Manufacturing method for mandrel bar and manufacturing apparatus for mandrel bar
Induction heating with precise parameter control addresses uneven hardness and toughness issues in mandrel bars, ensuring uniform quality and reducing energy consumption in mandrel bar manufacturing.
Patent Information
- Application Number
- JP2023047243
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Existing mandrel bar manufacturing methods face challenges in achieving uniform surface hardness and toughness due to temperature differences and high energy costs, particularly when using conventional heating methods like atmospheric furnaces, which can lead to uneven properties and increased energy consumption.
A method and apparatus utilizing induction heating to perform quenching and tempering heat treatments on mandrel bars, determining specific heating parameters and conditions to achieve targeted hardness and toughness without using atmospheric furnaces, employing one or multiple coils and FEM analysis for precise temperature control.
Enables uniform hardness and toughness distribution in mandrel bars, reducing energy costs and preventing uneven surface properties, thereby maintaining the quality of the mandrel bars for rolling processes.
Smart Images

Figure 2024136208000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method and an apparatus for manufacturing a mandrel bar. [Background technology]
[0002] Mandrel rolling is one of the processes for reducing the wall thickness of a tube. In this process, a mandrel bar that rolls the wall thickness from the inside of the tube is inserted into a blank tube, and both the blank tube and the mandrel bar are pulled between grooved rolls to reduce the wall thickness and elongate the tube. The grooved rolls are often installed in multiple stands with a phase difference in the tube circumferential direction so that the outer periphery of the tube can be uniformly reduced. Depending on the length of the tube to be manufactured and the number of stands, the mandrel bar, which is the inner tool, has a long shape of several meters to several tens of meters. In mandrel rolling, the wall thickness is determined by the roll gap of the grooved rolls and the diameter of the mandrel bar that rolls the tube from the inside, so a mandrel bar with high dimensional accuracy over its entire length is required. In addition, the surface of the mandrel bar is transferred to the inner surface of the tube, so good surface quality of the mandrel bar is required. After mandrel rolling, the mandrel bar is gripped at the end by a pulling device, removed from the tube, and recycled for use in mandrel rolling again.
[0003] The mandrel bar generates high contact pressure with the inner surface of the tube being rolled. In the case of hot rolling, the mandrel bar is exposed to high temperatures, and it is difficult to supply lubricant after it is inserted into the inner surface of the tube. Such harsh operating conditions cause the surface of the mandrel bar to wear due to friction. At the same time, cracks may occur on the surface of the mandrel bar due to sudden thermal contraction caused by temperature changes when the mandrel bar is removed from the inner surface of the tube. If the wear or cracks are large, they will have a negative effect on the wall thickness and inner surface quality of the tube being produced, making the mandrel bar unusable for rolling. For this reason, the mandrel bar needs to have high surface hardness and toughness.
[0004] As a method for imparting high surface hardness and toughness, for example, Patent Document 1 proposes a method in which a mandrel bar is heated by high-frequency induction heating means to harden the surface, and then the entire bar is heated to temper it. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-197112 [Patent Document 2] JP 2008-274433 A Summary of the Invention [Problem to be solved by the invention]
[0006] Here, in the method of Patent Document 1, the entire bar needs to be uniformly heated and tempered in the tempering process, and a very large atmospheric furnace is required to heat treat the entire long object such as a mandrel bar.
[0007] Furthermore, in an atmospheric furnace, when the mandrel bar is heated while placed on a hearth or skid, a temperature difference occurs between the part in contact with the hearth or skid and the part not in contact with the hearth or skid. In this case, a hardness difference occurs in the circumferential and longitudinal directions of the mandrel bar, which may cause unevenness in the surface properties of the mandrel bar. Furthermore, if the inside of the mandrel bar is sufficiently heated in a large atmospheric furnace, the energy cost increases.
[0008] To address this issue, the present inventors focused on a method of tempering heat treatment using induction heating (IH). The area of the mandrel bar that requires strength and toughness is within a range of several millimeters to several tens of millimeters from the surface, and it is believed that even with induction heating, which preferentially heats the surface, it is possible to temper the required area.
