Photoimagable dielectrics

Soluble polyimide resin compositions with tailored tetracarboxylic acid and diamine components address high CTE and curing temperature issues, offering improved mechanical and dielectric properties for semiconductor packaging, preventing wafer warping and enhancing adhesion.

JP2024137865APending Publication Date: 2024-10-07DUPONT ELECTRONIC MATERIALS INT LLC +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024044359
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-21
Filing Date
2024-03-21
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional polyimide resins used in semiconductor packaging face challenges with high cure imidization temperatures, high coefficient of thermal expansion (CTE), and high water absorption, leading to warping of silicon wafer chips, while low molecular weight polyimides offer poor mechanical properties and reduced solubility.

Method used

Development of soluble polyimide resin compositions comprising tetracarboxylic acid, diamine, and end-capping compounds, tailored to provide high tensile strength, low CTE, and low dielectric properties, suitable for low-temperature curing and advanced packaging applications.

Benefits of technology

The soluble polyimide resins exhibit improved mechanical properties, low dielectric constants, and reduced CTE, enabling stable film formation without warping, suitable for electronic devices requiring low curing temperatures and high adhesion to copper and silicon substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137865000001
    Figure 2024137865000001
  • Figure 2024137865000002
    Figure 2024137865000002
  • Figure 2024137865000003
    Figure 2024137865000003
Patent Text Reader

Abstract

To provide photoimagable dielectrics.SOLUTION: There is provided a soluble polyimide resin comprising: (a) one or more tetracarboxylic acid component residues: (b) one or more diamine component residues; and (c) one or more endcapping compounds, wherein the one or more endcapping compounds comprise one or more crosslinking groups. The soluble polyimide resin can be used in electronics applications.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to soluble polyimide resin compositions, methods for preparing such resins and their use in the manufacture of electronic devices. [Background technology]

[0002] Polymer resins are used in spin-on dielectric packaging, circuit boards, laminates, coatings for metal foils, antenna-in-packages and other electronic applications. The resins must provide films / coatings with good mechanical and adhesion properties as well as low dielectric properties. In particular, high tensile strength, high tensile elongation, high glass transition temperature (T g It is desirable to have a low coefficient of thermal expansion (CTE), good adhesion to copper, and low dielectric constant (Dk) and loss tangent (Df) at high frequencies. In addition, it is desirable to be able to cure the resin at lower temperatures without curing for excessively long periods of time.

[0003] Such a balance of properties would be possible only with a resin system designed to combine multiple polymers, fillers, other components, etc., to tailor the system properties and / or drive the reaction between the resins. Although there are many traditional packaging materials that have been employed over the years, polyimides have been the material of choice for semiconductor packaging applications due to their excellent electrical, mechanical, and thermal properties. However, the use of polyimides in this type of application presents challenges associated with their high cure imidization temperature, high CTE, and high water absorption. The high CTE leads to shrinkage of the cured polyimide film, and the associated high residual strain can cause chip warpage on silicon wafers.

[0004] Soluble polyimides are known and photosensitive compositions containing these polymers have been disclosed. In general, it has been found that low molecular weight polyimide polymers provide acceptable photolithographic properties. However, compositions using such polymers suffer from poor mechanical properties to the extent that they cannot be used as advanced packaging materials in packaging processes. Acceptable mechanical properties can be obtained by increasing the molecular weight of the polyimide. However, the resulting polyimide compositions may have poor developer solubility, which often results in poor lithographic performance.

[0005] An ideal polyimide for a photosensitive composition is one that not only has low loss, but is also photoimageable and compatible with the processing conditions used in packaging applications (i.e., low cure temperature and developable with organic solvents). The completed processed material should exhibit high elongation, acceptable mechanical properties, and good adhesion to substrates commonly used in advanced packaging applications (e.g., copper, silicon, silicon nitride, etc.). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] U.S. Patent No. 7,198,878 [Patent Document 2] U.S. Patent No. 8,143,360 [Patent Document 3] Korean Patent No. 10-2422883B1 Summary of the Invention [Problem to be solved by the invention]

[0007] Under these circumstances, there is a continuing need to develop such materials. [Means for solving the problem]

[0008] As used throughout this specification, the following abbreviations shall have the following meanings unless the context clearly indicates otherwise: °C = degrees Celsius; g = grams; nm = nanometers, μm = microns = micrometers; mm = millimeters; sec. = seconds; and min. = minutes. Unless otherwise specified, all amounts are weight percent ("wt %) and all ratios are molar ratios. All numerical ranges are inclusive and combinable in any order, except where it is clear that such numerical ranges are constrained to add up to 100%. Unless otherwise specified, all molecular weights of polymers and oligomers are weight average molecular weights ("Mw") in g / mole or Daltons, as determined by gel permeation chromatography relative to polystyrene standards.

[0009] The articles "a," "an," and "the" refer to the singular and plural unless the context clearly indicates otherwise. As used herein, the term "and / or" includes any and all combinations of one or more of the associated items.

[0010] As used herein, R, R a , R b , R', R" and any other variables are generic symbols and the variables defined within the formula may be the same or different.

[0011] As used herein, the term "addition polymerizable" as it applies to monomers is intended to mean unsaturated monomers that can be polymerized simply by linking groups without the concomitant formation of other products.

[0012] The term "adjacent," when referring to substituents, is intended to mean that the substituents are attached to a linked carbon by a single or multiple bond. Exemplary adjacent R groups are shown below:

[0013] [ka]

[0014] The term "alkoxy" is intended to mean the group RO--, where R is an alkyl group.

[0015] The term "alkyl" is intended to mean a group derived from an aliphatic hydrocarbon, and includes straight-chain, branched, or cyclic groups. A group "derived from" a compound refers to a group formed by removing one or more hydrogens or deuteriums. In some embodiments, an alkyl has 1 to 20 carbon atoms.

[0016] The term "amine" is intended to mean a compound containing a basic nitrogen atom with a lone pair, where lone pair refers to a set of two valence electrons that are not shared with another atom. The term "amino" refers to the functional groups -NH2, -NHR or -NR2, where R is the same or different in each occurrence and can be an alkyl or aryl group. The term "diamine" is intended to mean a compound containing two basic nitrogen atoms with lone pairs. The term "polyamine" is intended to mean a compound containing two or more basic nitrogen atoms with lone pairs. The term "aromatic diamine" is intended to mean an aromatic compound with two amino groups. The term "aromatic polyamine" is intended to mean an aromatic compound with two or more amino groups. The term "bent diamine" refers to a diamine in which the two basic nitrogen atoms and associated lone pairs are asymmetrically arranged around the center of symmetry of the corresponding compound or functional group, such as m-phenylenediamine:

[0017] [ka]

[0018] is intended to mean

[0019] The term "aromatic diamine residue" is intended to mean a moiety that is bound to two amino groups in an aromatic diamine. The term "aromatic polyamine residue" is intended to mean a moiety that is bound to two or more amino groups in an aromatic polyamine. The term "aromatic diisocyanate residue" is intended to mean a moiety that is bound to two isocyanate groups in an aromatic diisocyanate compound. The term "aromatic polyisocyanate residue" is intended to mean a moiety that is bound to two or more isocyanate groups in an aromatic polyisocyanate compound. This is further exemplified below.

[0020] [ka]

[0021] The terms "diamine residue" and "diisocyanate residue" are intended to mean moieties that are bonded to two amino groups or two isocyanate groups, respectively, and these moieties are aliphatic or aromatic. The terms "polyamine residue" and "polyisocyanate residue" are intended to mean moieties that are bonded to two or more amino groups or two or more isocyanate groups, respectively, and these moieties are aliphatic or aromatic.

[0022] The term "aromatic compound" is intended to mean an organic compound containing at least one unsaturated cyclic group having 4n+2 delocalized π-electrons.

[0023] The term "aryl" is intended to mean a group derived from an aromatic compound having one or more points of attachment. The term includes groups having a single ring and groups having multiple rings that may be linked by a single bond or fused together. Carbocyclic aryl groups have only carbon in the ring structure. Heteroaryl groups have at least one heteroatom in the ring structure.

[0024] The term "alkylaryl" is intended to mean an aryl group having one or more alkyl substituents.

[0025] The term "aryloxy" is intended to mean the group RO--, where R is an aryl group.

[0026] The term "crosslinking group" refers to a functional group that contains a bond or a short series of bonds that are used to link one polymer chain to another.

[0027] The term "curable" as applied to a composition is intended to mean a material that becomes harder and less soluble in solvents upon exposure to radiation and / or heat or under conditions of use.

[0028] The term "endcapping compound" refers to a discrete compound or group used in a resin to inhibit ongoing polymerization and thereby control the overall molecular weight of the resin.

[0029] The term "liquid composition" is intended to mean a liquid medium in which a material is dissolved to form a solution, in which a material is dispersed to form a dispersion, or in which a material is suspended to form a suspension or emulsion.

[0030] The term "(meth)acrylate" is intended to mean a group that is either an acrylate or a methacrylate.

[0031] The term "polyimide" refers to condensation polymers produced by the reaction of one or more polyfunctional anhydride components with one or more primary polyamines or polyisocyanates. They contain the imide structure -CO-NR-CO- as linear or heterocyclic units along the main chain of the polymer backbone.

[0032] The term "semiconductor wafer" as used herein is intended to encompass "semiconductor substrates," "semiconductor devices," and various packages for various levels of interconnection, such as single chip wafers, multi-chip wafers, packages for various levels, substrates for light emitting diodes (LEDs) or other assemblies requiring solder connections. Semiconductor wafers, such as silicon wafers, gallium arsenide wafers, and silicon germanium wafers, may be patterned or unpatterned. The term "semiconductor substrate" as used herein includes any substrate having one or more semiconductor layers or structures that include active or operable portions of a semiconductor device. The term "semiconductor substrate" is defined to mean any structure that includes semiconductor material, such as a semiconductor device. A semiconductor device refers to a semiconductor substrate on which at least one microelectronic device has been or will be fabricated. Thermally stable polymers include, but are not limited to, polyimides, e.g., KAPTON, ethylenediaminetetraacetate, propylene glycol, propylene glycol terephthalate ... TM Polyimides (DuPont, Wilmington, DE), liquid crystal polymers such as VECSTAR TM Examples of the polymer substrate include any polymer, such as LCP film (Kuraray Co., Ltd., Tokyo, Japan) and bismaleimide-triazine (BT) resin (MGC, Tokyo, Japan). Further polymer substrates include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride; polyester films such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate; or polycarbonate films. In addition, release paper and metal foils, such as copper foil and aluminum foil, can be used. The support and the protective film described below may be subjected to surface treatments such as matte treatment and corona treatment. Alternatively, the support and the protective film may be release-treated with a release agent such as a silicone resin-based release agent, an alkyd resin-based release agent, or a fluororesin-based release agent. In some non-limiting embodiments, the support has a thickness of 10 to 150 μm, and in some non-limiting embodiments, it is 25 to 50 μm.

[0033] The term "solvent" is intended to mean an organic compound that is liquid at the temperature of use. The term is intended to include a single organic compound or a mixture of two or more organic compounds.

[0034] The term "tetracarboxylic acid moiety residue" is intended to mean the moiety that is attached to the four carboxy groups in a tetracarboxylic acid moiety, as further exemplified below.

[0035] [ka]

[0036] The term "thermoset" is intended to mean a liquid or soft polymer that, upon exposure to heat or radiation, irreversibly crosslinks or irreversibly increases the molecular weight of the network such that the material cannot substantially reshape after such treatment.

[0037] The terms "film" and "layer" are used interchangeably throughout this specification.

[0038] All ranges are inclusive and combinable, for example the term "in the range of 50-3000 cPs or 100 cPs or more" would include each of 50-100 cPs, 50-3000 cPs, and 100-3000 cPs.

[0039] Unless otherwise expressly stated herein or the context of use indicates to the contrary, when an embodiment of the subject matter herein is stated or described as comprising, including, containing, having, consisting of or consisting of a particular feature or element, the embodiment may have one or more features or elements in addition to those expressly stated or described. Another embodiment of the subject matter disclosed herein is described as consisting essentially of a particular feature or element, in which the embodiment is free of any feature or element that would materially alter the principle of operation or distinguishing characteristics of the embodiment. Yet another embodiment of the subject matter described herein is described as consisting of a particular feature or element, in which the embodiment, or insubstantial variations thereof, have only the feature or element specifically stated or described.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs. Although methods and materials similar or equivalent to those described herein can be used to practice or test embodiments of the present disclosure, suitable methods and materials are described below. Furthermore, the materials, methods, and examples are illustrative only and are not intended to be limiting.

[0041] To the extent not described herein, many details regarding specific materials, processing operations and circuits are conventional and can be found in textbooks and other sources in the art of photoresists, dielectric materials and semiconducting components.

[0042] A soluble polyimide resin is provided, comprising: (a) one or more tetracarboxylic acid component residues; (b) one or more diamine component residues; and (c) one or more end-capping compounds, the one or more end-capping compounds comprising one or more crosslinking groups. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] The one or more tetracarboxylic acid component residues are not particularly limited and are derived from the corresponding tetracarboxylic acid dianhydrides selected from the group consisting of aromatic tetracarboxylic acid dianhydrides and aliphatic tetracarboxylic acid dianhydrides.

[0044] In some non-limiting embodiments, the aromatic tetracarboxylic dianhydride is 4,4'-(hexafluoro-isopropylidene)diphthalic anhydride (6FDA); 4,4'-oxydiphthalic dianhydride (ODPA); pyromellitic dianhydride (PMDA); 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA); 2,3,3',4'-biphenyltetracarboxylic dianhydride (s-BDA); asymmetric 2,3,3',4'-biphenyl-tetracarboxylic dianhydride (a-BPDA); 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA); 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA); 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride. 3,3',4,4'-Bicyclohexyltetracarboxylic dianhydride;Hexahydro-4,8-methano-1H,3H-benzo[1,2-c]furan-1,3-dione;Decahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-c]furan-1,3-dione;Hexahydro-4,9-methano-3H-furo[3,4-g][2]benzopyran-1,3,5,7(3aH)-tetrone;3,3',4,4'-Bicyclohexyltetracarboxylic dianhydride;Hexahydro-4,8-methano-1H,3H-benzo[1,2-c hexahydro-1H,3H-benzo[1,2-c:4,5-c']difuran-1,3,5,7-tetrone; hexahydro-1H,3H-benzo[1,2-c:4,5-c']difuran-1,3,5,7-tetrone; 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA); ethylene glycol bis(trimellitic anhydride) ester; 4,4'-bisphenol A dianhydride (BPADA); and the like.

