Method for manufacturing semiconductor device
By employing a reducing gas supply and controlled film-forming process, the method prevents whisker formation in semiconductor devices, ensuring the integrity and functionality of the oxide semiconductor layer as a channel, thereby improving transistor characteristics.
Patent Information
- Application Number
- JP2023047815
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024136644000001_ABST
Abstract
Description
[Technical field]
[0001] The present embodiment relates to a method for manufacturing a semiconductor device. [Background technology]
[0002] Some semiconductor devices include a film containing an oxide of indium and a film containing tungsten. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US Patent Application Publication US2020 / 0185386 [Patent Document 2] US Patent Application Publication US2021 / 0125988 [Patent Document 3] US Patent Application Publication US2022 / 0102505 Summary of the Invention [Problem to be solved by the invention]
[0004] In the manufacturing process of a semiconductor device, when indium adheres to a film containing a metal such as tungsten, whiskers may easily occur.
[0005] An object of the present disclosure is to provide a method for manufacturing a semiconductor device that is capable of suppressing the occurrence of whiskers in a film containing metal. [Means for solving the problem]
[0006] A method for manufacturing a semiconductor device according to the present disclosure includes loading a substrate including a structure having a first surface exposing indium and a second surface exposing metal into a chamber of a film formation apparatus, supplying an indium reducing gas into the chamber at a first temperature, and, after supplying the reducing gas, supplying a film forming gas into the chamber at a second temperature higher than the first temperature. [Brief description of the drawings]
[0007] [Figure 1] 2 is a circuit diagram for explaining an example of a circuit configuration of a memory cell array according to the first embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view for explaining a structural example of the semiconductor memory device according to the first embodiment, showing a cross-sectional view parallel to the ZX plane. [Diagram 3] 2A to 2C are schematic diagrams illustrating a manufacturing process of the semiconductor device according to the first embodiment. [Figure 4] 2A to 2C are schematic diagrams illustrating a manufacturing process of the semiconductor device according to the first embodiment. [Diagram 5] 2A to 2C are schematic diagrams illustrating a manufacturing process of the semiconductor device according to the first embodiment. [Figure 6] 2A to 2C are schematic diagrams illustrating a manufacturing process of the semiconductor device according to the first embodiment. [Figure 7] 2A to 2C are schematic diagrams illustrating a manufacturing process of the semiconductor device according to the first embodiment. [Figure 8] 1 is a schematic diagram showing an example of a problem in a manufacturing process of a semiconductor device; [Figure 9] 1 is a schematic diagram showing an example of a problem in a manufacturing process of a semiconductor device; [Figure 10] 1 is a schematic diagram showing an example of a problem in a manufacturing process of a semiconductor device; [Figure 11] 3A to 3C are schematic diagrams for explaining a reaction between an indium reducing gas and ITO in the semiconductor device according to the first embodiment. [Figure 12] 3A to 3C are schematic diagrams for explaining a reaction between an indium reducing gas and ITO in the semiconductor device according to the first embodiment. [Figure 13] 5A to 5C are schematic diagrams illustrating a manufacturing process of the semiconductor device according to the second embodiment. [Figure 14] 10A to 10C are schematic diagrams illustrating a manufacturing process of the semiconductor device according to the third embodiment. [Figure 15] 10A to 10C are schematic diagrams showing a manufacturing process of the semiconductor device according to the fourth embodiment. [Figure 16] 13A to 13C are schematic diagrams showing a manufacturing process of the semiconductor device according to the fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, the present embodiment will be described with reference to the accompanying drawings. In order to facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals as much as possible, and duplicated description will be omitted.
[0009] [First embodiment] The configuration of the semiconductor memory device according to the first embodiment will be described. Each drawing may show an X-axis, a Y-axis, and a Z-axis. The X-axis, the Y-axis, and the Z-axis form a right-handed three-dimensional Cartesian coordinate system. Hereinafter, the direction of the X-axis arrow may be called the X-axis + direction, and the direction opposite to the arrow may be called the X-axis - direction, and the same applies to the other axes. The Z-axis + direction and the Z-axis - direction may be called "upper" and "lower", respectively. Furthermore, the planes perpendicular to the X-axis, Y-axis, or Z-axis may be called the YZ plane, ZX plane, or XY plane, respectively. Furthermore, the Z-axis direction may be called the "vertical direction". "Upward", "downward", and "vertical direction" are terms that merely indicate the relative positional relationship in the drawing, and are not terms that define the orientation based on the vertical direction.
[0010] In this specification, the term "connection" includes not only a physical connection but also an electrical connection, and unless otherwise specified, includes not only a direct connection but also an indirect connection.
[0011] The semiconductor memory device 101 according to the first embodiment is an oxide semiconductor random access memory (OS-RAM) and includes a memory cell array.
[0012] As shown in FIG. 1, the memory cell array includes a plurality of memory cells MC, a plurality of word lines WL, and a plurality of bit lines BL.
[0013] FIG. 1 shows a word line WL n, word line WL n+1 and word line WL n+2 (where n is a positive integer). Also, in FIG. 1, as an example of the bit line BL, m , bit line BL m+1 and bit line BL m+2 (where m is a positive integer.) The number of memory cells MC is not limited to the number shown in FIG.
[0014] A plurality of memory cells MC are arranged in, for example, a matrix to form a memory cell array. The memory cell MC includes a memory transistor MTR, which is a field effect transistor (FET), and a memory capacitor MCP.
