Manufacturing method for plastering material, plastering material, and, plastering construction method
By kneading a grout composition with portland cement, a fluidizing agent, and fine aggregate, and adding dry ice, the method addresses on-site workability issues, enhancing sagging resistance and pot life in grout materials for concrete structures.
Patent Information
- Application Number
- JP2023048088
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Existing grout materials face challenges in achieving on-site workability adjustments, such as sagging resistance, plasterability, and pot life, due to difficulties in dispersing thickeners accurately and increased water-cement ratios when using liquid thickeners.
A manufacturing method involving kneading a grout composition with portland cement, a fluidizing agent, and fine aggregate, and adding dry ice in specific proportions to enhance sagging properties and pot life, without requiring special equipment.
The method produces a plastering material with improved sagging resistance, plasterability, and pot life, ensuring a good finished surface on concrete structures.
Smart Images

Figure 2024136822000001 
Figure 2024136822000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a manufacturing method of a plastering material, a plastering material, and a plastering method. [Background technology]
[0002] Grout, which is a cement-based material, is sometimes used to repair and reinforce ground, structures, etc. Grout generally has high fluidity and is therefore suitable for use as a filling material to fill gaps between components, narrow cavities, etc.
[0003] Grout materials are required to have various properties other than fluidity depending on the construction location and construction conditions. Therefore, in order to impart the required properties to the grout material, additives according to the required properties are sometimes added to the grout material. For example, Patent Documents 1 to 3 disclose grout materials to which a thickener is added. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-111343 A [Patent Document 2] JP 2019-006665 A [Patent Document 3] JP 2022-186934 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the application of cement-based materials has been expanded by adjusting the workability of the materials on-site. For example, when grout is used as a plastering material, it is necessary to provide the grout with all the required performance for the workability of a plastering material, namely (i) the material does not drip when applied to a vertical surface (drip resistance), (ii) good spreadability when spread with a trowel (plastering property), and (iii) the time required for work can be secured (pot life).
[0006] As a method for imparting the above-mentioned performance, for example, adding a thickener to a grout material (or grout composition) is considered. However, when trying to add a thickener to a grout composition at a construction site, if a powder thickener is used, there is a risk that the thickener will not disperse sufficiently, and since the optimal amount of thickener is very small, there is also a risk that it will be difficult to ensure the measurement accuracy at the site. When a liquid thickener is used, it is possible to increase the amount added compared to a powder, but the water-cement ratio of the plastering material increases, so there is a risk that the strength and crack resistance will decrease.
[0007] The present invention has been made in view of such a current situation, and aims to provide a method for producing a plastering material that can produce a plastering material with improved sagging properties, plastering properties, and pot life while using a grout composition. It also aims to provide a plastering material with improved sagging properties, plastering properties, and pot life while using a grout composition, and a plastering method using the plastering material. [Means for solving the problem]
[0008] The method for producing a plastering material according to the present invention is a method for producing a plastering material, and includes a kneading step of kneading a grout composition containing Portland cement, a fluidizing agent, and fine aggregate with water to obtain a kneaded mixture, and an adding step of adding dry ice to the kneaded mixture in an amount of 2.5% by mass or more and 30.0% by mass or less relative to the added amount of the Portland cement.
[0009] The method for producing the plastering material includes an addition step of adding 2.5% by mass or more and 30.0% by mass or less of dry ice relative to the amount of Portland cement added to the mixture formed by kneading a grout composition with water, thereby making it possible to produce a plastering material with improved dripping resistance, plastering properties, and pot life while using a grout composition.
[0010] Furthermore, since the manufacturing method of the plastering material includes the adding step, the plastering material can be easily manufactured at the construction site without using special equipment.
[0011] The plastering material according to the present invention contains water and a grout composition containing Portland cement, a fluidizing agent, and fine aggregate, and the carbon dioxide fixation rate in the plastering material is 4.1% or more and 5.5% or less.
[0012] The plastering material contains a grout composition containing Portland cement, a fluidizing agent, and fine aggregate, and water. Since the carbon dioxide fixation rate in the plastering material is 4.1% or more and 5.5% or less, it is possible to improve dripping resistance, plastering properties, and pot life while using the grout composition.
