Glass lens and optical instrument
The glass lens design with a chamfered surface and controlled roughness addresses the challenges of miniaturization by ensuring a large outer peripheral surface area and reducing defects, improving optical performance and measurement accuracy.
Patent Information
- Application Number
- JP2023047089
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Miniaturized glass lenses face challenges in achieving high centering accuracy and sufficient outer peripheral surface area while minimizing defects such as chips and cracks, which can lead to tilting and measurement inaccuracies in optical devices.
The glass lens design features a chamfered surface with an angle between 110° and 125°, smooth transitions, and controlled surface roughness to ensure a large outer peripheral surface area with minimal chipping, using a specific molding and chamfering process to maintain precision and reduce defects.
The solution provides high-quality, small-sized glass lenses with a sufficient outer peripheral surface area and minimal defects, enhancing optical performance and measurement accuracy in optical devices.
Smart Images

Figure 2024136109000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass lens and an optical instrument. [Background technology]
[0002] When manufacturing optical elements such as glass lenses, centering may be performed on a press-molded body. The centering is performed to remove unnecessary parts such as the outer periphery of the molded body, and to align the outer diameter center axis of the optical element to be obtained with the optical axis. However, for small lenses with a lens diameter of about 1 to 5 mm, it is difficult to perform centering with high accuracy to determine the optical axis by centering, and if the centering accuracy is insufficient, the alignment between the outer diameter center axis and the optical axis becomes poor.
[0003] In response to this, a method is known in which the optically functional surface of an optical element is molded by press molding, and the outer diameter is determined by molding the outer periphery with a mold member such as a barrel mold. With this method, the outer diameter central axis of the optical element to be obtained can be precisely aligned with the optical axis. In order to align the outer diameter central axis of the lens to be obtained with the optical axis by press molding alone, it is necessary to define the lens shape by performing press molding so that each mold member of the mold contacts not only the optical surface of the lens but also the outer periphery. Patent Document 1 states that in this case, the volume of the molding material (also called a preform) used in press molding must generally match the volume of the lens to be obtained.
[0004] The molding material used in press molding can be produced, for example, by cutting a block of optical glass to a predetermined size and cold-forming it into a spherical shape by polishing it, or by separating it by dropping molten glass into a receiving mold, and preforming it (hot forming). However, in either case, it is not easy to make the molding material have a uniform volume. It tends to be difficult to maintain the volume of the molding material uniform, especially when the volume is small and the weight is low. Therefore, a chamfer is formed on the outer circumferential corner of the molding surface of the mold. The surplus volume of the molding material can escape into the gap formed between the chamfer and the inner circumferential surface of the body mold. In other words, even if there is variation in the volume of the molding material and the volume of the molding material exceeds the specified amount, the variation in the volume of the molding material can be absorbed. Furthermore, damage to the molding mold can be effectively avoided.
[0005] However, when a chamfer is provided in a molding die, irregular protrusions are formed on the lens, which can lead to problems when mounting the lens on an optical device and can cause chipping at the protruding portion.
[0006] Patent Document 1 describes a method for easily and stably producing optical elements of uniform shape with high production efficiency and high yield rate, even when there is variation in the volume of the molding material, when manufacturing small-volume optical elements with high precision that exceed the limits of volume control of the molding material. In this method of manufacturing optical elements, a molded body is molded using a mold having chamfered corners on the outer periphery of the molding surface, and then chamfering is performed to remove the upper and lower mold corners of the molded body. The chamfering of the molded body is performed using a grindstone with a recess. Even if a protrusion occurs on the upper or lower mold corners of the molded body, this protrusion is completely removed. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 4848165 Summary of the Invention [Problem to be solved by the invention]
[0008] As glass lenses become smaller, there are increasing demands for quality assurance regarding defects such as chips and cracks in glass lenses, as well as for ensuring a sufficient peripheral surface area of the lens. If the peripheral surface area of a glass lens is large, it is easier to suppress the inclination of the lens within an optical device.
[0009] In the method of Patent Document 1, both the upper die side corners and the lower die side corners of the molded body are ground, and in addition, the grinding wheel has a small chamfer angle, so it is believed that the glass lens produced by this method does not have a sufficient outer peripheral surface.
