Steel and soft nitrided component
A steel with tailored compositions and dislocation density enhances cold forgeability and fatigue strength, addressing the limitations of conventional steels by achieving high hardness and strength in nitrocarburized components.
Patent Information
- Application Number
- JP2024020581
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2044-02-14
AI Technical Summary
Existing steels do not achieve both excellent cold forgeability and fatigue strength after nitrocarburizing, with conventional compositions either reducing cold forgeability or resulting in insufficient strength.
A steel composition with specific ranges of C, Si, Mn, Cr, P, S, Al, N, V, and Cu, along with optional elements, ensuring a dislocation density of 1.5×10^14 m^-2 at a depth of 0.2mm from the surface for enhanced hardness and fatigue strength.
The steel exhibits excellent cold forgeability and fatigue strength after nitrocarburizing, with a surface hardness of 580 HV or more at 0.2mm depth, suitable for components like engine crankshafts and gears.
Smart Images

Figure 2024137736000003 
Figure 2024137736000001 
Figure 2024137736000002
Abstract
Description
[Technical field]
[0001] The present invention relates to steels and nitrocarburized parts. [Background technology]
[0002] Cold forging allows for near-net-shape forming, and has the advantage of being able to reduce the amount of cutting after forging and suppress yield loss compared to hot forging. In addition, soft nitriding is a heat treatment that improves the fatigue properties of steel parts while reducing the generation of heat treatment distortion compared to carburizing and quenching, and is applied to various industrial parts such as automotive gears.
[0003] Patent Document 1 discloses a steel for machine structural use with excellent cold workability, a method for manufacturing the steel for machine structural use, and a method for manufacturing a processed part using the steel for machine structural use. The steel for machine structural use is characterized in that it contains C: 0.005-0.06 mass%, Si: 0.01-0.1 mass%, Mn: more than 1.0-3.0 mass%, P: 0.05 mass% or less, S: 0.005-0.05 mass%, Cr: 0.3-3.0 mass%, Al: 0.005-0.1 mass%, N: 0.008-0.02 mass%, the balance being Fe and unavoidable impurities, the amount of N in solid solution is 0.008-0.02 mass%, the cementite phase fraction in the structure is 2% or less, the balance is a ferrite phase, and the average crystal grain size of the ferrite phase is 10-100 μm. This steel for mechanical structural use contains a specified amount of Mn, which has a desulfurizing effect in which Mn bonds with S, improving the deformability of the steel while suppressing thermal softening of the aging strengthening caused by solute N.
[0004] Patent Document 2 discloses a high-strength nitrocarburizing steel with excellent cold forgeability. This nitrocarburizing steel contains, in mass%, C: 0.01% or less (including 0%), Si: 0.01% to 1.5%, Mn: 0.15% to 2%, Cu: 0.5% to 2%, N: limited to less than 0.005%, the balance being Fe and unavoidable impurity elements, and has a hardness of HV150 or less as hot rolled or hot forged. In this high-strength nitrocarburizing steel, excellent precipitation hardening is obtained by precipitating Cu in ferrite, and it is said that high fatigue strength is obtained after nitrocarburizing treatment. In addition, in this high-strength nitrocarburizing steel, the amount of C added is 0.01 mass% or less, thereby improving cold forgeability.
[0005] Patent Document 3 discloses a method for producing a steel material for soft nitriding and a soft nitriding part using the steel material. In this method for producing a steel material for soft nitriding, a steel having a chemical composition of, by weight, C: 0.15-0.45%, Si: 0.05-0.50%, Mn: 0.2-2.5%, Cu: 0.5-1.5%, Ni: 0.25-0.75%, and 1.8≦Cu / Ni≦2.2, Cr: 0.5-2.0%, V: 0.05-0.5%, Al: 0.01-0.3%, Mo: 0-0.3%, S: 0-0.13%, Pb: 0-0.35%, Ca: 0-0.01%, and the balance being Fe and unavoidable impurities, is hot worked, spheroidized annealed, and then cold worked to a hardness of Hv180 or less. This soft-nitriding part is made of the above-mentioned steel material for soft-nitriding, and has a surface hardness of Hv600 or more and an effective hardened depth of 0.1 mm or more after soft-nitriding. In this soft-nitriding part, the combined addition of Cu and Ni significantly manifests the effect of Cu, which hardens by precipitation during soft-nitriding.
