Raw material for nursing care bathtub, molding material for nursing care bathtub, and nursing care bathtub unit
A nursing bathtub material with aluminum hydroxide and calcium carbonate enhances chemical resistance and suppresses surface defects, ensuring hygiene in care settings.
Patent Information
- Application Number
- JP2023047621
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Nursing bathtubs require high chemical resistance and minimal surface defects to withstand cleaning with chemicals like hydrochloric acid and sodium hypochlorite, while maintaining a hygienic appearance.
A nursing bathtub raw material comprising a resin component with a specific ratio of aluminum hydroxide and calcium carbonate, along with reinforcing fibers, is used to create a molding material that forms a nursing bathtub with excellent chemical resistance and reduced surface defects.
The nursing bathtub exhibits superior chemical resistance, preventing surface defects and maintaining a clean appearance, essential for hygiene in care settings.
Smart Images

Figure 2024136488000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a raw material for a nursing care bathtub, a molding material for a nursing care bathtub, and a nursing care bathtub unit. [Background technology]
[0002] Conventionally, molded articles made of molding materials (e.g., unsaturated polyester resins) containing resin components (e.g., sheet molding compounds (SMCs) in particular) have excellent appearance, mechanical properties, water resistance, and corrosion resistance. For this reason, it is known that such molded articles are used as materials for bathtubs.
[0003] As such a molding material, a sheet molding compound (SMC) containing a resin component including a crystalline unsaturated polyester resin and a vinyl ester resin, Softon 1200 (calcium carbonate), and glass fibers has been proposed (for example, Example 1 of Patent Document 1 below). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-295714 Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, bathtubs, particularly those for nursing care use by people who require nursing care, are required to have a high level of chemical resistance and to suppress surface defects.
[0006] More specifically, in medical and nursing care facilities, nursing care bathtubs are cleaned every time a person requiring nursing care uses them. Since the nursing care bathtub may be stained with dirt from the person requiring nursing care, chemicals (e.g., hydrochloric acid, sodium hypochlorite) are used for such cleaning. For this reason, nursing care bathtubs are required to have a high level of chemical resistance and to have few defects on the surface to prevent the accumulation of dirt and the like.
[0007] The present invention provides a nursing care bath raw material for producing a nursing care bath that has excellent chemical resistance and can suppress surface defects, a nursing care bath molding material that contains the nursing care bath raw material, and a nursing care bath unit that includes a nursing care bath that contains a cured product of the nursing care bath molding material. [Means for solving the problem]
[0008] The present invention [1] is a raw material for nursing bathtubs, comprising a resin component and a filler, the filler containing aluminum hydroxide, and the content of the aluminum hydroxide is 50 parts by mass or more per 100 parts by mass of the filler.
[0009] The present invention [2] includes the raw material for nursing bathtubs described in [1] above, in which the filler further contains calcium carbonate, and the content of the calcium carbonate is 5 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the filler.
[0010] The present invention [3] includes a molding material for a nursing bathtub, which contains the raw material for a nursing bathtub described in [1] or [2] above and reinforcing fibers.
[0011] The present invention [4] includes a nursing bath unit equipped with a nursing bath containing a cured product of the nursing bath molding material described in [3] above.
[0012] The present invention [5] includes the nursing bath unit described in the above [4], wherein the nursing bath is a light color having a value of 6 or more and a chroma of 8 or less in the Munsell color system. Effect of the Invention
[0013] The raw material for nursing care bathtubs of the present invention contains a predetermined ratio of aluminum hydroxide, so that nursing care bathtubs having excellent chemical resistance can be manufactured.
[0014] The molding material for nursing care bath of the present invention contains the raw material for nursing care bath of the present invention. Therefore, a nursing care bath having excellent chemical resistance can be manufactured.
[0015] The nursing care bath unit of the present invention includes a nursing care bath containing a cured product of the nursing care bath molding material of the present invention, and therefore has excellent chemical resistance and can suppress surface defects. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of a nursing bath unit of the present invention (a nursing bath unit equipped with a supine position bathing device as a bathing assistance device). [Diagram 2] FIG. 2 is a schematic diagram showing one embodiment of the nursing bath unit of the present invention (a nursing bath unit equipped with a sitting position bathing device as a bathing assistance device). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] 1. Materials for nursing bathtubs The raw material for nursing bathtubs includes a resin component and a filler.
[0018] <Resin component> The resin component includes a radical polymerizable resin.
[0019] Examples of the radical polymerizable resin include unsaturated polyester resin, vinyl ester resin, and urethane (meth)acrylate. From the viewpoint of excellent physical properties (toughness, strength, durability, weather resistance, hot water resistance, and transparency), the radical polymerizable resin is preferably unsaturated polyester resin or vinyl ester resin.
[0020] The unsaturated polyester resin contains an unsaturated polyester and a polymerizable monomer, that is, the unsaturated polyester resin is an unsaturated polyester resin composition containing an unsaturated polyester and a polymerizable monomer.
[0021] The unsaturated polyester is not particularly limited, but a compound obtained by the reaction of a polybasic acid with a polyhydric alcohol is suitable. Each raw material used in this reaction may be used alone or in combination with two or more kinds depending on the required performance. In addition, it may be modified with dicyclopentadiene (DCPD).
[0022] The polybasic acid includes a polybasic acid having an ethylenically unsaturated double bond as an essential component (hereinafter referred to as an ethylenically unsaturated bond-containing polybasic acid) and a polybasic acid not having an ethylenically unsaturated double bond as an optional component (hereinafter referred to as an ethylenically unsaturated bond-free polybasic acid).
[0023] Examples of the ethylenically unsaturated bond-containing polybasic acid include ethylenically unsaturated aliphatic dibasic acids and their anhydrides, halides of ethylenically unsaturated aliphatic dibasic acids, and alkyl esters of ethylenically unsaturated aliphatic dibasic acids.
