base resin component and the fiber bundles is such that the rise height of the base resin component measured by the following measurement method is 2.5 cm or more.

[0024] Method for measuring the rise height of the base resin component: The fiber bundle is cut to obtain fiber bundle X having a length of 50 cm and 24,000 fibers. A weight of 25 g is hung from one end of the fiber bundle X, and the fiber bundle X together with the weight is immersed in the molten base resin component from the one end of the fiber bundle X to a position 5 cm toward the other end. After 24 hours or more have passed since the immersion, the distance between the top surface of the base resin component at a position away from the fiber bundle X and the top surface of the base resin component at a position in contact with the fiber bundle X is measured, and this distance is taken as the rise height of the base resin component.

[0025] The material set according to the present invention has the above-mentioned configuration, and therefore the bending strength of the resulting fiber reinforced composite material can be increased and the variation in bending strength can be suppressed. In the material set according to the present invention, the combination of the matrix resin component and the fiber bundle is such that the rise height of the matrix resin component is 2.5 cm or more, so that the matrix resin component is well impregnated into the inter-fiber portions of the fiber bundle in the impregnation step during the manufacture of the fiber reinforced composite material. Therefore, a fiber reinforced composite material with few voids can be well obtained, and therefore a fiber reinforced composite material with high bending strength and reduced variation in bending strength can be well obtained.

[0026] The method for measuring the rise height of the base resin component will be described in more detail with reference to FIG.

[0027] Fig. 1 is a diagram for explaining a method for measuring the rising height of the base resin component. Fig. 1(a) is a diagram when the measurement of the rising height of the base resin component is started (when the fiber bundle X together with the weight is immersed in the molten base resin component), and Fig. 1(b) is a diagram when the measurement of the rising height of the base resin component is completed (when 24 hours or more have passed since the fiber bundle X together with the weight is immersed in the molten base resin component).

[0028] First, the fiber bundle is cut to obtain a fiber bundle X having a length of 50 cm and 24,000 fibers. When the fiber bundle X is a carbon fiber bundle, the weight of the fiber bundle X is about 0.8 g. In FIG. 1, the fiber bundle X is indicated by the symbol X. The fiber bundle X has one end Xa and the other end Xb. The one end Xa and the other end Xb are both ends of the fiber bundle X in the longitudinal direction. A weight 5 weighing 25 g is hung from the one end Xa of the fiber bundle X, and the other end Xb of the fiber bundle X is fixed to a stand. The weight 5 is a weight with a hook. That is, the weight 5 includes a weight body and a hook. Next, the fiber bundle X from which the weight 5 is hung is immersed in the molten base resin component 1 so that the direction connecting the one end Xa and the other end Xb of the fiber bundle X is the direction of gravity. More specifically, the fiber bundle X together with the weight 5 is immersed in the molten matrix resin component 1 from one end Xa of the fiber bundle X toward the other end Xb to a position of 5 cm. In FIG. 1, L is the immersion distance of the fiber bundle X. That is, the distance indicated by L in FIG. 1 is 5 cm. Also, since the weight 5 is suspended, the fiber bundle X has a certain degree of tension. The molten matrix resin component 1 is placed in, for example, a container.

[0029] An example of a commercially available weight 5 is "Mechanical Experiment Weight (made of brass): C15-1400-01" manufactured by Narica Co., Ltd. The shape of the weight 5 is not particularly limited. In order to make the buoyancy uniform, it is preferable that the specific gravity of the weight 5 is 8.45.

[0030] Also, as a method of fixing the weight 5 to one end Xa of the fiber bundle X, a method of tying a knot in the fiber bundle and hooking the hook of the weight 5 on the knot can be given. Note that near the knot of the fiber bundle X, twisting or the like may occur in the fiber bundle X, which may impair the straightness of the fiber bundle X. Therefore, it is preferable that the distance from the upper surface of the weight body of the weight 5 to the liquid surface (upper surface) of the molten base resin component 1 is 4 cm or more.