[0015] A series of memory cells MC arranged in the row direction are connected to a word line WL (e.g., word line WL n A series of memory cells MC arranged in the column direction is connected to a bit line BL (e.g., bit line BL m+2 )
[0016] Specifically, the gate of the memory transistor MTR included in the memory cell MC is connected to a word line WL corresponding to the row to which the memory cell MC belongs, and one of the source and drain of the memory transistor MTR is connected to a bit line BL corresponding to the column to which the memory cell MC belongs.
[0017] One electrode of a memory capacitor MCP included in a memory cell MC is connected to the other of the source or drain of a memory transistor MTR included in the memory cell MC, and the other electrode of the memory cell MC is connected to a power supply line (not shown) that supplies a specific potential.
[0018] The memory cell MC is configured to be able to hold data by storing charge in the memory capacitor MCP due to a current flowing through the corresponding bit line BL, by switching the memory transistor MTR based on the potential of the corresponding word line WL.
[0019] As shown in FIG. 2, the semiconductor memory device 101 includes a semiconductor substrate 10, a circuit 11, a capacitor 20, a semiconductor device 30, a conductor 33, and insulating layers 34, 35, 45 and 63.
[0020] Capacitor 20 includes a conductor 21, an insulating film 22 (an example of a "dielectric film"), a conductor 23, a capacitor electrode 24 (an example of a "first capacitor electrode"), and a capacitor electrode 25 (an example of a "second capacitor electrode").
[0021] The semiconductor device 30 includes a field effect transistor 40 (an example of a "semiconductor element"), an upper electrode 50 provided above the field effect transistor 40, and a lower electrode 32 (an example of a "second conductive film") provided below the field effect transistor 40.
[0022] The field effect transistor 40 includes an oxide semiconductor layer 70 (an example of an "oxide semiconductor") corresponding to a channel, a gate insulating film 43 (an example of a "film"), and a conductive layer 42 (an example of a "gate electrode").
[0023] The oxide semiconductor layer 70 is formed in the insulating layer 45, and has an upper end 70a (an example of a "first end") and a lower end 70b (an example of a "second end"). The oxide semiconductor layer 70 is a columnar body extending in the Z-axis + direction (an example of a "first direction") from the lower end 70b to the upper end 70a. The oxide semiconductor layer 70 forms a channel of the field effect transistor 40, and the oxide semiconductor layer 70 has an amorphous structure.
[0024] The conductive layer 42 functions as a gate electrode of the field effect transistor 40, and faces between the upper end 70a and the lower end 70b of the oxide semiconductor layer 70 via the gate insulating film 43. The conductive layer 42 corresponds to the word line WL (see FIG. 1), and extends along an extension axis parallel to the Y axis.
[0025] The gate insulating film 43 is, for example, a silicon nitride film (Si3N4) containing silicon and nitrogen.
[0026] The upper electrode 50 is formed in the positive Z-axis direction with respect to the oxide semiconductor layer 70. The upper electrode 50 includes a metal oxide layer 50a (an example of a "first conductive film"), a barrier metal layer 50b, and a metal film 50c.
[0027] The metal film 50c includes tungsten (W) (an example of a "first metal"). The metal oxide layer 50a is formed between the metal film 50c and the upper end 70a of the oxide semiconductor layer 70. The metal oxide layer 50a includes indium. The metal oxide layer 50a includes, for example, indium and oxygen. The metal oxide layer 50a includes, for example, a metal oxide. The metal oxide includes, for example, indium and tin as metal elements. In this embodiment, the metal oxide layer 50a is formed of indium-tin-oxide (ITO).
[0028] The barrier metal layer 50b contains titanium and nitrogen, and is formed between the metal oxide layer 50a and the metal film 50c. In this embodiment, the barrier metal layer 50b is made of, for example, titanium nitride (TiN).
[0029] The conductive layer 51 is formed so as to be in contact with at least a portion of the upper surface of the upper electrode 50. The conductive layer 51 corresponds to the bit line BL (see FIG. 1), and extends along an extension axis parallel to the X-axis.
[0030] The insulating layer 63 is formed above the insulating layer 45. The insulating layer 63 covers the upper electrode 50 and the conductive layer 51.
[0031] The lower electrode 32 contacts a lower end 70b (an example of a "second end") of the oxide semiconductor layer 70. The lower electrode 32 contains indium. The lower electrode 32 contains, for example, indium and oxygen. The lower electrode 32 contains, for example, a metal oxide. The lower electrode 32 is formed, for example, by an ITO layer containing a metal oxide such as indium-tin-oxide, or ITO (an example of an "oxide of indium").
[0032] The circuit 11 constitutes peripheral circuits such as a decoder for selecting a specific memory cell MC from among a plurality of memory cells MC, i.e., capacitors 20 and field effect transistors 40, of the semiconductor memory device 101, a sense amplifier connected to the bit line BL, and a register constituted by an SRAM. The circuit 11 may include a CMOS circuit having field effect transistors, that is, a P-channel field effect transistor (Pch-FET) and an N-channel field effect transistor (Nch-FET), formed by a CMOS process.
