Method for forming semiconductor structure

A dual layer hardmask with aluminum and hafnium oxide layers addresses CMOS fabrication challenges by preventing pinholes and ensuring accurate epitaxial deposition in CMOS devices.

JP2024137830APending Publication Date: 2024-10-07ASM IP HLDG BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024042169
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-21
Filing Date
2024-03-18
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Traditional hardmask materials face challenges in CMOS device fabrication, particularly in forming suitable hardmasks for PMOS and NMOS regions, leading to issues like pinholes and undesired epitaxial deposition.

Method used

Employ a dual layer hardmask comprising a first metal oxide layer, such as aluminum oxide, and a second metal oxide layer with a lower etch rate, like hafnium oxide, to protect specific regions during CMOS fabrication processes, using cyclical deposition methods to form a bilayer hardmask.

Benefits of technology

The dual layer hardmask effectively prevents pinhole formation and ensures precise epitaxial deposition by selectively removing the top layer in targeted regions, maintaining protection for other regions, thus enhancing CMOS fabrication accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137830000001_ABST
    Figure 2024137830000001_ABST
Patent Text Reader

Abstract

To provide a method for forming a semiconductor structure.SOLUTION: A method for forming a semiconductor structure is disclosed. The method including depositing a first hard mask layer and a second hard mask layer on a substrate including a first region and a second region, thereby forming a double layer hard mask. A formed exemplary structure includes a CMOS device structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates generally to methods for forming semiconductor structures, and in particular to methods for forming semiconductor structures that include a bilayer hardmask. The present disclosure also relates generally to structures that include a bilayer hardmask. Background of the disclosure [Background technology]

[0002] The scaling of semiconductor devices, such as complementary metal-oxide-semiconductor (CMOS) devices, has led to significant improvements in the speed and density of integrated circuits. However, traditional device scaling techniques face significant challenges for future technology nodes.

[0003] For example, it has been a challenge to find suitable hardmask materials for use in the fabrication of PMOS and NMOS regions of a CMOS device structure. Thus, new hardmask materials and hardmask structures are desirable for improved CMOS fabrication methods.

[0004] Any discussion, including discussion of the problems and solutions described in this section, is included in this disclosure solely for the purpose of providing a context for the disclosure and should not be construed as an admission that any or all of the information was known at the time the invention was made or otherwise constitutes prior art. Summary of the Invention

[0005] This Summary may introduce selected concepts in a simplified form that may be described in more detail below. This Summary is not necessarily intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.

[0006] Various embodiments of the present disclosure relate to semiconductor structures and methods for forming certain semiconductor structures, including hardmask layers and structures, that may be utilized, for example, in fabrication processes such as etching processes employed in the fabrication of CMOS device structures.

[0007] According to an exemplary embodiment of the present disclosure, a method of forming a semiconductor structure is disclosed. The method of the present disclosure includes seating a substrate including a first region and a second region in a reaction chamber, and forming a bilayer hardmask on the substrate. In some embodiments, forming the bilayer hardmask includes performing one or more deposition cycles of a first cyclic deposition process to deposit a first hardmask layer including a first metal oxide on the substrate, and performing one or more deposition cycles of a second cyclic deposition process to deposit a second hardmask layer including a second metal oxide on the first metal oxide hardmask layer.

[0008] In some embodiments, a first unit deposition cycle of the first cyclical deposition process includes providing a first metal precursor to the reaction chamber and providing a first oxidant to the reaction chamber.

[0009] In some embodiments, the first hardmask layer comprises aluminum oxide.

[0010] In some embodiments, a second unit deposition cycle of the second cyclical deposition process includes providing a second metal precursor to the reaction chamber and providing a second oxidant to the reaction chamber.

[0011] In some embodiments, the second hardmask layer is selected from the group consisting of hafnium oxide, yttrium oxide, and zirconium oxide.

[0012] In some embodiments, the methods of the present disclosure further include selectively removing the bilayer hardmask from over a first region of the substrate to expose a surface of the first region of the substrate.

[0013] In some embodiments, selectively removing the bilayer hardmask from the first region of the substrate further comprises forming a patterned resist layer over the second region of the substrate and contacting the exposed regions of the bilayer hardmask with a wet etchant.

[0014] In some embodiments, the wet etchant is selected from the group consisting of hydrofluoric acid, sulfuric acid, and phosphoric acid.

[0015] In some embodiments, the methods of the present disclosure further include performing a cleaning process on the exposed surface of the first region of the substrate, thereby forming a cleaned first region surface.

[0016] In some embodiments, the cleaning process includes contacting the exposed surface of the first region of the substrate with a plasma generated from a gas mixture comprising a fluorine-containing gas and ammonia.