[0031] When the matrix resin component 1 has a thermosetting resin and a curing agent, it is preferable to immerse the fiber bundle X together with the weight 5 in the matrix resin component 1 in the molten state immediately after obtaining the matrix resin component 1 in the molten state by mixing the thermosetting resin and the curing agent in the blending ratio of the thermosetting resin and the curing agent when manufacturing the fiber reinforced composite material. The blending ratio of the thermosetting resin and the curing agent when carrying out the method for measuring the rise height of the matrix resin component can be, for example, 27 parts by weight of the curing agent per 100 parts by weight of the thermosetting resin. The temperature for carrying out the method for measuring the rise height of the matrix resin component can be 25°C. When the thermosetting resin is a quick-setting resin, the evaluation can be performed using only the main agent excluding the curing agent.

[0032] In the case where the base resin component 1 is a thermoplastic resin, the method for measuring the rise height of the base resin component is carried out using a thermoplastic resin (a molten thermoplastic resin) having the same temperature as the impregnation temperature in the impregnation step in manufacturing the fiber reinforced composite material. For example, when the impregnation temperature is 250°C, the method for measuring the rise height of the base resin component is also carried out with the base resin component 1 at 250°C. In this case, when the fiber bundle X is immersed together with the weight 5 in the base resin component 1 (thermoplastic resin), the base resin component 1 may cool and harden, but the time when the hardened base resin component 1 is melted again by heating is set as the start time of the immersion. In addition, since the base resin component 1 (thermoplastic resin) may cool and harden as the liquid level rises, it is necessary to carry out the method for measuring the rise height of the base resin component in an environment with a uniform atmosphere, for example, in an oven.

[0033] The fiber bundle X together with the weight is immersed in the molten base material resin component 1 and left for 24 hours or more. At this time, the molten base material resin component 1 penetrates into the fiber bundle X due to capillary action. Also, by immersing the fiber bundle X together with the weight in the molten base material resin component 1 and leaving it for 24 hours or more, the upper surface of the base material resin component 1 at a position away from the fiber bundle X and the upper surface of the base material resin component 1 at a position in contact with the fiber bundle X reach a state of equilibrium.

[0034] After 24 hours or more have passed since the immersion, the distance H between the upper surface of the base material resin component 1 at a position away from the fiber bundle X and the upper surface of the base material resin component 1 at a position in contact with the fiber bundle X is measured, and the distance H is taken as the rise height of the base material resin component. Note that, depending on the structure of the fiber bundle X, the height of the upper surface of the base material resin component 1 at a position in contact with the fiber bundle X may not be constant. In this case, the distance H between the upper surface of the base material resin component 1 at a position away from the fiber bundle X and the maximum height position of the upper surface of the base material resin component 1 at a position in contact with the fiber bundle X is measured, and the distance H is taken as the rise height of the base material resin component.

[0035] When the molten base resin component 1 contains a thermosetting resin and a curing agent, the rise in the liquid level of the base resin component and the curing reaction proceed simultaneously, but the rise in the height of the base resin component is measured 24 hours or more after the fiber bundle X is immersed in the molten base resin component 1. However, the base resin component 1 may cure before 24 hours have passed since the fiber bundle X was immersed in the molten base resin component 1.

[0036] In order to obtain the effect of the present invention, the rise height of the base resin component is 2.5 cm or more.

[0037] The rising height of the base resin component is preferably 3.0 cm or more, more preferably 3.4 cm or more. When the rising height of the base resin component is equal to or more than the lower limit, the effect of the present invention can be more effectively exhibited. The rising height of the base resin component may be 5.0 cm or less, or 4.0 cm or less.

[0038] Examples of methods for making the rise height of the base resin component 2.5 cm or more include the following: (1) A method of using a fiber bundle opened by a filler as the fiber bundle. (2) A method of discretely attaching a sizing agent to the outer surface of the fibers of the fiber bundle. Examples of the above method (2) include (2-1) a method of partially removing the sizing agent attached to the outer surface of the fibers of the fiber bundle using an organic solvent or the like, and (2-2) a method of burning off or carbonizing the sizing agent attached to the outer surface of the fibers of the fiber bundle by heat treatment.

[0039] The material set according to the present invention will be further described below.

[0040] <Base resin component> The material set includes a base resin component, which includes a base resin and a hardener.