[0033] The field effect transistors of the circuit 11 can be formed using a semiconductor substrate 10 such as a single crystal silicon substrate. The Pch-FET and Nch-FET are so-called horizontal field effect transistors that have a channel region, a source region, and a drain region in the semiconductor substrate 10 and have a channel for flowing carriers in the X-axis direction or the Y-axis direction approximately parallel to the surface of the semiconductor substrate 10 in a region close to the surface of the semiconductor substrate 10. The semiconductor substrate 10 may have a conductivity type of P type to N type. For convenience, FIG. 2 illustrates an example of the field effect transistor of the circuit 11.
[0034] The capacitor 20 is a memory capacitor MCP included in the memory cell MC (see FIG. 1). Although four capacitors 20 are illustrated in FIG. 2, the number of capacitors 20 is not limited to four.
[0035] In this embodiment, the capacitor 20 is provided above the semiconductor substrate 10. The capacitor electrode 24 of the capacitor 20 is connected to the conductor 21 and the lower electrode 32. The capacitor electrode 25 faces the capacitor electrode 24. The insulating film 22 is provided between the capacitor electrodes 24 and 25.
[0036] The capacitor 20 is a three-dimensional capacitor such as a pillar-type capacitor. Note that, as the capacitor of this embodiment, other capacitors having a configuration capable of storing electric charge may be adopted.
[0037] The conductor 21 abuts against the lower end face of the lower electrode 32 and has a shape extending downward from that end. The capacitor electrode 24 is formed so as to cover the lower electrode 32 and the conductor 21. The insulating film 22 is formed so as to cover the capacitor electrode 24. The capacitor electrode 25 surrounds a lower portion of the insulating film 22 and has a lower end abutting against the upper end face of the conductor 23.
[0038] The conductor 21 may include a material such as amorphous silicon. The insulating film 22 may include a material such as hafnium oxide. The conductor 23 and the capacitor electrodes 24 and 25 may include a material such as tungsten (W) and titanium nitride (TiN).
[0039] The conductor 33 includes a wiring that electrically connects the circuit 11 and the semiconductor device 30. The conductor 33 may include a via wiring, and has a via wiring that extends in the Z-axis direction as shown in Fig. 2, for example, and connects the word line WL and the circuit 11 provided on the semiconductor substrate 10. The conductor 33 includes, for example, copper.
[0040] The insulating layer 34 is provided between the plurality of capacitors 20. The insulating layer 34 is, for example, a silicon oxide film containing silicon and oxygen.
[0041] The insulating layer 35 is provided above the insulating layer 34. The insulating layer 35 is, for example, a silicon nitride film containing silicon and nitrogen.
[0042] The semiconductor device 30 is provided above the capacitor 20. A field effect transistor 40 in the semiconductor device 30 corresponds to the memory transistor MTR of the memory cell MC (see FIG. 1).
[0043] In the semiconductor device 30, the field effect transistor 40 is provided above the lower electrode 32. In particular, the oxide semiconductor layer 70 of the field effect transistor 40 is located in a direction away from the semiconductor substrate 10 with respect to the lower electrode 32, that is, above the lower electrode 32.
[0044] The upper electrode 50 is located in a direction away from the semiconductor substrate 10, i.e., above the oxide semiconductor layer 70. With this configuration, the field-effect transistor 40 is a so-called vertical transistor having a channel extending in the Z-axis direction (up-down direction) that is approximately perpendicular to the surface of the semiconductor substrate 10.
[0045] The oxide semiconductor layer 70 is a semiconductor in which oxygen vacancies serve as donors, and contains indium (In), zinc (Zn), and gallium (Ga) as metal elements. In particular, the oxide semiconductor layer 70 is an oxide of indium, gallium, and zinc, that is, IGZO (InGaZnO). The oxide semiconductor layer 70 may be another type of oxide semiconductor.
[0046] Although the structure in which the semiconductor device 30 is provided above the capacitor 20 has been shown, the capacitor 20 may be provided above the semiconductor device 30 .
[0047] [Method of manufacturing semiconductor device] A method for manufacturing the semiconductor device 30 will be described below as an example of a method for manufacturing the semiconductor device according to the first embodiment.
[0048] First, as shown in FIG. 3, a hole 71 (an example of a "structure") is formed so as to penetrate vertically by etching the insulating layer 45 and the conductive layer 42 formed on the semiconductor substrate.
[0049] The hole 71 is, for example, a transistor hole. The lower part of the hole 71 is a bottom surface 71a. The bottom surface 71a includes a surface 151 (an example of a "first surface") where the ITO is exposed. Specifically, the surface 151 is a part of the lower electrode 32 that is exposed when the hole 71 is formed.
[0050] The X-axis and Y-axis directions of the hole 71 are side surfaces 71b. The side surfaces 71b include a surface 152 (an example of a "second surface") where the tungsten is exposed. Specifically, the surface 152 is a part of the conductive layer 42 that is exposed when the hole 71 is formed.
[0051] Next, the gate insulating film 43 is formed in the hole 71. The gate insulating film 43 is formed according to the flow shown in FIG. 4. First, the semiconductor substrate including the semiconductor device 30 is loaded in a film forming apparatus at time t0. The film forming apparatus forms a film using, for example, atomic layer deposition (ALD). The film forming apparatus includes a chamber into which the semiconductor substrate is carried. The chamber includes a holder on which the carried-in semiconductor substrate is placed. Furthermore, the semiconductor substrate can be heated by a heater provided inside the holder.
