Method of producing graphite fine particle comprising film-like carbon and nitrogen-containing coating layer

By applying solution plasma treatment and heat treatment to graphite fine particles with a nitrogen-containing solvent, a carbon and nitrogen-containing coating layer is formed, addressing the challenges of controlling the coating layer's properties and improving the performance of graphite as a negative electrode in lithium ion batteries.

JP2024135990APending Publication Date: 2024-10-04TOYOTA JIDOSHA KK +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023046931
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for modifying the surface of natural graphite in lithium ion batteries face challenges in controlling the thickness, elements, and structure of the carbon-containing coating layer, making it difficult to achieve desired properties.

Method used

Applying solution plasma treatment to graphite fine particles using a solvent containing a nitrogen-containing compound followed by a heat treatment process forms a carbon and nitrogen-containing coating layer in the form of a thin film on the graphite surface.

Benefits of technology

The method enables the formation of a coating layer with desired properties on graphite fine particles, enhancing their crystallinity and conductivity, suitable for use as a negative electrode active material in lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135990000001_ABST
    Figure 2024135990000001_ABST
Patent Text Reader

Abstract

To provide means of forming a coating layer of an intended property on the surface of a graphite fine particle.SOLUTION: An embodiment of the present invention relates to a method of producing graphite fine particles each comprising film-like carbon and a nitrogen-containing coating layer, which method includes a step of applying a solution plasma treatment to graphite fine particles using a solvent including a nitrogen-containing compound to form film-like carbon and a nitrogen-containing coating layer on the surface of the graphite fine particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing graphite microparticles having a carbon- and nitrogen-containing coating layer in the form of a thin film. [Background technology]

[0002] Lithium ion batteries are widely used not only as power sources for mobile terminals such as mobile phones and smartphones, but also as power sources for electric vehicles. Various carbon materials are usually used as the negative electrode active material for lithium ion batteries. Among these carbon materials, natural graphite is most commonly used.

[0003] When natural graphite is used as a negative electrode active material of a lithium ion battery, the surface properties of the natural graphite may affect the battery performance of the lithium ion battery. However, the surface properties of natural graphite vary depending on the mine from which the natural graphite is produced. In addition, it is usually difficult to control the surface properties of natural graphite. For this reason, there has been a demand for the development of a means for modifying the surface of natural graphite.

[0004] For example, Patent Document 1 describes a method for producing a negative electrode active material, which includes a first step of coating the surfaces of particles A of a carbon material capable of absorbing and releasing lithium with a nitrogen-containing organic substance, a second step of heat-treating the particles A to form a layer having a high nitrogen content on the surfaces of the particles A, and a third step of supporting particles B made of a material capable of alloying with lithium on the surfaces of the particles A.

[0005] Patent Document 2 describes a method for producing conductive graphite, which includes a solution plasma treatment step of performing a solution plasma treatment on a solution containing graphite oxide and a nitrogen-containing compound, and a step of obtaining conductive graphite from the solution that has been subjected to the solution plasma treatment, in which the conductive graphite has a nitrogen content of 0.5% by weight or more and 15% by weight or less.

[0006] Patent Document 3 describes a method for producing a carbon-based catalyst in which carbon particles are aggregated into carbon nanofibers, in which a carbon compound containing carbon and heterogeneous elements other than carbon, hydrogen, and oxygen and having at least one of a ring structure and an unsaturated bond is mixed with carbon nanofibers, and then a solution plasma treatment is performed.

[0007] Patent Document 4 describes a carbon material including a carbon material having a graphene structure and nitrogen-doped nanocarbon covering at least a part of the surface of the carbon material. The document describes a method of polymerizing the raw material compound on the surface of the carbon material by generating plasma in a liquid containing a cyclic compound having a ring structure at least in a part thereof, the carbon material having a graphene structure, and an acid, the raw material compound being polymerized on the surface of the carbon material. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2016-221830 A [Patent Document 2] JP 2016-102034 A [Patent Document 3] International Publication No. 2017 / 135386 [Patent Document 4] JP 2019-189495 A Summary of the Invention [Problem to be solved by the invention]

[0009] As a means for modifying the surface of natural graphite, a method has been known in which tar or the like is applied to the surface of natural graphite and then dried to form a coating layer containing carbon. However, this method has the problem that it is difficult to control the thickness of the coating layer, the elements to be introduced into the coating layer, and the structure of the coating layer.