[0009] For example, Patent Document 2 proposes a method of tempering a long object such as a bar by induction heating (IH). However, in general, induction heating heats the surface preferentially, so that for solid objects with a large diameter such as mandrel bars, the radial temperature deviation becomes large, making it difficult to heat the inside. In addition, if the heating temperature is set high in order to heat the inside sufficiently, the maximum temperature reached on the surface becomes high, and there is a possibility that the desired heat treatment cannot be performed. Patent Document 2 does not propose a method of tempering the inside using induction heating. Therefore, it is difficult to temper the required range by simply applying the conventional technology such as Patent Document 2.
[0010] The present disclosure has been made in consideration of the above-described circumstances, and has an object to provide a mandrel bar manufacturing method and a mandrel bar manufacturing apparatus that are capable of performing a tempering heat treatment on a mandrel bar without using an atmospheric furnace. [Means for solving the problem]
[0011] As a result of intensive research, the inventors have found that it is possible to set a heating pattern using induction heating that allows the parts requiring strength and toughness to be heated to an appropriate strength while suppressing the maximum temperature reached on the surface. The present disclosure is based on this finding. The gist of the disclosure is as follows.
[0012] (1) A method for manufacturing a mandrel bar according to one embodiment of the present disclosure includes: A method for manufacturing a mandrel bar, comprising the steps of: subjecting a mandrel bar to a quenching heat treatment and then a tempering heat treatment, determining the hardness of the mandrel bar to be achieved after the tempering heat treatment; Determine the heating temperature, holding time and upper limit temperature for achieving the determined hardness; determining a range required to achieve the determined hardness of the mandrel bar; Determine the heat treatment conditions of induction heating so that the heating temperature and holding time are achieved within the range required to achieve the determined hardness, and the upper limit temperature is not exceeded; The mandrel bar is subjected to a tempering heat treatment under the determined heat treatment conditions.
[0013] (2) As an embodiment of the present disclosure, in (1), The induction heater uses a coil to heat the mandrel bar.
[0014] (3) As an embodiment of the present disclosure, in (1), The induction heater uses multiple coils to heat the mandrel bar.
[0015] (4) As an embodiment of the present disclosure, in any one of (1) to (3), The heating temperature, the holding time and the upper limit temperature are determined based on data from an experiment using a steel piece having the same chemical composition as the mandrel bar.
[0016] (5) As an embodiment of the present disclosure, in any one of (1) to (4), The heat treatment conditions are determined based on temperature calculations using FEM coupled with electromagnetic field-thermal conduction analysis.
[0017] (6) An apparatus for manufacturing a mandrel bar according to an embodiment of the present disclosure, A mandrel bar manufacturing apparatus for manufacturing a mandrel bar by subjecting the mandrel bar to a quenching heat treatment and then a tempering heat treatment, a first determination unit for determining a hardness of the mandrel bar to be achieved after the tempering heat treatment; A second determination unit that determines a heating temperature, a holding time, and an upper limit temperature for achieving the determined hardness; a third determination unit that determines a range in which the determined hardness of the mandrel bar needs to be achieved; A fourth determination unit determines heat treatment conditions for induction heating that achieve the heating temperature and holding time within a range required to achieve the determined hardness and do not exceed an upper limit temperature; and a tempering heat treatment execution unit that performs a tempering heat treatment on the mandrel bar under the determined heat treatment conditions. Effect of the Invention
[0018] According to the present disclosure, there is provided a mandrel bar manufacturing method and a mandrel bar manufacturing apparatus that are capable of performing a tempering heat treatment on a mandrel bar without using an atmospheric furnace. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a diagram for explaining a tempering heat treatment by induction heating in an embodiment of the present disclosure in the case where one coil is used. [Diagram 2] FIG. 2 is a diagram for explaining a method for determining heat treatment conditions using the present disclosure. [Diagram 3] FIG. 3 is a diagram showing an example of the results of the experiment. [Figure 4] FIG. 4 is a diagram for explaining a form of tempering heat treatment by induction heating in an embodiment of the present disclosure when a plurality of coils are used. [Diagram 5] FIG. 5 is a diagram showing the temperature calculation results in the first embodiment. [Figure 6] FIG. 6 is a diagram showing the temperature calculation results in the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, a mandrel bar manufacturing method and a mandrel bar manufacturing apparatus according to an embodiment of the present disclosure will be described with reference to the drawings.
