Refractory material for iron making
By adding metal silicon fine powder to ironmaking refractories in a specific ratio with titania and optionally carbon black, the refractory structure is stabilized, addressing thermal shock-induced cracking and maintaining corrosion resistance, enhancing durability in blast furnaces.
Patent Information
- Application Number
- JP2023048725
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Existing ironmaking refractories using silicon carbide and titania suffer from significant cracking due to thermal shock during the initial stages of operation, particularly in blast furnace gutters, despite efforts to enhance corrosion resistance.
Incorporating metal silicon fine powder in a specific mass ratio to titania fine powder, along with carbon black if present, to stabilize the refractory structure and suppress cracking by generating titanium carbide and carbonitride fine particles, thereby restricting shrinkage and agglomeration.
The proposed refractory composition effectively suppresses cracking and maintains thermal shock resistance and corrosion resistance, ensuring durability in high-temperature ironmaking processes.
Smart Images

Figure 2024137267000002 
Figure 2024137267000001
Abstract
Description
[Technical field]
[0001] The present invention relates to refractories for ironmaking, such as pourable materials, pumped materials, precast blocks, sprayed materials, trowel coating materials, and tamping materials, which are used in blast furnaces, blast furnace troughs, torpedo cars, torpedo furnaces, etc. [Background technology]
[0002] In the field of refractories for pig iron making, a technique of using a large amount of silicon carbide or carbonaceous raw materials to ensure corrosion resistance is widely used. However, due to oxidation of silicon carbide, etc., a decrease in corrosion resistance can become a problem. As a countermeasure, for example, the use of titanium carbide as a raw material for refractories has been proposed as in Patent Document 1. However, since titanium carbide is expensive, it is not industrially realistic to use titanium carbide as a raw material for refractories.
[0003] On the other hand, for example, Patent Document 2 proposes a technique for maintaining and improving corrosion resistance by forming titanium carbide by reacting titania with silicon carbide during operation. That is, Patent Document 2 discloses a monolithic refractory material characterized in that, in 100 mass% of a refractory composition, 5 to 35 mass% of silicon carbide fine powder having a particle size of 0.3 mm or less is contained as refractory fine powder, 3 to 20 mass% of titania fine powder having a particle size of 0.3 mm or less is contained as refractory fine powder, and 0.5 to 8 mass% of alumina cement is contained as a hardener. Patent Document 2 also describes that titanium carbide and titanium carbonitride are produced by the reaction of silicon carbide and titania, and an example shows that the material has excellent corrosion resistance in an induction furnace corrosion test using molten iron and blast furnace slag as corrosion agents. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-16698 A [Patent Document 2] Patent No. 4922851 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors conducted a laboratory evaluation of cracking of the monolithic refractory material of Patent Document 2, assuming actual use in a plant, and found that cracking was prominent. This cracking phenomenon was found to occur prominently, for example, in a blast furnace trough, when the castable material was applied and the applied body was dried and directly exposed to high-temperature slag and molten iron in the initial stage of operation.
[0006] An object of the present invention is to suppress cracking due to thermal shock in the initial stage of operation in a refractory for pig iron making containing silicon carbide and titania. [Means for solving the problem]
[0007] The present inventors have found that in a refractory for iron-making containing silicon carbide fine powder and titania fine powder, the thermal shock resistance is significantly improved by containing metal silicon fine powder at a specific mass ratio to the titania fine powder. This will be specifically described below.
[0008] In refractories containing silicon carbide and titania fine powders, titanium carbide and carbonitride fine particles are generated in the high temperature range (when the temperature of the refractory in the ironmaking process is between about 1350°C and 1600°C), and these fine particles aggregate together. This aggregation causes contraction inside the refractory. This contraction causes destruction of the internal structure of the refractory, leading to cracking and spalling of the entire refractory. It has been found that this cracking phenomenon hardly occurs when the rate of temperature rise or heat reception is slow, but it almost certainly occurs when there is a large temperature change, such as when receiving pig iron from a temperature of several hundred degrees.