[0010] Therefore, an object of the present invention is to provide a means for forming a coating layer having desired properties on the surface of graphite particles. [Means for solving the problem]

[0011] The present inventors have investigated various means for solving the above problems. They have found that graphite fine particles having a thin-film carbon- and nitrogen-containing coating layer can be obtained by applying a solution plasma treatment to the graphite fine particles using a solvent containing a nitrogen-containing compound. Based on this finding, the present inventors have completed the present invention.

[0012] That is, the present invention includes the following aspects and embodiments. (Embodiment 1) A thin film formation step, which comprises subjecting graphite fine particles to a solution plasma treatment using a solvent containing a nitrogen-containing compound to form a thin film-type carbon and nitrogen-containing coating layer on the surface of the graphite fine particles; A method for producing graphite microparticles having a carbon and nitrogen-containing coating layer in the form of a thin film, comprising: (Embodiment 2) A heat treatment step of heat-treating the graphite microparticles obtained in the thin film formation step; 2. The method of embodiment 1, further comprising: (Embodiment 3) The method of embodiment 2, wherein the heat treatment step is carried out in the range of 400 to 600°C. (Embodiment 4) The method of any one of embodiments 1 to 3, wherein the nitrogen-containing compound is 2-pyrrolidone, aniline, pyrrolidine, 1-methylpyrrolidone, N,N,-dimethylformamide, or a mixture thereof. Effect of the Invention

[0013] The present invention makes it possible to provide a means for forming a coating layer having desired properties on the surface of graphite fine particles. [Brief description of the drawings]

[0014] [Figure 1]Transmission electron microscope (TEM) images of the coating layer formed on the surface of the graphite microparticles are shown in FIG. 1. In the figure, A is a TEM image of a carbon- and nitrogen-containing coating layer formed using an additive compound, and B is a TEM image of a carbon-containing coating layer formed using an additive compound. The dotted lines indicate the interface of the coating layer. (a), (b), and (c) indicate the measurement positions of the coating layer thickness. The scale bar in A indicates 5 nm, and the scale bar in B indicates 100 nm. [Diagram 2] TEM images of carbon- and nitrogen-containing coating layers formed on the surfaces of graphite particles using additive compounds. In the figure, A is a TEM image of untreated graphite particles, B is a TEM image of graphite particles having a carbon- and nitrogen-containing coating layer obtained in a thin film formation process, and C is a TEM image of graphite particles having a carbon- and nitrogen-containing coating layer obtained in a heat treatment process. The dotted lines indicate the boundaries of the coating layers. The scale bar indicates 5 nm. [Diagram 3] 1 shows Raman spectra of carbon- and nitrogen-containing coating layers formed on the surfaces of graphite particles using additive compounds. In the figure, A is the Raman spectrum of untreated graphite particles, B is the Raman spectrum of graphite particles having a carbon- and nitrogen-containing coating layer obtained in a thin film formation process, and C is the Raman spectrum of graphite particles having a carbon- and nitrogen-containing coating layer obtained in a heat treatment process. The horizontal axis shows the Raman shift value (cm-1), and the vertical axis shows the signal intensity. [Figure 4]1 shows Cole-Cole plots obtained by impedance measurement of batteries using untreated graphite particles, graphite particles having a carbon- and nitrogen-containing coating layer obtained in a thin film forming process, and graphite particles having a carbon- and nitrogen-containing coating layer obtained in a heat treatment process as negative electrode active materials. In the figure, the horizontal axis shows the real component of impedance, and the vertical axis shows the imaginary component of impedance. (a) is a plot of impedance measurement of a battery using untreated graphite particles as negative electrode active material, (b) is a plot of impedance measurement of a battery using graphite particles having a carbon- and nitrogen-containing coating layer obtained in a thin film forming process as negative electrode active material, and (c) is a plot of impedance measurement of a battery using graphite particles having a carbon- and nitrogen-containing coating layer obtained in a heat treatment process as negative electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Preferred embodiments of the present invention will now be described in detail.

[0016] One aspect of the present invention relates to a method for producing graphite particulates having a carbon- and nitrogen-containing coating layer in the form of a thin film.