[0006] Patent Document 4 discloses a method for producing a steel material for soft nitriding and a soft-nitrided part using the steel material. In this method, the steel material for soft nitriding contains, by weight, C: 0.15-0.45%, Si: 0.05-0.50%, Mn: 0.2-2.5%, Cu: 0.5-1.5%, Ni: 0.25-0.75%, and 1.8≦Cu / Ni≦2.2, Cr: 0.5-2.0%, V: 0.05-0.5%, Al: 0.005-0.3%, Mo+0.5W: 0-0.3%, Ti: 0. Steel having a chemical composition of 0.2%, Zr: 0-0.2%, Nb: 0-0.2%, Pb: 0-0.35%, Ca: 0-0.01%, S: 0.13% or less, and the balance being Fe and inevitable impurities, is hot worked and then spheroidized annealed to a core hardness of Hv180 or less, and then cold worked to a core hardness of Hv250 or more, and the decarburization depth is 0.1-0.4 mm from the surface of the steel. This soft-nitrided part is made of the above-mentioned steel for soft-nitriding, and has a surface hardness of Hv600 or more and an effective hardening depth of 0.2 mm or more after soft-nitriding. In this soft-nitrided part as well, the combined addition of Cu and Ni makes the effect of Cu, which precipitation hardens during soft-nitriding, more pronounced.
[0007] Non-Patent Document 1 discloses a method (so-called Williamson-Hall method) for estimating dislocation density by determining lattice strain caused by non-uniform deformation of the lattice from the half-width of an X-ray diffraction peak. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2011-236449 A [Patent Document 2] JP 2002-69571 A [Patent Document 3] Japanese Patent Application Publication No. 9-256045 [Patent Document 4] Japanese Patent Application Publication No. 10-226818 [Non-patent literature]
[0009] [Non-Patent Document 1] GK Williamson and WH Hall, “X-ray Line Broadening from Filed Aluminum and Wolfram,” Acta Metall., Vol. 1, 1953, pp. 22-31. Summary of the Invention [Problem to be solved by the invention]
[0010] If parts can be manufactured by cold forging, costs can be reduced compared to manufacturing parts by hot forging. Furthermore, if softening annealing before cold forging can be omitted, or cutting after cold forging can be omitted by using net shape forming, costs can be further reduced.
[0011] However, in the steel for machine structural use disclosed in Patent Document 1, Mn is added in an amount of more than 1.0 mass %, which reduces the cold forgeability of the steel, and may make it difficult to omit softening annealing or perform net shape forming.
[0012] In addition, in the high-strength nitrocarburizing steel disclosed in Patent Document 2, the amount of C added is reduced to 0.01 mass% or less to improve cold forgeability, but the strength after nitrocarburizing may be insufficient due to the reduction in the amount of C added.
[0013] In addition, in the steel materials for soft nitriding disclosed in Patent Documents 3 and 4, the amount of C added is set to 0.15% by weight or more and 0.45% by weight or less, and in some cases, excellent cold forgeability that allows soft annealing to be omitted cannot be obtained.
[0014] As described above, in the conventional technology, it has not been possible to obtain a steel that has both excellent cold forgeability and fatigue strength after soft nitriding. Therefore, it is desired to provide a steel that has both excellent cold forgeability and fatigue strength after soft nitriding.
[0015] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a steel having excellent cold forgeability and excellent fatigue strength after soft nitriding, and a soft-nitrided part formed from the steel. [Means for solving the problem]
[0016] In order to achieve the above object, the steel and the soft-nitrided part according to the present invention are as follows.
[0017] [1]C: more than 0.02% by mass and less than 0.15% by mass, Si: 0.03 mass% or more and 0.15 mass% or less, Mn: 0.10 mass% or more and 0.95 mass% or less, Cr: 0.50 mass% or more and 1.90 mass% or less, P: 0.1% by mass or less, S: 0.5% by mass or less, Al: 0.005% by mass or more and 0.080% by mass or less, N: 0.0010 mass% or more and 0.0120 mass% or less, V: 0.03 mass% or more and 0.30 mass% or less and Cu: 0.2% by mass or more and 1.5% by mass or less; The balance is Fe and impurities.