[0017] In some embodiments, the cleaning process removes the second hard mask layer from over the second region of the substrate.

[0018] In some embodiments, the methods of the present disclosure can further include forming a semiconductor layer on the cleaned first region surface.

[0019] In some embodiments, forming the semiconductor layer includes depositing the semiconductor layer directly on the cleaned first region surface by an epitaxial deposition process.

[0020] In some embodiments, methods of the present disclosure can further include removing any remaining portions of the bilayer hardmask from over the second region of the substrate.

[0021] The embodiments of the present disclosure may also include further methods for forming a semiconductor structure. In some embodiments, the method of the present disclosure includes seating a substrate including an NMOS region and a PMOS region in a reaction chamber, and depositing a bilayer hardmask on the NMOS region and on the PMOS region. In some embodiments, depositing the bilayer hardmask may include depositing a first hardmask layer on both the NMOS region and the PMOS region, and depositing a second hardmask layer on the first hardmask layer. The method of the present disclosure may further include selectively removing the bilayer hardmask on the NMOS region to expose a surface of the NMOS region, performing a cleaning process on the exposed surface of the NMOS region, thereby forming a clean NMOS surface, depositing a semiconductor layer on the clean NMOS surface, and removing the remaining portion of the bilayer hardmask disposed on the PMOS region.

[0022] In some embodiments, the bilayer hardmask is deposited by a cyclic deposition process.

[0023] In some embodiments, the semiconductor layer is deposited by an epitaxial deposition process.

[0024] In some embodiments, selectively removing the bilayer hardmask over the NMOS region can further include forming a patterned resist layer over the PMOS region and contacting the exposed regions of the bilayer hardmask with a wet etchant selected from the group consisting of hydrofluoric acid, sulfuric acid, and phosphoric acid.

[0025] In some embodiments, the cleaning process removes the second hardmask layer over the PMOS region while maintaining at least a portion of the first hardmask layer over the PMOS region.

[0026] Embodiments of the present disclosure also disclose semiconductor structures formed according to the methods disclosed herein.

[0027] These and other embodiments will become readily apparent to those skilled in the art from the following detailed description of certain embodiments, taken in conjunction with the accompanying drawings, in which: The invention is not limited to any particular embodiment disclosed.

[0028] A more complete understanding of the embodiments of the present disclosure may be obtained by reference to the detailed description and claims when considered in conjunction with the following illustrative drawings. [Brief description of the drawings]

[0029] [Figure 1] FIG. 1 illustrates an exemplary method according to an embodiment of the present disclosure. [Diagram 2] 1 illustrates a further exemplary method according to an embodiment of the present disclosure. [Diagram 3] FIG. 1 illustrates an exemplary structure according to an embodiment of the present disclosure. [Figure 4] FIG. 1 illustrates an exemplary structure according to an embodiment of the present disclosure. [Diagram 5] FIG. 1 illustrates an exemplary structure according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] It will be appreciated that elements in the figures are illustrated for simplicity and clarity and have not necessarily been drawn to scale, for example, the dimensions of some of the elements in the figures may be exaggerated relative to other elements to help improve understanding of the illustrated embodiments of the present disclosure.

[0031] The descriptions of exemplary embodiments of methods, structures, devices, and apparatus provided below are merely exemplary and are intended for illustrative purposes only, and the following descriptions are not intended to limit the scope of the present disclosure or the claims. Moreover, the recitation of multiple embodiments having described features is not intended to exclude other embodiments having additional features or other embodiments incorporating different combinations of the described features. For example, various embodiments are described as exemplary embodiments and may be recited in dependent claims. Unless otherwise stated, the exemplary embodiments or components thereof may be combined or applied separately from each other.

[0032] As described in more detail below, various embodiments of the present disclosure provide methods for forming semiconductor structures suitable for various applications. Exemplary methods can be used, for example, to form complementary metal-oxide-semiconductor (CMOS) device structures. For example, the methods of the present disclosure can include a bilayer hard mask that can be used to form logic devices, dynamic random access memories (DRAMs), and three-dimensional NAND devices. However, unless otherwise stated, the present invention is not necessarily limited to such examples.

[0033] In this disclosure, "gas" can include materials that are gases at ambient temperature and pressure (NTP), vaporized solids, and / or vaporized liquids, and can be comprised by a single gas or a mixture of gases, depending on the circumstances. Gases other than the process gas, i.e., gases introduced without passing through a gas distribution assembly, other gas distribution devices, etc., can be used, for example, to seal the reaction space and can include sealing gases, for example, noble gases. In some cases, the term "precursor" can refer to a compound that participates in a chemical reaction that produces another compound, and specifically a compound that constitutes the matrix of the film or the backbone of the film. The term "reactant" can be used interchangeably with the term precursor. The term "inert gas" can refer to a gas that does not participate in a chemical reaction and / or does not become part of the film matrix to any significant extent. Exemplary inert gases include helium, argon, and any combination thereof. In some cases, the inert gas can include nitrogen and / or hydrogen.