[0045] In some non-limiting embodiments, the aromatic tetracarboxylic dianhydride is selected from the group consisting of alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N-alkyl; (R')(R")N-alkoxyalkyl; (R')(R")N-alkylaryloxyalkyl; -S(O) S -aryl; and -S(O) S -heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" are the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0046] The amount of the aromatic tetracarboxylic dianhydride can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0047] In some non-limiting embodiments, the aliphatic tetracarboxylic dianhydride is cyclobutane dianhydride (CBDA); 3-(carboxymethyl)-1,2,4-cyclopentane tricarboxylic 1,4:2,3-dianhydride; bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride; 1,2,3,4-cyclopentane tetracarboxylic dianhydride; 1,2,4,5-cyclohexane-tetracarboxylic dianhydride; 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride; 1,3-dimethyl-1,2,3,4-cyclobutane-tetracarboxylic dianhydride; tricyclo[6.4.0.0 2,7 ]dodecane-1,8:2,7-tetracarboxylic dianhydride; meso-butane-1,2,3,4-tetracarboxylic dianhydride; 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydrophthalene-1,2-dicarboxylic anhydride; 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, and the like.

[0048] In some non-limiting embodiments, the aliphatic tetracarboxylic dianhydride is selected from the group consisting of alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N -alkyl; (R')(R")N-alkoxyalkyl; (R')(R")N-alkylaryloxyalkyl; -S(O)S-aryl; and -S(O)S-heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" are the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0049] The amount of the aliphatic tetracarboxylic dianhydride can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0050] In some embodiments, the ratio of aromatic tetracarboxylic dianhydride to aliphatic tetracarboxylic dianhydride can be 100 / 1, 90 / 1, 80 / 1, 70 / 1, 60 / 1, 50 / 1, 40 / 1, 30 / 1, 20 / 1, 10 / 1, 9 / 1, 8 / 1, 7 / 1, 6 / 1, 5 / 1, 4 / 1, 3 / 1, 2 / 1, 1 / 1, 1 / 2, 1 / 3, 1 / 4, 1 / 5, 1 / 6, 1 / 7, 1 / 8, 1 / 9, 1 / 10, 1 / 20, 1 / 30, 1 / 40, 1 / 50, 1 / 60, 1 / 70, 1 / 80, 1 / 90, or 1 / 100.

[0051] The one or more diamine component residues are not particularly limited and are derived from the corresponding diamines selected from the group consisting of aromatic diamines and aliphatic diamines.

[0052] In some non-limiting embodiments, the aromatic diamine is p-phenylenediamine (PPD); 2,2'-bis(trifluoromethyl)benzidine (TFMB); m-phenylenediamine (MPD); 4,4'-oxydianiline (4,4'-ODA), 3,4'-oxydianiline (3,4'-ODA); 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (BAHFP); 2,2-bis(4-aminophenoxy)hexafluoropropane (HFBAPP); 1,3-bis(3-aminophenoxy)hexafluoropropane (HFBAPP); 2,2-Bis[4-(4-aminophenoxy)phenyl]sulfone (m-BAPS);2,2-Bis[4-(4-aminophenoxy)phenyl]sulfone (p-BAPS);m-Xylylenediamine (m-XDA);2,2-Bis(3-amino-4-methylphenyl)hexafluoropropane (BAMF);9,9'-Bis(4-aminophenoxy)benzene (m-BAPB);4,4'-Bis(4-aminophenoxy)biphenyl (p-BAPB);2,2-Bis(3-aminophenyl)hexafluoropropane (BAPF);Bis[4-(3-aminophenoxy)phenyl]sulfone (m-BAPS);2,2-Bis[4-(4-aminophenoxy)phenyl]sulfone (p-BAPS);m-Xylylenediamine (m-XDA);2,2-Bis(3-amino-4-methylphenyl)hexafluoropropane (BAMF);9,9'-Bis(4-aminophenoxy) fluorene (FDA), 4,4'-(3,3,3',3'-tetramethyl-2,2',3,3'-tetrahydro-1,1'-spirobi[indene]-6,6'-diyl)dianiline, 3,3'-(3,3,3',3'-tetramethyl-2,2',3,3'-tetrahydro-1,1'-spirobi[indene]-6,6'-diyl)dianiline, 3,3'-(3,3,3',3'-tetramethyl-2,2',3,3'-tetrahydro-1,1'-spirobi[indene]-6,6'-diyl)dianiline, hexamethylenediamine amine (HMD), 1,4-cyclohexane-diamine (CHDA), 3,3',5,5'-tetramethyl-4,4'-diaminophenylmethane, 1,3-bis(4-aminophenoxy)benzene; 1,3'-bis(3-aminophenoxy)benzene (APB-133); 4,4'-methylenebis(2-ethyl-6-methylaniline) (MEMA), m-tolidine (2,2'-dimethylbenzidine), 3-(4-aminophenyl)-1,1,3-trimethyl-5-indanamine (TMDA), and the like.

[0053] In some non-limiting embodiments, the aromatic diamine is selected from the group consisting of alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N-alkyl. and -S(O)S-heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" may be the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0054] The amount of aromatic diamine can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0055] In some non-limiting embodiments, the aliphatic diamine is selected from the group consisting of 1,3-bis(aminoethyl)cyclohexane (m-CHDA); 1,4-bis(aminomethyl)cyclohexane (p-CHDA); 1,3-cyclohexanediamine; (8,8'-(4-hexyl-3-octylcyclohexane-1,2-diyl)bis(octan-1-amine); trans-1,4-diaminocyclohexane; 4,4'-methylenebi(cyclohexylamine); bis(aminomethyl)norbornane; α-,ω-diaminoalkanes (e.g., 1,6-hexanediamine; 1,8-octanediamine; 1,12-dodecanediamine); and the like.

[0056] In some non-limiting embodiments, the aliphatic diamine is selected from the group consisting of alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N-alkyl; (R')(R")N-alkoxyalkyl; (R')(R")N-alkylaryloxyalkyl; -S(O) S -aryl; and -S(O) S -heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" are the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0057] The amount of the aliphatic diamine can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0058] In some embodiments, the ratio of aromatic diamine to aliphatic diamine can be 100 / 1, 90 / 1, 80 / 1, 70 / 1, 60 / 1, 50 / 1, 40 / 1, 30 / 1, 20 / 1, 10 / 1, 9 / 1, 8 / 1, 7 / 1, 6 / 1, 5 / 1, 4 / 1, 3 / 1, 2 / 1, 1 / 1, 1 / 2, 1 / 3, 1 / 4, 1 / 5, 1 / 6, 1 / 7, 1 / 8, 1 / 9, 1 / 10, 1 / 20, 1 / 30, 1 / 40, 1 / 50, 1 / 60, 1 / 70, 1 / 80, 1 / 90, or 1 / 100.

[0059] The one or more end-capping compounds containing one or more crosslinking groups are not particularly limited and may be selected from the group consisting of aliphatic end-capping compounds, aromatic end-capping compounds, heteroaromatic end-capping compounds, alkynyl end-capping compounds, alkenyl end-capping compounds, maleimide end-capping compounds, vinyl end-capping compounds, allyl end-capping compounds, cyanate ester end-capping compounds, ester end-capping compounds, and the like.

[0060] In some non-limiting embodiments, the crosslinking groups of the endcapping compound are selected from the group consisting of radical crosslinking groups, cationic crosslinking groups, anionic crosslinking groups, crosslinking groups that can crosslink with themselves to form homopolymers, crosslinking groups that can crosslink with other crosslinking groups to form heteropolymers, and combinations thereof.

[0061] In some non-limiting embodiments, the crosslinking group of the endcapping compound is any group capable of forming a carbon-carbon or carbon-heteroatom bond and is selected from the group consisting of allyl groups, vinyl groups, alkynyl groups, alkenyl groups, (meth)acrylate groups, benzocyclobutene groups, maleimide groups, allyl-based groups, cyanate ester groups, and ester groups.

[0062] In some non-limiting embodiments, the one or more end-capping compounds comprising one or more crosslinking groups are selected from the group consisting of 4-ethynylaniline (4-EA), 2,4-diamino-6-diallylamino-1,3,5-triazine (DAMA), 4-aminostyrene (4AS), 4-ethynylphthalic anhydride, 4-phenylethynylphthalic anhydride, 5-(3-phenylpropioloyl)-1,3-isobenzofurandione, 4-methylethynylphthalic anhydride, 5-(1-oxo-3-phenyl-2-propyn-1-yl)-1,3-isobenzofurandione, 5-(1-oxo-3-phenyl-2-propyn-1-yl)-1,3-isobenzofurandione (PETA), and the like.

[0063] In some non-limiting embodiments, the soluble polyimide resins disclosed herein include residues of a single type of tetracarboxylic acid moiety. In some non-limiting embodiments, the soluble polyimide resins disclosed herein include two tetracarboxylic acid component residues, each of which is present at a mole percent between 0.1% and 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include three tetracarboxylic acid component residues, each of which is present at a mole percent between 0.1% and 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include four tetracarboxylic acid component residues, each of which is present at a mole percent between 0.1% and 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include five tetracarboxylic acid component residues, each of which is present at a mole percent between 0.1% and 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include six or more tetracarboxylic acid component residues, each of which is present at a mole percent between 0.1% and 99.9%.

[0064] In some non-limiting embodiments, the soluble polyimide resins disclosed herein include residues of a single diamine component. In some non-limiting embodiments, the soluble polyimide resins disclosed herein include two diamine component residues, each diamine component residue being present at a mole percent of 0.1% to 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include three diamine component residues, each diamine component residue being present at a mole percent of between 0.1% to 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include four diamine component residues, each diamine component residue being present at a mole percent of between 0.1% to 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include five diamine component residues, each diamine component residue being present at a mole percent of between 0.1% to 99.9%; in some non-limiting embodiments, the soluble polyimide resins disclosed herein include six or more diamine component residues, each diamine component residue being present at a mole percent of between 0.1% to 99.9%.

[0065] In some non-limiting embodiments, the soluble polyimide resins disclosed herein include a single type of end-capping compound; in some non-limiting embodiments, the soluble polyimide resins include two types of end-capping compounds; in some non-limiting embodiments, the soluble polyimide resins include three types of end-capping compounds; and in some non-limiting embodiments, the soluble polyimide resins include four or more types of end-capping compounds.

[0066] The amount of one or more endcapping compounds used in the soluble polyimide resins and / or related formulations disclosed herein will vary depending on the property targets of interest (e.g., thermal properties, mechanical properties, dielectric properties, etc.) The amount of one or more endcapping compounds used in the soluble polyimide resins and / or related formulations disclosed herein can range from 0.1-70 mol%, 1-65 mol%, 2-60 mol%, 5-55 mol%, 10-50 mol%, 15-45 mol%, 20-40 mol%, or 25-30 mol%. The amount of one or more endcapping compounds used in the soluble polyimide resins and / or related formulations disclosed herein can range from 2-10 mol%, 3-9 mol%, 4-8 mol%, 5-7 mol%, 2-6 mol%, 2-5 mol%, 2-4 mol%, 2-3 mol%, 3-6 mol%, 3-5 mol%, 3-4 mol%, 4-6 mol%, or 4-5 mol%.

[0067] Further provided is a soluble polyimide resin comprising: (a) one or more tetracarboxylic acid component residues; (b) one or more diamine component residues; and (c) one or more end-capping compounds; and further comprising one or more residues selected from the group consisting of: (d) one or more triamine component residues; (e) one or more tetraamine component residues; (f) one or more hexacarboxylic trianhydride component residues; and (g) one or more dicarboxylic acid monoanhydride component residues or dicarboxylic acid component residues, wherein the one or more end-capping compounds contain one or more crosslinking groups.

[0068] Specific embodiments of (a) one or more tetracarboxylic acid component residues; (b) one or more diamine component residues; and (c) one or more endcapping compounds, which contain one or more crosslinking groups for these soluble polyimide resins, are the same as those disclosed hereinabove.

[0069] The one or more triamine moiety residues are not particularly limited and are derived from the corresponding triamine selected from the group consisting of aromatic triamines and aliphatic triamines.

[0070] In some non-limiting embodiments, the one or more triamines are diethylenetriamine, 4,4',4"-methanetriyltrianiline, 5'-(4-aminophenyl)-[1,1':3',1"-terphenyl]-4,4"-diamine, 4,4',4"-(1,3,5-triazine-2,4,6-triyl)trianiline, N 1 ,N 1 -bis(4-aminophenyl)benzene-1,4-diamine, N1,N1-bis(3-aminophenyl)benzene-1,3-diamine, 4'-(3-aminophenyl)-[1,1':2',1"-terphenyl]-3,3"-diamine, 5'-(3-aminophenyl)-[1,1':3',1"-terphenyl]-3,3"-diamine and 5'-(4-aminophenyl)-[1,1':3',1"-terphenyl]-3,3"-diamine.

[0071] In some non-limiting embodiments, the triamine may be further substituted with a functional group selected from the group consisting of alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N-alkyl; (R')(R")N-alkoxyalkyl; (R')(R")N-alkylaryloxyalkyl; -S(O)S-aryl; and -S(O)S-heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" are the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl, or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0072] The amount of the triamine component residue can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0073] The one or more tetraamine moiety residues are not particularly limited and are derived from the corresponding tetraamine selected from the group consisting of aromatic tetraamines and aliphatic tetraamines.

[0074] In some non-limiting embodiments, the one or more tetraamines are selected from the group consisting of tetraaminoethylene, [1,1':3',1"-terphenyl]-3,3",5,5"-tetraamine, [1,1':4',1"-terphenyl]-3,3",5,5"-tetraamine, 5,5'-(1,3,5-triazine-2,4-diyl)bis(benzene-1,3-diamine), 5,5'-(9-methyl-9H-carbazole-3,6-diyl)bis(benzene-1,3-diamine), and 5,5'-(9H-carbazole-3,9-diyl)bis(benzene-1,3-diamine).

[0075] In some non-limiting embodiments, the tetraamine may be further substituted with functional groups selected from the group consisting of alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N-alkyl; (R')(R")N-alkoxyalkyl; (R')(R")N-alkylaryloxyalkyl; -S(O)S-aryl; and -S(O)S-heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" are the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl, or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0076] The amount of the tetraamine component residue can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0077] The one or more hexacarboxylic acid trianhydride moiety residues are not particularly limited and are derived from the corresponding tricarboxylic acid selected from the group consisting of aromatic hexacarboxylic acid trianhydrides and aliphatic hexacarboxylic acid trianhydrides.

[0078] In some non-limiting embodiments, the one or more hexacarboxylic acid trianhydrides are selected from the group consisting of 5,5',5"-nitrilotris(isobenzofuran-1,3-dione) and 5,5',5"-(benzene-1,3,5-triyl)tris(isobenzofuran-1,3-dione).