[0009] Here, when the titania fine powder contains metal silicon fine powder at a specific mass ratio, the metal silicon fine powder is oxidized, silica is generated in the fine powder region, and new solids are generated between particles larger than the fine powder region. As a result, a state in which pillars are formed inside the refractory is created, and the structure is stabilized. In such a stabilized structure, even if the refractory is exposed to a rapid heating condition in which the time from room temperature to high temperature is short and the temperature gradient inside the refractory is large, the shrinkage of the fine powder region due to the generation and aggregation of titanium carbide and carbonitride fine particles in the high temperature range is limited, and the occurrence of cracks, etc. can be suppressed.
[0010] Furthermore, in trough materials and the like, carbon black, which is a fine carbon powder with an average particle size of 1 μm or less, is sometimes added to prevent over-sintering and suppress the infiltration of slag. However, it has been found that when carbon black is present in combination with silicon carbide fine powder and titania fine powder, cracks will occur unless a larger amount of metal silicon powder is added compared to when neither is present.
[0011] The present invention has been made based on the above findings, and the gist of the present invention is as follows. A refractory for pig iron making, comprising, based on 100 mass% of a refractory composition, 5 mass% or more and 35 mass% or less of silicon carbide fine powder having a particle size of less than 0.3 mm, 3 mass% or more and 20 mass% or less of titania fine powder having a particle size of less than 0.3 mm, and 6 mass% or less of metal silicon fine powder having a particle size of less than 75 μm, and having a carbon black content of 5 mass% or less (including 0), and further wherein the content of the metal silicon fine powder (Si), the content of the titania fine powder (TiO2), and the content of the carbon black (C) satisfy the following formula (1): Si / TiO2≧0.11×C+0.1 … Formula (1) Effect of the Invention
[0012] According to the present invention, in an iron-making refractory containing silicon carbide and titania, cracking due to thermal shock in the initial stage of operation can be suppressed. [Brief description of the drawings]
[0013] [Figure 1]1 is a graph showing the results of a thermal shock test carried out on a refractory material for ironmaking intended as a pourable material for a blast furnace trough. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] As described above, in the formula (1) of the present invention, "Si" represents the content of metal silicon fine powder, which is metal silicon having a particle size of less than 75 μm, "TiO2" represents the content of titania fine powder, which is titania having a particle size of less than 0.3 mm, and "C" represents the content of carbon black. These "contents" refer to mass ratios in 100% by mass of the refractory composition. That is, in the formula (1), "Si / TiO2" means the mass ratio of metal silicon fine powder to titania fine powder. Therefore, in the following description, "Si / TiO2" will be expressed as "Si / TiO2 ratio".
[0015] In the case where the refractory composition of the ironmaking refractory of the present invention does not contain carbon black, the above formula (1) becomes Si / TiO2≧0.1, which means that the Si / TiO2 ratio must be 0.1 or more. In other words, if the Si / TiO2 ratio is less than 0.1, the thermal shock resistance becomes insufficient. On the other hand, if the content of the metal silicon fine powder exceeds 6 mass%, the by-product silica is generated in excess, which leads to a decrease in corrosion resistance. In other words, since silica has a high dissolution rate in slag, a refractory material containing an excess amount of silica has a high dissolution rate. Therefore, in the present invention, the upper limit of the content of the metal silicon fine powder is set to 6 mass%.
[0016] On the other hand, when the refractory composition of the present invention contains carbon black, when the carbon black in the refractory reacts with the titania fine powder to produce titanium carbide due to heat during use, the solid volume decreases and shrinks before and after the reaction. Therefore, it is necessary to increase the amount of metallic silicon according to the carbon black content to cancel the decrease in solid volume. As a result of various tests, it was found that it is necessary to satisfy formula (1).