[0034] The term "substrate" as used herein can refer to any underlying material or material that can be used to form a device, circuit, or film, or any underlying material or material on which a device, circuit, or film can be formed. The substrate can include a bulk material such as silicon (e.g., single crystal silicon), other Group IV materials such as germanium, or other semiconductor materials such as Group II-VI or Group III-V semiconductor materials, and can include one or more layers overlying or underlying the bulk material. Additionally, the substrate can include various features (such as recesses, protrusions, and the like) formed in or on at least a portion of the layers of the substrate. By way of example, the substrate can include a bulk semiconductor material and an insulating or dielectric material layer overlying at least a portion of the bulk semiconductor material.

[0035] The terms "film" and / or "layer" as used herein can refer to any continuous or non-continuous structures and materials, such as materials deposited by the methods disclosed herein. For example, films and / or layers can include two-dimensional materials, three-dimensional materials, nanoparticles, or even partial or complete molecular layers, or partial or complete atomic layers, or clusters of atoms and / or molecules. Films or layers can include materials or layers with pinholes, which may be at least partially continuous.

[0036] A "structure" as used herein can be or can include a substrate as described herein. A structure can include one or more layers on or within a substrate, e.g., one or more layers formed according to a method as described herein. An entire device or a partial device portion can be included within or on the structure.

[0037] The term "cyclic deposition process" or "cyclical deposition process" can refer to the sequential introduction of precursors (and / or reactants) into a reaction chamber to deposit layers on a substrate, and includes processing techniques such as atomic layer deposition (ALD), cyclic chemical vapor deposition (cyclic CVD), and hybrid cyclic deposition processes that include ALD and cyclic CVD components.

[0038] The term "atomic layer deposition" can refer to a deposition process in which a deposition cycle, typically multiple successive deposition cycles, is performed in a process chamber. The term atomic layer deposition as used herein is also meant to include processes represented by related terms, such as chemical vapor deposition atomic layer deposition, atomic layer epitaxy (ALE), molecular beam epitaxy (MBE), gas source MBE, metalorganic MBE, and chemical beam epitaxy, when performed with alternating pulses of precursor / reactive gases and purge (e.g., inert carrier) gases.

[0039] Generally, in an ALD process, during each deposition cycle, a precursor is introduced into the reaction chamber and chemisorbs onto the deposition surface (e.g., the substrate surface, which may include previously deposited material or other materials from a previous ALD cycle) to form a monolayer or submonolayer of material that does not readily react with another precursor (i.e., a self-limiting reaction). In some cases, a reactant (e.g., another precursor or reactant gas) may then be introduced into the process chamber for use in converting the chemisorbed precursor into a desired material on the deposition surface. The reactant may be capable of further reaction with the precursor. Purging steps may be utilized during one or more deposition cycles, e.g., during each step of each cycle, to remove any excess precursor from the process chamber and / or to remove any excess reactants and / or reaction by-products from the reaction chamber.

[0040] Furthermore, in this disclosure, any two numbers of a variable can constitute a workable range for that variable, and any range stated may include or exclude the endpoints. In addition, any value of a variable stated (whether they are stated with "about" or not) may refer to an exact or approximate value, and may include equivalents, such as an average, median, representative value, majority, or the like. Furthermore, in this disclosure, the terms "comprise", "comprise", and "have" refer independently in some embodiments to "typically or broadly include", "comprise", "consist essentially of", or "consist of". In this disclosure, any defined meaning does not necessarily exclude the ordinary and customary meaning in some embodiments.

[0041] It will be understood that the terms "on" or "over" may be used herein to describe relative positional relationships. Another element, film or layer may be directly on the layer referred to, or another layer (intermediate layer) or element may be interposed therebetween, or a layer may be disposed on the layer referred to but not completely cover the surface of the layer referred to. Thus, unless the term "directly" is used separately, the terms "on" or "over" will be interpreted as relative concepts. Similarly, the terms "under", "underlying" or "below" will be understood as relative concepts.

[0042] The present disclosure may include methods for forming semiconductor structures, particularly semiconductor structures that include a bilayer hardmask. More particularly, processes employed in the fabrication of CMOS device structures may require hardmask materials that are optimized to avoid epitaxial deposition of semiconductor layers, such as silicon germanium (SiGe) and phosphorus doped silicon (SiP), in undesired locations of the device structures.