[0017] In each embodiment of the present invention, graphite microparticles refer to graphite in the form of microparticles. Examples of graphite that is the raw material for graphite microparticles include natural graphite or artificial graphite (e.g., kish graphite, highly oriented pyrolytic graphite, or thermally expanded graphite, etc.) that is commonly used in the art. The average particle size of the graphite microparticles is usually in the range of 1 to 500 μm, and particularly in the range of 5 to 500 μm. In the case of the method of the prior art, it was known that solution plasma treatment can be applied to carbon materials of several nm scale such as carbon nanofibers (Patent Documents 3 and 4, etc.). In contrast, the method of the present embodiment can form a carbon and nitrogen-containing coating layer in the form of a thin film even when applied to graphite microparticles having an average particle size of several μm scale.

[0018] The method of this embodiment includes a thin film formation step and an optional heat treatment step. Each step will be described in detail below.

[0019] [1: Thin film formation process] The present inventors have found that a thin-film carbon- and nitrogen-containing coating layer can be formed on the surface of graphite fine particles by applying a solution plasma treatment to the graphite fine particles. Therefore, the present process includes subjecting graphite fine particles to a solution plasma treatment using a solvent containing a nitrogen-containing compound to form a thin-film carbon- and nitrogen-containing coating layer on the surface of the graphite fine particles.

[0020] In each aspect of the present invention, the "solution plasma treatment" refers to a treatment for generating plasma in a solution of a raw material mixture. A pulse voltage is applied between two electrodes arranged in a solution so as to face each other, thereby generating plasma between the two electrodes. Bubbles are generated around the generated plasma, and the bubbles exist in the solution in a state surrounding the plasma. This mechanism allows the high energy state of the plasma to be confined in the solution, promoting various chemical reactions in the surrounding gas phase, liquid phase, or the interface between them.

[0021] The solvent used in this step is preferably an aqueous solvent, more preferably water. By carrying out this step in the solvent exemplified above, the solution plasma treatment can be carried out efficiently. In addition, by carrying out this step in the solvent exemplified above, the cost required for waste liquid treatment can be reduced.

[0022] The solvent used in this step contains a nitrogen-containing compound. The nitrogen-containing compound is preferably 2-pyrrolidone, aniline, pyrrolidine, 1-methylpyrrolidone, N,N,-dimethylformamide, or a mixture thereof. By performing the solution plasma treatment in a solvent containing the nitrogen-containing compound, the nitrogen-containing compound reacts with the graphite fine particles to form a coating layer on the surface of the graphite fine particles. At this time, the solution plasma treatment causes a radical reaction between the nitrogen-containing compound and the graphite fine particles to form a thin-film-type carbon- and nitrogen-containing coating layer on the surface of the graphite fine particles. In contrast, when the solution plasma treatment is performed on the graphite fine particles in a solvent containing an organic compound such as a nitrogen-free alicyclic hydrocarbon or aromatic hydrocarbon (e.g., cyclopentanone, cyclohexanone, or benzene), a spherical agglomerate-type carbon-containing coating layer is formed. Therefore, by performing this step in a solvent containing the nitrogen-containing compound exemplified above, a thin-film-type carbon- and nitrogen-containing coating layer into which carbon atoms and nitrogen atoms derived from the nitrogen-containing compound are introduced can be formed.

[0023] The solvent used in this step may contain one or more additional components in addition to the nitrogen-containing compound. The one or more additional components may include an inorganic acid (e.g., hydrochloric acid). By containing one or more of the additional components exemplified above, the reaction by the solution plasma treatment can be promoted.

[0024] In this process, the content of the nitrogen-containing compound is preferably in the range of 0.1 to 10% by volume, more preferably in the range of 0.1 to 5% by volume, and even more preferably in the range of 0.1 to 1% by volume, based on the total volume of the solvent containing the nitrogen-containing compound. If the content of the nitrogen-containing compound is less than the lower limit, the carbon- and nitrogen-containing coating layer may not be sufficiently formed. If the content of the nitrogen-containing compound is more than the upper limit, by-products may be excessively generated. Therefore, by using the nitrogen-containing compound in the content range exemplified above, graphite microparticles having a thin-film-form carbon- and nitrogen-containing coating layer with high purity can be obtained.

[0025] In this step, the voltage of the solution plasma treatment is preferably in the range of 1 to 10 kV. The frequency of the solution plasma treatment is preferably in the range of 10 to 100 kHz. The pulse width of the solution plasma treatment is preferably in the range of 0.1 to 10 μs. The electrodes of the solution plasma treatment are preferably tungsten. The distance between the electrodes of the solution plasma treatment is preferably in the range of 0.1 to 10 mm. The time of the solution plasma treatment is preferably in the range of 1 to 60 minutes. By carrying out the solution plasma treatment under the conditions exemplified above, the reaction can be carried out efficiently.