[0079] In some non-limiting embodiments, the hexacarboxylic acid trianhydride is selected from the group consisting of alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N-alkyl; (R')(R")N-alkoxyalkyl; (R')(R")N-alkylaryloxyalkyl; -S(O) S -aryl; and -S(O) S -heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" are the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0080] The amount of the hexacarboxylic acid trianhydride component residue can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0081] The one or more dicarboxylic acid monoanhydride moiety residues are not particularly limited and are derived from the corresponding dicarboxylic acid selected from the group consisting of aromatic dicarboxylic acids and aliphatic dicarboxylic acids.

[0082] In some non-limiting embodiments, the one or more dicarboxylic acid monoanhydrides are selected from the group consisting of 5-ethenyl-1,3-isobenzofuran dione, 5-ethynylisobenzofuran-1,3-dione, 5-allylisobenzofuran-1,3-dione, 5-(vinyloxy)isobenzofuran-1,3-dione, and 5-(ethynyloxy)isobenzofuran-1,3-dione.

[0083] In some non-limiting embodiments, the dicarboxylic acid monoanhydride is alkyl; aryl; nitro; cyano; -N(R')(R"); halo; hydroxy; carboxy; alkenyl; alkynyl; cycloalkyl; heteroaryl; alkoxy; aryloxy; heteroaryloxy; alkoxycarbonyl; perfluoroalkyl; perfluoroalkoxy; arylalkyl; silyl; siloxy; siloxane; thioalkoxy; -S(O)2-; -C(=O)-N(R')(R"); (R')(R")N-alkyl; (R')(R")N-alkoxyalkyl; (R')(R")N-alkylaryloxyalkyl; -S(O) S -aryl; and -S(O) S -heteroaryl; and other groups capable of forming new C-C or C-heteroatom bonds during curing; R' and R" are the same or different at each occurrence and are optionally substituted with alkyl, cycloalkyl or aryl groups; 0 < S < 2; and the functional group optionally comprises a crosslinking group.

[0084] The amount of dicarboxylic acid monoanhydride component residues can be in the range of 1 to 99 mol%, 5 to 95 mol%, 10 to 90 mol%, 15 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, 35 to 65 mol%, 40 to 60 mol%, 45 to 55 mol%, 1 to 10 mol%, 10 to 20 mol%, 20 to 30 mol%, 30 to 40 mol%, 40 to 50 mol%, 50 to 60 mol%, 60 to 70 mol%, 70 to 80 mol%, 80 to 90 mol%, or 90 to 99 mol%.

[0085] Non-limiting examples of soluble PI resins disclosed herein include: ODPA / / TFMB / APB-133 / 4AS 100 / / 49 / 49 / 4; ODPA / / TFMB / APB-133 / DAMA / 4AS 100 / / 46.5 / 46.5 / 5 / 4; BPADA / / APB-133 / TFMB / 4AS 100 / / 42.5 / 42.5 / 30; BPADA / / APB-133 / TFMB / 4AS 100 / / 45 / 45 / 20; ODPA / 6FDA / / TFMB / Priamine TM 1075 / 4-AS 85 / 15 / / 91 / 05 / 08; ODPA / / APB-133 / TFMB / DAMA / 4-EA 100 / / 46.5 / 46.5 / 05 / 04; ODPA / / APB-133 / TFMB / M1309 / 4-AS 100 / / 46 / 46 / 04 / 08; BPADA / / APB-133 / 4-AS 100 / / 85 / 30; and BPADA / APB133 / TFMB / 1-(4-aminophenyl)-1H-pyrrole-2,5-dione) 100 / 42.5 / 42.5 / 30 ODPA / 4-EPA / / APB-133 / MEMA 98 / 2 / / 50 / 50 BPDA / 4-EPA / / APB-133 / MEMA 85 / 30 / / 50 / 50 BPADA / / APB-133 / m-Tolidine / 4AS 100 / / 42.5 / 42.5 / 30 BPADA / PETA / / APB-133 / TFMB 85 / 30 / / 50 / 50 BPADA / ODPA / / m-Tolidine / FDA / Priamine TM 1075 / 4AS 90 / 10 / / 77 / 10 / 05 / 16 BPADA / 4-EPA / / TMDA / m-Tolidine 98 / 04 / / 50 / 50.

[0086] Solutions containing the soluble polyimide resins disclosed herein can be prepared using a variety of available methods regarding how the components (i.e., monomers and solvents) are introduced. Some variations in producing solutions of soluble polyimide resins include the following: (1) The diamine component and the dianhydride component are premixed together and then this mixture is added in small portions to the solvent with stirring. (2) A method in which a solvent is added to a mixture of a diamine component and a dianhydride component while stirring (opposite to (a) above). (3) A method in which only the diamine is dissolved in a solvent, and then the dianhydride is added thereto in such a ratio that the reaction rate can be controlled. (4) A method in which only the dianhydride component is dissolved in a solvent, and then the amine component is added thereto in such a ratio that the reaction rate can be controlled. (5) A method in which the diamine component and the dianhydride component are dissolved in a solvent separately, and then these solutions are mixed in a reactor. (6) A method in which a polyamic acid containing an excess of an amine component and another polyamic acid containing an excess of a dianhydride component are preformed and then reacted with each other in a reactor in a manner that particularly produces nonrandom or block copolymers. (7) A method in which a specific portion of the amine component and the dianhydride component are reacted first and then the remaining diamine component is reacted, or vice versa. (8) A process in which some or all of the ingredients are added to either some or all of the solvent in any order, and some or all of any ingredient may be added as a solution in some or all of the solvent. (9) A method in which one of the dianhydride components is reacted with one of the diamine components to obtain a first polyamic acid, the other dianhydride component is then reacted with the other amine component to obtain a second polyamic acid, and the amic acids are then combined by any one of several methods prior to forming a membrane.

[0087] Generally, the solution containing the soluble polyimide resin can be obtained from any one of the preparation methods disclosed above or other similar methods as practiced by one skilled in the art.

[0088] The specific solvent or solvents used are generally not limited and can be selected by those skilled in the art.High boiling polar aprotic solvents are often preferred.Non-limiting examples of this type of solvent include N-methyl-2-pyrrolidone (NMP), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), dimethylformamide (DMF), butyrolactone, dibutylcarbitol, butylcarbitol acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and the like, and combinations thereof.

[0089] Non-limiting examples of methods for preparing soluble polyimide resins include, in order, performing the following steps: (a) dissolving one or more diamines in a high boiling polar aprotic solvent; (b) adding one or more endcapping compounds to the solution prepared in (a); (c) adding one or more dianhydrides to the solution prepared in (b); (d) stirring the solution prepared in (c) for a first predetermined period of time; (e) heating the solution prepared in (d) to a first predetermined temperature and, optionally, adding a solution of one or more imidization catalysts; (f) heating the solution prepared in (e) to a second predetermined temperature and stirring for a second predetermined period of time; and (g) cooling the solution prepared in (f) and isolating the solid polyimide resin.

[0090] In some non-limiting embodiments of the methods disclosed herein, one or more additional solutions are added stepwise to the solution prepared in step (c) above. In some non-limiting embodiments, the additional solutions have 10 mol % or less of the one or more dianhydrides, in some non-limiting embodiments, 5 mol % or less of the one or more dianhydrides, and in some non-limiting embodiments, 2.5 mol % or less of the one or more dianhydrides.

[0091] In some non-limiting embodiments of the methods disclosed herein, the one or more imidization catalysts used in step (e) are selected from the group consisting of aliphatic acid anhydrides, acid anhydrides, alcohol / acid cocatalysts, aliphatic tertiary amines, aromatic tertiary amines, and heterocyclic tertiary amines.

[0092] In some non-limiting embodiments disclosed herein, a thermal conversion process may be used that may or may not utilize a conversion agent (i.e., catalyst) to convert the polyamic acid cast liquid to a polyimide. If a conversion agent is used, the process is considered a modified thermal conversion process. In both types of thermal conversion processes, only thermal energy is used to heat the film to both dry the solvent in the film and to carry out the imidization reaction. In general, thermal conversion processes with or without a conversion catalyst are used to make the polyimide films disclosed herein.

[0093] Since it is not only the composition of the film that imparts the desired properties, the specific parameters of the method are preselected. Rather, the cure temperature and the temperature ramp profile also play an important role in achieving the most desirable properties for the intended use disclosed herein. The temperature at which the polyamic acid is imidized should be at or above the highest temperature of any subsequent processing steps (e.g., deposition of inorganic or other layers required for the manufacture of functional displays), but below the temperature at which significant decomposition / discoloration of the polyamide occurs. It should also be noted that an inert atmosphere is generally preferred, especially when using high processing temperatures for imidization.

[0094] To obtain the polyamic acid / polyimide disclosed herein, temperatures between 300°C and 400°C are typically used, although subsequent processing temperatures above 300°C are required. By selecting the correct cure temperature, it is possible to obtain a fully cured polyimide that achieves the best balance between thermal and mechanical temperature properties. Because this temperature is so high, an inert atmosphere is required. Typically, the oxygen concentration in the oven should be less than 100 ppm. The very low oxygen concentration allows the highest cure temperatures to be used without significant degradation / discoloration of the polymer. Catalysts that accelerate the imidization process are effective in achieving higher levels of imidization at cure temperatures of about 200°C to 300°C. This approach limits the upper cure temperature to the T of the polyimide. g This can optionally be used when fabricating flexible devices with a lower

[0095] The length of time for each of the possible curing steps is also an important process consideration. In general, the time used when curing at the maximum temperature should be kept to a minimum. For example, when curing at 320°C, the cure time in an inert atmosphere can be up to about 1 hour, but if the cure temperature is higher, this time should be reduced to avoid thermal degradation. Generally speaking, higher temperatures require shorter times. Those skilled in the art will know the balance of temperature and time to optimize the properties of the polyimide for a particular end use.

[0096] In certain embodiments, the soluble polyimide resin can be prepared by introducing nitrogen gas to provide an inert atmosphere into a three-necked reaction vessel equipped with a PTFE stirring shaft, O-rings, and bearing assembly. For most diamines, the desired amino compound can be dissolved in DMAc at room temperature. In certain embodiments, the DMAC can be warmed to an appropriate temperature to dissolve all of the added diamine. While stirring the solution of diamine, the desired dianhydride monomer can be added to the reaction mixture in small increments such that the internal temperature does not exceed the desired temperature. The reaction mixture can then be stirred until the viscosity of the resulting polyamic acid solution is in the desired range.

[0097] Acetic anhydride and β-picoline can then be added to the polyamic acid solution. The reaction mixture can be heated to 80° C. and maintained at this temperature for about 3 hours to maintain the reaction, followed by stirring overnight. The resulting polyimide can then be isolated as a powder by precipitation with water and / or additional precipitation co-solvents, e.g., methanol, acetone. The polymer can be washed with methanol and dried. The polyimide can be isolated as a white powder and characterized by GPC and NMR spectroscopy. Specific embodiments and variations thereof are illustrated in the examples.

[0098] The soluble polyimide resins prepared as disclosed herein generally have several mechanical, electronic and thermal properties that make them well suited for use in the electronic applications disclosed herein. In some non-limiting embodiments, the soluble polyimide resins have: (a) Mn less than 80,000; (b) Mw less than 150,000; (c) loss tangent less than 0.007; and (d) a coefficient of thermal expansion less than 50 ppm / K.

[0099] In some non-limiting embodiments, the Mn of the soluble PI resins disclosed herein is less than 70,000, in some non-limiting embodiments less than 60,000, in some non-limiting embodiments less than 50,000, in some non-limiting embodiments less than 40,000, in some non-limiting embodiments less than 30,000, in some non-limiting embodiments less than 20,000, and in some non-limiting embodiments less than 10,000.

[0100] In some non-limiting embodiments, the Mw of the soluble PI resins disclosed herein is less than 140,000, in some non-limiting embodiments, less than 1300,000, in some non-limiting embodiments, less than 120,000, in some non-limiting embodiments, less than 110,000, in some non-limiting embodiments, less than 100,000, in some non-limiting embodiments, less than 90,000, in some non-limiting embodiments, less than 80,000, in some non-limiting embodiments, less than 70,000, in some non-limiting embodiments, less than 60,000, in some non-limiting embodiments, less than 50,000, in some non-limiting embodiments, less than 40,000, in some non-limiting embodiments, less than 30,000, in some non-limiting embodiments, less than 20,000, and in some non-limiting embodiments, less than 10,000.

[0101] In some non-limiting embodiments, the loss tangent (D f ) is less than 0.006, in some non-limiting embodiments less than 0.005, in some non-limiting embodiments less than 0.004, in some non-limiting embodiments less than 0.003, in some non-limiting embodiments less than 0.002, and in some non-limiting embodiments less than 0.001.

[0102] In some non-limiting embodiments, the coefficient of thermal expansion (CTE) of the soluble PI resins disclosed herein is less than 40 ppm / K, in some non-limiting embodiments, less than 30 ppm / K, in some non-limiting embodiments, less than 20 ppm / K, and in some non-limiting embodiments, less than 10 ppm / K.

[0103] Further provided is a liquid composition comprising two or more of the following: (a) 15-90 wt % of one or more soluble polyimide resins; (b) 5-75 wt % of one or more crosslinking compounds; (c) 0-5 wt % of one or more photoinitiators or thermal radical initiators; (d) 0-5 wt % of one or more oxidation catalysts; and (e) 0-65 wt % of one or more solvents.

[0104] Specific embodiments of the one or more soluble polyimide resins are the same as those disclosed hereinabove.

[0105] Any suitable crosslinking compound ("crosslinker") can be used in the liquid composition of the present invention. Suitable crosslinkers are those that can react with the functional groups in the resin composition, such as alkenes, free radical curing mechanisms, functional groups that undergo Michael reactions, and Diels-Alder dienes, as selected by one skilled in the art. Such suitable crosslinkers can include polyfunctional thiols, polyfunctional azides, polyfunctional aziridines, and bisarylcyclobutene monomers, as well as (meth)acrylates, di(meth)acrylates, maleimides, bismaleimides, polyfunctional maleimides, allyl compounds, diallyl compounds, vinylsilane compounds, divinyl compounds, cyanate esters, and polyfunctional dienophiles such as di-, tri-, and polyfunctional amines, or other suitable dienophiles that crosslink with the polymers of the present disclosure under the conditions used to cure the composition. The selection of such crosslinkers is within the capabilities of one skilled in the art.

[0106] In some non-limiting embodiments, the one or more crosslinkers are selected from the group consisting of multifunctional thiols, multifunctional azides, multifunctional aziridines, bisarylcyclobutenes, (meth)acrylates, maleimides, allyl compounds, vinyl or other alkenyl compounds, vinylsilane compounds, dienophiles, and other suitable reaction partners. In some non-limiting embodiments, the one or more crosslinkers are (meth)acrylates. In some non-limiting embodiments, the one or more crosslinkers are maleimides. In some non-limiting embodiments, the maleimides include one or more biphenyl groups or long chain aliphatic groups. In some non-limiting embodiments, the one or more crosslinkers are selected from the group consisting of MIR3000, MIR5000, BMI4000, BMI5100, BMI-TMH, BMI689, SR454, triallyl isocyanurate (TAIC), triallyl cyanurate (TAC), and SPV-100.