[0021] The mandrel bar, which is the target of manufacture by the mandrel bar manufacturing method and the mandrel bar manufacturing apparatus according to the present embodiment, is an inner tool used in the mandrel rolling process. Hot work tool steel such as SKD6 or SKD61 specified in JIS is generally used as the steel type of material for manufacturing the mandrel bar. The mandrel bar is manufactured by processing to a predetermined dimension and then undergoing heat treatments of quenching and tempering (initial manufacture). The mandrel bar is used in the mandrel rolling process in the manufacture of steel pipes and the like, and after use, is subjected to annealing heat treatment, cut, and manufactured again (remanufacturing). The remanufactured mandrel bar is used again in the mandrel rolling process. The mandrel bar manufacturing method and the mandrel bar manufacturing apparatus according to the present embodiment perform the above initial manufacture or remanufacturing.
[0022] Here, the surface hardness of the mandrel bar after the heat treatment of quenching is about HV550 to 750 in Vickers hardness. The surface hardness is the hardness in the range of about 0 to 25 mm in the radial direction from the surface (outer surface) of the mandrel bar. Generally, hardening of tool steel is performed by induction heating, and hardening of mandrel bars in initial manufacture and remanufacturing is also performed by induction heating. In induction heating, the surface is mainly heated. Therefore, it is the vicinity of the surface that increases in hardness by the heat treatment of quenching.
[0023] <Tempering heat treatment> The mandrel bar manufacturing apparatus according to this embodiment performs a tempering heat treatment by induction heating on the mandrel bar after the quenching heat treatment.
[0024] In order to prevent harmful cracks from occurring in the mandrel bar as described above, it is effective to impart high toughness to the mandrel bar by tempering heat treatment. The range to be toughened is preferably 8 mm or more from the surface, more preferably 10 mm or more. In addition, in a Charpy impact test using a half-size test piece specified in JIS Z 2242:2018 taken from the above range, it is preferable that the mandrel bar has a toughness value of 4 J or more, more preferably 16 J or more.
[0025] FIG. 1 is a diagram for explaining a form of tempering heat treatment by induction heating in the case where one coil 2 is used. The coil 2 is a heating coil for induction heating that heats the mandrel bar 1. The dimensions of the mandrel bar 1 are not particularly limited, but as an example, the diameter may be about 50 mm to 400 mm and the length may be about 0.4 m to 100.0 m. The dimensions of the coil 2 are also not particularly limited, but since the mandrel bar 1 passes through the coil 2, the inner diameter of the coil 2 is set to be larger than the outer diameter of the mandrel bar 1. The heating frequency of the induction heating is not particularly limited, but in order to efficiently heat the surface of the mandrel bar 1, it is preferable that the frequency is 200 Hz or more, and more preferably 400 Hz or more.
[0026] <Transport> In order to perform the tempering heat treatment over the entire length of the mandrel bar 1, the conveying device 3 passes the mandrel bar 1 through the coil 2. The form of conveyance is not limited. For example, the conveying device 3 may convey the mandrel bar 1 by pinching it between pinch rolls and rotating the pinch rolls. Alternatively, the conveying device 3 may move the coil 2 along the longitudinal direction of the mandrel bar 1 without conveying the mandrel bar 1.
[0027] FIG. 2 is a diagram for explaining a method for determining heat treatment conditions (conditions for induction heating in tempering heat treatment). First, the hardness to be achieved after tempering heat treatment is determined, and the necessary temperature and time conditions are determined based on experiments. Next, using these temperature and time conditions, heat treatment conditions for achieving the hardness of the mandrel bar 1 within the required range are calculated. Next, the mandrel bar 1 is subjected to tempering annealing treatment under the determined heat treatment conditions. Each item will be described in detail below.
[0028] <Determination of hardness> First, as described above, the hardness after tempering heat treatment to be achieved is determined. The hardness after tempering heat treatment to be achieved is set as a target hardness that provides sufficient wear resistance of the bar during rolling, for example.
[0029] <Determining temperature, time and upper limit> The temperature and time conditions necessary to achieve the determined hardness after tempering are obtained by an experiment. The experiment may be to subject the same material as the mandrel bar 1 to be cut to tempering and investigate the hardness.