[0010] The present invention has been made in view of the above problems, and has an object to provide a high-quality, small glass lens that has a sufficient outer peripheral surface area and few defects. [Means for solving the problem]
[0011] The present disclosure provides a glass lens and an optical device having the following configurations [1] to
[11] . [1] An outer peripheral surface parallel to the optical axis; a first optical surface; and a second optical surface opposed to the first optical surface, a first flat surface on an outer circumferential side of the first optical surface; a second flat surface on an outer circumferential side of the second optical surface; A chamfered surface is provided between the first flat surface and the outer circumferential surface, In a cross section including the optical axis, the angle between the chamfered surface and the outer circumferential surface is greater than 110° and less than or equal to 125°; A surface having an arithmetic mean roughness Ra2, where Ra1 is an arithmetic mean roughness Ra1 of the chamfered surface, is provided between the outer peripheral surface and the second flat surface, such that Ra1>Ra2; A glass lens with an outer diameter of 5 mm or less. [2] The glass lens of [1], wherein the arithmetic mean roughness Ra3 of the outer peripheral surface is 0.2 μm or less. [3] The glass lens according to any one of [1] to [2], wherein the arithmetic mean roughness Ra2 is 0.2 μm or less. [4] The glass lens according to any one of [1] to [3], wherein, in at least one cross section including the optical axis, when A is the width in the optical axis direction of the chamfered surface and B is the distance between the outer circumferential surface and a line that passes through a point on the outer circumferential side on the second flat surface and forms an angle of 90° with the optical axis, B satisfies A>0.3B. [5] The glass lens according to any one of [1] to [4], wherein at least one of the first flat surface and the second flat surface is perpendicular to the optical axis. [6] The glass lens according to any one of [1] to [5], wherein the outer circumferential surface and the second flat surface are smoothly continuous with each other. [7] The glass lens according to any one of [1] to [6], wherein at least one of the first optical surface and the second optical surface is a convex lens. [8] The glass lens according to any one of [1] to [7], wherein the distance between the intersection point of the optical axis and the first optical surface and the outer diameter center axis of the outer peripheral surface, and the distance between the intersection point of the optical axis and the second optical surface and the outer diameter center axis of the outer peripheral surface are 5 μm or less. [9] Refractive index n at d line (587.6 nm) d A glass lens according to any one of [1] to [8], in which the refractive index is 1.5 or more.
[10] The glass lens according to any one of [1] to [9], wherein the glass lens has a cut surface that is circular in shape with the cut surface portion missing when viewed from the optical axis direction.
[11] An optical device comprising any one of the glass lenses [1] to
[10] . Effect of the Invention
[0012] According to the present invention, it is possible to provide a high-quality, small glass lens and optical device having a sufficient outer peripheral surface area and few defects. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a plan view of a glass lens according to an embodiment. [Diagram 2] 2 is a cross-sectional view including the optical axis of the glass lens of FIG. 1. [Diagram 3]1 is a cross-sectional view including an optical axis of a glass lens according to an embodiment. [Figure 4] FIG. 1 is a plan view of a glass lens according to an embodiment. [Diagram 5] FIG. 2 is a schematic diagram of a molding method for a precursor of the glass lens of FIG. 1. [Figure 6] FIG. 2 is a schematic diagram of a method for chamfering the glass lens of FIG. 1. [Figure 7] 1 is a cross-sectional view including an optical axis of a glass lens according to an embodiment. [Figure 8] FIG. 13 is a diagram showing the relationship between the angle of the chamfered surface and the size of the flat chipping. [Figure 9] FIG. 13 is a diagram showing the relationship between the angle of the chamfered surface and the size of side chipping. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiments of the present invention will be described. The present invention is not limited to the following embodiments, and other embodiments may also fall within the scope of the present invention as long as they correspond to the gist of the present invention. For clarity of explanation, the following description and drawings may be simplified appropriately, and the scale of each component in the drawings may differ significantly. In this specification, "parallel" does not mean strictly 0°, but means 0°±5°, preferably 0°±3°, and more preferably 0°±2°. "Perpendicular" does not mean strictly 90°, but means 90°±5°, preferably 90°±3°, and more preferably 90°±2°. The upper and lower limits of the numerical ranges in this specification can be appropriately combined.