[0052] Next, in a soak period T10 from time t10 to time t11, a reducing gas supply process is performed as a pre-processing for the process of forming the gate insulating film 43. In the reducing gas supply process, an indium reducing gas is supplied to the hole 71 including the surface 151 and the surface 152 at a first temperature.
[0053] The first temperature is preferably equal to or lower than 350° C. In this embodiment, the first temperature is, for example, 300° C. Note that the temperature in this embodiment is the set temperature of the heater.
[0054] The reducing gas for indium can be, for example, an inorganic material-based gas and an organic material-based gas, where the inorganic material-based gas contains, for example, a Si-X bond, where X is a halogen, such as F, Cl, Br, I, or At.
[0055] The inorganic material gas is, for example, a halide, such as HSiCl3 (trichlorosilane: TCS), H2SiCl2 (dichlorosilane: DCS), (SiCl3)2 (hexachlorodisilane: HCD), or SiH2I2 (diiodosilane).
[0056] The organic material gas includes, for example, at least one of a C-H bond and an N-C-H bond. Specifically, the organic material gas includes, for example, a gas in which three amino groups are bonded to SiH, such as [(CH3)2N]3SiH (Tris(dimethylamino)silane: TrisDMAS), a gas in which two amino groups are bonded to SiH2, such as [NH(C4H9)]2SiH2 (Bis(tertiary-butylamino)silane: BTBAS), a monoaminosilane-based material, and a carbon material.
[0057] The organic material gas may not contain silicon. The organic material gas may contain, for example, a metal such as Al, Ti, Zr, or Hf, and an amino group or C N -H M The organic material gas is, for example, trimethylaluminium (TMA).
[0058] In the reducing gas supply process in the soak period T10, the pressure in the chamber is 10 to 2000 Pa. The reducing gas for indium is, for example, HCD. HCD is supplied into the chamber together with N2 gas at 1 to 2000 sccm (standard cc / min).
[0059] The length of the soak period T10 (an example of the "first time") is 1 to 30 minutes. In this embodiment, the length of the soak period T10 is, for example, 10 minutes.
[0060] Next, a temperature rise process is performed during a temperature rise period T20 from time t11 to time t20. In the temperature rise process, the temperature of the semiconductor device 30 is raised from a first temperature to a second temperature without opening the chamber in which the semiconductor device 30 is stored to the atmosphere. That is, the supply of the indium reducing gas and the formation of the gate insulating film 43, which will be described later, are performed consecutively in the same chamber. In addition, during the temperature rise period T20, for example, N2 gas is supplied into the chamber.
[0061] Next, as shown in Fig. 4, a film formation process is performed during a film formation period T30 from time t20 to time t21. The film formation process is performed by supplying a film formation gas to the chamber at a second temperature higher than the first temperature. As shown in Fig. 5, a gate insulating film 43 is formed in the hole 71 in the semiconductor device 30.
[0062] In particular, the second temperature is equal to or higher than 400 degrees Celsius. In this embodiment, the second temperature is, for example, 450 degrees Celsius.
[0063] The formation of the gate insulating film 43 includes repeatedly supplying a first gas containing silicon for a second time period less than the length of the first time period and supplying a second gas containing nitrogen for a third time period less than the length of the first time period, where the second time period is less than or equal to 0.2 times the first time period, and the third time period is less than or equal to 0.2 times the first time period.
[0064] The first gas may be the same type of gas as the reducing gas used in the soak period T10. Specifically, the first gas is, for example, HCD. The second gas is, for example, NH3.
[0065] Specifically, in the film formation process, the supply of a first gas, which is a silicon supplying material, and the supply of a second gas, which is a nitriding agent such as NH3, N2H2, N2H4, or N3H8, are sequentially repeated.
[0066] In this embodiment, in the film formation process in the film formation period T30, the ALD unit process P300 is repeatedly executed. The ALD unit process P300 is repeated, for example, about 100 times.
[0067] The ALD unit process P300 includes processes P1, P2, P3, and P4. The processes P1, P2, P3, and P4 are executed in this order.
[0068] In the process P1, the first gas is supplied for a second time. Specifically, HCD, which is an example of the first gas, is supplied. The supply time of HCD (an example of the "second time") is, for example, 5 seconds or more and 30 seconds or less.
[0069] In process P2, the chamber is evacuated and then purged. The time for evacuating the chamber is, for example, 5 seconds or more and 60 seconds or less. The time for purging is, for example, 5 seconds or more and 60 seconds or less.
[0070] In the process P3, the second gas is supplied for a third time. Specifically, NH3, which is an example of the second gas, is supplied. The supply time of NH3 (an example of the "third time") is, for example, 10 seconds or more and 60 seconds or less.
[0071] In process P4, the chamber is evacuated and then purged for the next ALD unit process P300. The chamber is evacuated for, for example, 5 to 60 seconds. The purge time is, for example, 5 to 60 seconds.
[0072] By the film formation process in the film formation period T30, the gate insulating film 43 is formed on the bottom surface 71a and the side surface 71b of the hole 71 in the semiconductor device 30 (see FIG. 5).
[0073] Next, as shown in FIG. 6, the gate insulating film 43 formed above the lower electrode 32 is etched, so that the surface 151 of the lower electrode 32 is exposed.
[0074] Next, after the semiconductor substrate is unloaded from the chamber (Load out), an oxide semiconductor layer 70 is deposited inside the hole 71, as shown in Fig. 7. As a result, a channel is formed which is connected to the lower electrode 32 and has an opposing surface 70c which faces the conductive layer 42 via the gate insulating film 43.