[0018] [2] The composition further comprises Ni: 1.5% by mass or less, Mo: 1.0% by mass or less, B: 0.01% by mass or less, Ti: 0.1% by mass or less, Nb: 0.1% by mass or less, Sn: 0.1% by mass or less, Sb: 0.1% by mass or less, Se: 0.3% by mass or less, Ca: 0.1% by mass or less, Pb: 0.3% by mass or less and Bi: 0.3% by mass or less Steel according to [1], comprising one or more selected from the group consisting of: [3] The steel according to [1] or [2], wherein the chemical composition includes Cu: 0.41 mass% or more and 1.5 mass% or less.
[0019] [4] It is made of any of the steels [1] to [3] above, The dislocation density at a depth of 0.2 mm from the surface is 1.5×10 14 (m -2 ) or higher. Effect of the Invention
[0020] According to the present invention, it is possible to provide a steel having excellent cold forgeability and excellent fatigue strength after soft nitriding, and a soft-nitrided part formed from the steel. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a schematic diagram showing the shape of a test piece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The steel according to this embodiment will be described below.
[0023] First, an overview of the steel according to this embodiment will be described.
[0024] The steel according to this embodiment has a component composition (chemical composition) including C (carbon): more than 0.02% by mass and less than 0.15% by mass, Si (silicon): 0.03% by mass or more and 0.15% by mass or less, Mn (manganese): 0.10% by mass or more and 0.95% by mass or less, Cr: 0.50% by mass or more and 1.90% by mass or less, P (phosphorus): 0.1% by mass or less, S: 0.5% by mass or less, Al (aluminum): 0.005% by mass or more and 0.080% by mass or less, N (nitrogen): 0.0010% by mass or more and 0.0120% by mass or less, V (vanadium): 0.03% by mass or more and 0.30% by mass or less, and Cu (copper): 0.2% by mass or more and 1.5% by mass or less, with the balance being Fe and impurities.
[0025] The steel according to this embodiment has excellent cold forgeability and excellent fatigue strength after soft nitriding.
[0026] The steel according to this embodiment and the soft-nitrided part realized by using this steel will be described in detail below.
[0027] An example of a soft-nitrided part realized by the steel according to this embodiment (hereinafter referred to as the soft-nitrided part according to this embodiment) is a part forming a vehicle such as an automobile. For example, examples of parts in the automobile field include engine crankshafts, timing gears, etc., transmission gears, ring gears, sun gears, planetary gears, etc., of a transmission, steering pinions, worms, etc., of a suspension, and worms for power windows in an interior.
[0028] Nitriding includes both a nitriding treatment in which only nitrogen is introduced into steel, and a soft nitriding treatment in which nitrogen and carbon are introduced into steel at the same time, and both are treatments that do not cause martensitic transformation of steel. Of these, nitriding in this embodiment refers to soft nitriding.
[0029] The steel according to this embodiment is nitrided before use as described above. That is, the body of the soft-nitrided component according to this embodiment has a surface layer that is nitrided and has high hardness.
[0030] The hardness of the surface layer of the body of the soft-nitrided part, i.e., the steel material after nitriding, for example, at a depth of 0.2 mm from the surface, should be 580 HV or more, which gives the soft-nitrided part excellent fatigue strength. Here, the hardness at a depth of 0.2 mm from the surface can be measured by the method described in the Examples.
[0031] As described above, the fatigue strength of a nitrocarburized part is strongly correlated with the hardness at a depth of 0.2 mm from the surface. In addition, when dislocations introduced into steel by cold forging are restored during nitrocarburizing, the hardness of the steel material decreases according to the amount of restoration. In the steel of this embodiment, the dislocation density is 1.5×10 14 (m -2), hardness will decrease. Therefore, the dislocation density at a depth of 0.2 mm from the surface in the body of the soft-nitrided part (steel after nitriding) is 1.5×10 14 (m -2 In order to obtain a high surface hardness in the body of the soft-nitrided part (steel material after nitriding), it is more preferable that the dislocation density at a depth of 0.2 mm from the surface is 3.0×10 or more. 14 (m -2 ) or more. Here, the dislocation density at a depth of 0.2 mm from the surface can be measured by the method described in the Examples.
[0032] The soft-nitrided component according to the present embodiment may be a component in which the main body is combined with another structure that is made of a metal or a metal alloy and has a non-nitrided surface. The soft-nitrided component according to the present embodiment may be a component in which the main body is combined with another structure that is not made of metal.
[0033] The steel according to this embodiment forms a portion at a depth of 0.5 mm or more from the surface of the body of the soft-nitrided component according to this embodiment. Note that the surface layer of the body of the soft-nitrided component according to this embodiment may be a steel obtained by nitriding the steel according to this embodiment, as described above.