[0024] Examples of ethylenically unsaturated aliphatic dibasic acids include maleic acid, fumaric acid, itaconic acid, and dihydromuconic acid. Examples of ethylenically unsaturated bond-containing polybasic acids include acid anhydrides derived from the above ethylenically unsaturated aliphatic dibasic acids. Examples of ethylenically unsaturated bond-containing polybasic acids include maleic anhydride. Examples of ethylenically unsaturated bond-containing polybasic acids include maleic anhydride.
[0025] Examples of polybasic acids not containing ethylenically unsaturated bonds include saturated aliphatic polybasic acids, saturated alicyclic polybasic acids, aromatic polybasic acids, anhydrides of these acids, halides of these acids, and alkyl esters of these acids.
[0026] Examples of the saturated aliphatic polybasic acid include saturated aliphatic dibasic acids.
[0027] Examples of saturated aliphatic dibasic acids include oxalic acid, malonic acid, succinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, hexylsuccinic acid, glutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylsuccinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. Examples of saturated aliphatic polybasic acids include acid anhydrides derived from the above-mentioned saturated aliphatic dibasic acids. Examples of acid anhydrides derived from saturated aliphatic dibasic acids include oxalic anhydride and succinic anhydride.
[0028] Examples of the saturated alicyclic polybasic acid include saturated alicyclic dibasic acids.
[0029] Examples of saturated alicyclic dibasic acids include HET acid, 1,2-hexahydrophthalic acid, 1,1-cyclobutanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid (cis- or trans-1,4-cyclohexanedicarboxylic acid or a mixture thereof). Examples of saturated alicyclic polybasic acids include acid anhydrides derived from the above-mentioned saturated alicyclic dibasic acids. Examples of acid anhydrides derived from saturated alicyclic dibasic acids include HET acid anhydride.
[0030] Examples of aromatic polybasic acids include aromatic dibasic acids.
[0031] Examples of aromatic dibasic acids include phthalic acid (orthophthalic acid, isophthalic acid, terephthalic acid), trimellitic acid, and pyromellitic acid. Examples of aromatic polybasic acids include acid anhydrides derived from the above aromatic dibasic acids. Examples of acid anhydrides derived from aromatic dibasic acids include phthalic anhydride. Examples of aromatic dibasic acids include orthophthalic acid, terephthalic acid, and isophthalic acid. Examples of aromatic dibasic acids include more preferably terephthalic acid and isophthalic acid. Examples of aromatic dibasic acids include even more preferably isophthalic acid.
[0032] The polybasic acids can be used alone or in combination of two or more kinds.
[0033] When the polybasic acid includes an ethylenically unsaturated bond-containing polybasic acid and an ethylenically unsaturated bond-free polybasic acid, the mixing ratio of the ethylenically unsaturated bond-containing polybasic acid is, for example, 50 mol% or more, preferably 60 mol% or more, more preferably 70 mol% or more, and, for example, 95 mol% or less, preferably 90 mol% or less, based on 100 mol of the total polybasic acid. The mixing ratio of the ethylenically unsaturated bond-free polybasic acid is, for example, 5 mol% or more, preferably 10 mol% or more, and, for example, 50 mol% or less, preferably 40 mol% or less, more preferably 30 mol% or less.
[0034] Polyhydric alcohols include, for example, dihydric and trihydric alcohols.
[0035] Examples of dihydric alcohols include aliphatic diols, alicyclic diols, and aromatic diols. Examples of aliphatic diols include alkane diols and ether diols. Examples of alkane diols include ethylene glycol, propylene glycol (1,2- or 1,3-propane diol or a mixture thereof), butylene glycol (1,2- or 1,3- or 1,4-butylene glycol or a mixture thereof), 1,5-pentane diol, 1,6-hexane diol, neopentyl glycol, 2-methyl-1,3-propane diol, 2-butyl-2-ethyl-1,3-propane diol, 3-methyl-1,5-pentane diol, 2,2,2-trimethylpentane diol, and 3,3-dimethylol heptane. Examples of ether diols include diethylene glycol, triethylene glycol, and dipropylene glycol. Examples of alicyclic diols include cyclohexanediol (1,2- or 1,3- or 1,4-cyclohexanediol or a mixture thereof), cyclohexanedimethanol (1,2- or 1,3- or 1,4-cyclohexanedimethanol or a mixture thereof), cyclohexanediethanol (1,2- or 1,3- or 1,4-cyclohexanediethanol or a mixture thereof), and hydrogenated bisphenol A. Examples of aromatic diols include an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A.
[0036] Examples of trihydric alcohols include glycerin, trimethylolpropane, and triisopropanolamine.
[0037] The polyhydric alcohol is preferably a dihydric alcohol. The polyhydric alcohol is more preferably an aliphatic diol. The polyhydric alcohol is further preferably an alkanediol. The polyhydric alcohol is particularly preferably propylene glycol, neopentyl glycol, hydrogenated bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A.
[0038] The polyhydric alcohols can be used alone or in combination of two or more kinds.
[0039] The unsaturated polyester is prepared by reacting a polybasic acid with a polyhydric alcohol.
[0040] The equivalent ratio of the polyhydric alcohol to the polybasic acid (hydroxyl groups of the polyhydric alcohol / carboxyl groups of the polybasic acid) is, for example, 0.9 or more, preferably 0.95 or more, and for example, 1.2 or less, preferably 1.1 or less.
[0041] The reaction temperature is, for example, 150° C. or more, preferably 190° C. or more, and for example, 250° C. or less, preferably 230° C. or less.
[0042] In the above reaction, a known solvent and a known reaction catalyst can be added, if necessary.
[0043] This allows the preparation of an unsaturated polyester.
[0044] The acid value of the unsaturated polyester (measurement method: in accordance with JIS K6901 (2008)) is, for example, 5 mgKOH / g or more, preferably 10 mgKOH / g or more, and for example, less than 40 mgKOH / g, preferably 30 mgKOH / g or less.
