Hydrogen storage alloy
The CaCu5 hydrogen storage alloy with engineered lattice porosity and reduced cobalt content addresses the challenges of cost and pulverization in nickel-metal hydride batteries, enhancing life characteristics and reducing material costs.
Patent Information
- Application Number
- JP2024020078
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hydrogen storage alloys for nickel-metal hydride batteries face challenges in maintaining life characteristics and reducing material costs, particularly due to the high cost and increased pulverization from repeated hydrogen absorption and release when the cobalt content is reduced.
A hydrogen storage alloy with a CaCu5 crystal structure is developed, where the cobalt content is minimized, and the crystal lattice is engineered to have a porosity of 23.20% or more by replacing some constituent atoms with elements having different metal bond radii, ensuring minimal volume change during hydrogen absorption and release, thereby suppressing pulverization.
The alloy effectively reduces raw material costs and maintains or improves the life characteristics of the negative electrode by preventing pulverization, making it suitable for use in nickel-metal hydride batteries.
Smart Images

Figure 2024137734000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a CaCu alloy used as the negative electrode of a nickel-metal hydride battery. 5 The present invention further relates to a negative electrode using this hydrogen storage alloy and a battery using this negative electrode. [Background technology]
[0002] Nickel-metal hydride batteries, which use a hydrogen storage alloy in the negative electrode, were commercialized in the early 1990s and have since become widely used.
[0003] When nickel-metal hydride batteries were first commercialized, they were used as power sources for mobile phones and laptops. They have since been gradually replaced by smaller, lighter lithium-ion batteries, and are now used in toys, small devices, and even hybrid cars due to their good balance of low cost, high safety, and energy density per volume.
[0004] The hydrogen storage alloy used in such nickel-metal hydride batteries is an alloy that reacts with hydrogen to form a metal hydride, and is capable of reversibly absorbing and releasing large amounts of hydrogen at around room temperature.
[0005] Hydrogen storage alloys include LaNi 5 AB, represented by 5 Type alloy, ZrV 0.4 Ni 1.5 AB, represented by 2 In addition to type alloys, AB type, A 2 Type B, AB 3 Various types of alloys are known, including those with a high affinity for hydrogen and a high hydrogen storage capacity (rare earth elements, Ca, Mg, Ti, Zr, V, Nb, Pt, Pd, etc.), and those with a relatively low affinity for hydrogen and a low storage capacity (Ni, Mn, Co, Al, etc.), which promote the hydrogenation reaction and lower the reaction temperature.
[0006] Among these, CaCu 5 AB type crystal structure 5 Hydrogen storage alloys of this type, for example, alloys that use misch metal (hereinafter referred to as "Mm"), a rare earth mixture, in the A site and elements such as Ni, Mn, Co, and Al in the B site, can form negative electrodes using relatively inexpensive materials compared to alloys of other compositions.
[0007] A.B. 5 In the case of hydrogen storage alloys, various characteristics such as the charge / discharge capacity, input / output characteristics, and cycle life of the negative electrode can be adjusted by adjusting the ratio of the B site atomic weight to the A site atomic weight (AB ratio) and the amount of Ni substituted with Co, Mn, Al, etc. 5 This type of hydrogen storage alloy makes it possible to produce nickel-metal hydride batteries for a variety of applications.
[0008] In order to popularize hybrid vehicles, it is necessary to reduce the manufacturing cost of nickel-metal hydride batteries and to further improve the life and input / output characteristics of the negative electrode. One of these is the AB 5 In hydrogen storage alloys of this type, there have been studies focusing on the "segregation phase" in the alloy in order to maintain and improve the life characteristics.
[0009] For example, in Patent Document 1, CaCu is used as the active material for the hydrogen storage alloy electrode. 5 The hydrogen storage alloy powder has a crystal structure of the type MmMgNiCoMnAl, and fine segregation phases of MgNiCoMnAl alloy phase are dispersed at least inside the hydrogen storage alloy powder. It is also proposed to preferably apply a hydrogen storage alloy powder having a surface layer of an alloy of Ni and Co on the surface of the hydrogen storage alloy powder. By doing so, it is said that the hydrogen storage alloy powder is prevented from becoming fine.
[0010] Patent Document 2 proposes a rare earth-based hydrogen storage alloy that contains a misch metal with a La content of 60-90 wt%, Mg, Ni, Co, Mn, and Al, and has a Mg content of 2-6 atomic % based on the total amount of the misch metal and Mg, and is characterized in that at least one segregated phase exists in the matrix, and the Mg concentration in the segregated phase is higher than that in the matrix. By doing so, the segregated phase in the alloy is selectively corroded during battery activation, and the surface area increases from the vicinity of the segregated phase, resulting in early activation of the alloy.