[0015] A glass lens 10 according to this embodiment will be described with reference to FIGS. The glass lens 10 has a first optical surface 11, a second optical surface 12, a first flat surface 13, a second flat surface 14, an outer peripheral surface 15, and a chamfered surface 16. In this specification, the optical surface refers to a light entrance surface and a light exit surface. The first optical surface 11 faces the second optical surface 12. The first flat surface 13 exists on the outer circumferential side of the first optical surface 11. The second flat surface 14 exists on the outer circumferential side of the second optical surface 12. The flat surfaces can serve as reference surfaces for positioning when mounting to a device. The first flat surface 13 and the second flat surface 14 are preferably perpendicular to the optical axis. The outer peripheral surface 15 is parallel to the optical axis 17. The optical axis 17 precisely coincides with the outer diameter center axis of the outer peripheral surface 15. Specifically, the distance between the intersection point of the optical axis 17 and the first optical surface 11 and the outer diameter center axis of the outer peripheral surface 15, and the distance between the intersection point of the optical axis 17 and the second optical surface 12 and the outer diameter center axis of the outer peripheral surface 15 are preferably 5 μm or less, more preferably 3 μm or less, and further preferably 1 μm or less. The chamfered surface 16 exists between the first flat surface 13 and the outer circumferential surface 15 .
[0016] The glass lens 10 is a small lens with an outer diameter of 5 mm or less. There is no particular lower limit to the outer diameter, and it is, for example, 1 mm or more. The outer diameter can be the diameter of a circle circumscribing the outer peripheral surface 15 when the glass lens 10 is observed from the optical axis direction.
[0017] The first optical surface 11 and the second optical surface 12 have a lens surface. A lens surface is a curved surface that bends the propagation direction of light, and converges or diverges light. FIG. 2 shows a form in which both the first optical surface 11 and the second optical surface 12 are convex lenses, but the lens surfaces are not limited to convex lenses. For example, both may be concave lenses, or one may be a convex lens and the other a concave lens. In addition, the first optical surface 11 and the second optical surface 12 are not limited to a form in which both have lens surfaces. As long as at least one optical surface has a lens surface, the other optical surface does not need to have a lens surface. From the viewpoint of facilitating the handling of the glass lens 10, it is preferable that at least one of the first optical surface 11 and the second optical surface 12 is a convex lens, and it is more preferable that both are convex lenses.
[0018] The chamfered surface 16 is formed by grinding. In a cross section including the optical axis 17, the angle that the chamfered surface 16 makes with the outer peripheral surface 15 is θ. In a cross section including the optical axis 17, if the width of the chamfered surface 16 in the direction perpendicular to the optical axis 17 is constant, the smaller the angle θ, the smaller the width of the chamfered surface in the direction of the optical axis 17. Therefore, the smaller the angle θ, the larger the area of the outer peripheral surface 15. The angle θ is 125° or less, preferably 123° or less, and more preferably 120° or less. When the angle θ is within the above range, the glass lens 10 has an outer peripheral surface 15 with a sufficient area. When the glass lens 10 is placed in an optical device, the inner peripheral surface of the lens mounting portion and the outer peripheral surface 15 come into contact with each other over a sufficient area, and the inclination of the glass lens 10 is suppressed. In addition, when the angle θ is within the above range, the amount of grinding required to prepare the chamfered surface 16 is also suppressed. As a result, wear of the grinding wheel and generation of grinding waste are suppressed, and manufacturing costs are suppressed.