[0043] In some CMOS fabrication methods, for example, aluminum oxide (AlO x Metal oxide hardmasks, such as aluminum oxide hardmasks, may be employed as metal oxide hardmasks during the etching process. However, single-layer metal oxide hardmasks, such as aluminum oxide, may contain pinholes that form during, for example, CMOS fabrication processes, and such pinholes may cause problems in downstream CMOS fabrication processes. For example, pinholes in single-layer metal oxide hardmasks may cause fabrication problems when the hardmask is employed to prevent epitaxial deposition of a semiconductor layer in certain regions of a substrate.

[0044] Thus, embodiments of the present disclosure may employ a bilayer hardmask including a first hardmask layer and a second hardmask layer, for example, the first hardmask layer can include a first metal oxide, such as, for example, aluminum oxide, that is disposed directly on the substrate, and the second hardmask layer can include a second metal oxide, such as, for example, hafnium oxide, yttrium oxide, or zirconium oxide, where the second hardmask layer has a lower dry etch rate compared to the first hardmask layer.

[0045] Thus, embodiments of the present disclosure provide a method for masking an epitaxial layer of a first metal oxide (MO) instead of a single metal oxide hardmask layer, particularly during fabrication processes that require masking of areas to prevent unwanted epitaxial deposition in undesired areas of a substrate. x1 ) and a second metal oxide (MO x2 In some embodiments, a bilayer hardmask composed of a first metal oxide and a second metal oxide can be in the form of a stacked structure. In some embodiments, a bilayer hardmask composed of a first metal oxide and a second metal oxide can be in the form of a mixed metal oxide structure.

[0046] In some embodiments, the top hardmask layer (second hardmask layer) can have a lower dry etch rate than the bottom hardmask layer (first hardmask layer), and the top hardmask layer can be formed to a thickness thin enough that it can be removed by employing a wet etching process used during a CMOS fabrication process. For example, the CMOS fabrication process of the present disclosure may employ a first wet etching step (e.g., employing dilute hydrofluoric acid) that can remove the bilayer hardmask from a first region (e.g., NMOS region) of the substrate, while maintaining the bilayer hardmask to protect a second region (e.g., PMOS region) of the substrate.

[0047] In subsequent fabrication processes of the disclosed steps, the bilayer hardmask remaining on the second region of the substrate (e.g., PMOS region) can be removed after epitaxial deposition of the desired semiconductor layer on the first region of the substrate (e.g., deposition on the NMOS region). The uppermost hardmask layer having a lower etch rate can be removed while keeping the underlying lower hardmask layer intact, thereby avoiding the formation of pinholes in the lower hardmask layer. As a result, for example, the subsequent epitaxial deposition process on the NMOS region maintains protection for the PMOS region. In some embodiments, the employment of the bilayer hardmask and the method of forming such a bilayer hardmask may be repeated again to protect the NMOS region during epitaxial deposition of a semiconductor layer (e.g., SiGe semiconductor layer) on the PMOS region.

[0048] Thus, the present disclosure may include a method for forming a semiconductor structure. In some embodiments, the method may include seating a substrate including a first region and a second region in a reaction chamber and forming a bilayer hardmask on the substrate. In some embodiments, forming the bilayer hardmask layer may include performing one or more deposition cycles of a first cyclical deposition process to deposit a first hardmask layer including a first metal oxide on the substrate and performing one or more deposition cycles of a second cyclical deposition process to deposit a second hardmask layer including a second metal oxide on the first metal oxide hardmask layer.

[0049] More specifically, Figure 1 illustrates an exemplary process 100 that can be used to form a bilayer hardmask on a substrate including a first region and a second region. Briefly, the exemplary method 100 may include providing a substrate in a reaction chamber and employing a first cyclical deposition process (cyclical process 105) for depositing a first hardmask layer including a first metal oxide on the substrate, followed by a second cyclical deposition process (cyclical process 135) for depositing a second hardmask layer including a second metal oxide on the first metal hardmask layer. The first hardmask layer (i.e., the first metal oxide) is disposed proximate to the substrate, and the second hardmask layer (i.e., the second metal oxide) is disposed distal to the substrate, with the combination of the first hardmask layer and the second hardmask layer constituting a bilayer hardmask.

[0050] More specifically, the exemplary method 100 may include providing a substrate in a reaction chamber. The reaction chamber employed to form the bilayer hard mask during the exemplary process 100 may be or may include a reaction chamber of an atomic layer deposition reactor system configured to perform one or more cyclic deposition processes. The reaction chamber may be a stand-alone reaction chamber or part of a cluster tool. The reaction chamber may be a batch processing tool. In some embodiments, a flow type reactor may be utilized. In some embodiments, a showerhead type reactor may be utilized. In some embodiments, a space-divided reactor may be utilized. In some embodiments, a high volume manufacturable single wafer reactor may be utilized. In other embodiments, a batch reactor including multiple substrates may be utilized. For embodiments in which a batch reactor is used, the number of substrates may range from 10 to 200, or from 50 to 150, or even from 100 to 130. The reactor may be configured as a thermal reactor without a plasma excitation device. Alternatively, the reactor may include a direct and / or remote plasma device.