[0013] In the plastering method according to the present invention, the plastering material is applied to a portion of a concrete structure that needs to be repaired or reinforced.
[0014] In the plastering method, the plastering material can improve dripping resistance, plastering properties, and pot life while using a grout composition. Therefore, by applying the plastering material to the repaired or reinforced portion of a concrete structure, a good finished surface can be obtained. Effect of the Invention
[0015] According to the present invention, it is possible to provide a method for producing a plastering material that can produce a plastering material with improved dripping properties, plastering properties, and pot life while using a grout composition. It is also possible to provide a plastering material with improved dripping properties, plastering properties, and pot life while using a grout composition, and a plastering method using the plastering material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The manufacturing method of the plastering material, the plastering material, and the plastering method according to this embodiment will be described below.
[0017] <Manufacturing method of plastering materials> The manufacturing method of the plastering material according to the present embodiment includes a kneading step of kneading a grout composition containing Portland cement, a fluidizing agent, and fine aggregate with water to obtain a kneaded mixture, and an adding step of adding 2.5% by mass to 30.0% by mass of dry ice relative to the amount of Portland cement added to the kneaded mixture. Each material used in the manufacturing method of the plastering material according to the present embodiment will be described below, followed by a description of the manufacturing method of the plastering material.
[0018] The grout composition includes Portland cement, a fluidizing agent, and fine aggregate. In this specification, the grout composition is a material that is mixed with water and is preferably used as a filling material with high fluidity to fill gaps between components, narrow cavities, etc., and has a high fluidity of 300 mm or more without impact, measured based on JIS R 5201:2015, immediately after mixing with water. The grout composition may be a mixture of the materials constituting the grout composition in advance, or may be a mixture of the materials constituting the grout composition on-site.
[0019] Examples of Portland cement include ordinary Portland cement, high-early-strength Portland cement, ultra-high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, sulfate-resistant Portland cement, and white Portland cement, which are specified in JIS R 5210. Note that one type of Portland cement may be used alone, or two or more types may be used in combination.
[0020] The content of the Portland cement is preferably 20% by mass or more and 50% by mass or less, and more preferably 20% by mass or more and 45% by mass or less, based on the grout composition. When two or more types of Portland cement are contained, the above content is the total content. The content of the Portland cement is expressed, for example, by unit amount (kg / m 3 : 1 m of grout composition and water 3 Mass per unit: 300 kg / m 3 More than 1000kg / m 3It can be less than 400 kg / m 3 More than 900kg / m 3 In addition, when two or more types of Portland cement are contained, the above content is the total content.
[0021] Examples of the fluidizing agent include polycarboxylate-based, naphthalenesulfonate-based, ligninsulfonate-based, melaminesulfonate-based, etc. The fluidizing agent may be used alone or in combination of two or more kinds.
[0022] The content of the fluidizing agent is preferably 0.01% by mass or more and 2.0% by mass or less, and more preferably 0.01% by mass or more and 1.0% by mass or less, based on the grout composition. When two or more types of fluidizing agents are included, the above content is the total content.
[0023] Fine aggregate refers to aggregate that passes entirely through a 10 mm mesh sieve and 85% or more by mass through a 5 mm mesh sieve (JIS A 0203:2014). Examples of fine aggregate include naturally occurring sand such as mountain sand, river sand, land sand, sea sand, crushed sand, and limestone crushed sand, as specified in JIS A 5308 Appendix A Aggregates for Ready Mixed Concrete, sand derived from slag such as blast furnace slag, electric furnace oxidized slag, and ferro-nickel slag, recycled aggregate, artificial lightweight aggregate, and recycled aggregate. These fine aggregates may be used alone or in combination of two or more types.
[0024] The content of the fine aggregate is preferably 30% by mass or more and 80% by mass or less, and more preferably 40% by mass or more and 70% by mass or less, based on the grout composition. When two or more types of fine aggregate are included, the above content is the total content.