[0034] As described above, the steel according to this embodiment has a chemical composition containing C, Si, Mn, Cr, P, S, Al, N, V, and Cu, with the balance being Fe and impurities. This steel may further contain the following optional components. The optional components include the following groups A to E, and may contain any one or more of the groups.
[0035] Group A: This steel may contain 1.5 mass % or less of Ni (nickel) as an optional component.
[0036] Group B: This steel may contain, as optional components, at least one selected from the group consisting of 1.0 mass % or less of Mo (molybdenum) and 0.01 mass % or less of B (boron).
[0037] Group C: This steel may contain, as an optional component, at least one selected from the group consisting of 0.1 mass % or less of Ti (titanium) and 0.1 mass % or less of Nb (niobium).
[0038] Group D: This steel may contain, as an optional component, at least one selected from the group consisting of 0.1 mass % or less of Sn (tin) and 0.1 mass % or less of Sb (antimony).
[0039] Group E: This steel may contain, as optional components, one or more selected from the group consisting of 0.3 mass% or less of Se (selenium), 0.1 mass% or less of Ca (calcium), 0.3 mass% or less of Pb (lead), and 0.3 mass% or less of Bi (bismuth).
[0040] The content and effects of each component in the steel will be described in detail below. In the following description, when the content is simply stated, it means the content (mass%) in the steel.
[0041] C: More than 0.02% by mass and less than 0.15% by mass The content of C is more than 0.02% by mass and less than 0.15% by mass. The more C is added, the more the strength of the steel is improved. However, the more C is added, the more the cold forgeability of the steel is reduced. If the content of C is within the above range, the effect of reducing the cold forgeability is small, and the dislocations introduced by cold forging do not recover during soft nitriding, and work hardening is maintained even after soft nitriding, so that high surface hardness can be achieved in the steel material (soft-nitrided part) even after soft nitriding. In order to achieve both cold forgeability and fatigue strength after soft nitriding, the content of C is preferably 0.04% by mass or more and 0.13% by mass or less.
[0042] Si: 0.03 mass% or more and 0.15 mass% or less The Si content is 0.03 mass% or more and 0.15 mass% or less. In nitrided steel, Si serves as a deoxidizer. Excessive Si content in steel reduces the cold workability of the steel. The Si content is preferably 0.05 mass% or more and 0.10 mass% or less.
[0043] Mn: 0.10 mass% or more and 0.95 mass% or less The Mn content is 0.10% by mass or more and 0.95% by mass or less. Mn improves hardenability and strengthens the pre-nitriding structure of steel, thereby strengthening the post-nitriding structure (nitrided steel). In order to obtain sufficient fatigue strength, the Mn content must be 0.10% by mass or more. If the steel contains excessive Mn, it may lead to an increase in deformation resistance. The Mn content is preferably 0.13% by mass or more and 0.55% by mass or less, and more preferably 0.15% by mass or more and 0.25% by mass or less.
[0044] Cr: 0.50 mass% or more and 1.90 mass% or less The Cr content is 0.50% by mass or more and 1.90% by mass or less. Cr has the effect of forming a Cr nitride layer during soft nitriding to increase hardness and the effect of inhibiting the recovery of work hardening introduced by cold forging. Excessive addition of Cr may reduce the amount of N penetrating into the interior, thereby decreasing the effective hardened layer depth. The Cr content is preferably 0.65% by mass or more and 1.35% by mass or less, and more preferably 0.70% by mass or more and 0.85% by mass or less.
[0045] P: 0.1% by mass or less The P content is 0.1 mass% or less. Since P segregates at the grain boundaries of nitriding steel and reduces toughness, the lower the P content, the more desirable it is. The P content is permitted up to 0.1 mass%. The P content is preferably 0.02 mass% or less. Although there is no problem if there is no particular limit on the P content, since the inclusion of P is usually unavoidable, unnecessary reduction in P content may increase the refining time and the refining cost. Therefore, it is reasonable and preferable to set the P content to 0.003 mass% or more.
[0046] S: 0.5% by mass or less The S content is 0.5% by mass or less. S exists as sulfide-based inclusions and is an element effective in improving machinability. Excessive S inclusion in steel may lead to a decrease in cold workability. There is no particular limit to the S content, but since the inclusion of S is usually unavoidable, excessive reduction in S content may increase refining costs. Therefore, it is reasonable to set the S content to 0.003% by mass or more. The S content is preferably 0.004% by mass or more and 0.3% by mass or less, and more preferably 0.005% by mass or more and 0.09% by mass or less.