[0019] On the other hand, the inventors have found that when the angle θ is greater than a certain value, a glass lens with fewer large chips near the boundary between the chamfered surface and the outer circumferential surface can be obtained. When a glass lens has a large chip, the optical quality may be degraded due to scattering at the chipped area, or fragments from the chipped area may fall off inside the optical equipment, causing equipment malfunction. These adverse effects are particularly problematic for small lenses with an outer diameter of 5 mm or less, which require high quality. In addition, for small lenses, the attachment position on the optical equipment may be determined from the lens outer diameter measured by image recognition. Large chips may also lead to a decrease in the measurement accuracy of the lens outer diameter during image recognition. For these reasons, it is necessary to suppress chipping, particularly in small lenses with an outer diameter of 5 mm or less. In small lenses with an outer diameter of 5 mm or less, the diameter of the longest chipping around the chamfered surface is preferably 0.1 mm or less, more preferably 0.08 mm or less, and even more preferably 0.04 mm or less.
[0020] The angle θ of the glass lens 10 is greater than 110°, preferably greater than 115°, and more preferably greater than 118°. With the angle θ within the above range, the glass lens 10 has fewer large chips near the boundary between the chamfered surface 16 and the outer peripheral surface 15, and the adverse effects of the chipping described above are suppressed. It is believed that the occurrence of large chipping is suppressed because, as the angle θ increases, the amount of machining per unit time near the boundary between the chamfered surface 16 and the outer peripheral surface 15 decreases, reducing the load during machining.
[0021] In a cross section including the optical axis 17, the width of the chamfered surface 16 in the optical axis direction is A, and the distance between the outer circumferential surface 15 and a straight line passing through the outermost point on the second flat surface 14 and forming an angle of 90° with the optical axis is B. In at least one cross section among the cross sections including the optical axis 17, the relationship between A and B is preferably A>0.3B, more preferably A>0.5B, and even more preferably A>B. When A and B have the above relationship, a larger area of the outer circumferential surface 15 is easily ensured. Even if the value of B differs between the left and right sides of the cross section, it is sufficient that at least one of them satisfies the above-mentioned relationship. When the second flat surface 14 is at 90° to the optical axis, in a cross section including the optical axis 17, a straight line that passes through the outermost point on the second flat surface 14 and forms an angle of 90° with the optical axis includes the second flat surface 14. If the first flat surface 13 and the second flat surface 14 are not perpendicular to the optical axis, but are, for example, inclined so that the first flat surface 13 and the second flat surface 14 approach the opposing surfaces as they move toward the outer periphery, A and B will be as shown in Figure 3.
[0022] When the arithmetic mean roughness of the chamfered surface 16 is Ra1, the glass lens 10 has a surface 19 having an arithmetic mean roughness Ra2, where Ra1>Ra2, between the outer peripheral surface 15 and the second flat surface 14. Specifically, the arithmetic mean roughness Ra2 is preferably 0.2 μm or less, more preferably 0.1 μm or less, even more preferably 0.05 μm or less, and particularly preferably 0.02 μm or less. By having the surface 19 having the arithmetic mean roughness Ra2 between the outer peripheral surface 15 and the second flat surface 14, it is possible to suppress adverse effects due to light scattering on the surface between the outer peripheral surface 15 and the second flat surface 14. In the examples of FIG. 2 and FIG. 3, the surface 19 having the arithmetic mean roughness Ra2 is a surface that connects the outer peripheral surface 15 and the second flat surface 14, and is curved. 2 and 3, the above-mentioned distance B can be said to be the length (width) of the surface 19 with the arithmetic mean roughness Ra2 in the direction along the optical axis 17. However, without being limited thereto, the surface 19 with the arithmetic mean roughness Ra2 may be a part of the surface connecting the outer circumferential surface 15 and the second flat surface 14, in other words, it may be at least a part of the surface connecting the outer circumferential surface 15 and the second flat surface 14.
[0023] The arithmetic mean roughness Ra3 of the outer peripheral surface 15 is preferably 0.2 μm or less, more preferably 0.1 μm or less, and even more preferably 0.05 μm or less. When the arithmetic mean roughness Ra3 is within the above range, the adverse effects of light scattering on the outer peripheral surface 15 can be suppressed. In addition, the angle of reflected light of light incident on the outer peripheral surface 15 from within the glass lens 10 can be roughly predicted. If the angle of reflected light can be predicted, for example, the destination of the reflected light can be made outside the effective range of the lens and then painted black, thereby further suppressing the effects of reflected light on the outer peripheral surface 15.