[0011] Patent Document 3 also proposes using, as the negative electrode active material, a hydrogen storage alloy containing Mm (Mm represents a mixture of two or more rare earth elements containing 30% by weight or more of La) and at least Ni, Co, Mn, and Al as constituent elements, in which the hydrogen storage alloy has a segregation phase mainly composed of Ni, and the number of segregation phases exposed in any 15 μm square region of the alloy cross section (the number of segregation phases having a minimum diameter of a circle circumscribing the segregation phase and a diameter of 0.05 μm or more) is 1 to 40. This is said to achieve high capacity, high rate discharge at low temperature, and excellent high-temperature storage characteristics.
[0012] In Patent Document 4, CaCu 5A hydrogen storage alloy has been proposed that has a mother phase of the crystalline structure, and that is characterized in that the Fe / Mn peak ratio [Fe / Mn ratio], which is the ratio of the Fe peak intensity of the segregated phase to the Fe peak intensity of the mother phase when analyzed by point analysis with an energy dispersive X-ray analyzer (EDX), [{(Fe peak intensity of segregated phase) / (Fe peak intensity of mother phase)}×100(%)], and the Mn peak intensity ratio [{(Mn peak intensity of segregated phase) / (Mn peak intensity of mother phase)}×100(%)], is the ratio of the Mn peak intensity of the segregated phase to the Mn peak intensity of the mother phase, is 0.12<[Fe / Mn ratio]<0.37. This is because it is known that the pulverization characteristics (life characteristics) are improved by containing Fe, and therefore by substituting a part of Ni with Fe, excellent cycle characteristics are obtained. More specifically, the segregation phase acts as a cushion to reduce distortion caused by the expansion and contraction of the lattice due to hydrogen absorption and release in the parent phase.
[0013] Furthermore, in Patent Document 5, there is disclosed an alloy represented by the general formula MmNixMy (Mm is a mixture of misch metal or rare earth elements, M is at least one element selected from the group consisting of Al, Mn, Co, Cu, Fe, Cr, Ti and V, and 5.0≦x+y≦5.5), and the alloy structure is CaCu 5 A hydrogen storage alloy has been proposed that is composed of a phase having a crystal structure of the type that reversibly absorbs and releases hydrogen, and one or more phases that are mainly composed of elements other than Mm and do not absorb hydrogen, with the latter phase being dispersed in the former phase like islands. By doing so, it is said that it is possible to combine a long life and excellent high-rate discharge characteristics without containing a large amount of Co. In other words, it is said that some of these alloys have compositions in which Ni is partially replaced by Fe or Cr, and as a result, it is said that the phase that does not absorb hydrogen makes the hydrogen-absorbing phase itself structure resistant to stress.
[0014] Furthermore, in Patent Document 6, Mm (misch metal) consisting of La and Ce occupies the A site, and Ni, Co, Mn and Al, or Ni, Mn and Al occupy the B site, AB 5In this type of hydrogen storage alloy, if the Co content is reduced to 0.11 or less in terms of the Co / Mm molar ratio, the Al / Mn molar ratio is 0.35 to 1.10, and the c-axis length / a-axis length of the crystal is 0.8092 or more, it is possible to prevent a decrease in the battery life characteristics when used as the negative electrode active material of a nickel-metal hydride battery while reducing the Co content. According to the above description, only La and Ce occupy the A site, but in a composition where the molar ratio x of ABx is 5.0 or more, CaCu 5 It is extremely difficult to form a crystal structure of this type. This is because when the A site is filled with only La and Ce and the ABx molar ratio is 5+α, the crystal structure is [A 5 / (5+α) V A 1-5 / (5+α) ]B 5 This is because, although it is necessary to form 1-5 / (5+α) A-site vacancies at the A site, in reality, some B atoms will occupy part of the A site. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] JP 2005-93297 A [Patent Document 2] JP 2004-269929 A [Patent Document 3] JP 2000-353542 A [Patent Document 4] JP 2009-30158 A [Patent Document 5] Japanese Patent Application Publication No. 7-286225 [Patent Document 6] WO2021-220824 Summary of the Invention [Problem to be solved by the invention]
[0016] As mentioned above, the maintenance and improvement of life characteristics has been considered. In recent years, the trading price of Co has risen sharply, and AB containing Co 5In order to maintain or reduce the raw material costs of this type of hydrogen storage alloy, it is desirable to further reduce the Co content or to eliminate it altogether.
[0017] However, A.B. 5 When the Co content of the hydrogen storage alloy is reduced, the alloy is pulverized due to repeated absorption and release of hydrogen, and the life characteristics of the negative electrode tend to decrease. In the examples of Patent Documents 1 to 6, attention is paid to the segregation phase, and some of the constituent atoms are replaced with other elements to maintain the life characteristics, but in reality, a certain amount of Co is contained, and further study is required to achieve both a reduction in the Co content and the life characteristics of the negative electrode.