[0041] Examples of the base resin include thermoplastic resin and thermosetting resin. The base resin component preferably has the thermosetting resin and a curing agent, or is a thermoplastic resin, and more preferably has the thermosetting resin and a curing agent. When the base resin component has the thermosetting resin and a curing agent, the base resin component in the material set is usually in a state before the thermosetting resin and the curing agent are mixed.

[0042] Examples of the base resin include polyvinyl chloride resin, ethylene-vinyl alcohol copolymer (EVOH), polyether ether ketone resin (PEEK), polyaryl ether ketone resin (PAEK), polyether sulfone resin (PES), polyether ketone ketone resin (PEKK), thermoplastic polyimide resin (PI), polyphenylene sulfide resin (PPS), polyphthalamide resin (PPA), polyamide resin (PA), polycarbonate resin (PC), polymethyl methacrylate resin (PMMA), polypropylene resin (PP), polytetrafluoroethylene resin (PTFE), polyvinylidene fluoride resin (PVDF), polyethylene resin (PE), polyethylene terephthalate resin (PET), epoxy resin, unsaturated polyester resin, vinyl ester resin, phenolic resin, melamine resin, and polyurethane resin.

[0043] From the viewpoint of facilitating the formation of a composite with fibers and further enhancing impregnation properties, the above-mentioned base resin is preferably a thermosetting resin, more preferably an epoxy resin or a polyurethane resin, and even more preferably an epoxy resin.

[0044] As the curing agent, a conventionally known curing agent suitable for the type of thermosetting resin can be used.

[0045] <Fiber bundle> The material set has a fiber bundle. The fiber bundle includes fibers. The fiber bundle preferably includes fibers and a sizing agent attached to the outer surface of the fibers. The fiber bundle preferably includes fibers and a filler disposed between the fibers. The fiber bundle more preferably includes fibers, a sizing agent attached to the outer surface of the fibers, and a filler disposed between the fibers. Only one type of fiber bundle may be used, or two or more types may be used in combination.

[0046] The form of the fiber bundle may be unidirectional continuous fiber (UD), woven fabric, knitted fabric, etc. The knitted fabric may be NCF (non-crimp fabric), etc.

[0047] From the viewpoint of further increasing the strength of the obtained fiber-reinforced composite material, the form of the fiber bundle is preferably a unidirectional continuous fiber, a knitted fabric or a woven fabric, more preferably a woven fabric. The fiber bundle may be a fiber bundle in which a plurality of fiber bundles are laminated in the thickness direction.

[0048] <<Textile>> The fiber bundle includes a plurality of fibers. The fibers may be of one type or of two or more types in combination.

[0049] The fibers include carbon fibers, glass fibers, ceramic fibers, metal fibers, silicon carbide fibers, basalt fibers, natural fibers, aramid fibers, etc. The natural fibers include bamboo fibers, hemp fibers, etc.

[0050] From the viewpoint of further increasing the bending strength and compressive strength of the resulting fiber-reinforced composite material, it is preferable that the fibers include carbon fibers, glass fibers, or aramid fibers.

[0051] From the viewpoint of reducing the weight of the resulting fiber-reinforced composite material and further increasing the mechanical strength of the resulting fiber-reinforced composite material, the above-mentioned fiber is preferably carbon fiber or aramid fiber, and more preferably carbon fiber.

[0052] From the viewpoint of reducing the production costs of the fiber-reinforced composite material, the fibers are preferably glass fibers.

[0053] Examples of the carbon fiber include PAN-based carbon fiber and PITCH-based carbon fiber.

[0054] The fibers are preferably continuous fibers. The continuous fibers are, for example, unidirectional continuous fibers (UD; Uni Directional fibers) and fibers contained in woven fabrics, and exist continuously in the cross-sectional direction.

[0055] <<Sizing agent>> The fiber bundle preferably contains a sizing agent attached to the outer surface of the fiber. In this case, the rise height of the base resin component is easily increased, and the effect of the present invention can be more effectively achieved. The sizing agent may be used alone or in combination of two or more kinds.