[0047] Al: 0.005 mass% or more and 0.080 mass% or less The Al content is 0.005% by mass or more and 0.080% by mass or less. Al forms oxides and is an element effective in deoxidizing nitrided steel. Furthermore, Al has the effect of suppressing the formation of coarse oxide-based inclusions in nitrided steel. If the Al content is less than 0.005% by mass, these effects may not be obtained. If the steel contains excessive Al, it may increase the inclusions (Al oxides), increase the starting points of fatigue fracture, and cause low fatigue strength. The Al content is preferably 0.015% by mass or more and 0.065% by mass or less.
[0048] N: 0.0010 mass% or more and 0.0120 mass% or less The N content is 0.0010% by mass or more and 0.0120% by mass or less. Excessive N content in steel may cause surface cracks in the steel slab after casting. There is no particular lower limit for the N content, but since the inclusion of N is usually unavoidable, excessive reduction in N content may increase refining costs. The N content is preferably 0.0010% by mass or more. The N content is preferably 0.0030% by mass or more and 0.0080% by mass or less.
[0049] V: 0.03 mass% or more and 0.30 mass% or less The V content is 0.03% by mass or more and 0.30% by mass or less. V combines with carbon and nitrogen to form fine precipitates during soft nitriding, thereby improving the strength of the steel. V also has an effect of suppressing the recovery of work hardening introduced by cold forging. In order to obtain this effect of V, it is preferable to contain at least 0.03% by mass or more of V in the steel. If an excessive amount of V is contained in the steel, the cold forgeability will be reduced. The V content is more preferably 0.10% by mass or more and 0.15% by mass or less.
[0050] Cu: 0.2 mass% or more and 1.5 mass% or less The content of Cu is 0.2% by mass or more and 1.5% by mass or less. Cu has the effect of suppressing the recovery of dislocations introduced by cold forging during soft nitriding. In addition, due to this effect, Cu contributes to increasing the hardness of the surface layer of the steel material after soft nitriding. Even if the Ni content in the steel exceeds 1.5% by mass, the above effect is saturated. Cu also has the effect of embrittling the steel during hot working, and may reduce the manufacturability of the steel. Considering the effect of Cu embrittling the steel during hot working, the content of Cu is preferably 0.2% by mass or more and 0.8% by mass or less, more preferably 0.3% by mass or more and 0.7% by mass or less. In addition, when there is a purpose to prevent surface cracks during hot rolling, it is preferable to set the Cu content to 0.41% by mass or less.
[0051] The optional components of the steel will be described below.
[0052] Ni: 1.5% by mass or less The Ni content may be 1.5 mass% or less. Ni has the effect of mitigating embrittlement of steel during hot working when Cu is added. Ni may be added to improve the manufacturability of steel. In order to obtain this effect of Ni, it is preferable to contain Ni in an amount of 0.05 mass% or more in the steel. Even if the Ni content in the steel exceeds 1.5 mass%, the above effect is saturated. The Ni content is preferably 1.0 mass% or less.
[0053] Mo: 1.0% by mass or less The Mo content may be 1.0% by mass or less. Mo improves hardenability and strengthens the pre-nitriding structure, thereby strengthening the post-nitriding structure. However, if the Mo content exceeds 1% by mass, the hardenability becomes excessive, the hardness after rolling increases, and the workability and machinability may decrease. In order to realize the effect of Mo in improving the strength of the steel material, it is preferable to contain Mo in an amount of 0.01% by mass or more in the steel. The Mo content is more preferably 0.03% by mass or more and 0.50% by mass or less, and even more preferably 0.05% by mass or more and 0.25% by mass or less.
[0054] B: 0.01% by mass or less The content of B may be 0.01% by mass or less. B segregates at grain boundaries and inhibits diffusion-type transformation, which is effective in improving hardenability, and also has the effect of strengthening grain boundaries, inhibiting the occurrence and progression of fatigue cracks, and improving fatigue strength. In order to obtain this effect of B, it is preferable to contain B in steel at 0.0003% by mass or more. If the content of B exceeds 0.01% by mass, the toughness of the steel decreases, so the content of B is preferably 0.01% by mass or less. The content of B is more preferably 0.0005% by mass or more and 0.005% by mass or less, and even more preferably 0.0007% by mass or more and 0.002% by mass or less.