[0045] The weight average molecular weight of the unsaturated polyester is, for example, 2,000 or more, preferably 4,000 or more, and for example, 25,000 or less, preferably 20,000 or less.
[0046] The weight average molecular weight is a weight average molecular weight calculated in terms of polystyrene by gel permeation chromatography (GPC), and can be determined by measuring the unsaturated polyester by GPC.
[0047] The unsaturated polyesters can be used alone or in combination of two or more kinds.
[0048] The vinyl ester resin contains a vinyl ester and a polymerizable monomer, that is, the vinyl ester resin is a vinyl ester resin composition containing a vinyl ester and a polymerizable monomer.
[0049] Vinyl esters are the addition reaction products of epoxy resins and unsaturated monocarboxylic acids.
[0050] The epoxy resin contains at least one epoxy group. Examples of the epoxy resin include bisphenol type epoxy resins (e.g., bisphenol A type epoxy resins, bisphenol F type epoxy resins, brominated bisphenol A type epoxy resins, etc.), novolac type epoxy resins (e.g., phenol novolac type epoxy resins, cresol novolac type epoxy resins, brominated novolac type epoxy resins, etc.), aliphatic type epoxy resins, alicyclic epoxy resins, hydrogenated bisphenol type epoxy resins, and amine type epoxy resins. Examples of the epoxy resin include preferably bisphenol type epoxy resins. Examples of the epoxy resin include more preferably bisphenol A type epoxy resins.
[0051] The epoxy resins can be used alone or in combination of two or more kinds.
[0052] The epoxy equivalent of the epoxy resin is, for example, 100 or more, preferably 200 or more, and for example, 700 or less, preferably 500 or less, and more preferably 400 or less. The epoxy equivalent can be measured in accordance with JIS K 7236.
[0053] The unsaturated monocarboxylic acid contains at least one unsaturated double bond and at least one carboxy group. Examples of the unsaturated monocarboxylic acid include unsaturated monofatty acids (e.g., (meth)acrylic acid, crotonic acid, sorbic acid, etc.), aromatic unsaturated monocarboxylic acids (e.g., cinnamic acid, etc.), and ester bond-containing unsaturated monocarboxylic acids (e.g., reaction products of acid anhydrides and unsaturated alcohols, etc.). Note that (meth)acrylic is synonymous with methacrylic and / or acrylic. A preferred example of the unsaturated monocarboxylic acid is methacrylic acid.
[0054] The unsaturated monocarboxylic acids can be used alone or in combination of two or more kinds.
[0055] The vinyl ester is prepared by subjecting the epoxy group of the above-mentioned epoxy resin and the carboxy group of the above-mentioned unsaturated monobasic acid to a ring-opening addition reaction.
[0056] The radical polymerizable resin can be used alone or in combination of two or more. When the unsaturated polyester and the vinyl ester are used in combination, the content of the unsaturated polyester is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, more preferably 70 parts by mass or more, and for example, 80 parts by mass or less, based on 100 parts by mass of the total of the unsaturated polyester and the vinyl ester. The content of the vinyl ester is, for example, 20 parts by mass or more, and, for example, 50 parts by mass or less, preferably 40 parts by mass or less, and more preferably 30 parts by mass or less, based on 100 parts by mass of the total of the unsaturated polyester and the vinyl ester.
[0057] From the viewpoint of preventing poor appearance due to resin separation during curing, the radical polymerizable resin preferably does not contain a vinyl ester resin or a urethane (meth)acrylate, and is made of an unsaturated polyester resin.
[0058] Examples of the polymerizable monomer include styrene-based monomers and (meth)acrylic acid ester-based monomers.
[0059] Styrenic monomers include, for example, styrene, vinyltoluene, t-butylstyrene, and chlorostyrene.
[0060] Examples of (meth)acrylic acid ester monomers include (meth)acrylic acid alkyl esters, (meth)acrylic acid allyl esters, ring-containing (meth)acrylic acid esters, (meth)acrylic acid hydroxyalkyl esters, (meth)acrylic acid alkoxyalkyl esters, (meth)acrylic acid aminoalkyl esters, (meth)acrylic acid fluoroalkyl esters, and polyfunctional (meth)acrylic acid esters. Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate. Examples of (meth)acrylic acid allyl esters include allyl (meth)acrylate. Examples of ring-containing (meth)acrylic acid esters include cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate. Examples of hydroxyalkyl (meth)acrylic acid esters include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. Examples of alkoxyalkyl (meth)acrylic acid esters include 2-methoxyethyl (meth)acrylate and 2-ethoxyethyl (meth)acrylate. Examples of aminoalkyl (meth)acrylic acid esters include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and chloride salts thereof. Examples of the fluoroalkyl (meth)acrylate include trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate.Examples of polyfunctional (meth)acrylic acid esters include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0061] As the polymerizable monomer, preferably, styrene-based monomer and (meth)acrylic acid alkyl ester are mentioned. As the polymerizable monomer, more preferably, styrene and methyl methacrylate are mentioned. As the polymerizable monomer, more preferably, styrene is mentioned.
[0062] The polymerizable monomers can be used alone or in combination of two or more kinds.
[0063] The unsaturated polyester resin is prepared by dissolving the unsaturated polyester in a polymerizable monomer (preferably styrene) and, if necessary, adding an additive.
[0064] In preparing the unsaturated polyester resin, the blending ratio of the polymerizable monomer is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, and for example, 80 parts by mass or less, preferably 70 parts by mass or less, relative to 100 parts by mass of the unsaturated polyester.
[0065] The vinyl ester resin is prepared by dissolving the vinyl ester in a polymerizable monomer (preferably styrene) and, if necessary, adding an additive.
[0066] In preparing the vinyl ester resin, the mixing ratio of the polymerizable monomer is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, and for example, 80 parts by mass or less, preferably 70 parts by mass or less, relative to 100 parts by mass of the vinyl ester.