[0030] Here, the inventors have conducted extensive research and found that heating with a certain or higher tempering parameter is necessary to reduce the hardness based on the hardness after quenching heat treatment. It has also been found that if the heating temperature is too high or the holding time is too long, the hardness will be reduced too much. Here, the lowest heating temperature value among the heating conditions under which the hardness is reduced too much obtained by experiment may be used as the upper limit temperature for preventing the material hardness from being reduced too much. In this way, the heating temperature, holding time, and upper limit temperature for achieving the target hardness are determined by experiment. Here, in the experiment, the condition for a long holding time is preferably 60 seconds or more, and more preferably 100 seconds or more. The condition for a short holding time is preferably 20 seconds or less, and more preferably 10 seconds or less.
[0031] FIG. 3 is a diagram showing an example of the results of an experiment. The vertical axis indicates the heating temperature (°C). The horizontal axis indicates the holding time (seconds). "◯" indicates that the Vickers hardness is HV400 to 550. "×" indicates that the Vickers hardness is greater than HV550. "△" indicates that the Vickers hardness is less than HV400. In the example of FIG. 3, it is shown that heating with a tempering parameter of 15400 or more is effective for reducing the hardness. In addition, among the heating conditions obtained by the experiment that cause the hardness to drop too much, the lowest heating temperature value is 800°C, and it is shown that it is effective to use 800°C as the upper limit temperature to prevent the material hardness from dropping too much. Here, the heating conditions that cause the hardness to drop too much are the conditions that are "△", which indicates that the Vickers hardness is less than HV400. The tempering parameter (TP) is calculated by the following formula.
[0032] TP=(Temp+273)×(20+log(Time / 3600))
[0033] Here, Temp is the heating temperature [°C], and Time is the holding time [seconds].
[0034] <Determining the range of hardness that needs to be achieved> The range in which the hardness of the mandrel bar 1 must be achieved is determined. For this range, the hardness must be brought within a target range by tempering heat treatment. The range in which the hardness of the mandrel bar 1 must be achieved is determined according to the required specifications, for example, as a range of 0 to 10 mm in the radial direction from the outer surface.
[0035] <Determining heat treatment conditions> The heat treatment conditions for induction heating are determined so that the heating temperature and holding time are achieved within the entire range in which hardness needs to be achieved, and the upper limit temperature is not exceeded.
[0036] Due to the characteristics of induction heating, the surface is heated preferentially. Therefore, the heat treatment conditions of induction heating are determined so that the innermost position of the range in which hardness needs to be achieved achieves the determined heating temperature and holding time. Here, if the determined heating temperature is achieved at the innermost position, the temperature will be higher at positions radially outward from that position. Therefore, the heat treatment conditions of induction heating are determined so that the maximum temperature reached at the surface position where the temperature is highest does not exceed the upper limit temperature.
[0037] Here, in order to achieve the above heating temperature and holding time, the conveying speed of the mandrel bar 1 may be determined as the heat treatment conditions in addition to the induction heating output. In determining the induction heating output, a heat transfer calculation may be performed based on the temperature history of the mandrel bar 1. For example, the calculation may be performed using a finite element method (FEM) that couples an electromagnetic field-thermal conduction analysis. The induction heating output and the conveying speed of the mandrel bar 1 are determined by the calculation so that the previously determined heating temperature and holding time are achieved and the upper limit temperature is not exceeded. Then, a tempering heat treatment of the mandrel bar 1 is performed under the determined heat treatment conditions.
[0038] Referring again to FIG. 1 , an exit thermometer 4 for measuring the temperature of the mandrel bar 1 may be provided on the exit side of the coil 2. In the tempering heat treatment of the mandrel bar 1, the output of the coil 2 may be adjusted so that the surface temperature of the mandrel bar 1 on the exit side of the coil 2 follows the calculation when determining the heat treatment conditions. Also, an entry thermometer 5 for measuring the temperature of the mandrel bar 1 may be provided on the entry side of the coil 2. The output of the coil 2 may be adjusted so that the surface temperature of the mandrel bar 1 on the entry side of the coil 2 follows the calculation when determining the heat treatment conditions. Here, the exit thermometer 4 and the entry thermometer 5 may be non-contact measuring devices such as radiation thermometers, or may be contact thermometers.
[0039] <Multiple coil configuration> Fig. 4 is a diagram for explaining a form of tempering heat treatment by induction heating when there are multiple coils 2. By arranging multiple coils 2 at a distance (coil-to-coil distance) as shown in Fig. 4 and heating them, it is possible to reduce the radial temperature deviation of the mandrel bar 1, which is a solid object with a large diameter. This is because the temperature distribution becomes smaller due to the radial heat transfer of the mandrel bar 1 after it is heated by the first coil 2 (the coil 2 on the upstream side in the conveying direction) and before it is heated by the second coil 2 (the coil 2 on the downstream side in the conveying direction). There may be three or more coils 2.