[0107] In some non-limiting embodiments, the liquid compositions disclosed herein include 5-75% by weight, in some non-limiting embodiments, 10-60% by weight, in some non-limiting embodiments, 15-50% by weight, in some non-limiting embodiments, 20-40% by weight, and in some non-limiting embodiments, 12-18% by weight of one or more crosslinkers.

[0108] Any suitable photoinitiator or thermal radical initiator can be used as the curing agent of the liquid composition of the present invention. A variety of curing agents can be used in the liquid compositions of the present disclosure useful for photolithography. Suitable curing agents are those that can aid in the curing of polyimide-containing materials and can be activated by heat or light. Exemplary curing agents can include, but are not limited to, thermally generated initiators and photoactive compounds (photogenerated initiators). The selection of such curing agents is within the ability of one of ordinary skill in the art. Preferred thermally generated initiators are free radical initiators such as, but not limited to, azobisisobutyronitrile, dibenzoyl peroxide, and dicumyl peroxide (DCP). In some non-limiting embodiments, the photoinitiator is selected from the group consisting of acylphosphine oxides, alpha-aminoalkylphenones, alpha-dialkyloxyacetophenones, and oxime esters. Preferred photoactive curing agents are free radical photoinitiators available from BASF under the Irgacure brand and diazonaphthoquinone (DNQ) compounds, including sulfonate esters of DNQ compounds. Suitable DNQ compounds are any compounds having a DNQ moiety, such as a DNQ sulfonate moiety, and any compounds that function as photoactive compounds in the present compositions, i.e., they function as dissolution inhibitors when exposed to appropriate radiation. Suitable DNQ compounds are disclosed in U.S. Patent No. 5,399,623 and U.S. Patent No. 5,399,623, the entire contents of which are incorporated herein by reference.

[0109] The amount of photoinitiator or thermal initiator varies between 0-30% by weight, based on the total weight of polymer solids. When a photoactive compound is present, it is typically used in an amount of 5-30% by weight, or 5-25% by weight, or 10-25% by weight, based on the total weight of polymer solids.

[0110] Any suitable oxidation catalyst can be used in the liquid compositions of the present invention. In some non-limiting embodiments, the one or more oxidation catalysts are selected from the group consisting of TEMPO, 4-hydroxy-TEMPO, 4-amino-TEMPO, alkylated hydroquinones, alkylated hydroxytoluenes, alkylated hydroxyanisoles, and others that would be known to one of skill in the art.

[0111] The amount of oxidation catalyst varies between 0-30% by weight, based on the total weight of polymer solids. When present, the oxidation catalyst is typically used in an amount of 5-30% by weight, or 5-25% by weight, or 10-25% by weight, based on the total weight of polymer solids.

[0112] Any suitable solvent can be used in the liquid composition of the present invention as long as the components of the composition are soluble or dispersible therein.Non-limiting examples of one or more solvents include cyclopentanone, cyclohexanone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, gamma-butyrolactone, 3-methoxypropionate, dipropylene glycol dimethyl ether, 3-methoxybutyl acetate, anisole, mesitylene, 2-heptanone, silane, 2-butanone, ethyl lactate, amyl acetate, n-butyl acetate, n-methyl-2-pyrrolidone, N-butyl-2-pyrrolidone, 2-butanone, toluene, acetone, methyl ethyl ketone, etc., and combinations thereof.

[0113] The solvent may be present in an amount of 10-90% by weight, or 20-80% by weight, or 30-70% by weight, or 40-60% by weight, based on the total weight of the components of the liquid composition.

[0114] Further provided is a liquid composition as described herein above, further comprising one or more of the following: (f) one or more additional resins in an amount from 10 to 60% by weight; (g) one or more surface levelling agents in an amount from 0 to 10% by weight; (h) one or more organic or inorganic fillers in an amount from 0 to 70% by weight and (i) one or more adhesion promoters in an amount from 0 to 25% by weight.

[0115] Specific embodiments of (a) 15-90 wt. % of one or more soluble polyimide resins; (b) 5-75 wt. % of one or more crosslinking compounds; (c) 0-5 wt. % of one or more photoinitiators or thermal radical initiators; (d) 0-5 wt. % of one or more oxidation catalysts; and (e) 0-65 wt. % of one or more solvents are the same as those disclosed herein above.

[0116] The use of additional resins in the compositions disclosed herein can provide materials with optimal properties for targeted electronic formulations. Non-limiting examples of additional resins include MIR-3000, NC-3000, epoxy resins, novolac resins, and others that would be known to one skilled in the art. When present, the additional resin can be present in an amount of 0.5-60% by weight, or 1-40% by weight, or 5-30% by weight, or 10-20% by weight.

[0117] Any suitable surface leveling agent or "leveling agent" may be used in the liquid compositions of the present disclosure, the selection of which is well within the ability of one of ordinary skill in the art. The majority of leveling agents are monomers such as: Si(R 1 )(R 2 )(OR 3 )2(wherein, R 1 , R 2 or R 3 is C1~C 20 Alkyl or C5~C 20 Aliphatic group or C1-C 20 The leveling agent may include silicone units derived from polymerizing a C3-C6 alkyl group (each independently selected from an aryl group). In one non-limiting embodiment, the leveling agent is non-ionic and may include at least two functional groups capable of chemically reacting with functional groups contained in the silicone and non-silicone resins under cationic photocuring processes or thermal curing conditions. In some non-limiting embodiments, there are leveling agents that include non-reactive groups. In addition to the silicon derived units, the leveling agent may include C3-C6 alkyl groups containing oxirane rings.20 It may also contain units derived from the polymerization of aliphatic molecules. In addition, the leveling agent may contain C1-C hydroxyl groups. 50 It may also include units derived from aliphatic molecules. In some non-limiting embodiments, the leveling agent does not include halogen substituents. In some non-limiting embodiments, the molecular structure of the leveling agent may be predominantly linear, branched, hyperbranched, or grafted.

[0118] In some non-limiting embodiments; the leveling agent is AD1700, MD700; Megaface F-114, F-251, F-253, F-281, F-410, F-430, F-477, F-510, F-551, F-552, F- 553, F-554, F-555, F-556, F-557, F-558, F-559, F-560, F-561, F-562, F-56 3, F-565, F-568, F-569, F-570, F-574, F-575, F-576, R-40, R-40-LM, R-41, R-94, RS-56, RS-72-K, RS-75, RS-76-E, RS-76-NS, RS-78, RS-90, DS-21 (DIC Sun Chemical);KY-164, KY-108, KY-1200, KY-1203 (Shin-Etsu Chemical Co., Ltd.);Dowsil 14, Dowsil 11, Dowsil 54, Dowsil 57, Dowsil FZ2110, FZ-2123;Xiameter OFX-0077;ECOSURF EH-3, EH-6, EH-9, EH-14, SA-4, SA-7, SA-9, SA-15; Tergitol 15-S-3, 15-S-5, 15-S-7, 15-S-9, 15-S-12, 15-S-15, 15-S-20, 15-S-30, 15-S-40, L61, L-62, L-64, L-81, L-101, XD, XDLW, XH, XJ, TMN-3, TMN-6, TMN-10, TMN-100X, NP-4, NP-6, NP-7, NP-8, NP-9, NP-9.5, NP-10, NP-11, NP-12, NP-13, NP-15, NP-30, NP-40, NP-50, NP-70; Triton CF-10, CF-21, CF-32, CF76, CF87, DF-12, DF-16, DF-20, GR-7M, BG-10, CG-50, CG-110, CG-425, CG-600, CG-650, CA, N-57, X-207, HW 1000, RW-20, RW-50, RW-150, X-15, X-35, X-45, X-114, X-100, X-102, X-165, X-305, X -405,X-705;PT250,PT700,PT3000,P425,P1000TB,P1200,P2000,P4000,15-200(Dow Chemical);DC ADDITIVE 3, 7, 11, 14, 28, 29, 54, 56, 57, 62, 65, 67, 71, 74, 76, 163(Dow Silicones);TEGO Flow 425, Flow 370, Glide 100, Glide 410, Glide 415, Glide 435, Glide 432, Glide 440, Glide 450, Flow 425, Wet 270, Wet 500, Rad 2010, Rad 2200N, Rad 2011, Rad 2250, Rad 2500, Rad 2700, Dispers 670, Dispers 653, Dispers 656, Airex 962, Airex 990, Airex 936, Airex 910(Evonik); BYK-300, BYK-301 / 302, BYK-306, BYK-307, BYK-310, BYK-315, BYK-31 3, BYK-320, BYK-322, BYK-323, BYK-325, BYK-330, BYK-331, BYK-333, BYK-337, BYK-3 41, BYK-342, BYK-344, BYK-345 / 346, BYK-347, BYK-348, BYK-349, BYK-370, BYK-375 , BYK-377, BYK-378, BYK-UV3500, BYK-UV3510, BYK-UV3570, BYK-3550, BYK-SILCLEAN 3700, Modaflow® 9200, Modaflow® 2100, Modaflow® Lambda, Modaflow® Epsilon, Modaflow® Resin, Efka FL, Additiol XL 480, Additol XW 6580 and BYK-SILCLEAN 3720;

[0119] In some non-limiting embodiments, the leveling agent can be present in an amount of 0-10% by weight, or 0-5% by weight, or 0-1% by weight, or 0.001-0.9% by weight, or 0.05-0.5% by weight, or 0.05-0.25% by weight, or 0.05-0.2% by weight, or 0.1-0.15% by weight.

[0120] In some non-limiting embodiments of the liquid composition disclosed herein, at least one or two inorganic particulate fillers are selected from the group consisting of inorganic fillers with a dielectric constant less than 5 and a dielectric loss (GHz band) less than 0.002. Any particulate filler having the above characteristics is generally useful, as long as it has an average diameter less than about 2 μm or an absolute diameter less than about 8 μm and has good insulating and / or good dielectric properties. In some non-limiting embodiments, the average particle size of the inorganic particulate filler is preferably less than or equal to 10 percent of the thickness of the layer of the dielectric composite in the final product. In some non-limiting embodiments, the inorganic particulate filler has a dielectric constant less than or equal to 4.0 and a dielectric loss less than 0.001. Non-limiting examples of inorganic particulate fillers include silica, alumina, boron nitride, glass, and quartz.

[0121] In some non-limiting embodiments of the liquid composition disclosed herein, at least one inorganic particulate filler is surface-modified by reacting with one or more silane coupling agents. The selection of the silane coupling agent used to surface-modify the at least one inorganic particulate filler is not particularly limited. In some non-limiting embodiments of the dielectric composite disclosed herein, the one or more acrylic silane coupling agents are represented by the formula:

[0122] [ka]

[0123] wherein R is the same or different at each occurrence and is selected from the group consisting of alkyl, aryl, acetyl, ketoimino, and alkenyl; X is an unsaturated group selected from the group consisting of acryloxy, methacryloxy, allyloxy, vinyl, maleimide, fumarate, maleate, ethynyl, phenylethynyl, phenylamino, phenyl, stilbene, propiolate, and phenylpropiolate; and n is an integer from 0 to 10. In some non-limiting embodiments, the silane coupling agent is acrylic. In some non-limiting embodiments, the silane coupling agent is monomeric, and in some non-limiting embodiments, the silane coupling agent is polymerized through a vinyl group.

[0124] Examples of acrylic silane coupling agents include, but are not limited to, bis(trimethoxysilyl)propyl fumarate, 8-methacryloxyoctyl-trimethoxysilane (KBM-5803), acryloxy and methylmethoxysilane oligomer (KR-513), methacryloxy and methylmethoxysilane oligomer (X-40-9296), mercapto and methylmethoxysilane oligomer (KR-519), mercaptomethoxysilane organic chain oligomer (X-12-1154), and 3-methacryloxypropyltrimethoxysilane (KBM-503), 3-methacryloxypropylmethyldimethoxysilane (KBM-502), 3-methacryloxypropyltriethoxysilane (KBE-503), N-phenyl-3-aminopropyltrimethoxysilane (KBM-573) and phenyltrimethoxysilane (KBM-103).

[0125] In some non-limiting embodiments of the dielectric composite materials disclosed herein, one or more acrylic silane coupling agents are used in combination with one or more polymeric silanes to surface modify the inorganic particulate filler. In some non-limiting embodiments, the one or more polymeric silanes have the formula:

[0126] [ka]

[0127] (In the formula, R 27 is selected from the group consisting of alkyl and H; R 28 is selected from the group consisting of alkyl, aryl, acetyl, ketoimino and alkenyl; R 29 is selected from the group consisting of COOCHCH=CH, CH and H; R 30 is selected from the group consisting of 4-allyloxyphenyl, COOCH2CH═CH2, and any group containing a reactive dienophile; X and Y are the same or different and are selected from the group consisting of methyl and H; m and n are the same or different and are integers from 10 to 1000; o is an integer from 0 to 1000; and p is an integer from 0 to 10.

[0128] In some non-limiting embodiments, the liquid compositions disclosed herein include 0-80% by weight, in some non-limiting embodiments, 20-75% by weight, in some non-limiting embodiments, 40-72% by weight, and in some non-limiting embodiments, 54-68% by weight of one or more inorganic particulate fillers.

[0129] In some non-limiting embodiments, the liquid composition disclosed herein includes one or more organic particulate fillers, which may be rubber particles or the like. The rubber particles are not soluble even in the organic solvent used to prepare the resin composition of the present disclosure, and are not miscible with the components of the resin composition, such as the arylcyclobutene resin. Thus, the rubber particles in the present disclosure are present in a dispersed state in the varnish of the resin composition of the present disclosure. Such rubber particles are usually prepared by increasing the molecular weight of the rubber component to such an extent that they are not soluble in the organic solvent and the resin, and forming them into particles. For example, if a rubber component that is soluble in a solvent and miscible with other components, such as the arylcyclobutene resin, in the resin composition is blended, the roughness after the roughening treatment is significantly increased, and the heat resistance of the product after curing is also reduced.