[0067] In addition, after preparing the unsaturated polyester resin or vinyl ester resin, when this unsaturated polyester resin is mixed with other components (fillers and additives (described later)), a polymerizable monomer can also be further blended.
[0068] The mixing ratio of the radical polymerizable resin is 20 parts by mass or more, preferably 30 parts by mass or more, more preferably 40 parts by mass or more, and for example, 70 parts by mass or less, 60 parts by mass or less, per 100 parts by mass of the resin component.
[0069] The resin component preferably contains a low shrinkage agent.
[0070] Examples of the low shrinkage agent include polyethylene, polystyrene, styrene-based thermoplastic elastomer, cross-linked polystyrene, polyvinyl acetate-polystyrene block copolymer, polyvinyl acetate, polymethyl methacrylate, and saturated polyester resin. Examples of the low shrinkage agent include polyethylene, cross-linked polystyrene, polyvinyl acetate-polystyrene block copolymer, and polystyrene. Examples of the low shrinkage agent include polyethylene, cross-linked polystyrene, and polystyrene, more preferably.
[0071] The low profile agents can be used alone or in combination of two or more.
[0072] Alternatively, the low shrinkage agent can be dissolved in the polymerizable monomer to prepare a polymerizable monomer solution of the low shrinkage agent.
[0073] In the polymerizable monomer solution of the low shrinkage agent, the solids concentration of the low shrinkage agent is, for example, 20% by mass or more and, for example, 70% by mass or less.
[0074] The mixing ratio of the low shrinkage agent relative to 100 parts by mass of the resin component is, for example, 1 part by mass or more, preferably 3 parts by mass or more, and for example, 20 parts by mass or less, preferably 10 parts by mass or less.
[0075] The resin component preferably contains a radical polymerizable resin and a low shrinkage agent, and more preferably consists of a radical polymerizable resin and a low shrinkage agent.
[0076] <Filling material> The filler contains aluminum hydroxide as an essential component.
[0077] Aluminum hydroxide is an ingredient that imparts chemical resistance and improves the appearance of nursing bathtubs (described below).
[0078] The average particle size of the aluminum hydroxide is, for example, 1 μm or more, and, for example, 50 μm or less, preferably 25 μm or less.
[0079] The average particle size of aluminum hydroxide can be determined by creating a particle size distribution curve using a laser diffraction / scattering type particle size distribution measurement device and calculating the 50% by mass equivalent particle size.
[0080] The content of aluminum hydroxide is, relative to 100 parts by mass of the filler, 50 parts by mass or more, preferably 70 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 85 parts by mass or more, and for example, 100 parts by mass or less, preferably 95 parts by mass or less.
[0081] When the content of aluminum hydroxide is equal to or higher than the above lower limit, a nursing bathtub (described later) having excellent chemical resistance and appearance can be produced.
[0082] On the other hand, if the content of aluminum hydroxide is less than the lower limit, the chemical resistance is reduced, and it is not possible to manufacture a nursing bathtub (described later) having excellent chemical resistance.
[0083] The filler also optionally contains calcium carbonate, which improves the gloss and appearance.
[0084] The content of calcium carbonate relative to 100 parts by mass of the filler is, for example, 5 parts by mass or more, and, for example, 50 parts by mass or less, preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less.
[0085] When the content of calcium carbonate is equal to or less than the upper limit, the occurrence of surface defects (scumming, waviness) and molding cracks can be suppressed.
[0086] Furthermore, the filler may contain other fillers than aluminum hydroxide and calcium carbonate, if necessary.
[0087] Other fillers include, for example, inorganic fillers. Examples of inorganic fillers include oxides (e.g., alumina, titanium oxide), hydroxides (e.g., magnesium hydroxide (excluding aluminum hydroxide)), carbonates (excluding calcium carbonate), sulfates (e.g., barium sulfate), silica (e.g., crystalline silica, fused silica, fumed silica, dry silica (aerosil)), hollow fillers, silicates (e.g., silica sand, diatomaceous earth, glass powder, glass balloons, mica, clay, kaolin, talc), fluorides (e.g., fluorite), phosphates (e.g., calcium phosphate), and metal powders, ceramics, milled fibers, and clay minerals (e.g., smectite).
[0088] The other fillers can be used alone or in combination of two or more.
[0089] The content ratio of the other filler is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and for example, 20 parts by mass or less, preferably 10 parts by mass or less, relative to 100 parts by mass of the filler. In particular, when the other filler is barium sulfate, the content ratio of barium sulfate is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and for example, 40 parts by mass or less, preferably 20 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the filler, from the viewpoints of cost, appearance and moldability.
[0090] The filler preferably consists of aluminum hydroxide and calcium carbonate without other fillers.
[0091] The content ratio of the filler relative to 100 parts by mass of the resin component is 50 parts by mass or more, preferably 100 parts by mass or more, and for example, 300 parts by mass or less, preferably 200 parts by mass or less.
[0092] <Additives> If necessary, additives can be blended into the nursing bathtub raw material within the range that does not impair the effects of the present invention.
[0093] Examples of additives include polymerization inhibitors, curing agents, release agents, colorants, thickeners, flame retardants, wetting and dispersing agents, pattern materials, antibacterial agents, hydrophilic agents, photocatalysts, UV absorbers, UV stabilizers, separation inhibitors, silane coupling agents, antistatic agents, thixotropic agents, thixotropic stabilizers, and polymerization accelerators. The additives can be used alone or in combination of two or more.
[0094] The polymerization inhibitor is added to adjust the pot life and the curing reaction.
[0095] Examples of the polymerization inhibitor include hydroquinone compounds, benzoquinone compounds, catechol compounds, phenol compounds, and N-oxyl compounds.
[0096] As the polymerization inhibitor, preferably, a benzoquinone compound, a hydroquinone compound, and an N-oxyl compound are mentioned.