[0040] An exit thermometer 4 for measuring the temperature of the mandrel bar 1 may be provided on the exit side of the second coil 2. In the tempering heat treatment of the mandrel bar 1, the output of the coil 2 may be adjusted so that the surface temperature of the mandrel bar 1 on the exit side of the second coil 2 follows the calculation when determining the heat treatment conditions. Also, an entry thermometer 5 for measuring the temperature of the mandrel bar 1 may be provided on the entry side of the first coil 2. The output of the coil 2 may be adjusted so that the surface temperature of the mandrel bar 1 on the entry side of the first coil 2 follows the calculation when determining the heat treatment conditions. Also, an intermediate thermometer 6 for measuring the temperature of the mandrel bar 1 may be provided between the two coils 2. The output of the coil 2 may be adjusted so that the surface temperature of the mandrel bar 1 between the two coils 2 follows the calculation when determining the heat treatment conditions.
[0041] The manufacturing apparatus for the mandrel bar 1 according to the present embodiment may include the tempering heat treatment apparatus of FIG. 1 and FIG. 4 or may be an apparatus that controls the tempering heat treatment apparatus, and may be configured to include, for example, a computer. The manufacturing apparatus for the mandrel bar 1 may execute the above-mentioned manufacturing method for the mandrel bar 1 by, for example, a computer. The computer may be, for example, a computer that manages the manufacturing of the mandrel bar 1 and the mandrel rolling process using the mandrel bar 1. The configuration of the computer is not particularly limited, and may include, for example, a memory (storage device), a CPU (processing device), a hard disk drive (HDD), a communication control unit for connecting to a network, a display device, and an input device. Here, the method for determining the heat treatment conditions in FIG. 2 may be implemented by the CPU of the computer. Data (including experimental data) used in the heat treatment conditions may be input from the input device of the computer or via a network and stored in the memory or the hard disk drive. In addition, the above-mentioned process of "determining the hardness" may be executed by the first determination unit. The above-mentioned process of "determining the temperature, time, and upper limit value" may be executed by the second determination unit. The above-mentioned process of "determining the range in which the hardness needs to be achieved" may be executed by the third determination unit. The above-mentioned process of "determining heat treatment conditions" may be executed by a fourth determination unit. Also, the execution of the tempering heat treatment of the mandrel bar 1 may be executed by a tempering heat treatment execution unit. When one or more programs stored in the memory are loaded by the CPU of the computer, the CPU may function as a first determination unit, a second determination unit, a third determination unit, a fourth determination unit, and a tempering heat treatment execution unit. In this way, the manufacturing device for the mandrel bar 1 according to this embodiment includes a first determination unit, a second determination unit, a third determination unit, a fourth determination unit, and a tempering heat treatment execution unit, and executes the manufacturing method of the mandrel bar 1.
[0042] As described above, the manufacturing method and manufacturing apparatus for the mandrel bar 1 according to the present embodiment can perform the tempering heat treatment of the mandrel bar 1 without using an atmosphere furnace by using the above-mentioned configuration or process. That is, according to the present disclosure, the tempering heat treatment of the mandrel bar 1 can be realized without the need for a large atmosphere furnace. Therefore, the problem of a temperature difference occurring between the part in contact with the hearth or skid and the part not in contact with the hearth or skid does not occur. According to the present disclosure, the part to be cut is heated in a concentrated manner by induction heating, so that the energy cost can be reduced compared to an atmosphere furnace.
[0043] (Example) The effects of the present disclosure will be specifically described below based on examples, but the present disclosure is not limited to the contents of the examples.
[0044] In this example, a mandrel bar was manufactured.
[0045] (Example 1: One coil) A mandrel bar made of hot work tool steel (SKD6) having the chemical composition shown in Table 1 was subjected to induction quenching heat treatment, and then to induction tempering heat treatment as described in the above embodiment. The balance not shown in Table 1 is Fe and unavoidable impurities. The diameter of the mandrel bar is 120 mm. The length of the mandrel bar is 20000 mm. The hardness after tempering heat treatment to be achieved was set to a target value of HV400 to 550, which provides sufficient wear resistance for the bar. In addition, the target was that this hardness be obtained in a range of 0 to 10 mm in the radial direction from the outer surface. After the mandrel bar was subjected to quenching heat treatment, the end of the mandrel bar was cut and the Vickers hardness was measured in a range of 0 to 10 mm in the radial direction from the outer surface, and the hardness was in the range of HV595 to 608.