[0056] Examples of the sizing agent include epoxy resins, polyamide resins, polyurethane resins, olefin resins, polyimide resins, phenol resins, polyester resins, polyvinyl alcohol resins, and polyethylene glycol resins.

[0057] The sizing agent is preferably a resin having a functional group highly reactive with the base resin. For example, when the base resin is an epoxy resin, examples of the functional group highly reactive with the base resin include an epoxy group, a hydroxyl group, an amino group, a thiol group, a carboxyl group, and a sulfoxide group. In this case, the affinity with the base resin is good, and the rise height of the base resin component is easily increased.

[0058] The sizing agent may be attached to the entire outer surface of the fiber, or may be attached to only a portion of the outer surface of the fiber.

[0059] The sizing agent is preferably attached to a part of the outer surface of the fiber, and more preferably attached discretely on the outer surface of the fiber, which makes it easier to increase the rise height of the matrix resin component.

[0060] Examples of the method for discretely attaching the sizing agent to the outer surface of the fiber include the following methods (1) and (2): (1) A method for discretely attaching the sizing agent to the outer surface of the fiber by controlling the state of attachment to the fiber surface using a resin emulsion type sizing agent, and (2) A method for heating the fiber bundle having the sizing agent attached to the entire outer surface of the fiber at a high temperature (e.g., 300 degrees or higher).

[0061] In the fiber bundle, the content of the sizing agent (the amount of sizing agent adhering to the fibers) in the total of the fibers and the sizing agent (100% by weight) is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, even more preferably 1.0% by weight or more, preferably 7.0% by weight or less, more preferably 5.0% by weight or less, and even more preferably 3.0% by weight or less.

[0062] <<Filler>> The fiber bundle preferably contains a filler disposed between the fibers. The fiber bundle containing the filler is preferably a spread fiber bundle. The fiber bundle is preferably a spread fiber bundle containing a filler. In this case, it becomes easier to increase the rise height of the base resin component, and the effect of the present invention can be more effectively exhibited. Only one type of filler may be used, or two or more types may be used in combination.

[0063] The filler is preferably disposed on the outer peripheral surface of the fiber. The filler may be disposed on the outer peripheral surface of the fiber via a sizing agent.

[0064] The filler may be organic particles (organic filler) or inorganic particles (inorganic filler).

[0065] Examples of the organic particles include thermosetting resin particles such as epoxy resin particles, phenol resin particles, melamine resin particles, urea resin particles, unsaturated polyester resin particles, and oxazine resin particles; divinylbenzene resin particles; polyolefin resin particles; polybutylene terephthalate resin particles; polyethylene terephthalate resin particles; acrylic resin particles; polycarbonate resin particles, etc. The material of the organic particles may be the same as that of the base resin.

[0066] Examples of the inorganic particles include silica particles, metal particles, carbon particles, and calcium carbonate particles. Examples of the metal particles include alumina particles, titanium oxide particles, ferrite particles, iron particles, and copper particles. Examples of the carbon particles include amorphous carbon particles and graphite particles.

[0067] The filler is preferably inorganic particles or organic particles, more preferably inorganic particles. The fiber reinforced composite material preferably contains inorganic particles or organic particles, more preferably inorganic particles. In this case, the open state of the fiber bundles is well maintained, so that the impregnation of the matrix resin component can be further improved, and therefore various physical properties such as the compressive strength of the fiber reinforced composite material can be improved in a well-balanced manner.

[0068] The filler more preferably contains silica particles, metal particles, carbon particles, calcium carbonate particles, talc particles, or organic particles, and further preferably contains silica particles, alumina particles, titanium oxide particles, carbon particles, calcium carbonate particles, talc particles, or divinylbenzene resin particles. The filler is particularly preferably silica particles. In this case, the fiber bundles are well maintained in an open state, so that the impregnation of the matrix resin component can be further improved, and therefore various physical properties such as the compressive strength of the fiber-reinforced composite can be improved in a well-balanced manner.

[0069] The shape of the filler is not particularly limited. The shape of the filler may be spherical, or may be a shape other than a spherical shape, such as a flat shape, a scale shape, or a cube shape. The shape of the filler is preferably spherical.