[0051] The substrate disposed in the reaction chamber may be heated to a desired deposition temperature for subsequent deposition. For example, the substrate may be heated to a substrate temperature of less than 800° C., or less than 600° C., or less than 400° C., or even less than 200° C. In some embodiments of the present disclosure, the substrate temperature may be above room temperature, between 200° C. and 800° C., or between 200° C. and 600° C., or between 200° C. and 400° C. The temperature during the exemplary process 100 ( FIG. 1 ) (i.e., the cyclic deposition process for forming a bilayer hard mask) may also be within these ranges.

[0052] In addition to controlling the temperature of the substrate, the pressure in the reaction chamber may also be adjusted to enable deposition of a bilayer hard mask. For example, in some embodiments of the present disclosure, the pressure in the reaction chamber may be less than 760 Torr, or between 0.1 Torr and 10 Torr, or between 0.5 Torr and 5 Torr, or between 1 Torr and 4 Torr.

[0053] Once the temperature of the substrate is set to the desired deposition temperature and the pressure within the reaction chamber is adjusted as desired, the exemplary process 100 may proceed to step 105, which includes employing a first cyclical deposition process to deposit a first hard mask layer comprising a first metal oxide on the surface of the substrate, particularly on the first region and the second region of the substrate. For example, embodiments of the present disclosure may include performing one or more deposition cycles of a first cyclical deposition process to deposit a first metal oxide layer comprising aluminum oxide on the surface of the substrate, particularly on the surface of the first region and the surface of the second region.

[0054] In some embodiments, the first cyclic deposition process 105 may include providing a first metal precursor to the reaction chamber (process step 110) and providing a first oxidizer to the reaction chamber (process step 120). The first metal precursor and the first oxidizer can be provided to the reaction chamber separately and / or sequentially, with or without an intervening reaction chamber purge sequence. Process steps 110 and 120 (and any intervening purge sequences) may constitute a first unit deposition cycle, which may be repeated one or more times to deposit a first hard mask layer (e.g., a first metal oxide) to a desired thickness on the substrate, particularly on the first and second regions.

[0055] More specifically, process step 110 includes providing a first metal precursor to the reaction chamber. The first metal precursor can be pulsed into the reaction chamber. The term "pulse" can be understood to include providing a precursor into the reaction chamber for a predetermined amount of time. Unless otherwise stated, the term "pulse" does not limit the length or duration of the pulse, and the pulse can be of any length of time. The first metal precursor pulse can be provided to the reaction chamber with a carrier gas flow. In some embodiments, the first metal precursor can include a volatile metal species that reacts with the surface of the substrate. The first metal precursor pulse can self-saturate the substrate surface such that excess components of the gallium precursor pulse do not further react with the molecular layer formed by the process.

[0056] The first metal precursor pulse is preferably provided as a gas phase reactant. A first metal precursor gas may be considered "volatile" for purposes of this disclosure if the species exhibits sufficient vapor pressure under process conditions to be transported to the substrate surface in sufficient concentration to saturate the exposed surface.

[0057] According to some embodiments of the present disclosure, the first hard mask layer can include aluminum oxide, and providing the first metal precursor to the reaction chamber can include providing an aluminum precursor to the reaction chamber. In some embodiments, the aluminum precursor can include one or more of trimethylaluminum (TMA), dimethylaluminum chloride, aluminum trichloride (AlCl3), dimethylaluminum isopropoxide (DMAI), tris(tert-butyl)aluminum (TTBA), tris(isopropoxide)aluminum (TIPA), or triethylaluminum (TEA). In some embodiments, the aluminum precursor can include dimethylaluminum isopropoxide (DMAI).

[0058] The exemplary process 100 (FIG. 1) may continue with process step 120, which includes providing a first oxidant to the reaction chamber. In some embodiments, the first oxidant may include one or more of water (HO), hydrogen peroxide (HO), ozone (O), or nitrogen oxides, such as nitric oxide (NO), nitrous oxide (NO), or nitrogen dioxide (NO). In some embodiments of the present disclosure, the first oxidant precursor may include an organic alcohol, such as isopropyl alcohol.