[0017] FIG. 1 shows the results of a thermal shock test performed on a refractory for ironmaking, which is assumed to be a castable material for a blast furnace trough, under different conditions of carbon black content and Si / TiO2 ratio in the refractory composition, and plots the results. In FIG. 1, ◯ indicates that no cracks or cracks occurred, and × indicates that cracks or cracks occurred. The solid line in FIG. 1 is an approximation line based on three points (carbon black content, Si / TiO2 ratio) = (0, 0.1), (2, 0.35), and (5, 0.65). Specifically, the intercept is (0, 0.1), and the line is approximated by the least squares method, and the formula representing this line is the above formula (1). The results of this thermal shock test were performed under the same conditions as in the example, using the material of Example 14 described later as the base.
[0018] In the refractory for pig iron making of the present invention, the refractory composition contains silicon carbide fine powder, which is silicon carbide having a particle size of less than 0.3 mm, in addition to the titania fine powder and metal silicon fine powder described above. That is, in the present invention, in order to ensure corrosion resistance, particularly slag resistance, silicon carbide fine powder is used at a content of 5% by mass or more and 35% by mass or less as a carbon source for producing titanium carbide from titania fine powder. If the content of silicon carbide fine powder is less than 5% by mass, the slag resistance is insufficient and the amount of titanium carbide produced is insufficient, which also leads to insufficient slag resistance. On the other hand, if the content of silicon carbide fine powder exceeds 35% by mass, the corrosion resistance against molten pig iron decreases. As the silicon carbide fine powder, any powder that is generally used as a raw material for refractories can be used without any problems. Furthermore, the purity of the silicon carbide that can be used is 85% by mass or more.
[0019] In addition, titania fine powder is used at a content of 3% by mass or more and 20% by mass or less in order to improve corrosion resistance by becoming carbide during use. If the content of titania fine powder is less than 3% by mass, the generation of carbide is small, resulting in insufficient corrosion resistance. On the other hand, if the content of titania fine powder exceeds 20% by mass, the fine powder portion becomes too large, making it difficult to ensure uniformity of the structure, and for example, in the case of a cast material, the fluidity is easily impaired. As the titania fine powder, any titania commonly used as a raw material for refractories can be used without any problems. The purity of titania can be 90% by mass or more. From the viewpoint of improving corrosion resistance, the purity can be 93% by mass or more. The particle size of the titania fine powder is less than 0.3 mm, but it is also possible to use titania fine powder with a finer particle size, for example, a particle size of less than 44 μm, or even an average particle size of 1 μm or less.
[0020] In addition, by using titania fine powder that has been subjected to an easy-dispersion surface treatment (hereinafter referred to as "easy-dispersion surface treatment type"), the adsorption of dispersants, which are widely used in casting materials, is increased, and a casting material with good fluidity can be obtained. The easy-dispersion surface treatment of titania involves co-precipitating sodium aluminate, aluminum sulfate, sodium silicate, etc. with sulfuric acid or sodium hydroxide, and subjecting the surface of titania to an inorganic treatment in a wet manner, thereby modifying the interfacial potential of titania. In this way, by using the easy-dispersion surface treatment type titania fine powder, it becomes easier to ensure fluidity at low moisture, especially in the case of casting materials. In addition, when molding such as pressing, low moisture / low liquid differentiation is possible, making it easier to obtain a dense structure.
[0021] In the refractory composition for the pig iron making refractory of the present invention, other refractory raw materials may be used as required, such as electrically fused or sintered products of alumina, spinel, mullite, magnesia, zirconia, silica fume, clay, zircon, silicon nitride, carbons, etc. Also, graphite powder, pitches, etc. may be used as carbons.
[0022] The refractory for pig iron making of the present invention is a refractory used in the pig iron making process, which is produced by using water as mixing water, molding, and then heat treatment at 1200°C or less. More specifically, it can be an amorphous refractory such as a castable material, a precast block, a spraying material, a trowel coating material, and a tamping material. Among these, the castable material for blast furnace troughs contains a large amount of silicon carbide and is required to have corrosion resistance, so that by applying the present invention, a material excellent in corrosion resistance and thermal shock resistance can be obtained, and therefore, it is the most suitable application for the present invention.