[0070] The average particle size of the filler is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, and preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less. When the average particle size is equal to or more than the lower limit and equal to or less than the upper limit, the fiber bundles are well maintained in an open state, so that the impregnation with the matrix resin component can be further improved, and therefore various physical properties such as the compressive strength of the fiber reinforced composite can be improved in a well-balanced manner.

[0071] The average particle size of the filler is determined from an electron microscope photograph of the cross section of the fiber bundle using image analysis software (e.g., "WinROOF" manufactured by Mitani Shoji Co., Ltd.). It may also be determined from an electron microscope photograph of the cross section of the obtained fiber reinforced composite material using image analysis software (e.g., "WinROOF" manufactured by Mitani Shoji Co., Ltd.).

[0072] The average particle size of the filler is a number average particle size, which is the arithmetic mean value of the particle sizes of the filler observed in the cross section of the fiber bundle or fiber-reinforced composite material. The particle size means the diameter of the circle equivalent of the filler observed in the cross section.

[0073] The average particle size of the filler is preferably determined from 100 or more fillers. If there are not 100 or more fillers in the obtained electron microscope photograph, it is preferable to photograph a new region with the electron microscope until the number of fillers becomes 100 or more.

[0074] The content of the filler is preferably 0.01 part by weight or more, more preferably 0.1 part by weight or more, preferably 10.5 parts by weight or less, and more preferably 5.0 parts by weight or less, relative to 100 parts by weight of the total of the fibers and the sizing agent. When the content of the filler is equal to or more than the lower limit and equal to or less than the upper limit, the fiber bundle is well maintained in an open state, so that the impregnation of the matrix resin component can be further improved, and therefore various physical properties such as the compressive strength of the fiber-reinforced composite can be improved in a well-balanced manner.

[0075] Examples of methods for obtaining the above-mentioned filler-containing fiber bundle (spread fiber bundle) include the following methods (i), (ii), and (iii).

[0076] (i) A method in which a liquid containing a sizing agent and a filler is brought into contact with the fibers (body of the fiber bundle) to adhere the filler to the outer surface of the fibers.

[0077] (ii) A method in which a sizing agent is brought into contact with the fibers (fiber bundle body), and then a liquid containing a filler is brought into contact with the fibers to which the sizing agent is attached (fiber bundle body with sizing agent), thereby adhering the filler to the outer surface of the fibers.

[0078] (iii) A method in which fibers having a sizing agent attached thereto (a fiber bundle body with a sizing agent) are prepared, and this fiber bundle body with a sizing agent is brought into contact with a liquid containing a filler to adhere the filler to the outer surface of the fiber.

[0079] The method for bringing the liquid containing the filler into contact with the fibers includes spraying, coating, immersion, and the like.

[0080] By rotating or vibrating the fibers (fiber bundle body) that have come into contact with the filler, or by handling them with a roller or the like, the liquid containing the filler spreads over the fiber surface, and the filler penetrates between the fibers, thereby obtaining a fiber bundle containing the filler (open fiber bundle).

[0081] From the viewpoint of increasing the wetting and spreading property of the filler-containing liquid on the fiber surface, the filler-containing liquid preferably contains an organic solvent. The organic solvent is not particularly limited. From the viewpoint of workability, the organic solvent preferably contains methanol, ethanol, propanol, tetrahydrofuran, or acetone. The particle-containing liquid may contain water.

[0082] In order to remove the solvent (organic solvent, water, etc.), the fibers are brought into contact with a liquid containing a filler, and then the solvent is removed by heating or drying, thereby obtaining the spread fiber bundle.

[0083] <Other ingredients> The material set may have other components (other materials) different from both the base resin component and the fiber bundles.

[0084] (Method of manufacturing fiber-reinforced composite materials) A fiber-reinforced composite material can be manufactured using the above-mentioned material set. The manufacturing method of the fiber-reinforced composite material according to the present invention includes an impregnation step of impregnating the inter-fiber portions of the fiber bundle with the matrix resin component.

[0085] The method of impregnating the inter-fiber portions of the fiber bundle with the matrix resin component is not particularly limited, and examples thereof include a method in which the molten matrix resin component is extruded into a film shape using a sheet die or the like, laminated on the fiber bundle, and then compressed while being heated, thereby impregnating the inter-fiber portions of the fiber bundle with the matrix resin component.