[0026] This step may optionally include a washing step of washing the reaction product obtained by the solution plasma treatment with a washing solution, and an alkali treatment step of treating the reaction product obtained by the solution plasma treatment with an alkali. Either the washing step or the alkali treatment step may be performed, or both may be performed. In addition, the number of times and the order of the washing step and the alkali treatment step are not particularly limited.

[0027] The cleaning liquid used in the cleaning step is preferably the solvent exemplified above. The cleaning liquid preferably contains hydrogen peroxide. By cleaning the reaction product with the cleaning liquid exemplified above, it is possible to remove unreacted nitrogen-containing compounds and by-products generated by the reaction.

[0028] The alkali used in the alkali treatment step is used as a solution in the solvent exemplified above. The alkali is preferably potassium hydroxide or sodium hydroxide, more preferably potassium hydroxide. By treating the reaction product with the alkali exemplified above, by-products generated in the reaction can be removed.

[0029] By carrying out this process under the conditions described above, a thin-film carbon- and nitrogen-containing coating layer containing carbon atoms and nitrogen atoms derived from a nitrogen-containing compound can be formed on the surface of the graphite particles.

[0030] [2: Heat treatment process] The method of this embodiment may optionally include a heat treatment step, which involves heat treating the graphite particles obtained in the thin film formation step.

[0031] In this step, the temperature for heat-treating the graphite fine particles is preferably in the range of 400 to 600° C., more preferably in the range of 400 to 500° C. The time for heat-treating the graphite fine particles is preferably in the range of 1 to 5 hours, more preferably in the range of 1 to 2 hours. By carrying out the heat treatment under the conditions exemplified above, it is possible to improve the crystallinity and / or the electrical conductivity of the thin-film carbon- and nitrogen-containing coating layer.

[0032] This step is preferably carried out under an air atmosphere. By carrying out this step under an air atmosphere, the crystallinity and / or electrical conductivity of the carbon- and nitrogen-containing coating layer in the form of a thin film can be improved.

[0033] The graphite fine particles produced and / or producible by the method of this aspect have a carbon and nitrogen-containing coating layer. The carbon and nitrogen-containing coating layer is usually in the form of a thin film. The film thickness of the carbon and nitrogen-containing coating layer in the form of a thin film is usually in the range of 1 to 100 nm, for example, in the range of 1 to 50 nm, and particularly in the range of 1 to 20 nm.

[0034] As described in detail above, by the method of this aspect, graphite fine particles having a carbon and nitrogen-containing coating layer in the form of a thin film can be produced. The carbon and nitrogen-containing coating layer in the form of a thin film on the surface of the graphite fine particles obtained by the method of this aspect contains carbon atoms and nitrogen atoms. Further, the graphite fine particles obtained by the method of this aspect have high crystallinity and conductivity. Therefore, the graphite fine particles obtained by the method of this aspect can be suitably used as a negative electrode active material of a lithium ion battery. A lithium ion battery provided with the graphite fine particles obtained by the method of this aspect as a negative electrode active material can exhibit high battery characteristics.

Examples

[0035] Hereinafter, the present invention will be described more specifically using examples. However, the technical scope of the present invention is not limited to these examples.

[0036] <I: Preparation of Graphite Fine Particles Having a Coating Layer> [I-1: Thin Film Formation Step] 1000 mg of graphite microparticles were put into a solvent consisting of 1.25 mL of an additive compound, 125 mL of 1 M hydrochloric acid aqueous solution, and 30 mL of deionized water and stirred. This reaction solution was subjected to solution plasma treatment for 15 minutes under the conditions of electrode: tungsten, inter-electrode distance: 1 mm, pulse width: 1.3 μs, frequency: 45 kHz, and voltage: 2.0 kV. After the solution plasma treatment, 60 mL of 6 mass% hydrogen peroxide aqueous solution was added to the reaction solution and stirred for 6 hours. The reaction solution was filtered using a filter paper (pore size: 0.1 μm). The filtrate was washed. The obtained filtrate was dried in an oven at 60 °C. The dried filtrate was suspended in 1 M potassium hydroxide aqueous solution. The suspension was filtered using a filter paper (pore size: 11 μm). The filtrate was washed with 1 M potassium hydroxide aqueous solution. The obtained filtrate was dried in an oven at 60 °C. Thereby, graphite microparticles having a coating layer were obtained.