[0025] The grout composition may further contain an admixture. Examples of the admixture include inorganic fine powders such as silica fume, fly ash, ground granulated blast furnace slag, cement kiln dust, blast furnace fume, ground granulated converter slag, anhydrous gypsum, hemihydrate gypsum, dihydrate gypsum, expanding agent, ground limestone, ground quicklime, and ground dolomite, and inorganic fillers such as sodium bentonite, calcium bentonite, attapulgite, sepiolite, activated clay, acid clay, allophane, imogolite, shirasu (volcanic ash), shirasu balloon, kaolinite, metakaolin (calcined clay), synthetic zeolite, artificial zeolite, artificial zeolite, mordenite, and clinoptilolite. The admixture may be used alone or in combination of two or more kinds.
[0026] The content of the admixture may be 1.0% by mass or more and 20.0% by mass or less, and may be 5.0% by mass or more and 15.0% by mass or less, based on the grout composition. When two or more kinds of admixtures are included, the content is the total content.
[0027] The grout composition may further contain other admixtures other than the superplasticizer. Examples of the other admixtures include air-entraining agents, air-entraining water-reducing agents, high-performance water-reducing agents, separation-reducing agents, setting retarders (e.g., tartaric acid, etc.), setting accelerators (e.g., aluminum sulfate, etc.), quick-setting agents, shrinkage-reducing agents, foaming agents, foaming agents, waterproofing agents, and defoamers. The other admixtures may be used alone or in combination of two or more.
[0028] The content of the other admixtures may be 0.01% by mass or more and 5.0% by mass or less, and may be 0.05% by mass or more and 3.0% by mass or less, based on the grout composition. When two or more kinds of other admixtures are contained, the above content is the total content.
[0029] The water is not particularly limited, and for example, tap water, industrial water, recycled water, groundwater, river water, rainwater, etc. can be used.
[0030] Examples of dry ice include pellet-shaped dry ice, powdered dry ice, etc. One type of dry ice may be used alone, or different types of dry ice may be used in combination.
[0031] In the kneading step, a grout composition containing Portland cement, a fluidizing agent, and fine aggregate is kneaded with water to obtain a kneaded product. The method for kneading each material is not particularly limited, and for example, it can be kneaded by a conventionally known method using a mixer such as a hand mixer or a twin-axis forced kneading mixer. The kneading time can be, for example, 60 to 180 seconds, which is a time when the mixture is visually confirmed to be uniform.
[0032] The ratio (W / C) of the water (W) to the Portland cement (C) is preferably 30% to 80%, more preferably 35% to 70%, from the viewpoint of improving strength and workability. The ratio (W / B) of the water to the grout composition (B) is preferably 10% to 30%, more preferably 15% to 25%, from the viewpoint of improving strength and workability.
[0033] In the adding step, dry ice is added to the mixture obtained in the mixing step. The amount of dry ice added is 2.5% by mass or more and 30.0% by mass or less relative to the amount of Portland cement added, and from the viewpoint of ensuring workability as a plastering material, it is preferable that the amount of dry ice added is 2.8% by mass or more and 28.0% by mass or less relative to the amount of Portland cement added.
[0034] The manufacturing method of the plastering material according to the present embodiment may further include a dry ice kneading step of kneading the kneaded material with dry ice. In the dry ice kneading step, it is preferable to knead the kneaded material so that the evaporated carbon dioxide does not escape. For example, it is preferable to knead the kneaded material and dry ice in a container with a lid. The kneading time can be, for example, 60 to 300 seconds at which it is confirmed to be uniform by visual inspection (no white grains of dry ice remaining). The kneading time can be appropriately changed depending on the amount of dry ice added and the environmental temperature.
[0035] The manufacturing method of the plastering material according to the present embodiment includes the above-mentioned mixing step and adding step, and thus can manufacture a plastering material with improved dripping property, plastering property, and pot life while using a grout composition. In addition, the manufacturing method of the plastering material includes the adding step, and thus can manufacture the plastering material easily at a construction site without using special equipment.
[0036] <plastering materials> The plastering material according to this embodiment will be described below.
[0037] The plastering material according to this embodiment contains the grout composition containing Portland cement, a fluidizing agent, and fine aggregate described above, and water, and the carbon dioxide fixation rate in the plastering material is 4.1% or more and 5.5% or less.