[0059] In some embodiments, the first cyclic deposition process 105 may be repeated one or more times until a desired termination criterion is reached (process step 130) and the first cyclic deposition process may terminate. In some embodiments, the termination criterion for process step 130 may be reached based on a desired thickness of the first hard mask layer (e.g., a first metal oxide layer), or alternatively, the termination criterion for process step 130 may be reached upon performing a predetermined number of deposition cycles of the first cyclic deposition process 105. As a non-limiting example, the first cyclic deposition process 105 may be terminated after a desired thickness of aluminum oxide is deposited on the substrate, and in particular on the first and second regions of the substrate.

[0060] The exemplary process 100 (FIG. 1) may continue by performing one or more deposition cycles of a second cyclical deposition process (cyclical deposition process 135) to deposit a second hardmask layer comprising a second metal oxide, where the second hardmask layer (i.e., the second metal oxide) is deposited on the first hardmask layer (i.e., the first metal oxide). In some embodiments, the second hardmask layer is deposited directly on the first hardmask layer, thereby forming a bilayer hardmask. The second cyclical deposition process 135 may be similar to that of the first cyclical deposition process 105, and thus differences in the second cyclical deposition process 135 are described below.

[0061] More specifically, a second cyclical deposition process can be employed to deposit a second hardmask layer (e.g., a second metal oxide) onto the first hardmask layer, and in certain embodiments, directly onto the first hardmask layer, thereby forming a bilayer hardmask.

[0062] More specifically, in some embodiments, the second cyclical deposition process 135 can include providing a second metal precursor to the reaction chamber (process step 140) and providing a second oxidizer to the reaction chamber (process step 150). In some embodiments, the second hardmask layer is compositionally different from the first hardmask layer. In some embodiments, the second hardmask layer includes a second metal oxide that is different from the first metal oxide. In some embodiments, the second hardmask layer can be selected from the group consisting of hafnium oxide, yttrium oxide, and zirconium oxide.

[0063] For example, in embodiments in which the second hard mask layer comprises hafnium oxide, providing a second metal precursor to the reaction chamber can include providing a hafnium precursor to the reaction chamber. For example, the hafnium precursor can be selected from the group consisting of hafnium halide precursors and hafnium organometallic precursors. In some embodiments, the hafnium halide precursor comprises at least one of hafnium tetrachloride (HfCl4), hafnium tetraiodide (HfI4), or hafnium tetrabromide (HfBr4). In some embodiments, the hafnium organometallic precursor comprises at least one of tetrakis(ethylmethylamido)hafnium (Hf(NEtMe)4), tetrakis(dimethylamido)hafnium (Hf(NMe2)4), tetrakis(diethylamido)hafnium (Hf(NEt2)4), (tris(dimethylamido)cyclopentadienylhafnium HfCp(NMe2)3, or bis(methylcyclopentadienyl)methoxymethylhafnium (MeCp)2Hf(CH)3(OCH3).

[0064] In some embodiments, the second hard mask layer can include a zirconium oxide layer. Thus, in such embodiments, the second metal precursor can be, for example, Zr(NEtMe)4, ZrCp2(NMe2)2, Zr(O t The zirconium precursor may include a zirconium precursor such as ZrO2).

[0065] In some embodiments, the second hard mask layer can include an yttrium oxide layer. Thus, in such embodiments, the second metal precursor can include an yttrium precursor, such as, for example, Y(CpBu)3, Y(CpEt)3, or Y(CpMe)3.

[0066] The exemplary process 100 (FIG. 1) may continue with process step 150, which includes providing a second oxidant to the reaction chamber. In some embodiments, the second oxidant may include one or more of water (H2O), hydrogen peroxide (H2O2), ozone (O3), or nitrogen oxides, such as nitric oxide (NO), nitrous oxide (N2O), or nitrogen dioxide (NO2). In some embodiments of the present disclosure, the first oxidant precursor may include an organic alcohol, such as isopropyl alcohol. In some embodiments, the first oxidant and the second oxidant may be the same, while in other embodiments, the first oxidant and the second oxidant may be different.

[0067] In some embodiments, the second cyclic deposition process 135 may be repeated one or more times until a desired termination criterion is reached (process step 160) and the second cyclic deposition process may terminate. In some embodiments, the termination criterion for process step 160 may be reached based on a desired thickness of the second hardmask layer (e.g., second metal oxide layer), or alternatively, the termination criterion for process step 160 may be reached upon completing a predetermined number of deposition cycles of the second cyclic deposition process 105. As a non-limiting example, the second cyclic deposition process 135 may be terminated after a desired thickness of hafnium oxide is deposited on the first hardmask layer substrate. The exemplary process 100 may then terminate via process step 170 upon completion of the formation of the bilayer hardmask.

[0068] In some embodiments, the bilayer hardmask of the present disclosure may be employed in the fabrication of CMOS device structures. More specifically, exemplary process 200 (FIG. 2) illustrates the employment of the bilayer hardmask of the present disclosure in the fabrication of CMOS device structures.