[0024] The arithmetic mean roughness Ra is measured, for example, using a NewView6200 MICROSCOPE manufactured by Zygo, with a measurement range of 0.005 mm. 2 The average roughness Ra of the glass lens is 0.005 mm or more, and is the average value of the arithmetic mean roughness Ra measured in five areas not including the ridge line. 2 If it is difficult to secure the above measurement range, the measurement range is set to 0.005 mm.2 Less than is also fine.
[0025] From the viewpoint of suppressing the occurrence of chipping, it is preferable that the outer circumferential surface 15 and the second flat surface 14 are smoothly continuous with each other.
[0026] As shown in FIG. 4, the glass lens 10 may have a cut surface 18 that is a cut surface of the glass lens 10 that is not circular when viewed in a direction parallel to the optical axis 17. A lens having one cut surface as shown in FIG. 4 is known as a D-cut lens. The glass lens 10 may have a plurality of cut surfaces. A lens having one cut surface facing another cut surface is known as an I-cut lens. From the viewpoint of reducing the size and weight of the lens, it is preferable that the glass lens 10 has a cut surface. From the viewpoint of suppressing the occurrence of defects in the lens, it is preferable that the glass lens 10 does not have a cut surface.
[0027] From the viewpoint of making the glass lens thin, the refractive index n of the glass lens 10 at the d line (587.6 nm) is d is preferably 1.49 or more, more preferably 1.50 or more, and even more preferably 1.51 or more.
[0028] Next, we will explain the molding method of the glass lens 10. Fig. 5 is a schematic diagram showing the molding method of the glass lens precursor 24, which is the precursor of the glass lens 10. The glass lens precursor 24 is molded by press molding using a molding die 20. As shown in Fig. 5, a glass material (preform) 23 is placed on a second mold 22 that defines the second optical surface 12, the second flat surface 14, and the outer circumferential surface 15. The preform 23 is heated to a temperature equal to or higher than the glass transition point, and the preform 23 is pressed by a first mold 21 that defines the first optical surface 11 and the first flat surface 13. As a result, a glass lens precursor 24 is obtained, as shown in Fig. 5. The glass lens precursor 24 has a protrusion 27 on the peripheral edge of the first flat surface 25. The outer peripheral corners of the molding surface of the first die 21 are chamfered to prevent damage to the outer peripheral corners of the molding surface and to absorb excess volume of the preform 23 during pressing. During pressing, the preform 23 enters the gap between the chamfered portion of the first die 21 and the inner peripheral surface of the second die 22, forming the protrusion 27. The protrusion 27 is removed by chamfering through grinding because it can cause problems when mounting the glass lens precursor 24 on an optical device and can cause chipping. On the other hand, the second flat surface 26 does not have a protrusion on the peripheral edge, and does not require chamfering. This is because, in the second mold 22, the molding surface that defines the second optical surface 12 and the second flat surface 14 and the molding surface that defines the outer circumferential surface 15 are integrated. Instead of the second mold 22, a mold having a molding surface that defines the second optical surface 12 and the second flat surface 14, and a mold having a molding surface that defines the outer circumferential surface 15 may be used. In this case, it is preferable that the mold having the molding surface that defines the second optical surface 12 and the second flat surface 14 has the outer circumferential corners of the molding surface chamfered to prevent damage to the outer circumferential corners of the molding surface. However, the width of the chamfering needs to be small enough so that no protrusions are formed on the second flat surface 14.