[0037] [I-2: Heat Treatment Step] The graphite microparticles having a coating layer obtained in the thin film forming step were heat-treated under the conditions of 500 °C for 2 hours in an air atmosphere. Thereby, graphite microparticles having a heat-treated coating layer were obtained.

[0038] [II: Evaluation of Graphite Microparticles with Coating Layer] [II-1: Morphology Observation and Raman Spectrum Analysis] The morphology of the coating layer formed on the surface of the graphite fine particles was observed using a transmission electron microscope (TEM). In addition, the Raman spectrum of the graphite fine particles was measured using a Raman spectrometer. The introduction of nitrogen atoms into the coating layer was confirmed using the D' peak in the obtained Raman spectrum as an index. The additive compounds used and the morphology of the coating layer of the graphite fine particles prepared are shown in Table 1. In the table, "○" in the "Nitrogen Atom Introduction" column indicates that nitrogen atoms were introduced into the coating layer, and "×" indicates that nitrogen atoms were not introduced into the coating layer. In the "Formation of Coating Layer" column, "○" indicates that a coating layer in the form of a thin film was formed, "△" indicates that a coating layer in the form of a mixed thin film and spherical aggregates was formed, and "×" indicates that a coating layer in the form of spherical aggregates was formed. In addition, a TEM image of the coating layer formed on the surface of the graphite fine particles is shown in Figure 1. In the figure, A is a TEM image of a carbon- and nitrogen-containing coating layer formed using an additive compound, and B is a TEM image of a carbon-containing coating layer formed using an additive compound. The dotted lines indicate the boundary surface of the coating layer. (a), (b), and (c) show the positions at which the thickness of the coating layer was measured. The scale bar in A indicates 5 nm, and the scale bar in B indicates 100 nm.

[0039] [Table 1]

[0040] As shown in Table 1 and FIG. 1A, when nitrogen-containing compounds, 2-pyrrolidone, aniline, pyrrolidine, 1-methylpyrrolidone, and DMF, were used as additive compounds, a carbon- and nitrogen-containing coating layer in the form of a thin film was formed on the surface of the graphite particles. The film thickness of this carbon- and nitrogen-containing coating layer was about 5 nm. In contrast, as shown in Table 1 and FIG. 1B, when nitrogen-free organic compounds, cyclopentanone, cyclohexanone, and benzene, were used as additive compounds, a carbon-containing coating layer was formed on the surface of the graphite particles. However, the form of the coating layer was a spherical aggregate form or a mixed form of a thin film and a spherical aggregate form. The film thickness of this carbon-containing coating layer was 108 nm at position (a), 75 nm at position (b), and 38 nm at position (c).

[0041] FIG. 2 shows TEM images of the carbon- and nitrogen-containing coating layer formed on the surface of the graphite microparticles using the additive compound. In the figure, A is a TEM image of untreated graphite microparticles, B is a TEM image of graphite microparticles having a carbon- and nitrogen-containing coating layer obtained in the thin film formation process, and C is a TEM image of graphite microparticles having a carbon- and nitrogen-containing coating layer obtained in the heat treatment process. The dotted lines indicate the interface of the coating layer. The scale bar indicates 5 nm.

[0042] As shown in Figure 2, a thin film-type carbon- and nitrogen-containing coating layer was formed on the surface of the graphite microparticles by carrying out a thin film formation process (Figure 2B). By carrying out a heat treatment process on the graphite microparticles, the crystallinity of the thin film-type carbon- and nitrogen-containing coating layer was improved (Figure 2C).

[0043] The Raman spectrum of the carbon- and nitrogen-containing coating layer formed on the surface of the graphite fine particles using the additive compound is shown in FIG. 3. In the figure, A is the Raman spectrum of untreated graphite fine particles, B is the Raman spectrum of graphite fine particles having a carbon- and nitrogen-containing coating layer obtained in the thin film formation process, and C is the Raman spectrum of graphite fine particles having a carbon- and nitrogen-containing coating layer obtained in the heat treatment process. The horizontal axis represents the Raman shift value (cm-1 ) and the vertical axis indicates signal intensity.