[0086] The melting temperature of the base resin is defined as T° C. The impregnation temperature in the impregnation step is preferably (T+20)° C. or higher, more preferably (T+40)° C. or higher, and preferably (T+150)° C. or lower, more preferably (T+100)° C. or lower. When the impregnation temperature is equal to or higher than the lower limit and equal to or lower than the upper limit, the impregnation property can be further improved, and the effects of the present invention can be more effectively exhibited.

[0087] The melting temperature (T) of the base resin can be measured by a differential scanning calorimeter (DSC).

[0088] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.

[0089] The following base resin components were prepared:

[0090] (Base resin component) Epoxy resin and its hardener (Nagase ChemteX Corporation, base resin "XNR6715", hardener "XNH6815")

[0091] The following fiber bundle materials were prepared:

[0092] (fiber) Carbon fiber 1 (Toray Industries, Inc. "T700-60E") Carbon fiber 2 with sizing agent attached (Teijin "HTS-40", sizing agent: polyethylene glycol-based sizing agent) Carbon fiber 3 with sizing agent attached (Toray Industries, Inc. "T700-50C", sizing agent: epoxy-based sizing agent)

[0093] (Sizing agent) Polyimide emulsion (MICHELMAN "HP-1632")

[0094] (Filler) Silica particles (AGC Si-Tech "Sunsphere L-31")

[0095] <Preparation of fiber bundle A> Fiber bundle A, which is a spread fiber bundle, was produced using carbon fiber 1, polyimide emulsion (sizing agent), and silica particles (filler) as follows. 2 parts by weight of polyimide emulsion and 100 parts by weight of ethanol water (ethanol content: 60% by weight) were mixed to obtain a mixed solution. 2 parts by weight of silica particles were added to the obtained mixed solution to obtain a fiber-spreading liquid. Carbon fiber 1 was passed through the fiber-spreading liquid to obtain fiber bundle A, which is a spread fiber bundle. In fiber bundle A, the polyimide resin contained in the emulsion was discretely attached on the outer surface of the carbon fiber. In addition, in fiber bundle A, the filler was arranged between the fibers.

[0096] <Preparation of fiber bundle B> Carbon fiber 2 was stored at room temperature indoors in the air for one year to obtain fiber bundle B. The amount of sizing agent attached to fiber bundle B was very small, and it was attached discretely on the outer surface of the carbon fiber.

[0097] <Preparation of fiber bundle C> Carbon fiber 3 was stored at room temperature indoors and in the air for 2 years to obtain fiber bundle C. In fiber bundle C, the sizing agent was discretely attached to the outer surface of the carbon fiber.

[0098] <Preparation of fiber bundle D> Carbon fiber 3 was heated at 350°C for 10 minutes to obtain fiber bundle D. Heating was performed in an air atmosphere using a muffle furnace. In fiber bundle D, the sizing agent was partially removed by baking and was discretely attached to the outer surface of the carbon fiber.

[0099] <Preparation of fiber bundle E> Carbon fiber 3 was designated as fiber bundle E. In fiber bundle E, the sizing agent was attached to the entire outer surface of the carbon fiber.

[0100] (Examples 1 to 4 and Comparative Example 1) (1) Material set (combination of base resin component and fiber bundle): A material set was obtained so that the combination of the base resin component and the fiber bundles was as shown in Table 1.

[0101] (2) Measurement of the rise height of the base resin component: The height of rise of the base resin component was measured according to the method described above. The weight used was a Narica "Mechanical Experiment Weight (made of brass): C15-1400-01". The base resin component was prepared in a molten state by mixing 27 parts by weight of hardener with 100 parts by weight of main agent (base resin). The height of rise of the base resin component was measured in an environment at a temperature of 25°C. The results of the height of rise of the base resin component are shown in Table 1 below.