[0069] More specifically, the process 200 may begin with seating a substrate including a first region and a second region in a reaction chamber and forming a bilayer hard mask on the substrate as previously described herein. The exemplary process 200 may then proceed through process step 220, which includes selectively removing the bilayer hard mask from over the first region of the substrate to expose a surface of the first region of the substrate. In some embodiments, selectively removing the bilayer hard mask from the first region of the substrate further includes forming a patterned resist layer over the second region of the substrate and contacting the exposed region of the bilayer hard mask with a wet etchant. In some embodiments, the wet etchant is selected from the group consisting of hydrofluoric acid, sulfuric acid, and phosphoric acid, as well as dilute and hydrogen peroxide mixtures of the aforementioned wet etchants.

[0070] The exemplary process 200 may continue through process step 230, which includes performing a cleaning process on the exposed surface of the first region of the substrate, thereby forming a cleaned first region surface. In some embodiments, the cleaning process includes cleaning the exposed surface of the first region of the substrate with a fluorine-containing gas (e.g., hydrofluoric acid, NF3, NF3 * ) and ammonia. In some embodiments, the cleaning process removes at least a portion of the second hardmask layer from over the second region of the substrate. In some embodiments, the cleaning process removes the second hardmask layer from over the second region of the substrate.

[0071] The exemplary process 200 may continue through process step 240, which includes forming a semiconductor layer on the cleaned first region surface. In some embodiments, forming the semiconductor layer includes depositing the semiconductor layer directly on the cleaned first region surface by an epitaxial deposition process. In some embodiments, an epitaxial deposition process may be employed to deposit a SiGe layer or a SiP layer on the cleaned first surface.

[0072] The exemplary process 200 may continue through process step 240, which includes removing any remaining portions of the bilayer hardmask from over a second region of the substrate.

[0073] The bilayer hardmask of the present disclosure may be employed in other methods of fabricating CMOS device structures. More specifically, the process of the present disclosure may include seating a substrate including an NMOS region and a PMOS region in a reaction chamber, and depositing a bilayer hardmask on the NMOS region and on the PMOS region. In some embodiments, depositing the bilayer hardmask includes depositing a first hardmask layer on both the NMOS region and the PMOS region, and depositing a second hardmask layer on the first hardmask layer. In some embodiments, the bilayer hardmask is deposited by a cyclic deposition process.

[0074] The process of the present disclosure may further include selectively removing the bilayer hardmask over the NMOS region to expose a surface of the NMOS region and performing a cleaning process on the exposed surface of the NMOS region, thereby forming a clean NMOS surface. In some embodiments, selectively removing the bilayer hardmask over the NMOS region further includes forming a patterned resist layer over the PMOS region and contacting the exposed region of the bilayer hardmask with a wet etchant selected from the group consisting of hydrofluoric acid, sulfuric acid, and phosphoric acid.

[0075] The process of the present disclosure may further include depositing a semiconductor layer on the clean NMOS surface. In some embodiments, the semiconductor layer is deposited by an epitaxial deposition process.

[0076] The embodiments of the present disclosure also include semiconductor structures formed by the methods disclosed herein. For example, FIG. 3(a) illustrates a substrate including a first region 304 (e.g., an NMOS region) and a second region 302 (e.g., a PMOS region). A first hard mask layer 306 (e.g., aluminum oxide) may be deposited on the surface of the first region and the second region, as illustrated in FIG. 3(b). A second hard mask layer 308 (e.g., hafnium oxide) may be deposited on the surface of the first hard mask layer 306, thereby forming a bilayer mask 300, as illustrated in FIG. 3(c).

[0077] 4(a-c) illustrate further semiconductor structures that may be formed according to embodiments of the present disclosure. For example, as illustrated in FIG. 4(a), a patterned resist layer 310 may be formed and disposed on the second region 302 (e.g., PMOS region). A selective etching process may then be performed to remove the bilayer hard mask from the region above the first region 304 (e.g., NMOS region), as shown in FIG. 4(b), and after removal of the above layers, the remaining patterned resist may be removed. The structure illustrated in FIG. 4(b) may then be subjected to a cleaning process to provide a cleaned first region surface (e.g., clean NMOS surface region), during which the second hard mask layer 308 overlying the second region 302 (e.g., PMOS region) may be removed, as illustrated in FIG. 4(c). In some embodiments, the cleaning process may remove a portion of the second hard mask layer 308 overlying the second region.