[0130] Non-limiting examples of the rubber particles of the present invention include core-shell type rubber particles, cross-linked acrylonitrile butadiene rubber particles, cross-linked styrene butadiene rubber particles, and acrylate rubber particles. Core-shell type rubber particles are rubber particles having a core layer and a shell layer, examples of which include a two-layer structure in which the outer shell layer is a glassy polymer and the inner core layer is a rubbery polymer, and a three-layer structure in which the outer shell layer is a glassy polymer, the middle layer is a rubbery polymer, and the core layer is a glassy polymer. The glass layer is composed of, for example, a polymer of methyl methacrylate, while the rubbery polymer is composed of, for example, a polymer of butyl acrylate (butyl rubber). Specific examples of core-shell type rubber particles include Staphyloid AC 3832 and AC 3816 N (trade names of Ganz Chemical Co., Ltd.) and Metablen KW-4426 (trade name of Mitsubishi Rayon Co., Ltd.). Specific examples of acrylonitrile butadiene rubber (NBR) particles include XER-91 (average particle size: 0.5 μm; manufactured by JSR Corporation). Specific examples of styrene butadiene rubber (SBR) particles include XSK-500 (average particle size: 0.5 μm; manufactured by JSR Corporation). Specific examples of acrylate rubber particles include Metablen W300A (average particle size: 0.1 μm) and W450A (average particle size: 0.2 μm) (manufactured by Mitsubishi Rayon Co., Ltd.). Such rubber particles can impart effects such as improving the mechanical strength of the cured product and reducing the stress of the cured product.

[0131] The average particle size of the rubber particles to be blended is generally in the range of 0.005 to 1 μm, and in some non-limiting embodiments, in the range of 0.2 to 0.6 μm. The average particle size of the rubber particles in the present invention can be measured using a dynamic light scattering method. This measurement is carried out, for example, by uniformly dispersing the rubber particles in a suitable organic solvent by ultrasonication or the like, and creating a particle size distribution based on the mass of the rubber particles using FPRA-1000 (manufactured by Otsuka Electronics Co., Ltd.), and the median size is adopted as the average particle size.

[0132] In some non-limiting embodiments, the liquid compositions disclosed herein include 0-80% by weight, in some non-limiting embodiments, 20-75% by weight, in some non-limiting embodiments, 40-72% by weight, and in some non-limiting embodiments, 54-68% by weight of one or more organic particulate fillers.

[0133] Any suitable adhesion promoter may be used in the liquid composition of the present disclosure, the selection of which is well within the ability of one of ordinary skill in the art. In some non-limiting examples, the adhesion promoter is a silane-containing material or a tetraalkyl titanate or a trialkoxysilane-containing material. Exemplary adhesion promoters include, but are not limited to, bis(trialkoxysilylalkyl)benzenes, such as bis(trimethoxysilylethyl)benzene; aminoalkyltrialkoxysilanes, such as aminopropyltrimethoxysilane, aminopropyltriethoxysilane, and phenylaminopropyltriethoxysilane; and other silane coupling agents and mixtures of the foregoing. In some non-limiting embodiments, the adhesion promoter used is selected from the group consisting of dienophiles. The adhesion promoter may be applied first as a primer layer or as an additive to the composition. Some non-limiting examples of suitable adhesion promoters include AP3000, AP8000, and AP9000C (DuPont de Nemours, Wilmington, DE).

[0134] Other suitable adhesion promoters include organophosphorus compounds that may or may not contain other heteroatoms. Such species are not particularly limited and are generally selected from the group consisting of organophosphorus compounds of P(III), P(V) and their derivatives.

[0135] Non-limiting examples of organophosphorus compounds of P(III) include phosphines (PR3, including alkyldiarylphosphines, bidentate alkyldiarylphosphines, bidentate triarylphosphines, dialkylarylphosphines, trialkylphosphines, and triarylphosphines), aminophosphines (PR2(NR2)), phosphinites (PR2(OR)), diaminophosphines (PR(NR2)2), phosphonamidites (PR(OR)(NR2), phosphonites (PR(OR)2, including dialkylarylphosphonites and bidentate arylphosphonites), triaminophosphines (P(NR2)3), phosphorodiamidites (P(OR)(NR2)2), phosphoroamidites (P(OR)2(NR2) and phosphites (including P(OR)3, triaryl phosphites and bidentate aryl phosphites). Typically, in these P(III) compounds, R is selected from the group consisting of hydrogen, substituted or unsubstituted (C1-C30) alkyl, substituted or unsubstituted (C2-C30) alkenyl, substituted or unsubstituted (C5-C30) aryl, substituted or unsubstituted 5-30 membered heteroaryl or CN; or may be linked to adjacent substituents to form a substituted or unsubstituted monocyclic or polycyclic (C5-C30) aliphatic or aromatic ring, the carbon atoms of which may be replaced by at least one heteroatom selected from nitrogen, oxygen, sulfur, Si, PO, SO, SO2 and SeO2.

[0136] In some non-limiting embodiments of the organophosphorus compound of P(III), at least one of R is C1-C30 alkyl, and in some embodiments, all of R are C1-C30 alkyl.

[0137] Non-limiting examples of organophosphorus compounds of P(V) include phosphine oxides (PR3(O), including trialkylphosphine oxides and triarylphosphine oxides), phosphinates (PR2(O)(OR), including arylphosphinic acids and dialkylphosphinic acids), phosphinamides (PR2(O)(NR2)), phosphonates (PR(O)(OR)2, including trialkylphosphonates, triarylphosphonates and dialkylarylphosphonates), phosphonamidates (PR(O)(OR)(NR2)), phosphonamides (PR(O)(NR2)2), phosphates (P(O)(OR)3, including alkylphosphoric acids), phosphoramidates (P(O)(OR)2(NR2)), phosphorodiamidates (P(O)(OR)(NR2)2), and phosphoroamides (P(O)(NR2)3). Typically, in these P(V) compounds, R is the same or different at each occurrence and is selected from the group consisting of hydrogen, substituted or unsubstituted (C1-C30) alkyl, substituted or unsubstituted (C2-C30) alkenyl, substituted or unsubstituted (C5-C30) aryl, substituted or unsubstituted 5-30 membered heteroaryl or CN; or may be linked to adjacent substituents to form a substituted or unsubstituted monocyclic or polycyclic (C5-C30) aliphatic or aromatic ring, the carbon atoms of which may be replaced by at least one heteroatom selected from nitrogen, oxygen, sulfur, Si, PO, SO, SO2 and SeO2.

[0138] In some non-limiting embodiments of the organophosphorus compound of P(V), at least one of R is a C1-C30 alkyl, and in some embodiments, all R are C1-C30 alkyl. In some non-limiting embodiments, the organophosphorus compound can be a phosphoric acid ester amide compound such as SP670 and SP703 (Shikoku Chemical Industry Co., Ltd.), a phosphazene compound such as SPB-100, SPV-100 and SPE-100 (Otsuka Chemical Co., Ltd.) and FP series (Fushimi Pharmaceutical Co., Ltd.). Potentially useful metal hydroxides include magnesium hydroxides such as UD65, UD650 and UD653 (Ube Materials Corporation); and aluminum hydroxides such as B-30, B-325, B-315, B-308, B-303 and UFH-20 (Tomoe Engineering Co., Ltd.).

[0139] Preferred adhesion promoters include those capable of crosslinking one or more components of the coating composition of the present disclosure, such adhesion promoters include one or more functional groups selected from the group consisting of vinyl, styryl, maleimide, acrylic, methacrylic, allylic, alkynyl, or functional equivalents.

[0140] The liquid composition of the present disclosure may contain 0 to 25% by weight, or 1 to 20% by weight, or 2 to 15% by weight, or 5 to 10% by weight of the adhesion promoter, based on the total weight of the composition.

[0141] Further provided are crosslinked resins comprising one or more of the liquid compositions disclosed herein.

[0142] The specific embodiments regarding the components of the crosslinked resin are the same as those disclosed herein above.

[0143] The crosslinked resins prepared as disclosed herein generally possess several mechanical, electronic and thermal properties that make them well suited for use in the electronic applications disclosed herein. In some non-limiting embodiments, the crosslinked resins exhibit: (1) a coefficient of thermal expansion less than 50 ppm / K; (2) a Tg greater than 180° C.; (3) a Df less than 0.007; (4) a Dk less than 3.3; and (5) a tensile strength greater than 90 MPa.

[0144] In some non-limiting embodiments, the crosslinked resins prepared herein have a coefficient of thermal expansion less than 40 ppm / K, in some non-limiting embodiments less than 30 ppm / K, in some non-limiting embodiments less than 20 ppm / K, and in some non-limiting embodiments less than 10 ppm / K.

[0145] In some non-limiting embodiments, the crosslinked resins prepared herein have a Tg greater than 180°C, in some non-limiting embodiments greater than 190°C, in some non-limiting embodiments greater than 200°C, in some non-limiting embodiments greater than 210°C, in some non-limiting embodiments greater than 220°C, in some non-limiting embodiments greater than 230°C, in some non-limiting embodiments greater than 240°C, and in some non-limiting embodiments greater than 250°C.

[0146] In some non-limiting embodiments, the crosslinked resins prepared herein have a Df of less than 0.006, in some non-limiting embodiments less than 0.005, in some non-limiting embodiments less than 0.004, in some non-limiting embodiments less than 0.002, and in some non-limiting embodiments less than 0.001.

[0147] In some non-limiting embodiments, the crosslinked resins prepared herein have a Dk less than 3.2, in some non-limiting embodiments less than 3.1, in some non-limiting embodiments less than 3.0, in some non-limiting embodiments less than 2.9, in some non-limiting embodiments less than 2.8, in some non-limiting embodiments less than 2.7, in some non-limiting embodiments less than 2.6, in some non-limiting embodiments less than 2.5, in some non-limiting embodiments less than 2.4, in some non-limiting embodiments less than 2.3, in some non-limiting embodiments less than 2.2, in some non-limiting embodiments less than 2.1, and in some non-limiting embodiments less than 2.0.

[0148] In some non-limiting embodiments, the crosslinked resins prepared herein have a tensile strength greater than 100 MPa, and in some non-limiting embodiments, greater than 110 MPa, and in some non-limiting embodiments, greater than 120 MPa, and in some non-limiting embodiments, greater than 130 MPa, and in some non-limiting embodiments, greater than 140 MPa, and in some non-limiting embodiments, greater than 150 MPa, and in some non-limiting embodiments, greater than 160 MPa, and in some non-limiting embodiments, greater than 170 MPa, and in some non-limiting embodiments, greater than 180 MPa, and in some non-limiting embodiments, greater than 190 MPa, and in some non-limiting embodiments, greater than 200 MPa.

[0149] A non-limiting example of a method for preparing a crosslinked resin comprising a soluble polyimide resin disclosed herein comprises the following sequence of steps: (a) applying a liquid composition disclosed herein onto a substrate; (b) soft baking the coated substrate at one or more preselected temperatures for one or more preselected times; (c) exposing the coated substrate to UV radiation at a preselected wavelength and a preselected dose for a preselected time; (d) treating the coated, UV irradiated substrate at multiple preselected temperatures for multiple preselected times; (e) allowing the coated, UV irradiated, heat treated substrate to cool; and (f) developing and rinsing the coating in a solvent bath.

[0150] The liquid composition of the present disclosure can be prepared by combining one or more soluble polyimides of the present disclosure, any organic solvent, water or additional components, and a photoactive compound as a curing agent in any order. The organic solvent is the same as described above. When the composition contains a photoactive compound such as diazonaphthoquinone, onium salt, or photoinitiator, it is preferred to first dissolve the curing agent in a suitable organic solvent or aqueous alkaline solution, then mix with one or more of the present polymers and any optional surfactant, and then mix with any optional adhesion promoter. The selection of a suitable photoactive compound is within the ordinary level of skill in the art.

[0151] In some non-limiting embodiments, the liquid composition of the present disclosure can be applied or deposited on a substrate by any suitable method. The substrate can be the same as described above. Suitable methods for applying the composition can include, but are not limited to, spin coating, curtain coating, spray coating, roller coating, dip coating, vapor deposition, and lamination such as vacuum lamination and hot roll lamination, among others. In the semiconductor manufacturing industry, spin coating is a preferred method to utilize existing equipment and processes. In spin coating, the solid content of the composition can be adjusted along with the spinning speed to achieve the desired thickness of the composition on the surface to be applied.

[0152] If the liquid composition of the present disclosure does not contain an adhesion promoter, the surface of the substrate on which the composition is applied can be optionally first contacted with a suitable adhesion promoter or steam treated.Various steam treatments, such as plasma treatments, known in the art, can enhance the adhesion of the polymer of the present disclosure to the substrate surface.In certain applications, it may be preferable to treat the substrate surface with an adhesion promoter before applying the composition to the surface.The adhesion promoter is the same as described above.

[0153] Typically, the liquid composition of the present disclosure is spin-coated at a spin speed of 400-4000 rpm. The amount of the composition dispensed onto the wafer or substrate depends on the total solids content in the composition, the desired thickness of the resulting layer, and other factors known to those skilled in the art. When a film or layer of the composition is cast by spin-coating, much (or all) of the solvent evaporates during deposition of the film. Preferably, the composition after deposition on the surface is heated (soft baked) to remove any residual solvent. Typical bake temperatures are 80-120° C., although other temperatures may be suitably used. Such baking to remove residual solvent is typically performed for approximately 1-5 minutes, although longer or shorter times may be suitably used.

[0154] The compositions of the present disclosure are typically cured by heating for a period of time. Suitable curing temperatures are in the range of 140 to 300° C.; or 170 to 250° C. Typically, curing times are in the range of 1 to 600 minutes, or 30 to 240 minutes, or 30 to 120 minutes.

[0155] Generally, the thickness of the formed resin composition layer is equal to or greater than the thickness of the conductive layer. Since the thickness of the conductive layer of the circuit board is generally within the range of 5 to 70 μm, the thickness of the resin composition layer is generally 10 to 100 μm.

[0156] Further provided is a surface-treated metal foil, at least one surface of the metal foil comprising a surface treatment agent comprising: (a) one or more soluble polyimide resins; (b) one or more inorganic fillers; (c) one or more adhesion promoters; and (d) one or more initiators; the one or more adhesion promoters can function as crosslinkers with one or more components of the surface treatment agent.

[0157] Non-limiting examples of metal foils are selected from the group consisting of copper foil, nickel foil, cobalt foil, titanium foil, stainless steel foil and others known to those skilled in the art.

[0158] In one embodiment, the liquid composition comprising the polymer described herein can be coated onto a copper foil, resulting in some non-limiting embodiments of a surface-treated copper foil comprising, on at least one side of the surface-treated copper foil, (a) 15-90% by weight of one or more soluble polyimide resins; (b) 5-75% by weight of one or more crosslinking compounds; (c) 0-5% by weight of one or more photoinitiators; (d) 0-5% by weight of one or more oxidation catalysts; (e) 0-65% by weight of one or more solvents; (f) 0-60% by weight of one or more additional resins; (g) 0-10% by weight of one or more surface leveling agents; (h) 0-70% by weight of one or more organic or inorganic fillers; and (i) 0-25% by weight of one or more adhesion promoters. The embodiments relating to (a)-(i) of this composition are generally the same as those disclosed elsewhere herein with respect to the corresponding components contained in the resins, compositions, and the like.