[0018] The present invention has been made in consideration of the above problems, and 5 The objective of the present invention is to provide a hydrogen storage alloy having a crystalline structure that can suppress raw material costs by reducing the Co content and can suppress pulverization of the alloy due to repeated absorption and release of hydrogen, as well as a negative electrode and a battery using the hydrogen storage alloy. [Means for solving the problem]
[0019] In order to solve the above problems, the present inventors have conducted extensive research and have discovered 5 In hydrogen storage alloys with a crystalline structure, we reduced the Co content to reduce raw material costs, and then investigated methods to replace the pulverization suppression effect of Co. As a result, we came to the conclusion that it is possible to suppress pulverization of the alloy due to repeated absorption and release of hydrogen by ensuring sufficient intralattice porosity in the crystal lattice formed by the filling of the atoms that make up the hydrogen storage alloy, so that the volume change is small even when hydrogen atoms enter. 5 The present inventors have found that by substituting a part of the constituent atoms of a hydrogen storage alloy having a crystalline structure with an element X and ensuring a predetermined range of intralattice porosity, it is possible to reduce the Co content while suppressing pulverization, thereby completing the present invention.
[0020] The gist of the present invention is as follows.
[0021] (1) General formula MmNi a Mn b Al c Co d (wherein Mm is a misch metal, and the formula is represented by 4.30≦a≦4.75, 0.25≦b≦0.50, 0.25≦c≦0.45, 0≦d≦0.12, and 5.20≦a+b+c+d≦5.55) 5 A hydrogen storage alloy having a crystalline structure, in which a part of the constituent atoms represented by the general formula is substituted with another substitution element X, and the intralattice void ratio represented by the following formula is 23.20% or more and 23.70% or less. Intra-lattice void ratio = (crystal lattice volume - total volume of constituent atoms) / crystal lattice volume x 100 (2) Among the constituent atoms represented by the general formula, one or more target elements Y2 selected from the group consisting of Ni, Mn, and Al are replaced by the replacement element X to form a composition formula of MmNi a-a1 Mn b-b1 Al c-c1 X e Co d (wherein e=a1+b1+c1, 5.20≦a+b+c+d+e≦5.55) is satisfied. (3) The hydrogen storage alloy according to (2), wherein the X atom has a metallic bond radius larger than that of the atom to be substituted. (4) The hydrogen storage alloy according to (1) or (2), wherein Mm contains a rare earth metal having an atomic radius smaller than that of Ce. (5) The hydrogen storage alloy according to (1) or (2), characterized in that the pulverization difficulty of the hydrogen storage alloy is 0.55 or more. (6) A negative electrode comprising the hydrogen storage alloy according to (1) or (2) as a negative electrode active material. (7) A battery using the negative electrode according to (6). Effect of the Invention
[0022] According to the present invention, it is possible to provide a hydrogen storage alloy in which the raw material cost is reduced by reducing the Co content and the pulverization of the alloy due to repeated hydrogen absorption and release is suppressed, and the alloy can be effectively used in anodes and batteries. When the hydrogen storage alloy of the present invention is used as the anode active material of a battery, the amount of Co used can be reduced while maintaining or improving the life characteristics. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a schematic diagram showing the crystal structure of an AB5 type alloy, where (a) shows the case where the stoichiometric ratio of A and B is 5.0, and (b) shows the case where the stoichiometric ratio exceeds 5.0, in which some of the A-site atoms are missing. [Diagram 2] FIG. 2 is a schematic diagram showing the state in which two B atoms are substituted in a dumbbell shape at the A site of the crystal structure shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will be described in detail below.
[0025] The present inventors have 5 In hydrogen storage alloys having the crystalline structure, the pulverization caused by hydrogen absorption and desorption and its suppression were investigated in detail, taking into consideration the suppression effect of Co on pulverization and alternative methods for Co. First, the effect of suppressing fine powder by Co is shown in CaCu 5 When Co is added to a hydrogen storage alloy with the crystalline structure (when it is replaced with Co), the metallic bond radius of Co is replaced by LaNi 5 Since the atomic radius of Ni in the crystal lattice is almost the same (see Non-Patent Document 1, "Sanderson Inorganic Chemistry Vol. 1," translated by Fujiwara Yasuo, Hirokawa Shoten, 1969, p. 87), the crystal lattice size (crystal lattice volume) hardly changes even when Ni atoms are substituted with Co atoms. However, in the crystals of hydrogen storage alloys to which Co has been added, the volume change during hydrogenation (hydrogen absorption) is small, making them difficult to pulverize.
[0026] Here, cracking of hydrogen storage alloys due to hydrogenation (hydrogen absorption) occurs because hydrogen atoms H enter the alloy crystals in an interstitial manner, causing the crystals to expand. It is believed that during the hydrogenation process, stress is generated between the part that has expanded due to hydrogenation and the part that has not yet been hydrogenated at the interface between the part that has not yet been hydrogenated. This is because stress is also generated in the reverse reaction of hydrogenation (hydrogen release). In other words, if the stress generated above exceeds the strength of the alloy crystal, it will crack, so if the deformation (expansion) of the alloy crystal due to hydrogenation is small, the generated stress will also be small, making the alloy crystal less likely to crack, i.e., less likely to pulverize.