[0038] From the viewpoint of ensuring the workability as a plastering material, the carbon dioxide fixation rate is 4.1% or more and 5.5% or less, and preferably 4.3% or more and 5.1% or less. The carbon dioxide fixation rate is determined by performing thermogravimetric differential thermal analysis (TG-DTA) on the plastering material and the grout composition. More specifically, immediately after the plastering material is mixed, 30 g is taken out in a zipper bag and sealed so as not to come into contact with air. The material is cured in an environment of room temperature 20°C and humidity 60% until the material age of 7 days, and on the 7th day, the material is finely crushed in an agate mortar or the like to be used as a sample for thermogravimetric differential thermal analysis (TG-DTA). The sample is heated to 1000°C at a heating rate of 10°C / min using a thermogravimetric differential thermal analyzer (atmosphere gas: air) to obtain a weight loss curve. The mass reduction in the endothermic peak range of 550 to 800°C in this weight loss curve is judged to be due to decarbonation of calcium carbonate contained in the plastering material, and the fixation rate (mass%) of carbon dioxide contained in the plastering material is calculated from the amount of reduction. Separately, a grout composition is used as a sample and subjected to thermogravimetric differential thermal analysis in the same manner to determine the carbon dioxide originally contained in the grout composition (i.e., the fixation rate of carbon dioxide contained in the grout composition) by the same measurement. The fixation rate of carbon dioxide in the plastering material is determined by subtracting the fixation rate of carbon dioxide contained in the grout composition from the fixation rate of carbon dioxide contained in the plastering material.
[0039] The plastering material according to the present embodiment can be manufactured by kneading the above-mentioned grout composition, dry ice, and water. The kneading method is not particularly limited, and for example, the mixture can be kneaded by a conventionally known method using a conventionally known mixer or the like.
[0040] The plastering material according to the present embodiment can be suitably used in the plastering method, spraying method, etc., which will be described later. In the spraying method, the plastering material is sprayed onto a portion of a concrete structure to be repaired or reinforced, using a device such as a mortar pump.
[0041] The plastering material of this embodiment contains a grout composition containing Portland cement, a fluidizing agent, and fine aggregate, and water. The carbon dioxide fixation rate in the plastering material is 4.1% or more and 5.5% or less, so that it is possible to improve dripping resistance, plastering properties, and pot life while using the grout composition.
[0042] <Plastering method> The plastering method according to this embodiment will be described below.
[0043] In the plastering method according to the present embodiment, the above-mentioned plastering material is applied to the portion of the concrete structure to be repaired or reinforced. More specifically, a craftsman places an appropriate amount of mortar on a mortarboard and applies the plastering material to the portion of the concrete structure to be repaired or reinforced using a metal trowel or the like.
[0044] In the plastering method according to the present embodiment, the plastering material can improve dripping, plastering properties, and pot life while using a grout composition. Therefore, by applying the plastering material to the repaired or reinforced portion of a concrete structure, a good finished surface can be obtained.
[0045] The present invention includes the following aspects. [1] A method for producing a plastering material, comprising the steps of: A kneading step of kneading a grout composition containing Portland cement, a fluidizing agent, and fine aggregate with water to obtain a kneaded mixture; and an adding step of adding to the kneaded mixture 2.5% by mass or more and 30.0% by mass or less of dry ice relative to the amount of Portland cement added. [2] A grout composition comprising Portland cement, a fluidizing agent, and fine aggregate, and water; A plastering material with a carbon dioxide fixation rate of 4.1% or more and 5.5% or less. [3] A plastering method in which the plastering material described in [2] is applied to the repair or reinforcement areas of a concrete structure. EXAMPLES
[0046] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0047] The grout composition and water were put into a container with a lid having a hole in the lid for the shaft of a hand mixer so as to obtain the composition shown in Table 1, and mixed for 2 minutes with a hand mixer (Makita Corporation mixer UT1305) using a crown-shaped blade at a rotation speed of 1300 rpm to obtain a mixed material (mixing step). More specifically, the mixing was performed for 30 seconds while the grout composition was put into the water, and then for 60 seconds, after which the hand mixer was stopped and scraped off for 30 seconds. Next, the dry ice shown in Table 1 was put into the mixed material at the addition rate shown in Table 1 (addition step), the lid of the container was immediately closed, and the mixture was mixed for 120 seconds with the hand mixer to obtain plastering materials of each Example and each Comparative Example. The room temperature when the plastering materials were produced was 20°C, and the humidity was 60% RH.