[0102] (3) Preparation of fiber-reinforced composites: A fiber-reinforced composite material was produced by infusion molding. Specifically, the fiber-reinforced composite material was produced as follows. First, the fiber bundles were arranged so that the fibers of the fiber bundles were parallel to each other, and bagged together with a release cloth and an outer medium. After bagging, the system was evacuated using a vacuum pump, and the fiber bundles were impregnated with the base resin component. As the base resin component, a mixture of 27 parts by weight of a curing agent and 100 parts by weight of a main agent (base resin) was used. In a state where the fiber bundles were impregnated with the base resin component, the mixture was left to stand for 24 hours in an environment at a temperature of 25°C, and then left to stand for 2 hours in an oven at 80°C to cure the base resin component. After the curing was completed, the obtained fiber-reinforced composite material was taken out of the oven. The fiber volume content (Vf) of the obtained fiber-reinforced composite material is shown in Table 1.

[0103] (evaluation) (1) Bending strength and its variation of fiber-reinforced composite materials The obtained fiber reinforced composite material was cut out to obtain a fiber reinforced composite material having a size of 80 mm length × 15 mm width × 2 mm thickness in accordance with the bending test standard (JIS K7074). The bending strength of this fiber reinforced composite material was measured at 25°C in accordance with JIS K7074. The test was repeated four times, and the average value and standard deviation of the bending strength were obtained. The bending strength and its variation of the fiber reinforced composite material were evaluated according to the following criteria.

[0104] <Average bending strength of fiber-reinforced composite material> ○: Average bending strength is 800 MPa or more ×: Average bending strength is less than 800 MPa

[0105] <Bending strength variation of fiber-reinforced composite materials> ○: Standard deviation of bending strength is less than 100 MPa ×: Standard deviation of bending strength is 100 MPa or more

[0106] The configuration and results are shown in Table 1 below.

[0107] [Table 1] [Explanation of symbols]

[0108] 1…Base resin component 5…Weight (weight with hook) H…Distance (height of rise of base resin component) L…Immersion distance of fiber bundle X (5 cm) X…Fiber bundle (Fiber bundle X) Xa…One end Xb: other end

Claims

1. A material set for manufacturing a fiber-reinforced composite material, comprising: A material set of a base resin component and a fiber bundle, A material set for manufacturing a fiber-reinforced composite material, in which the combination of the base resin component and the fiber bundles is such that the rise height of the base resin component measured by the measurement method described below is 2.5 cm or more. Method for measuring the rise height of the base resin component: The fiber bundle is cut to obtain a fiber bundle X having a length of 50 cm and containing 24,000 fibers. A weight of 25 g is hung from one end of the fiber bundle X, and the fiber bundle X together with the weight is immersed in the molten base resin component up to a position 5 cm from the one end toward the other end of the fiber bundle X. After 24 hours or more have passed since the immersion, the distance between the upper surface of the base resin component at a position away from the fiber bundle X and the upper surface of the base resin component at a position in contact with the fiber bundle X is measured, and this distance is defined as the rise height of the base resin component.

2. The material set for manufacturing a fiber-reinforced composite material according to claim 1 , wherein the fiber bundle comprises fibers and a sizing agent deposited on an outer surface of the fibers.

3. The material set for manufacturing a fiber-reinforced composite material according to claim 2 , wherein the sizing agent is discretely attached on the outer surface of the fiber.

4. The material set for manufacturing a fiber-reinforced composite material according to any one of claims 1 to 3, wherein the fiber bundle includes fibers and a filler disposed between the fibers.

5. The material set for manufacturing a fiber-reinforced composite material according to any one of claims 1 to 3, wherein the fibers of the fiber bundles are carbon fibers.

6. The material set for manufacturing a fiber-reinforced composite material according to any one of claims 1 to 3, wherein the matrix resin component comprises a thermosetting resin and a curing agent.

7. A method for producing a fiber-reinforced composite material using the material set for producing a fiber-reinforced composite material according to any one of claims 1 to 3, comprising: A method for producing a fiber-reinforced composite material, comprising: an impregnation step of impregnating inter-fiber portions of the fiber bundle with the matrix resin component.

Citation Information

Patent Citations

  • Production of opened sheet and device for producing the same

    JP1999172562A

  • Fiber sheet for fiber-reinforced resin and production method of the same, and molded body using the same and production method of the molded body

    JP2016056491A