[0097] An example of the benzoquinone compound is parabenzoquinone.
[0098] Examples of the hydroquinone compound include hydroquinone, methylhydroquinone, and t-butylhydroquinone. A preferred example of the hydroquinone compound is t-butylhydroquinone.
[0099] More preferred examples of the polymerization inhibitor include benzoquinone compounds and N-oxyl compounds.
[0100] The mixing ratio of the polymerization inhibitor is, per 100 parts by mass of the resin component, for example, 0.01 part by mass or more, preferably 0.05 part by mass or more, and for example, 0.5 part by mass or less, preferably 0.2 part by mass or less, and more preferably 0.15 part by mass or less.
[0101] Examples of the curing agent include peroxides. Examples of the peroxides include benzoyl peroxide, t-butylperoxyisopropyl carbonate, t-amylperoxyisopropyl carbonate, t-hexylperoxyisopropyl monocarbonate, 1,1-bis(t-butylperoxy)cyclohexane, t-butylperoxy-2-ethylhexanoate, amylperoxy-2-ethylhexanoate, 2-ethylhexylperoxy-2-ethylhexanoate, t-butylperoxybenzoate, t-hexylperoxybenzoate, and t-hexylperoxyacetate. Examples of the curing agent include preferably t-butylperoxyisopropyl carbonate, t-amylperoxyisopropyl carbonate, t-butylperoxybenzoate, t-butyl-2-ethylhexanoate, and t-hexylperoxyacetate. More preferred examples of the curing agent include t-butyl peroxy isopropyl carbonate, t-amyl peroxy isopropyl carbonate, and t-hexyl peroxy acetate. More preferred examples of the curing agent include t-amyl peroxy isopropyl carbonate and t-hexyl peroxy acetate.
[0102] The curing agents can be used alone or in combination of two or more kinds.
[0103] The mixing ratio of the curing agent relative to 100 parts by mass of the resin component is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and for example, 5 parts by mass or less, preferably 2 parts by mass or less.
[0104] Examples of the release agent include fatty acids, fatty acid metal salts, liquid waxes, fluoropolymers, and silicon-based polymers. Examples of the fatty acids include stearic acid and lauric acid. Examples of the fatty acid metal salts include zinc stearate and calcium stearate.
[0105] The release agent is preferably a fatty acid metal salt, more preferably zinc stearate.
[0106] The release agents can be used alone or in combination of two or more kinds.
[0107] The mixing ratio of the release agent relative to 100 parts by mass of the resin component is, for example, 1 part by mass or more, preferably 3 parts by mass or more, and for example, 10 parts by mass or less.
[0108] The colorant is not particularly limited, and examples of the colorant include polyester toners mixed with known pigments such as titanium oxide, carbon black, red iron oxide, and phthalocyanine blue.
[0109] The colorant is preferably a polyester toner.
[0110] The colorants can be used alone or in combination of two or more kinds.
[0111] The mixing ratio of the colorant relative to 100 parts by mass of the resin component is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and for example, 20 parts by mass or less.
[0112] The thickener is blended to thicken the raw material for nursing bathtub to a viscosity suitable for heat compression molding. The thickener is preferably blended before (preferably immediately before) impregnating the raw material for nursing bathtub with the reinforcing fiber (described later).
[0113] Examples of the thickener include alkaline earth metal oxides and alkaline earth metal hydroxides. Examples of the alkaline earth metal oxides include magnesium oxide. Examples of the alkaline earth metal hydroxides include magnesium hydroxide and calcium hydroxide.
[0114] As the thickener, preferably, an alkaline earth metal oxide is used, and more preferably, magnesium oxide is used.
[0115] The thickeners can be used alone or in combination of two or more kinds.
[0116] The mixing ratio of the thickener relative to 100 parts by mass of the resin component is, for example, 0.5 parts by mass or more, and for example, 10 parts by mass or less, preferably 3 parts by mass or less.
[0117] <Preparation of raw materials for nursing bathtubs> The nursing bathtub raw material is prepared by mixing a resin component, a filler, and additives that are added as required.
[0118] The raw material for the nursing bath contains a predetermined ratio of aluminum hydroxide, which allows the production of a nursing bathtub (described later) with excellent chemical resistance.
[0119] Therefore, this raw material for nursing care bathtubs is suitable for use in producing nursing care bathtubs (described below) and in producing nursing care bathtub molding materials for molding the nursing care bathtubs (described below).
[0120] 2. Molding materials for nursing bathtubs The molding material for a nursing bathtub contains a raw material for a nursing bathtub and reinforcing fibers.
[0121] <Reinforced fiber> Examples of reinforcing fibers include inorganic fibers, organic fibers, and natural fibers. Examples of inorganic fibers include glass fibers, carbon fibers, metal fibers, and ceramic fibers. Examples of organic fibers include polyvinyl alcohol-based fibers, polyester-based fibers, polyamide-based fibers, fluororesin-based fibers, and phenol-based fibers. Examples of natural fibers include hemp and kenaf.
[0122] As the reinforcing fiber, preferably, inorganic fiber is used, and more preferably, glass fiber is used.
[0123] Examples of the shape of the reinforcing fibers include cloth (e.g., roving cloth), mat (e.g., chopped strand mat, preformable mat, continuous strand mat, and surfacing mat), strand, roving, nonwoven fabric, and paper.
[0124] The length of the reinforcing fibers is not particularly limited and is, for example, 1.5 mm or more, and from the viewpoint of improving strength, preferably 5 mm or more, more preferably 15 mm or more, and for example, 80 mm or less, preferably 40 mm or less.
[0125] <Preparation of molding material for nursing bathtub> To prepare the molding material for the nursing bathtub, the raw material for the nursing bathtub is mixed with the reinforcing fiber. Specifically, the raw material for the nursing bathtub is impregnated into the reinforcing fiber.