[0075] The gate insulating film 43 may be, for example, a silicon oxide film or a laminate of a silicon oxide film and a silicon nitride film. The gate insulating film 43 may include, for example, a high dielectric material such as alumina (Al2O3). When the gate insulating film 43 is a silicon oxide film, the supply of a first gas which is a silicon supply material and the supply of a second gas which is an oxidizing agent such as O2, O3, or H2O are sequentially repeated.
[0076] (assignment) 8, it is assumed that the semiconductor device 30 is subjected to a heat treatment in a state in which the ITO is exposed at a surface 151 and the tungsten is exposed at a surface 152. For example, the heat treatment for forming the gate insulating film 43 is assumed.
[0077] At surface 151, the temperature rises due to heat, and indium contained in ITO sublimes. The sublimated indium may adhere to surface 152 to form indium chunks 91 on surface 152. Indium chunks 91 are, for example, metal crystal pieces or aggregates of minute atoms.
[0078] It should be noted that the adhesion of indium to the surface 152 may also occur when the holes 71 are formed by, for example, reactive ion etching.
[0079] 9, when heat treatment is performed with indium chunks 91 attached to surface 152 where tungsten is exposed, whiskers may form on surface 152. Whiskers are, for example, beard-like tungsten crystals that protrude outward from surface 152. Whiskers are likely to form at temperatures of 350 degrees Celsius or higher.
[0080] If the reducing gas supply process (see FIG. 4) during the soak period T10 is not performed and the film formation process is performed at 450° C., there is a high possibility that whiskers will be formed. When the whiskers grow, they may block part or all of the hole 71.
[0081] As shown in FIG. 10 , when a gate insulating film 93 and an oxide semiconductor layer 94 are formed on a semiconductor device 30 in which a part or all of the hole 71 is blocked, the oxide semiconductor layer 94 does not completely fill the hole 71, and therefore the oxide semiconductor layer 94 does not function as a channel, which is not preferable.
[0082] (effect) In this embodiment, as shown in Fig. 4, a reducing gas supply process is performed during the soak period T10, so that the indium lump 91 (see Fig. 8) on the surface 152 can be sublimated and reduced by the indium reducing gas. This makes it possible to prevent the hole 71 from being partially or entirely blocked, so that the gate insulating film 43 and the oxide semiconductor layer 70 can be formed well, and the oxide semiconductor layer 70 can function well as a channel. As a result, a semiconductor memory device having excellent transistor characteristics can be formed.
[0083] In the reducing gas supply process and film formation process, the following reaction occurs in the lower electrode 32 containing ITO. That is, as shown in FIG. 11, when a gas containing Si-X bonds is used as a reducing gas for indium, the indium contained in the ITO of the lower electrode 32 sublimes as an indium halide. The gas containing Si-X bonds is, for example, an inorganic material gas. The gas is, for example, HCD.
[0084] When indium sublimes, oxygen in ITO remains in ITO. Therefore, it is possible to suppress an increase in oxygen vacancies in ITO. The movement of oxygen from the oxide semiconductor layer 70 to the lower electrode 32 including ITO is suppressed. This stabilizes the amount of oxygen vacancies that become carriers in the oxide semiconductor layer 70, and thus stabilizes the threshold voltage.
[0085] When a gas containing Si-X bonds, such as HCD, is used as the reducing gas for indium, halogen may be contained in the lower electrode 32. When halogen atoms having a high electronegativity are contained in the lower electrode 32, the movement of oxygen in the ITO can be suppressed. The movement of oxygen in the oxide semiconductor layer 70 to the ITO can be suppressed.
[0086] Further, the lower electrode 32 includes portions 32a and 32b (see FIG. 7). The portion 32a is located at an upper portion inside the lower electrode 32 and includes a surface 151. The portion 32b is located below the portion 32a and does not include the surface 151. The lower electrode 32 includes a portion, such as the portion 32a, having a higher concentration of halogen atoms compared to the concentration of halogen atoms in a part or the entirety of the metal oxide layer 50a. For example, the portion 32a of the lower electrode 32 has a higher concentration of halogen atoms compared to the portion 32b.
[0087] 12, when an organic material-based gas is used as the reducing gas for indium, the oxygen contained in the ITO of the lower electrode 32 easily combines with hydrogen, reducing the oxygen in the ITO. As a result, the amount of indium that is not combined with oxygen increases, and indium sublimes because of its low melting point.
[0088] In this case, oxygen in the ITO in the lower electrode 32 is reduced, and the contact resistance between the lower electrode 32 and the oxide semiconductor layer 70 can be reduced, so that the on-current Ion of the field effect transistor 40 can be increased. In addition, the oxide semiconductor layer 70 may be formed in a tapered shape, and the contact area between the oxide semiconductor layer 70 and the lower electrode 32 at the lower end 70b may be smaller than the contact area between the oxide semiconductor layer 70 and the metal oxide layer 50a at the upper end 70a. In this case, the contact resistance between the lower electrode 32 and the oxide semiconductor layer 70 is lower than the contact resistance between the upper electrode 50 and the oxide semiconductor layer 70, so that good transistor characteristics can be obtained. Note that DCS containing both Si-X bonds and CH bonds is considered to cause the reaction shown in FIG. 12 because hydrogen in DCS reacts with indium first.