[0046] [Table 1]
[0047] Experiments were conducted in advance using SKD6 steel billets with the same chemical composition as the mandrel bar. After heat treatment with the same temperature pattern as the quenching performed in the manufacture of the mandrel bar, the hardness became HV546 when held at 600°C for 60 seconds. From this result, it was decided that the heating temperature would be 600°C and the holding time would be 60 seconds (tempering parameter 15908). In addition, experiments were conducted under multiple conditions of changing the heating temperature and holding time. As a result, the hardness became less than HV400 under multiple conditions. Among these conditions, the lowest heating temperature was 790°C. From this result, it was decided that the upper limit temperature would be 790°C.
[0048] Tempering heat treatment was performed using a tempering heat treatment device as shown in Figure 1. The inner diameter of the coil is 140 mm. The outer diameter of the coil is 180 mm. The length (coil length) is 200 mm. The heating frequency of the induction heating is 3000 Hz. An exit thermometer, which is a radiation thermometer, is installed at the exit side of the coil to measure the temperature of the mandrel bar. The position of the coil is fixed. The mandrel bar is transported at a constant speed by pinch rolls installed on the entrance and exit sides of the coil.
[0049] Prior to the tempering heat treatment, temperature calculations were performed using FEM coupled with electromagnetic field-thermal conduction analysis. Figure 5 shows the results of calculating the temperature change over time at the surface and at a point 10 mm from the surface (two evaluation points). If the mandrel bar transport speed is 1.5 mm / s and the temperature of the mandrel bar at the coil exit is 744°C, the time for the position 10 mm from the surface to be maintained at 600°C or higher is 61 seconds, and the maximum temperature reached at the surface is 746°C, which is below the upper limit temperature. Here, the position 10 mm from the surface corresponds to the innermost position of the range in which hardness must be achieved. Therefore, the mandrel bar transport speed was set to 1.5 mm / s, and the induction heating output was adjusted so that the measurement value of the thermometer at the exit side would be 744°C.
[0050] With the above settings, the entire length of the mandrel bar was subjected to a tempering heat treatment. After the tempering treatment, the ends of the mandrel bar were cut and the Vickers hardness was measured in the range of 0 to 10 mm in the radial direction from the outer surface. The hardness was in the range of HV462 to 538, which was within the target range.
[0051] (Example 2: Multiple coils) A mandrel bar made of hot work tool steel (SKD6) having the chemical composition shown in Table 1 was subjected to induction quenching heat treatment, and then to induction tempering heat treatment as described in the above embodiment. The balance not shown in Table 1 is Fe and unavoidable impurities. The diameter of the mandrel bar is 170 mm. The length of the mandrel bar is 20000 mm. The hardness after tempering heat treatment to be achieved was set to a target value of HV400 to 550, which provides sufficient wear resistance for the bar. In addition, the target was that this hardness be obtained in a range of 0 to 10 mm in the radial direction from the outer surface. The end of the mandrel bar after quenching heat treatment was cut and the Vickers hardness was measured in a range of 0 to 10 mm in the radial direction from the outer surface, and the hardness was in the range of HV590 to 602.
[0052] Experiments were conducted in advance using SKD6 steel billets with the same chemical composition as the mandrel bar. After heat treatment with the same temperature pattern as the quenching performed in the manufacture of the mandrel bar, the hardness became HV548 when held at 600°C for 60 seconds. From this result, it was decided that the heating temperature would be 600°C and the holding time would be 60 seconds (tempering parameter 15908). In addition, experiments were conducted under multiple conditions of changing the heating temperature and holding time. As a result, the hardness became less than HV400 under multiple conditions. Among these conditions, the lowest heating temperature was 790°C. From this result, it was decided that the upper limit temperature should be 790°C.
[0053] Tempering heat treatment was performed using a tempering heat treatment device as shown in Figure 4. Both coils have the same dimensions. The inner diameter of the coil is 190 mm. The outer diameter of the coil is 230 mm. The length (coil length) is 200 mm. The heating frequency of the induction heating is 3000 Hz. An exit thermometer, which is a radiation thermometer, is installed at the exit side of the coil to measure the temperature of the mandrel bar. The position of the coil is fixed. The mandrel bar is transported at a constant speed by pinch rolls installed on the entrance and exit sides of the coil.