[0023] When the refractory for pig iron making of the present invention is used as a castable material, a binder generally used in conventional castable materials can be used, for example, a water-soluble binder such as alumina cement, silica sol, alumina sol, sodium silicate, sodium aluminate, phosphates, etc. The content of the binder in the refractory composition can be 0.5% by mass or more and 5% by mass or less in terms of solid content. Furthermore, dispersants generally used in conventional pouring materials can also be used. Examples of dispersants include sodium tripolyphosphate, sodium hexametaphosphate, sodium ultrapolyphosphate, acidic sodium hexametaphosphate, sodium polymetaphosphate, polyacrylates, polycarboxylates, β-naphthalenesulfonates, naphthalenesulfonic acid, melaminesulfonates, etc. The content of the dispersant in the fireproof composition can be 0.01% by mass or more and 1% by mass or less. Furthermore, drying accelerators and antioxidants that are generally used in conventional pouring materials can also be used. Drying accelerators that can be used include organic fibers, foaming agents, basic aluminum lactate, etc. Specific examples of organic fibers include polymeric organic fibers such as vinylon (including polyvinyl alcohol), rayon, polyester, nylon, polypropylene, and polyethylene. Borides, glass powder, etc. can be used as antioxidants. In addition, in the case of materials other than pourable materials, binders and dispersants used in conventional spray materials, trowel coating materials, tamping materials, etc. can also be used.
[0024] Here, the particle size in the present invention refers to the size of the sieve openings when the refractory raw material particles are sieved to separate them. For example, metallic silicon having a particle size of less than 75 μm refers to metallic silicon that passes through a sieve with 75 μm openings, and metallic silicon having a particle size of 75 μm or more refers to metallic silicon that does not pass through a sieve with 75 μm openings. The average particle size in the present invention refers to the volume average particle size corresponding to the median cumulative value (D50) of a cumulative curve measured with a laser diffraction scattering type particle size distribution analyzer. EXAMPLES
[0025] Table 1 shows the evaluation results of the refractory compositions and the resulting refractories in the examples of the present invention and the comparative examples. In the refractory compositions of each example shown in Table 1, the spinel was an electrofused spinel containing 72% by mass of Al2O3 and 28% by mass of MgO, with a particle size of less than 8 mm, the titania fine powder was TiO2 containing 93% by mass and having an average particle size of 1 μm or less, the silicon carbide fine powder was SiC containing 95% by mass and having a particle size of less than 75 μm, the carbon black was C containing 98% by mass and having an average particle size of 1 μm or less, and the calcined alumina was Al2O3 containing 99% by mass and having an average particle size of 4 μm or less. In addition, except for Example 17, the titania was a readily dispersible surface-treated type that had been subjected to a readily dispersible surface treatment using alumina and silica hydrate in combination. In Example 17, a non-easily dispersible surface-treated type that had not been subjected to a readily dispersible surface treatment was used.
[0026] [Table 1]
[0027] The kneaded mixture obtained by adding 5% by mass of water to 100% by mass of the fire-resistant composition of each example and kneading the mixture was evaluated for thermal shock resistance, corrosion resistance, and fluidity in the following manner. <Thermal shock resistance> The above mixture was vibrated and poured into a 40 x 40 x 160 mm mold, cured (24 hours at 20°C) and dried (24 hours at 110°C) to obtain a test piece. The test piece was then heated at 500°C for 3 hours. The reason for heating at 500°C is that there is a risk of explosion if volatile matter such as moisture from the binder remains when the test piece is immersed in 1550°C molten iron. The crucible was set in a high-frequency induction furnace, and after it was confirmed that the pig iron had melted in the furnace and reached 1550℃, the test piece was dropped into the molten iron, and after 20 minutes had passed, the test piece was pulled out and visually inspected for the presence of cracks or breaks to evaluate thermal shock resistance. Specifically, if no cracks or breaks were found after pulling up, they were rated as ◎ (pass (excellent)), if microcracks were found, they were rated as ◯ (pass (good)), and if moderate to low cracks or breaks were found, they were rated × (fail). <Corrosion resistance> The kneaded material was vibrated and poured into a mold, cured (at 20°C for 24 hours) and dried (at 110°C for 24 hours) to obtain a test piece. The test piece was then set on the wall of a high-frequency induction furnace, and after confirming that the pig iron had melted in the furnace, blast furnace slag was added on top of it to evaluate the corrosion resistance. The test temperature and time were 1550°C x 6 hours. The dimensional difference between each test piece before and after the test was taken as the corrosion damage dimension, and the corrosion damage index was calculated with the corrosion damage dimension of Comparative Example 1 taken as 100. The smaller the corrosion damage index value, the better the corrosion resistance. Specifically, the corrosion damage index was 80 or less, ⊚ (pass (excellent)), 80 to 100, ◯ (pass (good)), and over 100, × (fail). <Liquidity> In the evaluation of fluidity, the tap flow value of the above kneaded product was measured in accordance with JIS R2521. A tap flow value of 150 mm or more was rated as ⊚ (pass (excellent)), a value of 130 mm or more but less than 150 mm was rated as ◯ (pass (good)), and a value less than 130 mm was rated as × (fail).