[0055] Ti: 0.1% by mass or less The Ti content may be 0.1 mass% or less. Ti improves the strength of the steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. However, even if the Ti content in the steel exceeds 0.1 mass%, the effect is saturated. The Ti content is preferably 0.005 mass% or more and 0.08 mass% or less, and more preferably 0.01 mass% or more and 0.06 mass% or less.
[0056] Nb: 0.1% by mass or less The Nb content may be 0.1 mass% or less. Nb improves the strength of the steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. However, even if the Nb content in the steel exceeds 0.1 mass%, the effect is saturated. The Nb content is preferably 0.005 mass% or more and 0.08 mass% or less, and more preferably 0.01 mass% or more and 0.06 mass% or less.
[0057] Sb: 0.1% by mass or less The Sb content may be 0.1 mass% or less. Sb is an element effective in suppressing decarburization of the steel surface and preventing a decrease in surface hardness. In order to realize this effect, it is preferable to contain Sb in the steel at 0.0003 mass% or more. If an excessive amount of Sb is contained in the steel, the workability of the steel decreases. The Sb content is more preferably 0.001 mass% or more and 0.05 mass% or less, and further preferably 0.0015 mass% or more and 0.035 mass% or less.
[0058] Sn: 0.1% by mass or less The Sn content may be 0.1 mass% or less. Sn is an element effective for improving the corrosion resistance of the steel surface. From the viewpoint of improving the corrosion resistance, it is preferable that the steel contains 0.003 mass% or more of Sn. If the steel contains an excessive amount of Sn, the workability decreases. The Sn content is more preferably 0.0010 mass% or more and 0.050 mass% or less, and further preferably 0.0015 mass% or more and 0.035 mass% or less.
[0059] Se: 0.3% by mass or less The Se content may be 0.3 mass% or less. Se improves machinability by combining with Mn and Cu and dispersing as precipitates in the steel. To obtain this effect, it is preferable to contain at least 0.001 mass% Se in the steel. Even if the Se content in the steel exceeds 0.3 mass%, the effect is saturated. The Se content is more preferably 0.005 mass% to 0.1 mass%, and further preferably 0.008 mass% to 0.09 mass%.
[0060] Ca: 0.1% by mass or less The Ca content may be 0.1% by mass or less. Ca improves machinability by combining with S and dispersing in the steel as sulfides. To obtain this effect, it is preferable to contain at least 0.0005% by mass of Ca in the steel. If the Ca content in the steel exceeds 0.1% by mass, the effect is saturated. The Ca content is more preferably 0.0010% by mass or more and 0.0500% by mass or less, and further preferably 0.0015% by mass or more and 0.0300% by mass or less.
[0061] Pb: 0.3% by mass or less The Pb content may be 0.3% by mass or less. Pb has the effect of refining chips during cutting. Addition of Pb is effective when it is desired to improve chip disposability. To obtain this effect, it is preferable to contain 0.01% by mass or more of Pb in the steel. Even if excessive Pb is contained in the steel, the effect of improving chip disposability becomes saturated. The Pb content is preferably 0.01% by mass or more and 0.2% by mass or less, and more preferably 0.01% by mass or more and 0.1% by mass or less.
[0062] Bi: 0.3% by mass or less The Bi content may be 0.3 mass% or less. Bi has the effect of refining chips during cutting. Addition of Bi is effective when it is desired to improve chip disposability. To obtain this effect, it is preferable to contain Bi at 0.01 mass% or more. Even if an excessive amount of Bi is contained in the steel, the effect of improving chip disposability becomes saturated. The Bi content is preferably 0.01 mass% or more and 0.2 mass% or less, and more preferably 0.01 mass% or more and 0.1 mass% or less.
[0063] The balance other than the above-described elements is Fe and impurities. The impurities are substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment during industrial production of steel material, and are allowed within a range that does not adversely affect the characteristics of this embodiment.
[0064] The steel according to the present invention may be a steel obtained by melting a steel having a predetermined composition, or may be a rolled material obtained by hot rolling a steel having a predetermined composition. If the rolled material has a Vickers hardness of 105 HV or less, it can be said to have excellent cold forgeability, and cold forging is possible without softening annealing.