[0048] Details of each material shown in Table 1 are given below. Grout compositions (1) to (3): Commercially available grout compositions (containing fine aggregate, flow inhibitor, and fly ash in addition to Portland cement) Dry ice: Dry ice pellets (φ3m×1cm) Dry ice snow (powdered carbon dioxide) Water: Tap water
[0049] [Table 1]
[0050] [Flow test] For the plastering materials of each Example and Comparative Example, the flow values were measured immediately after mixing and 15 minutes after mixing, based on JIS R 5201: 2015, at no impact and after 15 impacts. The measured values are shown in Table 2.
[0051] [Carbon dioxide fixation rate] The plastering materials of each Example and Comparative Example were subjected to thermogravimetric differential thermal analysis (TG-DTA) to determine the fixation rate of carbon dioxide. More specifically, immediately after the plastering material was mixed, 30 g was taken into a zipper bag and sealed to prevent contact with air. The material was cured in an environment of room temperature 20°C and humidity 60% until the material was 7 days old, and on the 7th day old, it was finely crushed in an agate mortar or the like to be used as a sample for thermogravimetric differential thermal analysis (TG-DTA). The sample was heated to 1000°C at a heating rate of 10°C / min using a thermogravimetric differential thermal analyzer (atmosphere gas: air) to obtain a weight loss curve. The mass reduction in the endothermic peak range of 550 to 800°C in this weight loss curve was determined to be due to decarbonation of calcium carbonate contained in the plastering material, and the fixation rate (mass%) of carbon dioxide contained in the plastering material was calculated from the reduction amount. Separately, the grout composition was used as a sample and subjected to a thermogravimetric differential thermal analysis in the same manner to determine the carbon dioxide originally contained in the grout composition (i.e., the fixation rate of carbon dioxide contained in the grout composition) in the same manner. The value obtained by subtracting the fixation rate of carbon dioxide contained in the grout composition from the fixation rate of carbon dioxide contained in the plastering material was regarded as the fixation rate of carbon dioxide of the plastering material.
[0052] [Sagging] The sagging property was evaluated as "good" when the flow value without impact, measured immediately after mixing, was 150 mm or less, and "poor" when it exceeded 150 mm. The evaluation results are shown in Table 2.
[0053] [Plastering] The plastering properties were evaluated as follows: if the difference in flow value between 15 blows and no blows, measured 15 minutes after mixing, was 30 mm or more, it was evaluated as "Good", and if it was less than 30 mm, it was evaluated as "Poor". The evaluation results are shown in Table 2.
[0054] [Pot life] The pot life was evaluated as "good" when the difference between the flow value without impact measured 15 minutes after mixing and the flow value without impact measured immediately after mixing was less than 40 mm, and as "poor" when it was 40 mm or more. The evaluation results are shown in Table 2. The evaluation results are shown in Table 2.
[0055] [Table 2]
[0056] As can be seen from the results in Table 2, the plastering materials of the respective Examples which satisfy all of the constituent requirements of the present invention can improve dripping properties, plastering properties, and pot life while using a grout composition.
Claims
1. A method for producing a plastering material, comprising the steps of: A kneading step of kneading a grout composition containing Portland cement, a fluidizing agent, and fine aggregate with water to obtain a kneaded mixture; and an adding step of adding dry ice to the kneaded mixture in an amount of 2.5% by mass or more and 30.0% by mass or less relative to the amount of Portland cement added.
2. A grout composition including Portland cement, a flow agent, and fine aggregate, and water, A plastering material having a carbon dioxide fixation rate of 4.1% or more and 5.5% or less.
3. A plastering method comprising applying the plastering material according to claim 2 to a portion of a concrete structure to be repaired or reinforced.
Citation Information
Patent Citations
Concrete placing method
JP1999303398A
Method and device for mixing carbon dioxide with concrete
JP1999324324A
Method for fixing carbon dioxide
JP2022131308A
Production method of cement composition
JP2023018308A
Repair material, repair mortar composition, and cured product
JP2023030482A