[0126] The method of preparing the molding material for nursing bathtub can be a known method.Specifically, SMC (sheet molding compound), TMC (thick molding compound), BMC (bulk molding compound) can be mentioned.Preferably, SMC and TMC can be mentioned, and more preferably, SMC can be mentioned.
[0127] The content of the reinforcing fibers is, for example, 15 mass % or more and, for example, 60 mass % or less with respect to the molding material.
[0128] This results in a molding material for a nursing bathtub (preferably a sheet-like molding material for a nursing bathtub) containing the raw material for the nursing bathtub and the reinforcing fibers.
[0129] The molding material for the nursing care bath contains the raw materials for the nursing care bath, and therefore it is possible to manufacture a nursing care bath (described later) having excellent chemical resistance.
[0130] 3. Nursing bath unit The nursing bathtub unit includes a nursing bathtub and a bathing assistance device. More specifically, the nursing bathtub unit includes a nursing bathtub and a bathing assistance device for assisting a person requiring nursing care to bathe. The nursing bathtub unit is also distinguished from a bathtub provided for use by people who do not require nursing care (hereinafter, such a bathtub may be referred to as a general bathtub) in that it includes a bathing assistance device.
[0131] The nursing bath unit will be described in detail with reference to FIG.
[0132] The nursing bath unit 1 includes a nursing bath 2 and a supine position bathing device 3 as a bathing assistance device.
[0133] The nursing bath 2 has a box shape with one side open, and has a size and shape that allows a stretcher 4 (described later) to be accommodated inside.
[0134] The nursing bathtub 2 is made of the hardened product of the nursing bathtub molding material described above.
[0135] To harden the molding material for a nursing-care bathtub, the molding material for a nursing-care bathtub is first aged to thicken the material so that it can be subjected to heat compression molding (described later).
[0136] In the aging, the aging temperature is, for example, 20° C. or more and, for example, 50° C. or less. The aging time is, for example, 8 hours or more and, for example, 120 hours or less.
[0137] This allows the nursing bathtub molding material to retain its shape.
[0138] Next, the nursing bathtub molding material is heated and compressed and molded by a known method.
[0139] The conditions of the heat compression molding are appropriately set according to the purpose and use. In the heat compression molding, the molding temperature is, for example, 100° C. or more, and, for example, 200° C. or less. The molding pressure is, for example, 0.1 MPa or more, preferably 1 MPa or more, more preferably 5 MPa or more, and, for example, 20 MPa or less, preferably 15 MPa or less.
[0140] This causes the molding material for the nursing bathtub to be shaped and hardened, and the nursing bathtub 2 is obtained.
[0141] The nursing bathtub 2 is preferably light-colored since bleeding or the like of the person in need of care 10 needs to be noticed early. Light colors are those having a value of 6 or more and a chroma of 8 or less in the Munsell color system, preferably a value of 7 or more and a chroma of 7 or less, and more preferably a value of 8 or more and a chroma of 6 or less.
[0142] In the Munsell color system, if the lightness and saturation are within the above ranges, fading due to use will not be noticeable, and it will be easy to determine whether the color unevenness is due to fading of the bathtub or due to the adhesion of detergent, chemicals, or dirt, making this a suitable product for use in nursing bathtubs used as medical equipment.
[0143] The supine position bathing apparatus 3 includes a stretcher 4 and an electric circuit unit (not shown) that enables the stretcher 4 to be raised and lowered in the vertical direction.
[0144] The stretcher 4 has a substantially flat plate shape, and has a size and shape that allows it to be accommodated inside the nursing bathtub 2. The stretcher 4 is configured to be foldable from its center portion. The person in need of care 10 can take a bath while lying on the stretcher 4.
[0145] The nursing bath unit 1 includes a nursing bath 2 that contains the above-mentioned cured product of the nursing bath molding material, and therefore has excellent chemical resistance.
[0146] 4. Effects The raw material for nursing care bathtubs contains a specific amount of aluminum hydroxide, which allows the production of nursing care bathtubs with excellent chemical resistance.
[0147] Specifically, bathtubs, particularly nursing bathtubs for use by people requiring nursing care, are required to have a high level of chemical resistance.
[0148] Specifically, in medical and nursing care facilities, nursing care bathtubs are cleaned every time a person requiring nursing care uses them. Since the nursing care bathtub may be contaminated with dirt from the person requiring nursing care, acids (e.g., hydrochloric acid, sodium hypochlorite) are used for such cleaning. Therefore, nursing care bathtubs are required to have a high level of chemical resistance.
[0149] As a result of intensive research, it was found that the raw material for nursing care bathtubs must contain the specific ratio of aluminum hydroxide described above. As a result, nursing care bathtubs with excellent chemical resistance can be manufactured.
[0150] On the other hand, light-colored general-use bathtubs do not require the same chemical resistance as nursing care bathtubs. Rather, from the standpoint of improving the hygienic appearance and making them inexpensive, aluminum hydroxide is not used as a filler, and only calcium carbonate is used.
[0151] However, as described above, in order to ensure the high level of chemical resistance required for nursing care bathtubs, aluminum hydroxide is blended in place of calcium carbonate in the raw materials for nursing care bathtubs.
[0152] In addition, nursing bathtubs are required to suppress surface defects in order to prevent the accumulation of dirt and other debris. In particular, when the radical polymerizable resin contains unsaturated polyester resin, the surface of the SMC molded product may suffer from a poor appearance accompanied by a partial decrease in gloss, which is called the scumming phenomenon. The cause of scumming is a combination of factors, such as low-shrinkage agent components that are poorly compatible with unsaturated polyesters separating and precipitating during molding, contaminating the surface, and polymerizable monomers vaporizing during heat compression molding, gelling the surface of the molded product and causing roughness.