[0054] Prior to the tempering heat treatment, temperature calculations were performed using FEM coupled with electromagnetic field-thermal conduction analysis. Figure 6 shows the results of calculating the temperature change over time at the surface and at a point 10 mm from the surface (two evaluation points). The distance between the coils was set to 80 mm. If the mandrel bar transport speed is set to 1.5 mm / s and the temperature of the mandrel bar at the coil exit is 735°C, the time for the position 10 mm from the surface to be held at 600°C or higher is 63 seconds, and the maximum temperature reached at the surface is 736°C, which is below the upper limit temperature. Here, the position 10 mm from the surface corresponds to the innermost position of the range in which hardness must be achieved. Therefore, the distance between the coils was set to 80 mm, the mandrel bar transport speed was set to 1.5 mm / s, and the induction heating output was adjusted so that the measurement value of the thermometer at the exit side was 735°C.
[0055] With the above settings, the entire length of the mandrel bar was subjected to a tempering heat treatment. After the tempering heat treatment, the ends of the mandrel bar were cut and the Vickers hardness was measured in the range of 0 to 10 mm in the radial direction from the outer surface. The hardness was in the range of HV459 to 537, which was within the target range.
[0056] (Comparative Example 1: When the surface is heated too high) A mandrel bar made of hot work tool steel (SKD6) having the chemical composition shown in Table 1 was subjected to induction heating for quenching heat treatment, and then induction heating for tempering heat treatment. The balance not shown in Table 1 is Fe and unavoidable impurities. The diameter of the mandrel bar is 120 mm. The length of the mandrel bar is 20,000 mm. The end of the mandrel bar after quenching heat treatment was cut and the Vickers hardness was measured in the range of 0 to 10 mm in the radial direction from the outer surface, and the hardness was in the range of HV596 to 605.
[0057] Tempering heat treatment was performed using a tempering heat treatment device as shown in Figure 1. The inner diameter of the coil is 140 mm. The outer diameter of the coil is 180 mm. The length (coil length) is 200 mm. The heating frequency of the induction heating is 3000 Hz. An exit thermometer, which is a radiation thermometer, is installed at the exit side of the coil to measure the temperature of the mandrel bar. The position of the coil is fixed. The mandrel bar is transported at a constant speed by pinch rolls installed on the entrance and exit sides of the coil.
[0058] The mandrel bar was moved at a speed of 1.5 mm / s, and the output of the induction heater was adjusted so that the measurement value of the exit thermometer became 810°C.
[0059] With the above settings, the entire length of the mandrel bar was subjected to a tempering heat treatment. After the tempering treatment, the end of the mandrel bar was cut and the Vickers hardness was measured in the range of 0 to 10 mm in the radial direction from the outer surface. The hardness was in the range of HV324 to 480, which was outside the target range. This is thought to be because the surface hardness of the mandrel bar was reduced due to the temperature of the surface becoming too high.
[0060] (Comparative Example 2: When the surface is cooled too much) The mandrel bar after the quenching heat treatment similar to that of Example 2 was subjected to a tempering heat treatment in the same coil as that of Example 2.
[0061] The mandrel bar was moved at a speed of 1.5 mm / s, and the output of the induction heater was adjusted so that the measurement value of the exit thermometer was 650°C.
[0062] With the above settings, the entire length of the mandrel bar was subjected to tempering heat treatment. After tempering heat treatment, the ends of the mandrel bar were cut and the Vickers hardness was measured in the range of 0 to 10 mm in the radial direction from the outer surface. The hardness was in the range of HV509 to 580, which was outside the target range. This is thought to be because the heating temperature was low, and the heating temperature and holding time were not sufficient, so the hardness did not decrease sufficiently. In addition, a Charpy test was performed using half-size test pieces as specified in JIS Z 2242:2018. The test pieces were taken from the range of 0 to 10 mm in the radial direction from the outer surface. As a result, the toughness value was a low value of 2J, and there was a high possibility that harmful cracks would occur in the mandrel bar.