[0159] Copper foils include rolled annealed (RA) copper foils and electrodeposited (ED) copper foils. These foils are manufactured using various methods, so they may differ from each other in terms of mechanical properties, flexibility, and the required copper surface roughening treatment. Generally, ED copper foils have a dull side (deposit side) and a shiny side (drum side); whereas, RA copper foils have both surfaces that are smooth. Since the present copper foils are intended for use in flexible copper clad laminates (FCCLs) and flexible printed circuit boards (FPCBs) for high frequency and / or high speed applications, the preferred copper foils are surface-treated copper foils obtained by applying a conventional surface treatment to at least one surface of an untreated copper foil.

[0160] When the foil is incorporated into a flexible copper clad laminate, the side of the foil that faces the dielectric layer is called the "lamination side". The side opposite the "lamination side" is called the "resist side". If the present surface-treated foil has only one treated surface, that treated surface becomes the laminate side when incorporated into a flexible copper clad laminate.

[0161] By controlling the current density and / or plating time and / or plating bath temperature and / or plating solution additives, surface-treated copper foils with different grain sizes, surface roughness and thickness can be obtained.

[0162] In some non-limiting embodiments, the copper foil used herein is selected from the group consisting of Mitsui MT 18FL (1.5 μm with 18 μm carrier), BF-NN-HT, BFL-NN-HT, BFL-NN-Z, and the like.

[0163] In some non-limiting embodiments of the present invention, the average cross-sectional grain size of the surface treated copper foil is preferably 2.5 μm or more, or 2.0 μm or less.

[0164] From the viewpoint of ensuring adequate adhesion without increasing conductor loss, the surface roughness (Sz, 10-point average roughness) of at least one treated surface of the surface-treated copper foil measured by a laser microscope is 2.5 μm or less or 2.0 μm or less. The surface roughness (Sz) is measured using a laser microscope in accordance with ISO 25178.

[0165] The laminate side and / or resist side of the surface-treated copper foil may incorporate a nodule-forming layer, a passivation layer, and / or an adhesion-promoting layer to enhance the suitability of the foil for use in FPCs. The surface properties of the resist side of the surface-treated copper foil are affected by many subsequent printed circuit manufacturing processes, such as microetching, acid rinse, brown oxide treatment, black oxide treatment, and pre-solder mask treatment. Thus, the surface roughness, nodule density, and total amount of non-copper metal elements are the evaluation criteria for the laminate side of the surface-treated copper foil. In some non-limiting embodiments, at least one treated surface of the surface-treated copper foil has a nodule density of 300 pieces / 25 μm or more. 2 or less than 200 pieces / 25μm 2 or less than 100 pieces / 25μm 2 or less than 50 pieces / 25μm 2 The nodule-forming layer is:

[0166] After the nodule electrodeposition process, one or more passivation treatments can be applied to one or both sides of the copper foil to impart additional desired properties such as anti-tarnish, heat resistance, and chemical resistance. Passivation layers generally contain metallic elements other than copper, such as zinc, nickel, chromium, cobalt, molybdenum, tungsten, and combinations thereof.

[0167] When the surface-treated copper foil is incorporated into a flexible copper-clad laminate, the adhesion between the copper foil and the dielectric layer is due to mechanical adhesion due to the roughness of the copper foil, but also due to chemical bonding by the adhesion promoter, if an adhesion promoter layer is present. In general, the final surface treatment is performed by forming an adhesion promoter layer by treating with a known adhesion promoter, such as a phosphorus-based or silane-based coupling agent. After the treatment with the adhesion promoter is completed, the surface-treated copper foil of the present invention can be obtained by removing the moisture with an electric heater.

[0168] In some non-limiting embodiments, a structure is formed comprising a surface-treated metal foil as disclosed herein. The structure comprises a substrate having a metal surface and a surface treatment disposed on the metal surface, the surface treatment comprising a cured bulk polyimide resin and an inorganic filler, at least a portion of the inorganic filler being bonded to the cured bulk polymeric material; the dielectric layer comprises a first region adjacent to the metal surface. The structure further comprises a second region adjacent to the first region and opposite the metal surface, the first region comprising a relatively low amount of the inorganic filler and the second region comprising a relatively high amount of the inorganic filler. Forming such a structure can improve adhesion between the metal foil and the surface treatment, as described, for example, in (Patent Document 3).

[0169] The preparation of surface treated copper foils is further illustrated in the Examples section below.

[0170] Further provided is a dry film comprising a soluble polyimide resin comprising: (a) one or more tetracarboxylic acid component residues; (b) one or more diamine component residues; and (c) one or more end-capping compounds, the one or more end-capping compounds comprising one or more crosslinking groups.

[0171] Specific embodiments of (a) one or more tetracarboxylic acid component residues; (b) one or more diamine component residues; and (c) one or more end-capping compounds, wherein the one or more end-capping compounds contain one or more crosslinking groups, are the same as those disclosed herein above.

[0172] In making such dry films, the compositions disclosed herein can be cast through a slot die coater or other suitable equipment to form dry films desirable for microelectronic applications. The cast film can be soft baked at a temperature of 70-150°C or 90-120°C for 30 seconds to 10 minutes to remove residual solvent. The soft baked film can then be subjected to curing conditions of 150-250°C for 30 minutes to 4 hours.

[0173] In other non-limiting embodiments, a layer of the liquid composition of the present disclosure can be formed as a dry film and placed on a substrate surface by lamination. Non-limiting examples of suitable substrates include silicon, copper, silver, indium tin oxide, silicon dioxide, glass, silicon nitride, aluminum, gold, polyimide, and epoxy mold compound. In a process based on lamination, if the adhesive film has a protective film with a thickness of 1 to 40 μm, the protective film is first peeled off, and then the adhesive film and the circuit board are preheated as necessary, and the adhesive film is pressed and heated while being pressed onto the circuit board. In some non-limiting embodiments, a method of laminating the adhesive film to the circuit board under reduced pressure by a vacuum lamination method is preferably adopted. Non-limiting lamination conditions include a pressure bonding temperature (lamination temperature) of 70 to 140° C. and a pressure bonding pressure of 1 to 11 kgf / cm. 2 (9.8×10 4 ~107.9×10 4 N / m 2 ) and reducing the air pressure to 20 mHg (26.7 hPa) or less. The lamination method may be a batch type or a continuous type using rolls. Vacuum lamination can be performed using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum applicator manufactured by Nichigo-Morton Co., Ltd., a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a roll-type dry coater manufactured by Hitachi Industries Co., Ltd., and a vacuum laminator manufactured by Hitachi AIC Co., Ltd.

[0174] In some non-limiting embodiments, the surface roughness of the metal foil is 50 to 1000 nm, in some non-limiting embodiments, 100 to 1000 nm, in some non-limiting embodiments, 150 to 1000 nm, and in some non-limiting embodiments, 200 to 1000 nm. In some non-limiting embodiments, the thickness of the metal foil is 1 to 2.5 μm, in some non-limiting embodiments, 1 to 5.0 μm, in some non-limiting embodiments, 1 to 10 μm, and in some non-limiting embodiments, 1 to 20.0 μm.

[0175] In some non-limiting embodiments, the adhesion energy G1c of the dry film to the metal foil is 60 to 80 J / m 2 and in some non-limiting embodiments, 70 to 90 J / m 2 and in some non-limiting embodiments, 80 to 100 J / m 2 and in some non-limiting embodiments, 100 J / m 2 G1c refers to the adhesion energy at the onset of crack propagation. In some non-limiting embodiments, the peel strength of the dry film to the metal foil is greater than 0.3 N / mm, in some non-limiting embodiments, greater than 0.4 N / mm, in some non-limiting embodiments, greater than 0.5 N / mm, in some non-limiting embodiments, greater than 0.6 N / mm, and in some non-limiting embodiments, greater than 0.7 N / mm.

[0176] The lamination process, which involves heating and pressing under reduced pressure, can be carried out using a general vacuum heat press. For example, the lamination process can be carried out by pressing a heated metal plate such as a SUS plate against the support layer. Lamination is usually performed on a 1×10 -2 In some non-limiting embodiments, the pressure is reduced to 1×10 -3 Heating and pressing can be done in one step, but it is usually more advantageous to do so in two or more steps to prevent the resin from bleeding. For example, the first pressing step is done at 1 to 15 kgf / cm 2and a temperature of 70 to 150°C. The second pressing step can be performed at a pressure of 1 to 40 kgf / cm 2 and a temperature of 150-200° C. In some non-limiting embodiments, pressing is performed for 30-120 minutes at each stage. Examples of commercially available vacuum hot press machines include MNPC-V-750-5-200 (Meiki Seisakusho Co., Ltd.) and VH1-1603 (Kitagawa Seiki Co., Ltd.).

[0177] An insulating layer can be formed on a circuit board by laminating an adhesive film on the circuit board, cooling the laminate to about room temperature, and then heat-curing the resin composition layer after peeling off the support if peeling off the support. Appropriate conditions for heat-curing can be selected according to the type and content of each resin component in the resin composition disclosed herein. In some non-limiting embodiments, the temperature and time for heat-curing are selected from the ranges of 150 to 220°C and 20 to 180 minutes, and in some non-limiting embodiments, the temperature and time for heat-curing are selected from the ranges of 160 to 210°C and 30 to 120 minutes.

[0178] After the insulating layer is formed, the support is peeled off if it was not peeled off before curing. The insulating layer formed on the circuit board is then perforated as necessary to form via holes or through holes. Perforation can be performed by one or more methods known to those skilled in the art, including, for example, drilling, laser, plasma, and the like. In some non-limiting embodiments, perforation is accomplished using a laser, such as a carbon dioxide laser and a YAG laser.

[0179] Subsequently, a conductive layer is formed on the insulating layer by dry plating or wet plating. Non-limiting examples of dry plating methods include vapor deposition, sputtering, and ion plating. In wet plating, the surface of the insulating layer is sequentially subjected to a swelling treatment with a swelling liquid, a surface roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid, thereby forming an anchor with projections and recesses. The swelling treatment with a swelling liquid can be performed by immersing the insulating layer in the swelling liquid at 50 to 80°C for 5 to 20 minutes. Non-limiting examples of the swelling liquid include an alkaline solution and a surfactant solution. Examples of the alkaline solution include a sodium hydroxide solution and a potassium hydroxide solution. Examples of commercially available swelling liquids include Swelling Dip Securiganth P and Swelling Dip Securiganth SBU (Atotech Japan Co., Ltd.). The surface roughening treatment with an oxidizing agent can be performed by immersing the insulating layer in an oxidizing agent solution at 60 to 80°C for 10 to 30 minutes. Non-limiting examples of the oxidizing agent include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide, dichromate, ozone, hydrogen peroxide / sulfuric acid, and nitric acid. The concentration of permanganate in the alkaline permanganate solution can be about 5 to 10% by weight. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as Concentrate Compact CP and Dosing Solution Securiganth P (Atotech Japan Co., Ltd.). The neutralization treatment with a neutralizing solution can be performed by immersing the insulating layer in a neutralizing solution at 30 to 50°C for 3 to 10 minutes. In some non-limiting examples, the neutralizing solution can be an acidic aqueous solution. An example of a commercially available neutralizing solution is Reduction Solution Securiganth P (Atotech Japan Co., Ltd.).

[0180] Alternatively, a plating resist having a reverse pattern of the conductive layer may be formed, and the conductive layer may be formed by electroless plating alone. Subsequent patterning methods may be subtractive or semi-additive methods known to those skilled in the art.

[0181] Further provided is a multilayer printed wiring board comprising: an insulating layer formed from a soluble polyimide resin containing (a) one or more tetracarboxylic acid component residues; (b) one or more diamine component residues; and (c) one or more end-capping compounds, the one or more end-capping compounds containing one or more crosslinking groups; and a conductive layer formed by plating. Specific embodiments of the soluble polyimide resin and the conductive layer are the same as those disclosed herein above.

[0182] The present disclosure also relates to a wide variety of electronic devices comprising at least one layer of the dielectric film of the present application on an electronic device substrate. The electronic device substrate can be any substrate used in the manufacture of any electronic device. Exemplary electronic device substrates include, but are not limited to, semiconductor wafers, glass, sapphire, silicate materials, silicon nitride materials, silicon carbide materials, display device substrates, epoxy mold compound wafers, circuit board substrates, and thermally stable polymers.

[0183] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, suitable methods and materials are described below. Furthermore, the materials, methods, and examples are illustrative only and are not intended to be limiting. All publications, patent applications, patents, and other references mentioned herein are incorporated by reference in their entirety. EXAMPLES

[0184] The concepts described herein are further illustrated in the following examples, which do not limit the scope of the invention described in the claims.

[0185] raw materials: All reagents for diamine, dianhydride and polyimide synthesis were obtained from TCI America, Inc. and Sigma Aldrich. The (di)anhydrides, (di)amines, polyimides and related designations used in this disclosure include: 6FDA (4,4'-hexafluoroisopropylidenebisphthalic dianhydride), BPDA (3,3',4,4'-biphenyltetracarboxylic dianhydride), FDA (9,9'-bis(4-aminophenyl)fluorene), TFMB (2,2'-bis(trifluoromethyl)benzidine), BPADA (4,4'-bisphenol A type dianhydride), APB-133 (1,3'-bis(3-aminophenoxy)benzene), ODPA (4,4-oxydiphthalic anhydride), (4-ethynylaniline) (4-EA), (bis(3-aminopropyl) terminated poly(dimethylsiloxane) (average Mn approx. 2500)), DAMA (2,4-diamino-6-diallylamino-1,3,5-triazine), 4AS (4-aminostyrene), 4-EPA (4-ethynylphthalic anhydride), MEMA (4,4'-methylenebis(2-ethyl-6-methylaniline)), DMAC (dimethylacetamide), and PAA (polyamic acid). All other solvents and chemicals were obtained from Fisher Scientific and used as received without further purification.

[0186] A copper foil having a thickness of 18 μm was exposed to a roughening etching agent MEC CZ8101 (a product of MEC Corporation) until the roughness measured by optical microscopy reached an average of 400 nm.

[0187] Molecular weight measurement: (1) Polyimide resin: For molecular weight measurement of polyimide resin, Waters Model Breeze including pump and injector was used. TMThe mobile phase consisted of dimethylacetamide containing 0.1% (wt / v) lithium chloride and 0.025% (wt / v) para-toluenesulfonic acid. The separation columns were a set of two Shodex GPC KD806 styrene-divinylbenzene gels, one Waters Styragel HR 0.5 and one Waters Styragel HR1. The column temperature was 40°C, the flow rate was 1.0 ml / min, and the detector was a 2414 from Waters with a cell size of 10 microliters. TM A differential refractive index detector was used. The sample concentration was 1.0 mg / ml, and the sample injection volume was 0.100 ml. The molecular weight was determined by a polystyrene standard. The Breeze system from Waters was used for data collection and processing. TM v.2 was used.