[0153] Since the nursing bathtub 2 has a shape significantly different from that of a general bathtub, if the fluidity of the material during molding is not suitable, the upper edge and slope of the nursing bathtub 2 will cause waving and / or the above-mentioned scumming due to the material colliding with each other inside the mold, and fine cracks will occur at the corners of the slope and the bathtub standing surface. Waving and scumming are not only undesirable in appearance, but also cause poor cleaning of the surface of the nursing bathtub 2. Specifically, dirt and the like gets into the valleys of the waves and the fine gaps on the scumming surface, and is not easy to remove even by cleaning. In particular, dirt may not be able to be removed from the scumming surface. Since a high proportion of people who require nursing care have weak resistance to infection, and residual dirt can cause pathogen infection, in nursing bathtubs, waving and scumming are not desirable in order to prevent residual dirt. If cracks occur during molding, the product will be discarded.
[0154] On the other hand, it has been found that the raw material for nursing bathtubs must contain the above-mentioned specific ratio of aluminum hydroxide, which can suppress the above-mentioned waviness and scumming and improve the appearance.
[0155] In addition, the molding material for the nursing care bath contains the above-mentioned raw material for the nursing care bath. Therefore, it is possible to manufacture a nursing care bath with excellent chemical resistance.
[0156] The nursing bath unit includes a nursing bath containing the above-mentioned cured product of the nursing bath molding material, and therefore has excellent chemical resistance.
[0157] 5. Variations In the above description, a nursing bathtub unit equipped with a supine position bathing device as a bathing assistance device has been described in detail, however, the bathing assistance device is not limited to this, and examples thereof include a sitting position bathing device.
[0158] In this case, more specifically, as shown in FIG. 2, the nursing bath unit 1 includes a nursing bath 2 and a sitting position bathing device 5 as a bathing assistance device.
[0159] The sitting position bathing apparatus 5 is a wheelchair. In this nursing care bathtub unit 1, the sitting position bathing apparatus 5 is configured to be able to enter from one side of the nursing care bathtub 2. This allows the person in need of care 10 to take a bath while sitting in the sitting position bathing apparatus 5. EXAMPLES
[0160] Specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values (numerical values defined as "not more than" or "less than") or lower limit values (numerical values defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention." In addition, unless otherwise specified in the following description, "parts" and "%" are based on mass.
[0161] <Production of Unsaturated Polyester Resin> Manufacturing Example 1 A flask equipped with a thermometer, nitrogen gas inlet tube, reflux condenser, fractionator and stirrer was used as a reactor. 2.0 mol of isophthalic acid, 5.5 mol of propylene glycol and 5.0 mol of neopentyl glycol were charged into this reactor, and polycondensation reaction was carried out at a temperature of 200 to 210°C while stirring under a nitrogen gas atmosphere. When the acid value reached 10 mgKOH / g, the mixture was cooled to 150°C, 8.0 mol of maleic anhydride was charged, and the reaction was carried out again at 210 to 220°C for 8 hours to obtain an unsaturated polyester with an acid value of 29.0 mgKOH / g.
[0162] Next, 60 parts by mass of the obtained unsaturated polyester was mixed with 40 parts by mass of styrene, thereby obtaining an unsaturated polyester resin.
[0163] <Production of vinyl ester resin> Manufacturing Example 2 A flask equipped with a thermometer, a nitrogen gas inlet tube, a reflux condenser and a stirrer was used as a reactor. 1850 parts by mass (10.0 equivalents) of bisphenol A type epoxy resin (epoxy equivalent 185), 317 parts by mass (2.78 equivalents) of bisphenol A, and 0.5 parts by mass of triethylbenzylammonium chloride as a catalyst were charged into this reactor, and reacted at 170°C for 5 hours while blowing in nitrogen to obtain an epoxy resin with an epoxy equivalent of 300. After cooling to 120°C, 2.0 parts by mass of hydroquinone as a polymerization inhibitor, 5.0 parts by mass of triethylbenzylammonium chloride as a catalyst, and 636 parts by mass (7.40 equivalents) of methacrylic acid were added, and reacted at 110°C for 8 hours while blowing in air to obtain a vinyl ester with an acid value of 6.7 mgKOH / g.
[0164] Next, 1869 parts of styrene (66.7 parts by mass relative to 100 parts by mass of vinyl ester) was added to the obtained vinyl ester to obtain a vinyl ester resin containing 40% by mass of styrene.
[0165] <Preparation of raw materials for nursing bathtubs and molding materials for nursing bathtubs> Example 1 The following ingredients were added in order and mixed to prepare a nursing bathtub ingredient. Unsaturated polyester resin: 70 parts by mass of the unsaturated polyester resin of Production Example 1 (42 parts by mass of unsaturated polyester, 28 parts by mass of styrene) Polymerizable monomer: 15 parts by mass of styrene Shrinkage reducing agent: 15 parts by weight of polystyrene solution (5 parts by weight of polystyrene, 10 parts by weight of styrene) Filler: 150 parts by weight of aluminum hydroxide Polymerization inhibitor: parabenzoquinone 0.05 parts by mass Hardener: 1 part by mass of t-amylperoxyisopropyl carbonate Release agent: zinc stearate 5 parts by weight Colorant: Polyester toner (white toner) 10 parts by weight Thickener: Magnesium oxide 1.0 parts by mass Next, using a known sheet molding compound (SMC) impregnation machine, glass roving was continuously cut into 1-inch pieces onto the nursing bathtub raw material applied onto a carrier film through a doctor blade, and added so that the glass fiber content was 25% by mass. Through the impregnation process, a nursing bathtub molding material (sheet molding compound (SMC)) was obtained. Next, this nursing bathtub molding material was aged at 40°C for 48 hours, and the viscosity was increased until the nursing bathtub molding material was in a state where it could be heated and compressed.
[0166] Examples 2 to 5, Comparative Examples 1 to 3 The raw material for a nursing bathtub and the molding material for a nursing bathtub were prepared in the same manner as in Example 1. However, the formulation of each component was changed based on the description in Table 1.