[0044] As shown in Figure 3, in both Raman spectra, the peak at 1600 cm -1 The G band derived from graphite was observed around 1350 cm. -1 The D band is located near 1620 cm -1 The D' band, which is derived from nitrogen atoms, was observed near the Cr-Si layer (Fig. 3B and C). This result confirmed that nitrogen atoms were introduced into the carbon- and nitrogen-containing coating layer formed on the surface of the graphite particles by the thin film formation process. In addition, the ratio of the D band peak intensity to the G band peak intensity (I D / I G ) was calculated, the I D / I G is 0.14, and the I D / I G is 0.35, and the I of the Raman spectrum of the graphite particles having a carbon- and nitrogen-containing coating layer obtained by the heat treatment process D / I G After the heat treatment process, I D / I G Since the crystallinity of the thin carbon- and nitrogen-containing coating layer was improved by performing the heat treatment process, it was confirmed that the crystallinity of the thin carbon- and nitrogen-containing coating layer was improved by performing the heat treatment process.

[0045] [II-2: Electrical conductivity of graphite particles with carbon and nitrogen-containing coating layers] A test battery (coin cell) was prepared using graphite particles having a carbon- and nitrogen-containing coating layer prepared using the additive compound as the negative electrode active material. The battery capacity, capacity retention, and impedance were measured using this battery. The reaction resistance (Rct) was calculated from the impedance measurement results. Figure 4 shows the Cole-Cole plot obtained by impedance measurement of batteries using untreated graphite particles, graphite particles having a carbon- and nitrogen-containing coating layer obtained by the thin film formation process, and graphite particles having a carbon- and nitrogen-containing coating layer obtained by the heat treatment process as the negative electrode active material. In the figure, the horizontal axis indicates the real component of the impedance, and the vertical axis indicates the imaginary component of the impedance. (a) is a plot of impedance measurement of a battery using untreated graphite microparticles as the negative electrode active material, (b) is a plot of impedance measurement of a battery using graphite microparticles having a carbon and nitrogen-containing coating layer obtained in a thin film formation process as the negative electrode active material, and (c) is a plot of impedance measurement of a battery using graphite microparticles having a carbon and nitrogen-containing coating layer obtained in a heat treatment process as the negative electrode active material.

[0046] Table 2 shows the battery performance of batteries using untreated graphite particles, graphite particles having a carbon- and nitrogen-containing coating layer obtained by the thin film formation process, and graphite particles having a carbon- and nitrogen-containing coating layer obtained by the heat treatment process as the negative electrode active material.

[0047] [Table 2]

[0048] As shown in FIG. 4 and Table 2, the battery using the graphite microparticles after the thin film forming process, on whose surface a thin film-formed carbon- and nitrogen-containing coating layer is formed, as the negative electrode active material, had a lower battery capacity and an increased reaction resistance compared to the battery using untreated graphite microparticles as the negative electrode active material. In contrast, the battery using the graphite microparticles after the heat treatment process, on whose surface a thin film-formed carbon- and nitrogen-containing coating layer is formed, had an increased battery capacity and a decreased reaction resistance compared to the battery using the graphite microparticles after the thin film forming process. From these results, it was revealed that the conductive properties of the graphite microparticles after the thin film forming process, on whose surface a thin film-formed carbon- and nitrogen-containing coating layer is formed, can be improved by carrying out the heat treatment process.

[0049] The present invention is not limited to the above-described embodiments, but includes various modified examples. For example, the above-described embodiments have been described in detail to clearly explain the present invention, and the present invention is not necessarily limited to those including all of the configurations described. In addition, it is possible to add, delete, and / or replace part of the configuration of each embodiment with other configurations.

Claims

1. a thin film forming step of performing a solution plasma treatment on the graphite particles using a solvent containing a nitrogen-containing compound to form a thin film-type carbon and nitrogen-containing coating layer on the surface of the graphite particles; A method for producing graphite microparticles having a carbon and nitrogen-containing coating layer in the form of a thin film, comprising:

2. a heat treatment step of heat-treating the graphite microparticles obtained in the thin film formation step; The method of claim 1, further comprising:

3. 3. The method of claim 2, wherein the heat treatment step is carried out in the range of 400 to 600°C.

4. 2. The method of claim 1, wherein the nitrogen-containing compound is 2-pyrrolidone, aniline, pyrrolidine, 1-methylpyrrolidone, N,N,-dimethylformamide, or a mixture thereof.

Citation Information

Patent Citations

  • Carbon material for nonaqueous electrolyte battery, electrode for nonaqueous electrolyte battery using the same, and nonaqueous electrolyte battery

    JP2004342463A

  • Manufacturing method of conductive graphite and conductive graphite

    JP2016102034A

  • Method for producing conductive graphite, and conductive film

    JP2016204184A

  • Carbon material

    JP2019189495A

  • Method for producing surface-modified nanodiamond