[0027] Next, consider why the volume change of a hydrogen storage alloy becomes smaller when Co atoms, which have almost the same metallic bond radius as Ni atoms, are added. As mentioned above, hydrogen storage alloys hydrogenate as an interstitial hydrogen atom, which enters between the atoms that make up the alloy crystal, and so the alloy crystal normally expands significantly. However, we came to the conclusion that the expansion of the alloy crystal is suppressed because the electron cloud of the Co atom easily overlaps with the electron cloud of the hydrogen atom to form a covalent bond. Comparing the d electron configurations of Co and Ni, they each have a 3d 7 4s 2 and 3D 8 4s 2 Therefore, the Co atom has a higher covalent bond order with the hydrogen atom through the d-electrons, and the electron clouds overlap more. In other words, even if the hydrogen atom H enters the alloy crystal lattice, there is little expansion.
[0028] In light of the above, when considering alternatives to Co, elements with a d-electron configuration capable of forming covalent bonds are considered. However, although iron (Fe) and manganese (Mn) have a d-electron configuration with a higher covalent bond order, their metallic bond radii are large (see Non-Patent Document 1 above), and they are less effective in reducing the expansion of alloy crystals through covalent bonds with hydrogen (H).
[0029] Another idea is to enlarge the lattice of the alloy crystal in advance. This is a simple idea that if the lattice of the alloy crystal is enlarged in advance, the expansion will be small even if hydrogenated. To enlarge the alloy crystal lattice, there are methods such as substituting an atom having a larger metallic bond radius than nickel (Ni) at the Ni site (B site) (for example, see J.-M. Jouberta, et.al., Journal of Alloys and Compounds 330-332 (2002) 208-214; see Non-Patent Document 2), or making the B / A molar ratio (x value of ABx) of the A site and the B site non-stoichiometric to 5.0 or more (for example, see M. Latroche, et.al., Journal of Solid State Chemistry 146, 343-321 (1999); see Non-Patent Document 3).
[0030] When the latter ABx composition is made non-stoichiometric with x being 5.0 or more, unlike the above-mentioned Patent Document 6, the crystal structure becomes [AB 2 / 7×α ]B 5+(5 / 7)α When a B atom occupies an A site, two B atoms are substituted for the A site in a dumbbell shape. 5 The crystal structure of the type alloy is shown diagrammatically, where (a) is the case where the stoichiometric ratio of A to B is 5.0, and (b) is the case where the stoichiometric ratio exceeds 5.0, with some of the A site atoms missing. Figure 2 shows the state where two B atoms are substituted in a dumbbell shape at the A site. The inventors have attempted various alloy designs, believing that expanding the lattice of the alloy crystal in this way, especially in the c-axis direction, can suppress cracking (pulverization) of the alloy crystal due to hydrogen absorption and release.
[0031] After further detailed investigations, the inventors found that alloys with expanded crystal lattice are not necessarily less prone to pulverization, and that in particular, when the Co content is low or zero, it becomes difficult to suppress pulverization simply by expanding the crystal lattice.
[0032] As a result of investigating the above-mentioned causes, the inventors discovered that even if the crystal lattice of the hydrogen storage alloy is expanded, if the space for hydrogen atoms H to enter is not secured, pulverization cannot be suppressed even for alloys with large crystal lattices, leading to the present invention. In other words, it is important to form larger spaces in the crystal lattice of the alloy so that there is little change even if hydrogen atoms H enter. Specifically, it was discovered that pulverization can be suppressed by setting the intralattice porosity, expressed by the following formula, to 23.20% or more. Intra-lattice void ratio = (crystal lattice volume - total volume of constituent atoms) / crystal lattice volume × 100 They also found that the change caused by the intrusion of hydrogen atoms becomes smaller when the electron density (= number of electrons / atomic volume) of the atoms constituting the hydrogen storage alloy, together with the intralattice porosity, becomes smaller. Note that the above intralattice porosity was calculated excluding the volume of each constituent atom in the crystal lattice volume of the hydrogen storage alloy.
[0033] Here, in order to increase the lattice void ratio, it is not enough to simply substitute with atoms having a large metallic bond radius or to expand the crystal lattice by performing dumbbell-shaped substitution at the A site as described above; it is necessary to select the atom to be substituted and the atom that actually substitutes (substituting element), and the inventors have found that it is particularly effective to secure space by appropriately substituting with atoms having a small metallic bond radius.