[0188] The molecular weight distribution and average molecular weight were measured by GPC method with relative calibration. Samples were prepared by placing 5.0 mg of solid polymer in a 20 ml bottle, adding 5.0 ml of eluent (N,N-dimethylacetamide containing 0.1% lithium chloride and 250 ppm toluenesulfonic acid) and mixing until the solution was fully dissolved and clear. Then, 2 ml of this solution was filtered through a 0.2 PTFE filter into a 2 ml injection vial. 100 microliters of the sample solution was injected into a Waters Model Breeze vial using a syringe. TM The test results reported were obtained by comparison to a calibration curve. All test procedures and subsequent reporting were in accordance with the OECD Guideline for Testing of Chemicals 118, as recommended in EPA document 744-B-97-001, “Polymer Exemption Guidance Manual.”

[0189] (2) Arylcyclobutene and other non-polyimide resins: Polymer samples were prepared as 0.5 wt% solutions in tetrahydrofuran and filtered through a 0.2 micron Teflon filter. The mobile phase was 0.5% triethylamine, 5% methanol, and 94.5% tetrahydrofuran. The column used was a Waters Styragel HR5E 7.8 x 300 mm column, lot number 0051370931. The injection volume was 100 microliters and the run time was 27 minutes. Molecular weight data are reported relative to polystyrene standards.

[0190] Test Method (1) Dielectric properties: The dielectric properties of the free-standing films were determined using IPC test method TM-650 2.5.5.13 (revised 01 / 07) using a copper split cylinder resonator machined to have a cavity frequency of 10 GHz each and a Keysight N5224A PNA or a Rohde & Schwarz ZNB40 network analyzer. The film geometry was such that the substrate extended beyond the diameter of the two cylindrical cavities. The thickness of the dielectric substrate can vary from 0.01 mm to 5.0 mm, but a substrate with a thickness of 0.03 mm was used for these tests. The free-standing film was placed in the cavity of the split cylinder resonator and the resonant frequency and quality factor of the TE011 resonant mode were measured using the network analyzer. The relative dielectric constant (Dk) and loss tangent (Df) of the film were calculated from the TE011 resonant mode using custom software written in MATLAB.

[0191] (2) Thermomechanical and gravimetric analysis: Free-standing films were cut into 10 mm x 25 mm shapes and mounted in a TA Instruments Dynamic Mechanical Analyzer Q800 instrument with a strain rate of 0.06%, a preload of 1 Newton, and a frequency of 1 Hertz. The specimens were equilibrated at a temperature of 50°C and then heated to 250°C at a rate of 5°C per minute. The maximum of the tan δ curve was taken as the glass transition temperature value. Thermomechanical analysis was performed in tensile mode using a TA Instruments Thermomechanical Analyzer Q400. The specimens were heated at a constant rate from 5°C to 200°C, then cooled to -50°C, and then cooled back down to 250°C at the same rate. The thermal expansion coefficient was determined as the linear change in dimensions from 25°C to 150°C in the final cycle.

[0192] (3) Peel test of 18μm copper foil After the copper foil samples were cured, a 1 cm wide peel strip was cut on the coupon using a suitable blade, and then the copper strip was peeled off at a 90 degree angle at a speed of 50 mm / min on an Instron tensile tester. Peel force values ​​were determined in kilogram force / centimeter. Values ​​above 0.75 kgf / cm were considered excellent, while values ​​below 0.4 kgf / cm were considered unacceptable for the embodiments disclosed herein.

[0193] (4) Instron Testing Free-standing membranes were cut into 51 mm x 13 mm specimens and placed in either an Instron 5943 or an Instron 68SC-1 Universal Testing System. Samples were tested according to ASTM-D822-12, Standard Test Method for Tensile Properties of Thin Plastic Sheeting. Data was collected and analyzed with Intron Bluehill® software.

[0194] (5) Instron Testing of Photosensitive Polyimide Compositions The free-standing membranes were cut into 1 cm x 6 cm specimens and placed in an Instron 68SC-1 Universal Testing System. Samples were tested according to ASTM-D822-12, Standard Test Method for Tensile Properties of Thin Plastic Sheeting. Data was collected and analyzed with Instron Bluehill® software.

[0195] (6) Dynamic Mechanical Analysis of Photosensitive Polyimide Composition The free-standing membrane was cut into a 10 mm x 25 mm shape and mounted in a TA Instruments dynamic mechanical analyzer Q800 instrument with a strain rate of 0.06%, a preload of 1 Newton, and a frequency of 1 Hertz. The temperature was equilibrated at 50°C and then increased to 200°C at a rate of 5°C per minute. The maximum value of the tan δ curve was taken as the glass transition temperature value.

[0196] General synthesis of soluble polyimide resins A three-necked reaction vessel equipped with a PTFE stirring shaft, O-rings and bearing assembly was charged under nitrogen. For most diamines, the desired amino compound was dissolved in DMAc at room temperature. In certain embodiments, the DMAC was warmed to an appropriate temperature to dissolve all added diamines. While stirring the solution of diamine, the desired dianhydride monomer was added to the reaction mixture in small increments such that the internal temperature did not exceed the desired temperature. The reaction mixture was then stirred until the viscosity of the resulting polyamic acid solution was in the desired range.

[0197] To the polyamic acid solution, acetic anhydride and β-picoline were added. The temperature of the reaction mixture was raised to 80° C. and the reaction was maintained at this temperature for about 3 hours, followed by stirring overnight. The resulting polyimide was then isolated as a powder by precipitation from water. The polymer was then washed with methanol and dried. The polyimide was isolated as a white powder and characterized by GPC and NMR spectroscopy.

[0198] Preparation of soluble PI resin 1-SPI1 Preparation of soluble styrene-terminated polyimide copolymer (ODPA / / TFMB / APB-133 / 4AS-100 / / 49 / 49 / 4) A 1 liter reaction flask equipped with nitrogen inlet and outlet and mechanical stirrer was charged with 31.38 g of trifluoromethylbenzidine (TFMB) and 175 g of dimethylacetamide (DMAC). The mixture was stirred at room temperature under nitrogen for approximately 30 minutes to dissolve the TFMB. Then, 28.65 g of 1,3,3-aminophenoxybenzene (APB-133) and 0.95 grams of 4-aminostyrene (4AS) were added along with 50 g of DMAC. Once the amine was dissolved, 60.80 g of oxydiphthalic anhydride (ODPA) was added along with 59 g of DMAC while stirring the reactants. The rate of addition of the dianhydride was adjusted to ensure that the maximum reaction temperature was less than 40° C. The dianhydride was allowed to dissolve and react, resulting in a polyamic acid (PAA) solution that was stirred for approximately 24 hours. Then, ODPA was added in controlled increments of 0.310 g to increase the molecular weight of the polymer and the viscosity of the polymer solution. A small sample was removed from the reaction flask for testing and the solution viscosity was monitored using a Brookfield cone and plate viscometer. A total of 1.24 g of ODPA was added. The reaction was allowed to proceed for an additional 72 hours at room temperature with gentle stirring to allow the polymer to reach equilibrium. The final viscosity of the polyamic acid was 10,600 cP.

[0199] 50.4 grams of acetic anhydride and 45.99 grams of 3-methylpyridine were added to the polyamic acid copolymer solution, which was then heated at 80° C. for 4 hours. The mixture was precipitated in water (1000 mL×2) and washed with methanol (1000 mL). The isolated solid polyimide was dried under vacuum at 70° C. for 2-3 days. The solid was subsequently dissolved and formulated in various solvents (NMP, DMAc, and cyclopentanone).

[0200] Preparation of soluble PI resin 2-SPI2 Preparation of a soluble styrene-terminated polyimide copolymer (ODPA / TFMB / APB-133 / 2,4-diamino-6-diallylamino-1,3,5-triazine (DAMA) / 4AS 100 / 46.5 / 46.5 / 5 / 4) A 500 mL reaction flask equipped with nitrogen inlet and outlet and mechanical stirrer was charged with 22.34 g of trifluoromethylbenzidine (TFMB) and 150 g of dimethylacetamide (DMAC). The mixture was stirred at room temperature under nitrogen for about 30 minutes to dissolve the TFMB. Then, 20.39 g of 1,3,3-aminophenoxybenzene (APB-133), 1.55 g of 2,4-diamino-6-diallylamino-1,3,5-triazine (DAMA) and 0.72 grams of 4-aminostyrene (4AS) were added along with 36 g of DMAC. Once the amine was dissolved, 45.6 g of oxydiphthalic anhydride (ODPA) was added along with 25 g of DMAC while stirring the reaction. The rate of addition of the dianhydride was adjusted to keep the maximum reaction temperature below 40° C. The dianhydride was allowed to dissolve and react, resulting in a polyamic acid (PAA) solution that was stirred for about 24 hours. ODPA was then added in controlled increments of 0.233 g to increase the molecular weight of the polymer and the viscosity of the polymer solution. A small sample was removed from the reaction flask for testing and the solution viscosity was monitored using a Brookfield cone-and-plate viscometer. A total of 0.931 g of ODPA was added. The reaction was allowed to proceed for an additional 72 hours at room temperature with gentle stirring to allow the polymer to reach equilibrium. The viscosity of the polyamic acid was 829 cP.

[0201] To this polyamic acid mixture, 37.67 grams of acetic anhydride and 34.36 grams of 3-methylpyridine were added and heated at 80°C for 4 hours. The mixture was precipitated in water (1000 mL x 2) and washed with methanol (1000 mL). The isolated solid polyimide was dried under vacuum at 70°C for 2-3 days. This solid was subsequently dissolved and formulated in various solvents (NMP, DMAc, and cyclopentanone).

[0202] Preparation of soluble PI resin 3-SPI3 Preparation of soluble styrene-terminated polyimide copolymer BPADA / / APB-133 / TFMB / 4AS 100 / / 42.5 / 42.5 / 30 A 1 L reaction flask equipped with nitrogen inlet and outlet, mechanical stirrer, and thermocouple was charged with 16.33 g (0.051 mol) of TFMB, 14.91 g (0.051 mol) of APB-133, 4.29 g (0.036 mol) of 4AS, and 217 mL of DMAC. The mixture was stirred at room temperature under nitrogen for approximately 30 minutes. 61.21 g (0.1176 mol) of BPADA was then added slowly in small portions to the stirred solution of diamine. Once the dianhydride addition was complete, an additional 24 mL of DMAC was used to wash any remaining dianhydride powder from the vessel and reaction flask walls and added as a wash. The resulting mixture was stirred for 24 hours. Separately, a 5% solution of BPADA in DMAC was prepared and added in small portions (approximately 6.25 g) every 24 hours over a period of 4 days. A total of 24.98 g of BPADA in DMAC was added. The resulting reaction mass was further stirred gently at room temperature for 1-2 days. The imidization of PAA was carried out by heating the solution to 40°C, followed by the addition of 56.04 g of acetic anhydride and 51.12 g of 3-methylpyridine. The reaction mixture was then heated at 80°C for 5-7 hours. The polymer solution was cooled to room temperature and then poured into 4 L of MeOH in a blender and stirred rapidly to pulverize the polymer solids. The pulverized polymer solids were stirred in the blender for 10 minutes and then collected by filtration. The polymer powder was air-dried overnight and further dried under vacuum at 60°C for 2 days. The amount of polymer obtained was 91 grams.

[0203] A soluble polyimide resin was prepared containing: SPI1:ODPA / / TFMB / APB-133 / 4AS 100 / / 49 / 49 / 4 SPI2:ODPA / / TFMB / APB-133 / DAMA / 4AS 100 / / 46.5 / 46.5 / 5 / 4 SPI3:BPADA / / APB-133 / TFMB / 4AS 100 / 42.5 / 42.5 / 30 SPI4:ODPA / 6FDA / / TFMB / Priamine TM1075 / 4-AS 85 / 15 / / 91 / 05 / 08 SPI5:ODPA / / APB-133 / TFMB / DAMA / 4-EA 100 / / 46.5 / 46.5 / 05 / 04 SPI6:ODPA / / APB-133 / TFMB / M1309 / 4-AS 100 / / 46 / 46 / 04 / 08 SPI7:BPADA / / APB-133 / 4-AS 100 / / 85 / 30 SPI8:ODPA / 4-EPA / / APB-133 / MEMA 98 / 2 / / 50 / 50 The relevant properties are shown in Table 1.

[0204] [Table 1]

[0205] Preparation of comparative PI resin 1-CPI1 A polyimide containing ODPA, BisP, and TFMB with an Mn of about 72,500 and Mw of about 314,300 relative to polystyrene standards was placed in cyclopentanone such that upon complete dissolution of the material a 20 wt % solution was formed. Even with extensive rotation of the vial, less than 5 wt % of the polymer redissolved.

[0206] General formulation and preparation and testing of free-standing films In a 20 mL scintillation vial, dry polyimide powder and N-methyl-2-pyrrolidone (NMP) are mixed. After the vial is capped and sealed, the mixture is rotated for an appropriate time to dissolve the polyimide polymer into solution, typically 24-48 hours. After the initial mixing period is completed, additional components such as crosslinkers, adhesion promoters, etc. are added to the polyimide solution. The vial containing the formulation is then rotated for an additional 24 hours to prepare a homogenous solution. The formulation is filtered through a 3 μm polypropylene filter membrane using a plastic syringe. For formulations containing particulate fillers or other non-homogeneous components, these components are added after filtration, and the formulation is rotated for an additional 6-24 hours to disperse the insoluble components.

[0207] An automated drawdown bar (DDB) coater is used to fabricate the film. The substrate to be coated is placed and fixed on the platform of the automated coater. The formulation is dispensed onto the substrate and a film is formed on the substrate using a DDB with an appropriate gap to obtain the desired film thickness. Immediately after coating, the substrate with the film is transferred to a hotplate set at 80°C and soft baked for 10 minutes. After the soft bake is complete, the coated substrate is removed from the hotplate and allowed to cool to room temperature.

[0208] The soft-baked films were cured in a nitrogen atmosphere using a belt furnace. The films were cured on the desired substrate. They were passed through successive heating zones in the belt furnace with a maximum cure temperature of 200° C. for 60 minutes or a maximum cure temperature of 300° C. for 20 minutes. A typical cure profile with a maximum cure temperature of either 200° C. or 300° C. and a belt speed of 0.7 inches per inch is shown in Table 2.

[0209] [Table 2]

[0210] The cured film was stripped from the substrate by immersing the coated substrate in deionized water for at least 24 hours or until the film detached from the substrate. Alternatively, the film was placed in a pressure cooker at 15-20 psi and 125°C for 18-24 hours and then cooled to room temperature. The stripped film was then dried in air or in a vacuum oven set at 70°C and less than 1 inHg pressure for 18-24 hours.