[0029] 6 is a schematic diagram showing a method of chamfering the glass lens precursor 24. The chamfering is performed using a centering machine. As shown in FIG. 6, the glass lens precursor 24 is supported by the holder 30 with the optical axis 29 coinciding with the rotation axis of the holder 30. In addition, in a cross section including the optical axis 29 and the rotation axis 33 of the grindstone 31, the chamfering angle φ between the grindstone 32 and the outer peripheral surface 28 is greater than 110° and less than 125°. In this state, the glass lens precursor 24 is rotated while the rotated grindstone 31 is moved in the direction of the arrow in FIG. 6 to perform chamfering of the glass lens precursor 24. At this time, a coolant is supplied to prevent the glass lens and the grindstone from burning. The glass lens precursor 24 in which the protrusion 27 has been completely removed by the chamfering process and the chamfered surface has been formed corresponds to the glass lens 10. The angle θ of the glass lens 10 is equal to the chamfering angle φ. In glass lens 10 molded by the above method, the arithmetic mean roughness Ra of the surface between outer peripheral surface 15 and second flat surface 14 is usually approximately the same as or smaller than the arithmetic mean roughness Ra3 of outer peripheral surface 15. This is because the surface between outer peripheral surface 15 and second flat surface 14 is formed without coming into contact with molding die 20.
[0030] <Example> Next, the present invention will be described more specifically with reference to examples.
[0031] <Chamfering> A glass plano-concave lens (outer diameter: 4.6 mm, outer peripheral thickness: 0.4 mm, center thickness: 0.2 mm) formed by press molding was subjected to chamfering. The chamfering was performed using a centering machine (Nakamura-Tome Precision Industry Co., Ltd., LC-50) equipped with an electroplated grinding wheel (Fuji Dies Co., Ltd., outer diameter: 160 mm, grit size: SD1000) while supplying a coolant (Nikko Sangyo Co., Ltd., RIS CUT C-80H-5). Figure 7 is a cross-sectional view of the glass lens including the optical axis after chamfering. Here, the width of the chamfered surface in the direction perpendicular to the optical axis is defined as the chamfering width x. Chamfering was performed under the following conditions, and 40 glass lenses each with angles θ = 100°, 110°, 115°, 120°, and 135° were produced. Grinding wheel rotation speed: 3500 rpm Lens rotation speed: 6 rpm Machining speed: 1mm / min Chamfer width x: 0.1mm Chamfer angle φ: 100°, 110°, 115°, 120°, 135°
[0032] <Arithmetic mean roughness Ra evaluation> The arithmetic mean roughness Ra of a glass lens with θ=120° was measured using a NewView6200 MICROSCOPE manufactured by Zygo Corporation for (1) the first flat surface, (2) the second flat surface, (3) the chamfered surface, (4) the outer peripheral surface, and (5) the surface between the outer peripheral surface and the second flat surface. (1) to (4) were measured under the following conditions. IMAGE ZOOM TUBE: 0.5x Eyepiece: 50x Analyze Controls -Remove:Plane Measurement Controls -Scan length: 40μ bipolar -FDA Res:High Measurements are performed with a mask on the program to remove areas outside the measurement area, and the measurement accuracy is 0.005 mm. 2 The measurement was performed in an area not including the ridge line. The average of the measurements obtained from five points on each surface was calculated as the arithmetic mean roughness Ra. (5) is a curved surface, so Analyze Controls-Remove was set to Cylinder. Otherwise, the arithmetic mean roughness Ra was calculated under the same conditions as (1) to (4). The results are shown in Table 1.
[0033] [Table 1]
[0034] <Chipping evaluation> The chipping near the ridge between the first flat surface and the chamfered surface (hereafter, flat chipping) and the chipping near the ridge between the outer peripheral surface and the chamfered surface (hereafter, side chipping) were evaluated. The ridge between the first flat surface and the chamfered surface was observed from a direction parallel to the optical axis (arrow a in Figure 7) using a measuring microscope (Olympus, STM7), and the diameter of the longest flat chipping in one glass lens was measured as d P From the direction perpendicular to the optical axis (arrow b in Figure 7), the area near the ridge between the outer peripheral surface and the chamfered surface was observed, and the diameter of the longest side chipping in one glass lens was measured as d S obtained.
[0035] Figure 8(a) shows the d P (b) to d P Figure 9(a) shows the box plot of d obtained from 40 glass lenses for each angle θ.S (b) to d S A box plot of the above is shown.