[0167] <Evaluation> [Production of test specimens] The molding material for nursing bathtubs of each Example and Comparative Example was subjected to heat compression molding using a flat metal plate to obtain a flat test piece of 300 mm x 300 mm x 4 mm.
[0168] [Chemical resistance] (Acid resistance test) The test pieces of each Example and Comparative Example were cut into 100 mm x 100 mm squares. The test pieces were then immersed in 10% hydrochloric acid and left at 25°C for 24 hours. The test pieces were then removed from the hydrochloric acid, thoroughly washed with water, and wiped with a dry cloth, after which the appearance of the test pieces was visually observed. The acid resistance test was evaluated based on the following criteria. The results are shown in Table 1. {standard} ◯: Almost no change in appearance was observed. ×: The gloss was reduced or the surface was corroded.
[0169] (Alkaline resistance test) The test pieces of each Example and Comparative Example were immersed in 10% sodium hypochlorite and left at 25°C for 48 hours. Thereafter, the test pieces were removed from the sodium hypochlorite solution, thoroughly washed with water, and wiped with a dry cloth, after which the appearance of the test pieces was visually observed. The alkali resistance test was evaluated based on the following criteria. The results are shown in Table 1. {standard} ◯: Almost no change in appearance was observed. ×: The gloss was reduced or the surface was corroded.
[0170] (Detergent resistance test) The test pieces of each Example and Comparative Example were immersed in a Magiclean Bath Cleaner (Kao Corporation) concentrate (undiluted detergent solution) and left at 25°C for 96 hours. The test pieces were then removed from the concentrate, thoroughly washed with water, and dried for 24 hours, after which the appearance of the test pieces was visually observed. The detergent resistance test was evaluated based on the following criteria. The results are shown in Table 1. {standard} ◯: Almost no change in appearance was observed. ×: The gloss was reduced or the surface was corroded.
[0171] (Bath additive resistance test) The test pieces of each Example and Comparative Example were immersed in a 50% solution of Bathclin Lavender Scent (manufactured by Bathclin Co., Ltd.) (bath additive solution) and left at 40°C for 96 hours. The test pieces were then removed from the bath additive solution, thoroughly washed with water, and dried for 24 hours, after which the ΔE of the test pieces was measured using a color difference meter. The bath additive resistance test was evaluated based on the following criteria. The results are shown in Table 1. {standard} ◯: ΔE was 2 or less. ×: ΔE exceeded 2.
[0172] [Molding of nursing bathtubs] A nursing bathtub was molded using the molding materials for each of the Examples and Comparative Examples. The molding temperature was upper mold / lower mold=145°C / 130°C, the molding holding time was 480 seconds, and the molding pressure was 10 MPa. A nursing bathtub molded product having a length of 1000 mm, a width of 2000 mm, and a height of 700 mm was obtained under the conditions of the following:
[0173] [exterior] (Glossy) The gloss of the upper edge surface of the nursing bathtub molded product of each Example and Comparative Example was measured in accordance with JIS Z8741 (1997) under the conditions of an incident angle of 60° and a receiving angle of 60°. The measurement was performed at each of the four corners of the upper edge surface of the bathtub, and the average of the four measured values was calculated. The results are shown in Table 1.
[0174] (Scumming) The upper edge surface and the slope surface of the nursing bathtub molded product of each Example and Comparative Example were visually inspected for the occurrence of scumming. Scumming was evaluated based on the following criteria. The results are shown in Table 1. {standard} ○: No scumming was observed by visual inspection. △: Slight scumming was observed visually. ×: A large amount of scumming was observed by visual inspection.
[0175] (Wavy) The upper edge surface and the slope surface of the nursing bathtub molded product of each Example and Comparative Example were visually checked for the presence or absence of waviness. The waviness was evaluated based on the following criteria. The results are shown in Table 1. {standard} ◯: No waviness was observed by visual inspection. △: Small waviness was observed by visual inspection. ×: Large waviness was observed by visual inspection.
[0176] (Number of cracks) The presence or absence of cracks was confirmed for the slope surface and the corners of the bathtub standing surface of the nursing care bathtub molded products of each Example and Comparative Example. The number of units in which cracks were observed during molding of 10 units is shown in Table 1.
[0177] [color] The color and Munsell color system (hue, value, saturation) of the test pieces of each Example and Comparative Example were confirmed. The results are shown in Table 1. The Munsell color system was displayed in accordance with JIS Z8721 (1993).
[0178] (Blood stain visibility) The blood adhesion visibility was evaluated for each Example and Comparative Example. Specifically, one drop (0.05 ml) of red dye as a substitute for blood was dropped into the bathtub using a microsyringe, and the adhesion was visually confirmed from a distance of 1 m. {standard} ○ The areas where the red dye had adhered were visible to the naked eye. ×: The areas where the red dye was attached were not visible to the naked eye.
[0179] [Table 1]
Claims
1. Contains a resin component and a filler, the filler comprises aluminum hydroxide; A raw material for nursing bathtubs, wherein the content of the aluminum hydroxide is 50 parts by mass or more per 100 parts by mass of the filler.
2. The filler further comprises calcium carbonate, The nursing bathtub raw material according to claim 1, wherein the content ratio of the calcium carbonate is 5 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the filler.
3. A molding material for a nursing bathtub comprising the raw material for a nursing bathtub according to claim 1 or 2 and reinforcing fibers.
4. A nursing care bath unit comprising a nursing care bath containing a cured product of the nursing care bath molding material according to claim 3.
5. The nursing bath unit according to claim 4, wherein the nursing bath is a light color having a lightness of 6 or more and a chroma of 8 or less in the Munsell color system.
Citation Information
Patent Citations
Unsaturated polyester resin composition, molding material and molding comprising the same
JP2006036839A
Photocurable resin composition and functional panel using the same
JP2011132479A
FRP molded article and member for bathroom using the same
JP2011183569A
Molding material, molded article, and artificial marble