[0078] 5(a,b) illustrate further structures that can be formed according to embodiments of the present disclosure. For example, a semiconductor layer 310 can be deposited on a first region 304 (e.g., an NMOS region) by an epitaxial deposition method, as illustrated in FIG. 5(a). As illustrated in FIG. 5(a), the remaining portion of the bilayer hard mask prevents deposition of the semiconductor layer 310 on a second region 302 (e.g., a PMOS region). After deposition of the semiconductor layer 310, the remaining bilayer hard mask remaining on the second region 302 may be removed by, for example, an etching method, as illustrated in FIG. 5(b).

[0079] The exemplary embodiments of the present disclosure described above are merely examples of embodiments of the present invention, as defined by the appended claims and their legal equivalents, and therefore do not limit the scope of the present invention. Any equivalent embodiments are intended to be within the scope of the present invention. Indeed, various modifications of the present disclosure, in addition to those shown and described herein, such as alternative useful combinations of the described elements, may become apparent to those skilled in the art from the description. Such modifications and embodiments are also intended to be included within the scope of the appended claims.

Claims

1. 1. A method of forming a semiconductor structure, the method comprising: Seating a substrate including a first region and a second region in a reaction chamber; forming a bilayer hard mask on the substrate, the forming of the bilayer hard mask comprising: performing one or more deposition cycles of a first cyclical deposition process to deposit a first hard mask layer comprising a first metal oxide on the substrate; performing one or more deposition cycles of a second cyclical deposition process to deposit a second hardmask layer comprising a second metal oxide on the first hardmask layer, forming a bilayer hardmask.

2. a first unit deposition cycle of the first cyclical deposition process comprising: providing a first metal precursor to the reaction chamber; providing a first oxidant to the reaction chamber.

3. The method of claim 2 , wherein the first hard mask layer comprises aluminum oxide.

4. a second unit deposition cycle of the second cyclical deposition process comprising: providing a second metal precursor to the reaction chamber; and providing a second oxidant to the reaction chamber.

5. 5. The method of claim 4, wherein the second hard mask layer comprises aluminum oxide and a second, different metal oxide.

6. 5. The method of claim 4, wherein the second hard mask layer is selected from the group consisting of hafnium oxide, zirconium oxide, and yttrium oxide.

7. 10. The method of claim 1, further comprising selectively removing the bilayer hardmask from over the first region of the substrate to expose a surface of the first region of the substrate.

8. 8. The method of claim 7, wherein selectively removing the bilayer hardmask from the first region of the substrate further comprises forming a patterned resist layer over the second region of the substrate and contacting exposed regions of the bilayer hardmask with a wet etchant.

9. The method of claim 8 , wherein the wet etchant is selected from the group consisting of hydrofluoric acid, sulfuric acid, and phosphoric acid.

10. The method of claim 7 , further comprising performing a cleaning process on the exposed surface of the first region of the substrate, thereby forming a cleaned first region surface.

11. The method of claim 10 , wherein the cleaning process comprises contacting the exposed surface of the first region with a plasma generated from a gas mixture comprising a fluorine-containing gas and ammonia.

12. 11. The method of claim 10, wherein the cleaning process removes the second hard mask layer from over the second region.

13. The method of claim 12 further comprising forming a semiconductor layer on the cleaned first region surface.

14. 14. The method of claim 13, wherein forming the semiconductor layer comprises depositing the semiconductor layer directly on the cleaned first region surface by an epitaxial deposition process.

15. 15. The method of claim 14, further comprising removing any remaining portions of the bilayer hardmask from over the second region.

16. 1. A method of forming a semiconductor structure, the method comprising: Seating a substrate including an NMOS region and a PMOS region in a reaction chamber; depositing a bilayer hardmask over the NMOS region and the PMOS region, wherein depositing the bilayer hardmask comprises: depositing a first hard mask layer over both the NMOS region and the PMOS region; depositing a bilayer hardmask, comprising: depositing a second hardmask layer over the first hardmask layer; selectively removing the dual layer hard mask over the NMOS region to expose a surface of the NMOS region; performing a cleaning process on the exposed surfaces of the NMOS regions, thereby forming a clean NMOS surface; depositing a semiconductor layer on the clean NMOS surface; and removing a remaining portion of the bilayer hardmask disposed over the PMOS region.

17. 17. The method of claim 16, wherein the bilayer hardmask is deposited by a cyclic deposition process.

18. The method of claim 16 , wherein the semiconductor layer is deposited by an epitaxial deposition process.

19. 17. The method of claim 16, wherein selectively removing the bilayer hardmask over the NMOS region further comprises forming a patterned resist layer over the PMOS region and contacting exposed areas of the bilayer hardmask with a wet etchant selected from the group consisting of hydrofluoric acid, sulfuric acid, and phosphoric acid.

20. 17. The method of claim 16, wherein the cleaning process removes the second hardmask layer over the PMOS region while maintaining at least a portion of the first hardmask layer over the PMOS region.