[0036] As shown in Figure 8, d P did not change significantly depending on the angle θ. It is considered that the flat chipping is hardly affected by the angle θ when the angle θ is in the range of 100° to 135°. d S As shown in Fig. 9, for the glass lens with θ = 100° and 110°, S Particularly large side chipping of >0.1 mm occurred. Particularly large side chipping can lead to a deterioration in the optical quality of the glass lens and equipment malfunctions. In contrast, no side chipping exceeding 0.1 mm was observed in the glass lenses with θ = 115°, 120°, and 135°, and the glass lenses with θ = 120° and 135° in particular had relatively small d S was obtained. However, when θ=135°, the width of the chamfered surface in the optical axis direction in the cross section including the optical axis (chamfer width y) was approximately 0.1 mm, and the reduction in the area of the outer peripheral surface due to chamfering was large. In contrast, the chamfer widths y of the glass lenses with θ=115° and 120° were approximately 0.05 mm and 0.06 mm, respectively. Therefore, the reduction in the area of the outer peripheral surface due to chamfering was small for the glass lenses with θ=115° and 120°, and an outer peripheral surface with sufficient area was obtained. [Explanation of symbols]
[0037] 10 Glass Lens 11 First Optical Surface 12 Second Optical Surface 13 First flat surface 14 Second Flat Surface 15 Outer surface 16 Chamfered surface 17 Optical axis 18 Cut Surface 20 mold 21 First Type 22 Second Type 23 Preform 24 Glass lens precursor 25 First flat surface 26 Second Flat Surface 27 Protrusion 28 Outer surface 29 Optical axis 30 Holder 31 Grindstone 32 Grinding surface 33 Rotation axis
Claims
1. An outer peripheral surface parallel to the optical axis; a first optical surface; and a second optical surface opposed to the first optical surface, a first flat surface on an outer circumferential side of the first optical surface; a second flat surface on an outer circumferential side of the second optical surface; A chamfered surface is provided between the first flat surface and the outer circumferential surface, In a cross section including the optical axis, the angle between the chamfered surface and the outer circumferential surface is greater than 110° and less than or equal to 125°; The chamfered surface has an arithmetic mean roughness Ra1, and a surface having an arithmetic mean roughness Ra2, where Ra1>Ra2, is provided between the outer circumferential surface and the second flat surface; A glass lens having an outer diameter of 5 mm or less.
2. 2. The glass lens according to claim 1, wherein the arithmetic mean roughness Ra3 of the outer peripheral surface is 0.2 μm or less.
3. 2. The glass lens according to claim 1, wherein the arithmetic mean roughness Ra2 is 0.2 μm or less.
4. 2. The glass lens according to claim 1, wherein, in at least one cross section including the optical axis, when A is a width of the chamfered surface in the optical axis direction and B is a distance between the outer circumferential surface and a straight line that passes through a point on the outer circumferential side on the second flat surface and forms an angle of 90° with the optical axis, B satisfies A > 0.3B.
5. 2. The glass lens according to claim 1, wherein at least one of the first flat surface and the second flat surface is perpendicular to the optical axis.
6. 2. The glass lens according to claim 1, wherein the outer peripheral surface and the second flat surface are smoothly continuous with each other.
7. 2. The glass lens according to claim 1, wherein at least one of the first optical surface and the second optical surface is a convex lens.
8. 2. The glass lens according to claim 1, wherein a distance between a point of intersection of an optical axis with the first optical surface and a central axis of an outer diameter of the outer peripheral surface, and a distance between a point of intersection of the optical axis with the second optical surface and a central axis of an outer diameter of the outer peripheral surface, are 5 μm or less.
9. Refractive index n at d line (587.6 nm) d 2. The glass lens according to claim 1, wherein the refractive index is 1.5 or more.
10. 2. The glass lens according to claim 1, wherein the glass lens has a cut surface which, when viewed in the optical axis direction, has a circular shape with the cut surface portion missing.
11. An optical device comprising the glass lens according to any one of claims 1 to 10.
Citation Information
Patent Citations
Mold for forming optical element and method for forming optical element using the mold
JP1997165226A
Manufacturing method of optical device and glass lens
JP2007091569A
Optical element and method for working the same, and chamfering and grinding stone
JP2010169971A
Glass lens, and molding die for glass lens
JP2012031020A
Mold for optical element
JP2014105118A