[0034] Thus, the present invention relates to a compound having the general formula MmNi a Mn b Al c Co d (wherein Mm is a misch metal, and is represented by 4.30≦a≦4.75, 0.25≦b≦0.50, 0.25≦c≦0.45, 0≦d≦0.12, and 5.20≦a+b+c+d≦5.55), and CaCu 5The present invention relates to a hydrogen storage alloy having a lattice void ratio of 23.20% or more and 23.70% or less, wherein some of the constituent atoms represented by the general formula above are replaced by atoms having a smaller metallic bond radius than the constituent atoms, or by atoms having a larger metallic bond radius than the constituent atoms, or by both atoms having a smaller metallic bond radius than the constituent atoms and atoms having a larger metallic bond radius than the constituent atoms, and the hydrogen storage alloy has an intralattice void ratio of 23.20% or more and 23.70% or less, as represented by the following formula: Intra-lattice void ratio = (crystal lattice volume - total volume of constituent atoms) / crystal lattice volume × 100
[0035] The CaCu of the present invention 5 Hydrogen storage alloys with AB type crystal structure 5 In the hydrogen storage alloy of the type, the metal (atom) constituting the A site will be described first. In the present invention, La or a misch metal (Mm) in which part or all of La is a rare earth metal mixture is used as the metal constituting the A site. In Mm, La and Ce preferably occupy a ratio within a range of 80 mass% to 100 mass% with respect to the total mass of Mm, and more preferably, La is in the range of 70 to 99 mass%, and Ce is in the range of 1 to 30 mass%, and more preferably, La is in the range of 74 to 97 mass%, and Ce is in the range of 3 to 26 mass%.
[0036] Next, the metals (atoms) constituting the B site will be described. In the present invention, Ni, Mn, Al, and Co are used as the metals constituting the B site. The molar ratio of these metals in the general formula satisfies the following conditions. Ni molar ratio (a) 4.30≦a≦4.75 Mn molar ratio (b) 0.25≦b≦0.50 Al molar ratio (c) 0.25≦c≦0.45 Co mole ratio (d) 0≦d≦0.12 A-B ratio 5.20≦(a+b+c+d)≦5.55 The preferred conditions are as follows: Ni molar ratio (a) 4.40≦a≦4.70 Mn molar ratio (b) 0.35≦b≦0.43 Al molar ratio (c) 0.38≦c≦0.42 Co mole ratio (d) 0≦d≦0.05 A-B ratio 5.25≦(a+b+c+d)≦5.46
[0037] The molar ratio d of Co is preferably as small as possible to reduce the cost of raw materials, and is set to 0≦d≦0.12. By making d larger than 0 and equal to or smaller than 0.12, i.e., by substituting Co, the alloy is less likely to pulverize even when hydrogen is repeatedly absorbed and released, and this tendency becomes more pronounced as the amount of substitution increases. However, even if d=0, i.e., no Co substitution is performed, the AB of the present invention can be obtained. 5 By making the alloy into a hydrogen storage alloy of this type, it is possible to make it difficult for the alloy to pulverize even if it repeatedly absorbs and releases hydrogen. Therefore, the Co molar ratio (d) is 0≦d≦0.12, and preferably 0≦d≦0.05. Note that if d exceeds 0.12, it will not lead to a reduction in raw material costs.
[0038] The reason why the ratio of La, Ce, Ni, Mn, and Al in Mm was set as above is that 5 This is because the hydrogen storage capacity (H / M) of the hydrogen storage alloy is set to 0.85 to 1.00 to ensure charge / discharge capacity, the equilibrium pressure is set to 0.04 to 0.07 MPa to facilitate initial activation, and the plateau region in the PCT curve is set as wide as possible. In Mm, by setting La and Ce to be within the range of 80 mass% or more and 100 mass% or less with respect to the total mass of Mm, the hydrogen storage capacity (H / M) can be set to 0.85 to 1.00, and the charge / discharge capacity can be ensured. As described above, the Ni ratio (a) is within the range of 4.30 to 4.75, and when a negative electrode is produced using the hydrogen storage alloy powder as an active material, the output characteristics are easily maintained and the life characteristics are not particularly deteriorated. As described above, the Mn ratio (b) is within the range of 0.25 to 0.50, and within this range, the difficulty of pulverizing the hydrogen storage alloy powder can be easily maintained. As described above, the Al ratio (c) is within the range of 0.25 to 0.45, and within this range, the hysteresis in the PCT characteristics is small, and the deterioration of the charge / discharge efficiency of the hydrogen storage alloy powder can be suppressed, and the decrease in the hydrogen storage capacity of the hydrogen storage alloy powder can be suppressed.
[0039] The above is the general formula MmNi a Mn b Al c Co d (wherein Mm is a misch metal, and the formula is represented by 4.30≦a≦4.75, 0.25≦b≦0.50, 0.25≦c≦0.45, 0≦d≦0.12, and 5.20≦a+b+c+d≦5.55) 5 This is a basic description of alloys having the type crystal structure.