[0065] The steel according to the present invention is suitable as a steel for cold forging and nitriding (soft nitriding). In particular, it is particularly suitable for cold forging a rolled material obtained by hot rolling a steel having a predetermined composition, followed by nitriding (soft nitriding). The steel according to the present invention can be cold forged without soft annealing the rolled material, but it may also be cold forged after soft annealing the rolled material.
[0066] The methods of the above hot rolling, cold forging and nitriding (soft nitriding) are not particularly limited, and known methods can be adopted. When soft annealing is performed, the method is not particularly limited, and known methods can be adopted.
[0067] The soft-nitrided part according to the present invention is formed from the steel according to the present invention, and can be manufactured by hot rolling a steel having a predetermined component composition to obtain a rolled material, optionally subjecting the rolled material to softening annealing, followed by cold forging and nitriding treatment (soft-nitriding treatment). EXAMPLES
[0068] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0069] First, steels (steels No. 1 to 58) having the composition shown in Table 1 were melted and formed into round bars (rolled materials) having a diameter of 32 mm by hot rolling. Among the values of the composition shown in Table 1, the underlined values are outside the ranges specified in this embodiment. In addition, in Table 1, "Others" refers to any component other than C, Si, Mn, Cr, P, S, Al, N, V, and Cu.
[0070] [Table 1]
[0071] The Vickers hardness (HV) of each of the obtained round bars was measured. The load used for measuring the Vickers hardness was 1 kgf (9.8 N). The Vickers hardness was measured at 10 points randomly selected from the surface of the round bar, and the average of these 10 measured values was obtained. Table 2 shows the average of the Vickers hardness measurements of the round bars as the hardness of the rolled material.
[0072] The surface of the round bar was visually inspected and evaluated according to the following criteria: A: No cracks B: Minor cracks C: Significant cracks
[0073] [Table 2]
[0074] Next, this round bar was cut to obtain a round bar with a diameter of 17 mm, which was then cold worked (pultrusion) to obtain a round bar with a diameter of 14 mm, and a cold working strain was imparted to the round bar.
[0075] Furthermore, the round bar to which the cold-working strain had been applied was cut to obtain test pieces having the shape shown in the schematic diagram in FIG.
[0076] As shown in FIG. 1, the test piece is a straight rod, and its cross section perpendicular to the extending direction is a circular rod. Both ends of the test piece in the extending direction of the rod are gripping parts 1,1 described later. A parallel part 2 is disposed between the gripping parts 1,1. The diameter of the central part in the axial direction of the parallel part 2 is 10 mm (10±0.05 mm). The diameter of the gripping parts 1,1 is 12 mm (the same diameter as a round bar). The length of the gripping part 1 in the direction along the axis G is 25 mm. The length between the gripping parts 1,1 including the parallel part 2 is 30 mm. Both ends of the parallel part 2 in the direction along the axis G are narrowed in a curved shape of R15 from the end of the gripping part 1 to the central part in the axial direction. A recess 4 is formed in the central part of the parallel part 2 along the circumferential direction of the test piece. The recess 4, when viewed in a direction intersecting the extension direction of the test piece (side view), has a shape (R1.0) along a circular arc with a diameter of 1 mm, and the maximum depth of this recess from the surface of the test piece is about 1 mm. The width of the recess in the direction along the extension direction of the test piece (extension direction of the bar) is about 2 mm. The diameter of the recess 4 of the parallel portion 2 is about 8 mm (8±0.02 mm).
[0077] Next, the test pieces were subjected to gas soft-nitriding heat treatment (nitriding) at 570℃ for 3 hours to obtain post-treatment test pieces (an example of a soft-nitrided part). The nitriding treatment was carried out in a mixed gas containing ammonia and carbon monoxide. Two or more post-treatment test pieces were prepared for each steel with the chemical composition shown in Table 1.
[0078] After the treatment, the surface hardness (Vickers hardness) of the recessed portion of the test piece was measured in accordance with the "Method for measuring surface hardness of nitrided layer of steel" specified in JIS G 0563-1993. This measurement was performed at a position 0.2 mm deep from the surface of the bottom of the notch portion in a cross section overlapping with the axis G of the test piece. In other words, this measurement was performed at a position 0.2 mm deep below the surface layer of the test piece. In addition, the dislocation density at a position 0.2 mm deep below the surface layer of the test piece was determined by the Williamson-Hall method using X-ray diffraction (see Non-Patent Document 1). The surface hardness measurement results and dislocation density are shown in Table 2.