[0089] Furthermore, the concentration of silicon in the portion 32a is greater than the concentration of silicon in the portion 32b, because silicon is deposited on the surface 151 when the gate insulating film 43 is formed.
[0090] Furthermore, the concentration of indium in portion 32a is smaller than the concentration of indium in portion 32b in lower electrode 32. This is because, due to the above reaction, indium on surface 151 is halogenated and sublimated, or sublimated as it is.
[0091] Furthermore, when an organic material-based gas is supplied as the reducing gas for indium, the carbon concentration in the portion 32a is greater than the carbon concentration in the portion 32b in the lower electrode 32. Since carbon is a member of the same family as tin, the carbon in the lower electrode 32 has the same function as tin and increases the conductivity of ITO. Therefore, the conductivity in the portion 32a is greater than that in the portion 32b.
[0092] [Second embodiment] A method for manufacturing the semiconductor device 30 according to the second embodiment will be described. From the second embodiment onwards, a description of matters common to the first embodiment will be omitted, and only the differences will be described. In particular, similar effects due to similar configurations will not be mentioned in each embodiment.
[0093] As shown in FIG. 13, the manufacturing method of the semiconductor device 30 according to the second embodiment differs from the manufacturing method of the semiconductor device 30 according to the first embodiment shown in FIG. 4 in that film formation is performed at a low temperature after the reducing gas supply process in the soak period T10.
[0094] In the method for manufacturing the semiconductor device 30 according to the second embodiment, a film is formed on the structure after the indium reducing gas has been supplied at a temperature equal to or higher than the first temperature and lower than the second temperature.
[0095] In detail, a low-temperature film formation period T16 is provided between the soak period T10 and the temperature rise period T20. In this embodiment, in the low-temperature film formation process in the low-temperature film formation period T16, the ALD unit process P300 is repeatedly executed. The ALD unit process 300 repeated in the low-temperature film formation process is similar to the ALD unit process P300 shown in FIG.
[0096] The low-temperature film formation period T16 is shorter than the film formation period T30. The number of repetitions of the ALD unit process P300 in the low-temperature film formation period T16 is smaller than the number of repetitions of the ALD unit process P300 in the film formation period T30. In the low-temperature film formation period T16, the ALD unit process P300 is repeated, for example, 10 times, 50 times, or 100 times.
[0097] The temperature at which the low-temperature film formation process is performed is, for example, the same as the first temperature in the soak period T10, for example, 300 degrees Celsius. The temperature at which the low-temperature film formation process is performed may be any temperature that is equal to or higher than the first temperature and lower than the second temperature.
[0098] 13, the indium lump 91 attached to the surface 152 can be sublimated by the low-temperature film formation process in the soak period T10. As in the first embodiment, a semiconductor memory device having excellent transistor characteristics can be formed.
[0099] Furthermore, since a film is formed on the ITO of the lower electrode 32 by the low-temperature film formation process in the low-temperature film formation period T16, it is possible to protect the surface 151. This makes it possible to suppress the desorption of indium and oxygen from the ITO of the lower electrode 32, for example, as in the mechanism shown in Fig. 12, so that damage such as densification of the ITO of the lower electrode 32 due to heat can be suppressed.
[0100] [Third embodiment] A method for manufacturing the semiconductor device 30 according to the third embodiment will be described. As shown in Fig. 14, the method for manufacturing the semiconductor device 30 according to the third embodiment is different from the method for manufacturing the semiconductor device 30 according to the first embodiment shown in Fig. 4 in that an annealing process using ammonia is performed immediately before the reducing gas supply process in the soak period T10.
[0101] In the manufacturing method of the semiconductor device 30 according to the third embodiment, a fourth gas containing nitrogen is supplied to a hole 71 including a surface 151 exposing the ITO and a surface 152 exposing the tungsten at a third temperature to form a film on at least the surface 151.
[0102] In detail, an ammonia annealing period T5 is provided immediately before the soak period T10. In this embodiment, in the ammonia annealing process in the ammonia annealing period T5, ammonia gas is supplied into the chamber.
[0103] The length of the ammonia annealing period T5 is longer than that of the process P3. The length of the ammonia annealing period T5 is, for example, 10 to 60 minutes. In this embodiment, the ammonia annealing process is performed at a third temperature in the ammonia annealing period T5. The third temperature is lower than the second temperature. The third temperature is, for example, the same as the first temperature in the soak period T10, for example, 300 degrees Celsius. Note that the third temperature is preferably 350 degrees Celsius or lower.
[0104] 14, the surface 151 of the lower electrode 32 can be nitrided by the ammonia annealing treatment in the ammonia annealing period T5. It is possible to suppress sublimation of indium from the ITO in the lower electrode 32. As in the first embodiment, a semiconductor memory device having excellent transistor characteristics can be formed.
[0105] Furthermore, in T5, annealing is performed with ammonia, thereby nitriding the tungsten on the surface 152 of the conductive layer 42. This makes it possible to suppress the formation of whiskers when the indium chunks 91 adhere to the tungsten surface.
[0106] [Fourth embodiment] A method for manufacturing the semiconductor device 30 according to the fourth embodiment will be described. As shown in Fig. 15, the method for manufacturing the semiconductor device 30 according to the fourth embodiment is different from the method for manufacturing the semiconductor device 30 according to the third embodiment shown in Fig. 14 in that, instead of the ammonia annealing process in the ammonia annealing period T5, an annealing process using ammonia is performed immediately after the reducing gas supply process in the soak period T10.