[0040] In the present invention, a part of the constituent atoms represented by the general formula is replaced by a substitution element X other than these. In this case, the atoms may be replaced by atoms having a smaller metallic bond radius than the constituent atoms. For example, when Mm is the element to be replaced (subject element Y1) among the constituent atoms represented by the general formula described above, specifically, when La or Ce is the target element Y1, the A site may be replaced by an atom (substituting element X) having a smaller metallic bond radius than these. In addition, the B site may be replaced by an atom having a smaller metallic bond atomic radius than one or more target elements Y2 selected from the group consisting of Ni, Mn, Al, and Co. More specifically, atoms having a smaller metallic bond atomic radius than La or Ce include Pr, Nd, Sm, Gd, Tb, Dy, Ho, Er, Tm, Y, Sc, etc. On the other hand, atoms having a smaller metallic bond atomic radius than Ni, Mn, Al, or Co include, for example, Be, B, C, N, etc.
[0041] Also, the constituent atoms may be replaced with atoms having a larger metallic bond radius than the constituent atoms. For example, among the constituent atoms represented by the above general formula, when replacing the target element Y1, the A site may be replaced with an atom having a larger metallic bond radius than the constituent atoms, and when replacing the target element Y2, the B site may be replaced with an atom having a larger metallic bond radius than the constituent atoms. More specifically, atoms having a larger metallic bond radius than La or Ce include Eu, Yb, Ba, Ca, etc. On the other hand, atoms having a larger metallic bond atomic radius than Ni, Mn, Al, Co include Fe, Cu, Zn, Ga, Ge, Cr, V, Ti, Zr, Nb, Mo, Mg, etc.
[0042] Alternatively, an atom having a smaller metallic bond radius than the constituent atoms may be combined with an atom having a larger metallic bond radius to substitute the A site, substitute the B site, or substitute both. In particular, as described above, by substituting an atom having a larger metallic bond radius or by dumbbell-shaped substitution at the A site to expand the crystal lattice and appropriately substituting an atom having a smaller metallic bond radius, the lattice void ratio can be increased to 23.20% or more, thereby suppressing pulverization. This is particularly effective when the Co content is low or zero.
[0043] In particular, the target element to be replaced is the target element Y2, and the replacement element X is a compound represented by the formula MmNi in which one or more of Ni, Mn, or Al are replaced. a-a1 Mn b―b1 Al c―c1 X e Co d It is more preferable to use a hydrogen storage alloy that satisfies the formula: e=a1+b1+c1, 5.20≦a+b+c+d+e≦5.55.
[0044] The crystal lattice volume of the present invention is determined as follows: That is, the crystal lattice volume can be determined from the lattice constants (a-axis, c-axis) calculated from the X-ray diffraction pattern measured by the X-ray diffraction method (PHL Notten, et.al., Journal of The Electrochemical Society 146(9), 3181-3189(1999); similar to Non-Patent Document 4).
[0045] On the other hand, the total volume of the atoms occupying the crystal lattice volume is calculated using a sphere model from the metallic bond radius of each atom constituting the crystal lattice. The intralattice void ratio of the present invention is calculated from the following formula: Intra-lattice void ratio = (crystal lattice volume - total volume of constituent atoms) / crystal lattice volume x 100 The metallic bond radius in the present invention is the value described in "Chemical Handbook: Basics" edited by the Chemical Society of Japan, published in 1984. In the case of a typical element, half the bond distance between atoms of the same kind described in the representative value of atomic intervals is used.
[0046] As mentioned above, if the intralattice porosity is 23.20% or more, pulverization due to hydrogen absorption can be suppressed, and the larger the porosity, the greater the effect of suppressing pulverization. Therefore, there is no upper limit to the intralattice porosity, but CaCu 5 From the viewpoint of the stability of the crystal structure, the content was set to 23.70% or less.
[0047] In the hydrogen storage alloy of the present invention, the pulverization difficulty index is 0.55 to 0.70, so that when the hydrogen storage alloy powder is used as a negative electrode, the negative electrode has long life characteristics and is easily activated in the initial stage. Here, the difficulty in pulverization is the value obtained by dividing the "particle size of the hydrogen storage alloy powder after 10 hydrogen absorption / release cycles in an environment of a holding temperature of 45°C and a hydrogen pressure adjustment of 1.82 MPa" by the "initial particle size of the hydrogen storage alloy powder." The plateau pressure is the equilibrium hydrogen pressure (MPa) at H / M=0.5 on the hydrogen release side at a measurement temperature of 45°C. More specifically, the method for measuring the difficulty in pulverization in the present invention is described below. In the examples described later, the difficulty in pulverization of the hydrogen storage alloy obtained according to the following method was measured.