[0028] In Examples 1 to 8, the Si / TiO2 ratios were different within the range of the present invention in systems that did not contain carbon black, but the results showed excellent thermal shock resistance and corrosion resistance. In contrast, Comparative Example 1 does not contain metal silicon fine powder, and the thermal shock resistance is poor. Comparative Examples 2 to 4 contain metal silicon fine powder, but the Si / TiO2 ratio is below the lower limit of the present invention, and the thermal shock resistance is poor. On the other hand, Comparative Example 5 contains metal silicon fine powder and the content rate exceeds the upper limit of the present invention, and the corrosion resistance is poor.
[0029] Examples 9 and 10 have different contents of titania fine powder, but they are within the range of the present invention and provide good results. Although Examples 11 and 12 have different contents of silicon carbide fine powder, they were within the range of the present invention and provided good results.
[0030] Examples 13 to 16 are carbon black-containing systems with Si / TiO2 ratios that are within the range of the present invention, but the thermal shock resistance and corrosion resistance are excellent. In contrast, Comparative Examples 6 to 9 are carbon black-containing systems with Si / TiO2 ratios that are outside the range of the present invention, and the thermal shock resistance is poor.
[0031] In Example 17, a non-easily dispersible surface-treated titania fine powder was used, and the fluidity was inferior to that of the case where an easily dispersible surface-treated titania fine powder was used, but the thermal shock resistance and corrosion resistance were sufficient.
Claims
1. The refractory composition contains, in 100 mass%, 5 mass% or more and 35 mass% or less of silicon carbide fine powder having a particle size of less than 0.3 mm, 3 mass% or more and 20 mass% or less of titania fine powder having a particle size of less than 0.3 mm, and 6 mass% or less of metal silicon fine powder having a particle size of less than 75 μm, and the carbon black content is 5 mass% or less (including 0), and further the content of metal silicon fine powder (Si), the content of titania fine powder (TiO 2 ), and a carbon black content (C) satisfying the following formula (1): Si / TiO 2 ≥ 0.11 × C + 0.1... Equation (1)
2. 2. The refractory for pig iron making according to claim 1, wherein the fine titania powder is surface-treated for easy dispersibility.
3. 3. The refractory for pig iron making according to claim 1 or 2, which is used in a location where pig iron making slag and molten pig iron coexist, or in a boundary area between pig iron making slag and molten pig iron.
4. 3. The refractory for pig iron making according to claim 1 or 2, which is a castable material used for a blast furnace trough.
Citation Information
Patent Citations
Refractory composition
JP1981005379A
Monolithic refractory
JP2009013036A
Monolithic refractory for blast furnace iron spout
JP2010235342A
JP1974022851A
Monolithic refractory containing silicon carbide and titanium carbide
JP2011016698A
Cited By
Aluminum sol combined silicon carbide spray coating, protective layer and preparation method and application thereof
CN119161754A