[0107] In the method for manufacturing the semiconductor device 30 according to the fourth embodiment, a third gas containing nitrogen is supplied to the hole 71 after the indium reducing gas has been supplied, at a temperature equal to or lower than the first temperature.
[0108] In detail, an ammonia annealing period T15 is provided between the soak period T10 and the temperature rise period T20.
[0109] In this embodiment, the ammonia annealing treatment in the ammonia annealing period T15 is similar to the ammonia annealing treatment in the ammonia annealing period T5 shown in Figure 14. Note that the ammonia annealing treatment in the ammonia annealing period T15 may be different from the ammonia annealing treatment in the ammonia annealing period T5 shown in Figure 14.
[0110] The length of the ammonia annealing period T15 is longer than that of the process P3. The length of the ammonia annealing period T5 is, for example, 10 to 60 minutes. In the ammonia annealing period T15, the ammonia annealing process is performed at a fourth temperature. The fourth temperature is, for example, the same as the first temperature of the soak period T10, for example, 300 degrees Celsius. As in the first embodiment, a semiconductor memory device having excellent transistor characteristics can be formed.
[0111] Furthermore, in the method for manufacturing the semiconductor device 30 shown in FIG. 15, the surface 151 of the lower electrode 32 can be nitrided by the ammonia annealing treatment in the ammonia annealing period T15.
[0112] Furthermore, in T15, an annealing treatment using ammonia is performed to nitride the tungsten on the surface 152 of the conductive layer 42. By nitriding the tungsten, it is possible to suppress the formation of whiskers when the indium chunks 91 adhere to the tungsten surface.
[0113] Furthermore, for example, if the reducing gas supply process is performed sufficiently during the soak period T10, one or more layers of film are formed on the tungsten on the surface 152 of the conductive layer 42 by the reducing gas supply process. Then, during the ammonia annealing period T15, an annealing process using ammonia is performed to nitride the film on the tungsten. This makes it possible to prevent exposure of tungsten on the surface 152 of the conductive layer 42, thereby protecting the surface 152 from the formation of whiskers.
[0114] [Fifth embodiment] A manufacturing method of the semiconductor device 30 according to the fifth embodiment will be described. In the first embodiment, the manufacturing method in which indium reducing gas is supplied to the hole 71 which is a transistor hole is described, but in the fifth embodiment, a manufacturing method in which indium reducing gas is supplied to a groove formed between bit lines as shown in Fig. 16 will be described.
[0115] In the semiconductor device 30 according to the fifth embodiment, a bit line (BL)-landing pad (LP) groove 321 (an example of a "structure") is formed between two adjacent conductive layers 51. A conductor is filled into this BL-LP groove 321 in a subsequent process.
[0116] The BL-LP groove 321 is formed by etching. The BL-LP groove 321 has a bottom surface 321a on the lower side, is open on the upper side, and extends along the X-axis direction.
[0117] The bottom surface 321a below the BL-LP groove 321 includes a surface 161 (an example of a "first surface") to which the ITO is exposed. Specifically, the surface 161 is a part of the metal oxide layer 50a of the upper electrode 50 that is exposed when the BL-LP groove 321 is formed.
[0118] Side surface 321b of BL-LP groove 321 in the positive Y-axis direction includes surface 162 (an example of a "second surface") on which tungsten (an example of a "first metal") is exposed. Specifically, surface 162 is a part of metal film 50c, which is a landing pad, that is exposed when BL-LP groove 321 is formed.
[0119] In this manner, with ITO exposed at surface 161 and tungsten exposed at surface 162, for example, a film may be formed above insulating layer 66 in semiconductor device 30.
[0120] Heat treatment during film formation may cause indium contained in ITO to sublime on surface 161 , and the sublimated indium may adhere to surface 152 to form indium chunks 91 on surface 152 .
[0121] It should be noted that indium may also be deposited on surface 162 when BL-LP groove 321 is formed by, for example, reactive ion etching.
[0122] Even in such a case, the indium chunks 91 on the surface 162 can be sublimated and reduced by applying the manufacturing process shown in Figures 4, 13, 14, and 15. This makes it possible to suppress the generation of whiskers on the surface 162 that contains tungsten.
[0123] In the (a) embodiment, a configuration in which tungsten is exposed on the surfaces 152 and 162 has been described, but the present invention is not limited to this. The surfaces 152 and 162 may have a configuration in which another metal is exposed.
[0124] (b) In the embodiment, the configuration in which ITO is exposed on the surfaces 151 and 161 has been described, but the present invention is not limited to this. The surfaces 151 and 161 may have a configuration in which indium is exposed. The object of the present invention can also be achieved with this configuration.
[0125] (c) An insulating layer; an oxide semiconductor formed in the insulating layer, extending in a first direction, and having a first end and a second end; a first conductive film formed of a metal oxide and in contact with the first end of the oxide semiconductor; a second conductive film in contact with the second end of the oxide semiconductor and formed of the metal oxide; a gate electrode made of a metal, the gate electrode being opposed to the first end and the second end of the oxide semiconductor via an insulating film; the second conductive film includes a portion having a higher concentration of halogen atoms than a portion or the entirety of the first conductive film; Semiconductor device.