[0079] In addition, the treated test pieces other than those used for measuring the surface hardness were subjected to a rotating bending fatigue test, and the fatigue limit (1×10 7 The fatigue limit evaluation results are also shown in Table 2.
[0080] In the case of a rolled material (a round bar with a diameter of 32 mm, before nitriding), if the Vickers hardness is 105 HV or less, the material has excellent cold forgeability. The rolled materials formed from the steels according to this embodiment (Nos. 1 to 29, and Nos. 45 to 58) have a Vickers hardness of 105 HV or less and have excellent cold forgeability.
[0081] In the treated test piece, if the surface hardness at 0.20 mm below the surface is 580 HV or more, the fatigue strength after nitriding is excellent. The treated test pieces (nitrocarburized parts) formed from the steels according to this embodiment (Nos. 1 to 29, 45 to 58) have a surface hardness of 580 HV or more at 0.20 mm below the surface, and are excellent in fatigue strength after nitrocarburizing.
[0082] If the fatigue limit of the treated test piece is 260 MPa or more, the fatigue strength after soft nitriding is excellent. The treated test pieces (soft nitriding parts) formed from the steels according to this embodiment (Nos. 1 to 29, Nos. 45 to 58) have a fatigue limit of 260 MPa or more and are excellent in fatigue strength after soft nitriding.
[0083] That is, the steels according to the present embodiment (Nos. 1 to 29 and Nos. 45 to 58) have excellent cold forgeability and excellent fatigue strength after soft nitriding. Furthermore, the soft-nitrided parts formed from the steels according to the present embodiment have excellent fatigue strength.
[0084] Furthermore, in the steels according to this embodiment (Nos. 5, 16, 17, and 45 to 58) in which the Cu content is 0.2 mass % or more and 41 mass % or less, surface cracks during hot rolling are prevented.
[0085] In this manner, it is possible to provide a steel having excellent cold forgeability and excellent fatigue strength after soft-nitriding, and a soft-nitrided part formed from the steel.
[0086] It should be noted that the embodiments disclosed in this specification are merely examples, and the present invention is not limited to these embodiments, and can be modified as appropriate without departing from the scope of the present invention. [Industrial Applicability]
[0087] The present invention is applicable to steel and nitrocarburized components. [Explanation of symbols]
[0088] 1: Grip part 2: Parallel section 4: Recess
Claims
1. C: 0.02% by mass or more and less than 0.15% by mass, Si: 0.03% by mass or more and 0.15% by mass or less, Mn: 0.10% by mass or more and 0.95% by mass or less, Cr: 0.50% by mass or more and 1.90% by mass or less, P: 0.1% by mass or less, S: 0.5% by mass or less, Al: 0.005% by mass or more and 0.080% by mass or less, N: 0.0010% by mass or more and 0.0120% by mass or less, V: 0.03% by mass or more and 0.30% by mass or less, and Cu: 0.2% by mass or more and 1.5% by mass or less; The balance of the steel is Fe and impurities.
2. The composition further comprises: Ni: 1.5% by mass or less, Mo: 1.0% by mass or less, B: 0.01% by mass or less, Ti: 0.1% by mass or less, Nb: 0.1% by mass or less, Sn: 0.1% by mass or less, Sb: 0.1% by mass or less, Se: 0.3% by mass or less, Ca: 0.1% by mass or less, Pb: 0.3% by mass or less and Bi: 0.3% by mass or less The steel of claim 1 , comprising at least one selected from the group consisting of:
3. The steel according to claim 1 or 2, wherein the composition includes Cu: 0.41 mass% or more and 1.5 mass% or less.
4. Made of a steel according to claim 1 or 2, The dislocation density at a depth of 0.2 mm from the surface is 1.5 × 10 14 (m -2 ) or higher.
5. Made of the steel according to claim 3, The dislocation density at a depth of 0.2 mm from the surface is 1.5 × 10 14 (m -2 ) or higher.
Citation Information
Patent Citations
Steel for soft-nitriding, excellent in cold forgeability and pitting resistance
JP1998306343A
Rolled steel for cold forging / nitriding
JP2013159794A
Steel and component for soft nitriding and manufacturing method therefor
JP2016056450A
Production of steel for soft-nitriding and soft-nitrided parts using the same steel
JP1997256045A
Production of steel for soft-nitriding and soft-nitrided parts using this steel
JP1998226818A