[0048] That is, using a PCT (hydrogen pressure-composition-isotherm) characteristic evaluation device, the "particle size of the hydrogen storage alloy powder after 10 hydrogen absorption / desorption cycles in an environment of a holding temperature of 45°C and a hydrogen pressure adjustment of 1.82 MPa" was divided by the "initial particle size of the hydrogen storage alloy powder" to obtain an index of the difficulty of pulverization. That is, the closer the difficulty of pulverization is to 1, the more difficult it is for the hydrogen storage alloy powder to pulverize, and the closer it is to 0, the more easily the hydrogen storage alloy powder is pulverized. In determining the difficulty of pulverization, the "initial particle size of the hydrogen storage alloy powder" refers to the average particle size D50 measured using a particle size distribution analyzer 7997SRA manufactured by Leeds & Northrup. "Particle size of hydrogen storage alloy powder after 10 hydrogen absorption / desorption cycles at a holding temperature of 45°C and a hydrogen pressure of 1.82MPa" refers to the average particle size D50 measured with a particle size distribution analyzer 7997SRA manufactured by Leeds & Northrup Co. after 10 hydrogen absorption / desorption cycles at a holding temperature of 45°C and a hydrogen pressure of 1.82MPa using a fully automatic PCT measuring device (1 / 2 inch straight tube sample cell, sample amount 3g) manufactured by Suzuki Shokan Co., Ltd. The activation process of the hydrogen storage alloy powder in the fully automatic PCT measuring device was performed in an activation temperature of 80°C and a hydrogen pressure of 1.82MPa, and the hydrogen absorption / desorption cycle of the hydrogen storage alloy powder in the same device was performed in an environment of a holding temperature of 45°C, a hydrogen absorption pressure of 1.82MPa, and a hydrogen desorption pressure of 0MPa.
[0049] The reason why the pulverization difficulty level is set to 0.55 to 0.70 is that if it is too high, initial activation becomes difficult and the input / output characteristics of the battery deteriorate, whereas if it is too low, the life characteristics of the battery cannot be ensured.
[0050] The hydrogen storage alloy of the present invention may be any alloy that satisfies the above-mentioned requirements of the present invention, and there is no particular restriction on the method for producing the alloy. The following shows an example of a method for producing the hydrogen storage alloy of the present invention.
[0051] The hydrogen storage alloy can be manufactured through a weighing process, a mixing process, a casting process, and a heat treatment process. To be used in a battery, the hydrogen storage alloy manufactured in this manner is crushed and used (used after the crushing process). In the weighing process, each raw material of the hydrogen storage alloy is weighed to obtain a desired alloy composition. At that time, each raw material including the substitution element X is weighed so as to obtain the hydrogen storage alloy according to the present invention. In the mixing process, the weighed raw materials are mixed. In the casting process, the mixed raw materials are charged into a high-frequency heating melting furnace, and the mixed raw materials are melted to form a molten metal, which is then poured into a mold, for example, and cast at a temperature in the range of 1150°C to 1550°C (casting temperature = molten metal temperature in the crucible at the start of casting).
[0052] The cast alloy is heat-treated in a heat treatment step at a temperature of 950°C to 1250°C in a non-oxidizing atmosphere. The heat treatment time varies depending on the size of the cast ingot (hydrogen storage alloy piece), but is, for example, 5 hours to 18 hours. The time can be set so that the temperature reaches the center of the ingot and grains grow to the desired crystal size. For use in batteries, the hydrogen storage alloy produced in this manner is pulverized. In this pulverization process, the hydrogen storage alloy powder is made to the required particle size through coarse pulverization and fine pulverization. For example, an ingot is pulverized to a size that passes through a 500 μm sieve to make hydrogen storage alloy powder.
[0053] The hydrogen storage alloy powder thus obtained can be used to prepare a negative electrode for a battery by a known method. That is, a hydrogen storage alloy negative electrode can be formed by mixing and molding a binder, a conductive additive, etc., by a known method. The hydrogen storage alloy powder is preferably used as a negative electrode for a nickel-metal hydride battery. EXAMPLES
[0054] The present invention will be described below based on examples, although the present invention is not limited to these examples.
[0055] [Examples 1 to 8, Comparative Examples 1 to 7] Each metal raw material of Ni, Mn, Al, Co, La and Ce as Mm, and the substitution element X was weighed so as to obtain the alloy composition shown in Tables 1 and 2. In these tables, La and Ce as Mm are the elements of the A site, and the other raw materials are the elements of the B site, and are shown in molar ratio. The raw materials were placed in a crucible in a melting furnace, evacuated, and then made into an argon gas atmosphere. Next, the melt was heated and melted with a high-frequency heating device, heated to 1540°C, held for 10 minutes, cooled to 1250°C, and cast into a mold at a casting temperature of 1230°C. The cast alloy ingot was heat-treated at 1080°C x 12 hours in an argon atmosphere to obtain an alloy ingot. The obtained alloy ingot was crushed coarsely with a crusher in an inert atmosphere, then crushed with a cutting mill (manufactured by Frutsch) in an inert atmosphere, and then made into a hydrogen storage alloy powder with a particle size (500μm or less) that passes through a sieve of 500μm.
[0056] <Evaluation method> The hydrogen storage alloy powders (samples) obtained in the Examples and Comparative Examples were subjected to various evaluations as follows.
[0057] (Measurement of Difficulty of Micronization) The difficulty of pulverization was measured using a particle size distribution measuring device and a PCT characteristic evaluation device according to the method described above.