[0063] (Comparative Example 3: When an atmospheric furnace is used) A tempering heat treatment was carried out in an atmosphere furnace on the mandrel bar after rolling similarly to Example 2. In the tempering heat treatment, the mandrel bar was inserted into an atmosphere furnace at a furnace temperature of 630° C., and after 80 minutes, it was removed and air-cooled.
[0064] The end of the mandrel bar after the tempering heat treatment was cut and the Vickers hardness was measured in the range of 0 to 10 mm in the radial direction from the outer surface. The hardness was in the range of HV459 to 542, which was within the target range. However, 1.5 times the energy cost was required compared to Example 2. This is because in the case of an atmospheric furnace, it is necessary to heat the entire large furnace to a high temperature, and the energy cost for heating is large.
[0065] In addition, visual inspection of the surface of the mandrel bar after the tempering heat treatment revealed that there were irregularities in the circumferential and longitudinal directions of the surface properties. This is thought to be due to the fact that the heating was performed in an atmospheric furnace, which resulted in a temperature difference between the part of the mandrel bar that was in contact with the skid and the part that was not, resulting in a difference in hardness after the tempering heat treatment. Such irregularities can be transferred to the product during rolling and can cause quality defects.
[0066] Although the embodiments of the present disclosure have been described based on the drawings and examples, it should be noted that those skilled in the art can easily make various modifications or corrections based on the present disclosure. Therefore, it should be noted that these modifications or corrections are included in the scope of the present disclosure. For example, the functions included in each component or each step can be rearranged so as not to be logically inconsistent, and multiple components or steps can be combined into one or divided. The embodiments of the present disclosure can also be realized as a storage medium on which a program executed by a processor included in the device is recorded. It should be understood that these are also included in the scope of the present disclosure. [Explanation of symbols]
[0067] 1 Mandrel bar 2 Coil 3. Conveyor 4 Outlet thermometer 5 Inlet thermometer 6 Intermediate thermometer
Claims
1. A method for manufacturing a mandrel bar, comprising the steps of: subjecting a mandrel bar to a quenching heat treatment and then a tempering heat treatment, determining the hardness of the mandrel bar to be achieved after the tempering heat treatment; Determine the heating temperature, holding time and upper limit temperature for achieving the determined hardness; determining a range required to achieve the determined hardness of the mandrel bar; Determine the heat treatment conditions of induction heating so that the heating temperature and holding time are achieved within the range required to achieve the determined hardness, and the upper limit temperature is not exceeded; and subjecting the mandrel bar to a tempering heat treatment under the determined heat treatment conditions.
2. The method of claim 1 , wherein the induction heating uses one coil to heat the mandrel bar.
3. The method of claim 1 , wherein the induction heating uses a plurality of coils to heat the mandrel bar.
4. The method for manufacturing a mandrel bar according to any one of claims 1 to 3, wherein the heating temperature, the holding time, and the upper limit temperature are determined based on data from an experiment using a steel slab having a similar chemical composition to that of the mandrel bar.
5. The method for manufacturing a mandrel bar according to any one of claims 1 to 3, wherein the heat treatment conditions are determined based on temperature calculations performed by FEM coupled with electromagnetic field-thermal conduction analysis.
6. A mandrel bar manufacturing apparatus for manufacturing a mandrel bar by subjecting the mandrel bar to a quenching heat treatment and then a tempering heat treatment, a first determination unit for determining a hardness of the mandrel bar to be achieved after the tempering heat treatment; A second determination unit that determines a heating temperature, a holding time, and an upper limit temperature for achieving the determined hardness; a third determination unit for determining a range in which the determined hardness of the mandrel bar needs to be achieved; A fourth determination unit determines heat treatment conditions for induction heating that achieve the heating temperature and holding time within a range required to achieve the determined hardness and do not exceed an upper limit temperature; a tempering heat treatment execution unit that performs a tempering heat treatment on the mandrel bar under the determined heat treatment conditions.
Citation Information
Patent Citations
Core metal for mandrel rolling with small extensional deformation during being used
JP1993069013A
Mandrel bar for hot-rolling seamless tube and manufacture thereof
JP1996197112A
Method for improving service life of mandrel bar for manufacturing hot seamless steel tube
JP1999226614A
Induction hardening of steel
US4599502A
Method and apparatus for continuously processing long bar by heat treatment using induction heating
JP2008274433A
Cited By
Material hardness matching method and system for avoiding manufacturing defects of rotary swaging shaft
CN120046363A