[0126] (d) An insulating layer; an oxide semiconductor formed in the insulating layer, extending in a first direction, and having a first end and a second end; a first conductive film formed of a metal oxide and in contact with the first end of the oxide semiconductor; a second conductive film in contact with the second end of the oxide semiconductor and formed of the metal oxide; a gate electrode disposed between the first end and the second end of the oxide semiconductor and facing the first end and the second end of the oxide semiconductor via an insulating film; The conductivity of the second conductive film is greater than the conductivity of the first conductive film. Semiconductor device.
[0127] (e) The semiconductor device; a first capacitor electrode connected to the first conductive film or the second conductive film; a second capacitor electrode facing the first capacitor electrode; a dielectric film provided between the first capacitor electrode and the second capacitor electrode. Semiconductor memory device.
[0128] The present embodiment has been described above with reference to specific examples. However, the present disclosure is not limited to these specific examples. Any design modifications made by a person skilled in the art to these specific examples are also included within the scope of the present disclosure as long as they have the features of the present disclosure. The elements of each of the above-mentioned specific examples and their arrangements, conditions, shapes, etc. are not limited to those exemplified and can be changed as appropriate. The combination of each of the elements of each of the above-mentioned specific examples can be changed as appropriate as long as no technical contradiction occurs. [Explanation of symbols]
[0129] 10...Semiconductor substrate 11...Circuit 20…Capacitor 21...Conductor 22...Insulating film 23...Conductor 24, 25...Capacitor electrodes 30...Semiconductor device 32…Lower electrode 32a, 32b...part 33...Conductor 34, 35…Insulating layer 40...Field effect transistor 42...Conductive layer 43...Gate insulating film 45…Insulating layer 50…Top electrode 50a...metal oxide layer 50b...Barrier metal layer 50c…Metal film 51...Conductive layer 63...Insulating layer 63a...side 64, 66…insulating layer 70...Oxide semiconductor layer 70a…Top end 70b…lower end 70c...Opposing surface 71...hole 71a…Bottom surface 71b…side 101...Semiconductor memory device 151, 152, 161, 162…Surface 321...BL-LP groove 321a…Bottom surface 321b…side P300…ALD unit processing T5, T15: Ammonia annealing period T10…Soak period T16…Low temperature film formation period T20: Temperature rise period T30…film formation period
Claims
1. Carrying a substrate including a structure having a first surface exposing indium and a second surface exposing a first metal into a chamber of a film forming apparatus; providing an indium reducing gas to the chamber at a first temperature; After supplying the reducing gas, supplying a film forming gas to the chamber at a second temperature higher than the first temperature. A method for manufacturing a semiconductor device.
2. The first metal includes tungsten. The method for manufacturing a semiconductor device according to claim 1 .
3. After the reducing gas is supplied, the film forming gas is supplied without opening the chamber to the atmosphere. The method for manufacturing a semiconductor device according to claim 1 .
4. The film forming gas includes the reducing gas. The method for manufacturing a semiconductor device according to claim 1 .
5. The second temperature is equal to or greater than 400 degrees Celsius. The method for manufacturing a semiconductor device according to claim 4 .
6. The supply of the film forming gas includes repeatedly supplying a first gas containing silicon and a second gas containing nitrogen; The method for manufacturing a semiconductor device according to claim 1 .
7. The supply of the reducing gas is performed for a first time period, The supply of the film forming gas includes repeatedly supplying the first gas for a second time period less than the first time period and supplying the second gas for a third time period less than the first time period. The method for manufacturing a semiconductor device according to claim 6 .
8. The second time is equal to or less than 0.2 times the first time. The method for manufacturing a semiconductor device according to claim 7 .
9. The first gas and the reducing gas are the same gas species. The method for manufacturing a semiconductor device according to claim 7 .
10. The method for manufacturing a semiconductor device includes: After supplying the reducing gas and before supplying the film forming gas at the second temperature, the method further includes supplying the film forming gas at a temperature lower than the second temperature. The method for manufacturing a semiconductor device according to claim 1 .
11. The method for manufacturing a semiconductor device includes: and prior to providing the reducing gas, providing a fourth gas containing nitrogen at a third temperature less than the second temperature. The method for manufacturing a semiconductor device according to claim 1 .
12. The method for manufacturing a semiconductor device includes: The method further includes supplying a third gas containing nitrogen at a fourth temperature that is equal to or lower than the first temperature after supplying the reducing gas and before supplying the film forming gas at the second temperature. The method for manufacturing a semiconductor device according to claim 1 .
13. The method for manufacturing a semiconductor device includes: and forming a structure having a bottom surface including the first surface where indium is exposed and a side surface including the second surface where the first metal is exposed by etching before supplying the reducing gas. The method for manufacturing a semiconductor device according to claim 1 .
14. The method for manufacturing a semiconductor device includes: After supplying the film forming gas, the substrate is removed from the chamber; forming an oxide semiconductor on the substrate removed from the chamber; the oxide semiconductor is connected to the first surface and faces the second surface via a film formed by supplying the film forming gas; The method for manufacturing a semiconductor device according to claim 12 .
15. The third temperature is less than or equal to 350 degrees Celsius. The method for manufacturing a semiconductor device according to claim 11 .
Citation Information
Patent Citations
Semiconductor device and method for manufacturing semiconductor device
US20200185386A1
Semiconductor Device and Method for Manufacturing Semiconductor Device
US20210125988A1
Semiconductor Device and Memory Device
US20220102505A1