[0058] (Intra-lattice porosity) As mentioned above, the intralattice porosity is defined by the following formula: Intra-lattice void ratio = (crystal lattice volume - total volume of constituent atoms) / crystal lattice volume x 100 The crystal lattice volume was calculated from the a-axis length and c-axis length obtained by Rietveld analysis, while the crystal lattice volume was measured using an X-ray diffractometer (SmartLab, Rigaku Corporation) and calculated from the a-axis length and c-axis length obtained by Rietveld analysis. Specifically, the hydrogen storage alloy pulverized to 20 μm or less was measured using a powder X-ray diffractometer (SmartLab, Rigaku Corporation) with a goniometer radius of 300 mm, an X-ray source of CuKα radiation, a tube voltage of 45 kV, and a tube current of 200 mA. At that time, the diffraction angle was in the range of 2θ = 15.0 to 85.0 °, the scan speed was 4.000 ° / min, and the scan step was 0.020 °. Based on the obtained X-ray diffraction results, the crystal structure was analyzed by the Rietveld method (analysis software SmartLab Studio II, PowderXRD plug-in).
[0059] On the other hand, the total volume of the constituent atoms was calculated from the metallic bond radius of each atom constituting the crystal lattice using a sphere model, as mentioned above. In this case, the metallic bond radius was the value listed in the "Chemical Handbook: Basics" published in 1984 by the Chemical Society of Japan. In addition, in the case of typical elements, half the bond distance between atoms of the same type as the representative value of the atomic interval was used. Furthermore, when the composition of ABx representing the crystal structure is ABx>5 (i.e., when the AB ratio is>5), as mentioned above, the element at the B site is substituted in a dumbbell shape at the A site, so when ABx=5+α, the total volume is the sum of the molar ratio of each element shown in Tables 1 and 2 divided by (1+1 / 7α) and multiplied by the atomic volume of each element calculated from the metallic bond radius, which is the total volume of the constituent atoms. In addition, the "Replacement Element" column in Tables 1 and 2 shows the replacement element and the site of the target element that the replacement element replaces. In addition, the "Radiity Relationship" shows the relationship between the metallic bond radius between the replacement element and the replacement element.
[0060] [Table 1]
[0061] [Table 2]
[0062] In addition to the above examples, based on the results of tests conducted by the inventors, the AB of Mm-Ni-Mn-Al-Co alloys 5 It was found that in order to make the pulverization difficulty index of the type hydrogen storage alloy 0.55 or more, it is preferable to replace a part of the constituent atoms with a predetermined substitution element and set the intralattice porosity to 23.30% or more and 23.70% or less. In Comparative Examples 1 to 7, although the composition was almost the same as that of the Examples, the intralattice porosity was 23.20% or less, and therefore it was not possible to obtain a pulverization difficulty index comparable to that of Examples 1 to 8. From this, it was confirmed that according to the present invention, an alloy having a low Co content, low raw material cost, excellent life characteristics, and suitable for a negative electrode for a nickel-metal hydride battery can be obtained.
Claims
1. General formula MmNi a Mn b A c Co d (wherein Mm is a misch metal, 4.30≦a≦4.75, 0.25≦b≦0.50, 0.25≦c≦0.45, 0≦d≦0.12, 5.20≦a+b+c+d≦5.55) 5 A hydrogen storage alloy having a crystalline structure of the above type, in which a part of the constituent atoms represented by the general formula is substituted with another substitution element X, and the intralattice porosity represented by the following formula is 23.20% or more and 23.70% or less. Intra-lattice void ratio=(crystal lattice volume−total volume of constituent atoms) / crystal lattice volume×100
2. Among the constituent atoms represented by the general formula, one or more target elements Y2 selected from the group consisting of Ni, Mn, and Al are substituted with the substitution element X to form a composition formula MmNi a-a1 Mn b-b1 A c-c1 X e Co d 2. The hydrogen storage alloy according to claim 1, wherein the formula e=a1+b1+c1 and 5.20≦a+b+c+d+e≦5.55 are satisfied.
3. 3. The hydrogen storage alloy according to claim 2, wherein the X atom has a metallic bond radius larger than that of the atom to be substituted.
4. 3. The hydrogen storage alloy according to claim 1, wherein Mm contains a rare earth metal having an atomic radius smaller than that of Ce.
5. 3. The hydrogen storage alloy according to claim 1, wherein the pulverization difficulty of said hydrogen storage alloy is 0.55 or more.
6. 3. A negative electrode comprising the hydrogen storage alloy according to claim 1 or 2 as a negative electrode active material.
7. A battery comprising the negative electrode according to claim 6.
Citation Information
Patent Citations
Hydrogen storage alloy and nickel-hydrogen storage battery using the same
JP1995286225A
Alkaline storage battery
JP2000353542A
Hydrogen storage alloy, and electrode using the same
JP2004269929A
Hydrogen storage alloy powder and its manufacturing method, hydrogen storage alloy electrode and nickel-hydrogen storage battery using the electrode
JP2005093297A
Hydrogen storage alloy
JP2009030158A