[0211] Preparation of free-standing film 1-FSF1 Following the procedure outlined above, a formulation of polyimide SPI3 (3.002 g) and crosslinker MIR-3000 (1.294 g) in NMP (7.977 g) was prepared, coated, soft-baked, and cured to produce a free-standing film with a thickness of 20.4 μm, Dk(10 GHz) of 2.83, Df(10 GHz) of 0.0038, average tensile modulus of 1.85 GPa (max 2.35 GPa), average tensile strength of 70.5 MPa (max 74.0 MPa), and average Eb of 6.4% (max 7.9%).

[0212] Preparation of free-standing film 2-FSF2 Following the procedure outlined above, a formulation of polyimide SPI3 (3.000 g) and crosslinker SR454 (1.283 g) in NMP (7.954 g) was prepared, coated, soft-baked, and cured to produce a free-standing film with a thickness of 27.2 μm, Dk(10 GHz) of 2.88, Df(10 GHz) of 0.0151, average tensile modulus of 1.84 GPa (max 2.02 GPa), average tensile strength of 69.8 MPa (max 88.5 MPa), and average Eb of 7.6% (max 12.0%).

[0213] Preparation of free-standing film 3-FSF3 Following the procedure outlined above, a formulation containing polyimide SPI3 (3.000 g), crosslinker MIR-3000 (0.643 g), and crosslinker Kowa DCP-M (0.643 g) in NMP (7.959 g) was prepared, coated, soft-baked, and cured. The free-standing film thus produced had a thickness of 31.8 μm, Dk (10 GHz) of 2.66, Df (10 GHz) of 0.0046, average tensile modulus of 2.32 GPa (max 2.62 GPa), average tensile strength of 83.6 MPa (max 125.7 MPa), and average Eb of 8.9% (max 10.8%). Film properties are summarized in Table 3.

[0214] [Table 3]

[0215] Preparation of free-standing film 4-FSF4 Following the procedure outlined above, a formulation containing polyimide SPI3 (3.000 g), crosslinker MIR-3000 (0.643 g), and crosslinker Kowa DCP-M (0.643 g) in NMP (7.959 g) was prepared, coated, soft-baked, and cured. The free-standing film thus produced had a thickness of 31.8 μm, a Dk(10 GHz) of 2.66, a Df(10 GHz) of 0.0046, an average tensile modulus of 2.32 GPa (max 2.62 GPa), an average tensile strength of 83.6 MPa (max 125.7 MPa), and an average Eb of 8.9% (max 10.8%).

[0216] General procedure for preparing PI-based formulations containing silica Formulation containing 50% silica by weight: A formulation with 45% solids by weight based on total mass was produced by adding 35.4% by weight of soluble polyimide (DM-120) to a vessel, followed by the addition of a solvent such as cyclopentanone. After mixing the polyimide thoroughly to fully dissolve it in the solvent, the polyimide solution was thoroughly mixed with 5% by weight of triallyl cyanurate (TAC) or triallyl isocyanurate (TAIC), 2.5% by weight of Homide 116, 2.5% by weight of Sartomer (SR454), 3.5% by weight of SPV-100, 1% by weight of dicumyl peroxide (DCP), a thermal radical initiator, and 0.1% by weight of Polyfox 656, a surfactant. Finally, 50% by weight of Admatech's silica 5GX-CM1 (70% by weight in methyl ethyl ketone) with an average particle size of 0.5 mm and a top cut diameter of 5 mm was added. The resulting mixture was homogenized before coating.

[0217] Formulation containing 70% silica by weight: 21.24 wt% of soluble polyimide (DM-120) was added to the vessel, followed by the addition of a solvent such as cyclopentanone to produce a formulation with a total mass of the components of 45 wt%. After the polyimide was thoroughly mixed with the solvent, the polyimide solution was thoroughly mixed with 3 wt% triallyl cyanurate (TAC) or triallyl isocyanurate (TAIC), 1.5 wt% Homide 116, 1.5 wt% Sartomer (SR454), 2.1 wt% SPV-100, 0.6 wt% thermal radical initiator dicumyl peroxide (DCP), and 0.06 wt% surfactant Polyfox 656. Finally, 70 wt% of Admatech's silica SC2050-MTM / 5GX-CM1 mixture (1:1, w / w) (70 wt% in methyl ethyl ketone) with an average particle size of 0.5 mm and a top cut diameter of 5 mm was added. The resulting mixture was homogenized before coating.

[0218] Preparation of PI-coated copper-RCC1 and RCC2: Soluble polyimide-based formulations were prepared by mixing all ingredients, including polyimide-based resin, crosslinker, surfactant, thermal radical initiator, and inorganic filler such as functionalized silica particles, in cyclopentanone to a solid content of typically 45%, followed by rolling overnight to ensure complete mixing. The formulation solution was then drawdown coated at a speed of 6 mm / s through a steel bar with a gap of 200 microns onto Nan Ya N738G release PET substrate for dry film or onto copper foil for resin coated copper (RCC), and the film was soft-baked on a hot plate at 90° C. for 3 minutes to ensure less than 1% residual solvent by GC. After soft-baking, the dry film or RCC was covered with a PE film for storage.

[0219] Soluble polyimide-based formulations were also coated using a slot die coater (i.e., nTact nRad Extrusion Deposition System) with a 2 mil shim, a coating gap of 150 μm, and a relative speed of 13 mm / sec. The coating fluid dispense rate was 238 μL / sec, and a chuck was used to provide a dispense delay of 1000 ms at the start of coating. Soft bake conditions were 12 minutes at 80° C. in a convection oven. Substrates included 1.5 and 18 μm BFL-NN-HT copper foil and Nan Ya N738G release PET.

[0220] Using a Meiki (MVLP 500 / 600) laminator, the dry film or RCC was laminated onto a suitable substrate by applying a vacuum of about 2 hPa for 30 seconds in the first step, a pressure of 0.95-1.00 MPa via a rubber contact for 60 seconds at 95-110°C, and a pressure of 1.2 MPa with a steel plate for 60 seconds in the second step.

[0221] After lamination, the dry film samples were cured in nitrogen (<100 ppm oxygen) using a SierraTherm belt oven (model no. 7K9-74C122-8ANLIR) at 135° C. for 40 minutes and 200° C. for 60 minutes. The specimens were then peeled to remove the PET, yielding free-standing membrane samples that could be cut to desired dimensions for analysis.

[0222] For copper foil peel testing, the samples were either coated directly onto the corresponding copper foil (i.e., RCC) and then laminated to a CCL board, or the dry film was laminated, dielectric side down, to the corresponding copper foil, then the PET was peeled off and the other side of the dielectric film was laminated to a CCL board. The laminated specimens were then cured under the same belt oven conditions as described above.

[0223] The compositions of the PI-coated copper prepared herein are summarized in Table 4.

[0224] [Table 4]

[0225] Relevant characteristics are summarized in Table 5.

[0226] [Table 5]

[0227] RCC1 and RCC2 are T g It was confirmed that the peel strength on the Cu foil was high and the CTE was relatively low, while the flexibility and dielectric properties of the film were maintained.

[0228] Preparation of PI-coated copper-RCC3 to RCC7: A soluble polyimide-based formulation was prepared and coated onto copper foil as described herein above, with the composition listed in Table 6.

[0229] [Table 6]

[0230] Relevant characteristics are summarized in Table 7.

[0231] [Table 7]

[0232] The use of SPV-100 in the coating composition was observed to increase the measured peel strength. In addition, the use of mixed silica was also observed to increase the peel strength of the coating compositions prepared herein.

[0233] Effect of copper foil selection on measured peel strength Various copper foils were coated with formulation RCC4 using the procedure described above and the properties are listed in Table 8.

[0234] [Table 8]

[0235] Peel strength and surface resistivity measurements were found to vary depending on the choice of copper foil and the presence or absence of a treatment on the foil surface.

[0236] Preparation of photosensitive polyimide composition

[0237] [Table 9]

[0238] [Table 10]

[0239] A soluble photosensitive polyimide based formulation was prepared by mixing all the ingredients listed in Table 9, rolling overnight, and then filtering through a 5.0 μm syringe filter.

[0240] For lithographic evaluation, the polymer formulations were deposited on silicon substrates by spin coating and soft baked at 90°C-110°C for 1-2 min. Film thickness was measured using optical Filmetrics and corresponding software tools. For lithographic processing, the wafers were exposed to a dose of up to 1000 mJ / cm2 with a Karl Suess mask aligner or an OAI broadband light source through a multi-transmission mask containing various features. The films were then optionally post-exposure baked at 65°C or 85°C for 60 s. The films were then subjected to puddle development with cyclopentanone, with puddle times ranging from 10-75 s or 2×60 s (with spin drying in between) or 2×60 s followed by 1×30 s (with spin drying in between), followed by spin drying. The length of puddle development was determined by the time required to remove the unexposed areas of the wafer. The photopatternability of the films was evaluated by measuring the film thickness before and after development.

[0241] For free-standing film samples, the polymer formulations were deposited on copper wafer substrates or silicon substrates by spin coating, soft-baked at 90°C–110°C for 1–2 min, and then irradiated with 1000 mJ / cm 2 The films were flood exposed at 400 K and then cured in a Blue M oven at 130° C. for 30 minutes, then at 200° C. for 1 hour in nitrogen with less than 100 ppm oxygen. The coated copper wafer substrates were cut to size and the films were peeled off in a water bath containing 5% ammonium sulfate, rinsed, and dried to obtain free-standing films for analysis. The coated silicon wafer substrates were immersed in heated water in a pressure cooker for 24 hours to lift off free-standing films for analysis. The properties are reported in Table 10.

[0242] [Table 11]

[0243] It should be noted that not all of the acts described above in the general description or examples are required, that some of the specific acts may not be required, and that one or more additional acts may be performed in addition to those described. Furthermore, the order in which the acts are listed is not necessarily the order in which the acts are performed.

[0244] In the foregoing specification, the concepts have been described with reference to specific embodiments. However, those skilled in the art will appreciate that various modifications and changes can be made without departing from the scope of the present disclosure as set forth in the following claims. Accordingly, the specification and drawings should be regarded in an illustrative rather than a restrictive sense, and all such modifications are intended to be included within the scope of the present disclosure.

[0245] Benefits, other advantages, and solutions to problems have been described above with respect to certain embodiments. However, this benefit, advantage, solution to a problem, and any features that may give rise to or make more prominent any benefit, advantage, or solution should not be construed as critical, required, or essential features of any or all claims.

[0246] It should also be appreciated that certain features described herein in the context of separate embodiments for clarity may be combined and provided in a single embodiment. Conversely, various features described in the context of a single embodiment for brevity may also be provided individually or in any subcombination. The use of various ranges of numerical values ​​specified herein is described as approximations, as if the minimum and maximum values ​​in the described ranges were both preceded by the word "about". In this format, slight variations above and below the described ranges can be used to achieve substantially the same results as the values ​​within the ranges. Also, the disclosure of these ranges is intended to be a continuous range including all values ​​between the minimum and maximum average values, including fractional values ​​that may result from combining some of the components of one value with the components of another value. Furthermore, when broader and narrower ranges are disclosed, it is within the contemplation of the present disclosure to combine the minimum value from one range with the maximum value from another range, and vice versa.

Claims

1. A soluble polyimide resin comprising: (a) one or more tetracarboxylic acid moiety residues; (b) residues of one or more diamine components; (c) one or more endcapping compounds; Including, The one or more end-capping compounds comprise one or more cross-linking groups, and the soluble polyimide resin.

2. 2. The soluble polyimide resin of claim 1, wherein the one or more end-capping compounds comprising one or more crosslinking groups are selected from the group consisting of aliphatic end-capping compounds, aromatic end-capping compounds, heteroaromatic end-capping compounds, alkynyl end-capping compounds, alkenyl end-capping compounds, maleimide end-capping compounds, vinyl end-capping compounds, allylic end-capping compounds, cyanate ester end-capping compounds and ester end-capping compounds.

3. 3. The soluble polyimide resin of claim 2, wherein the one or more crosslinking groups are selected from the group consisting of a radical crosslinking group, a cationic crosslinking group, an anionic crosslinking group, a crosslinking group capable of crosslinking with itself to form a homopolymer, a crosslinking group capable of crosslinking with other crosslinking groups to form a heteropolymer, and combinations thereof.

4. 4. The soluble polyimide resin of claim 3, wherein the one or more crosslinking groups are selected from the group consisting of allyl groups, vinyl groups, alkynyl groups, alkenyl groups, (meth)acrylate groups, benzocyclobutene groups, maleimide groups, allyl-based groups, cyanate ester groups, and ester groups.

5. A liquid composition comprising two or more of the following: (a) 1 to 90 weight percent of one or more soluble polyimide resins; (b) 2 to 75% by weight of one or more crosslinking compounds: (c) 0 to 5 wt. % of one or more photoinitiators or thermal radical initiators; (d) 0 to 5 wt. % of one or more oxidation catalysts; and (e) 0 to 85 weight percent of one or more solvents.

6. 6. The liquid composition of claim 5, further comprising one or more of the following: (f) 10 to 60 weight percent of one or more additional resins; (g) 0 to 10 wt. % of one or more surface leveling agents; (h) 0 to 70% by weight of one or more organic or inorganic fillers; and (i) 0 to 25 weight percent of one or more adhesion promoters.

7. 1. A surface-treated metal foil, at least one surface of the surface-treated metal foil comprising: (a) one or more soluble polyimide resins; (b) one or more organic or inorganic fillers; (c) one or more adhesion promoters; (d) one or more initiators; A surface treatment agent comprising The one or more adhesion promoters may function as crosslinkers with one or more components of the surface treatment.

8. 8. A structure comprising the surface-treated metal foil of claim 7, the structure comprising: a substrate having a metal surface, and a surface treatment disposed on the metal surface, the surface treatment including the cured bulk polyimide resin and the inorganic filler, at least a portion of the inorganic filler being bonded to the cured bulk polymer material; a dielectric layer comprising: a first region adjacent to the metal surface; a second region adjacent to the first region and opposite the metal surface, wherein the first region comprises a relatively low amount of the inorganic filler and the second region comprises a relatively high amount of the inorganic filler.

9. 2. A dry film comprising the soluble polyimide resin of claim 1, comprising: (a) 5% to 50% by weight of the soluble polyimide resin; (b) from 0% to 50% by weight of one or more surface-functionalized crosslinkable organic or inorganic fillers; (c) 15% to 30% by weight of one or more additives selected from the group consisting of photoinitiators, thermal radical initiators, crosslinkers, additional resins, surface leveling agents, and adhesion promoters; Including dry film.

10. 2. A multilayer printed wiring board comprising an insulating layer made of the soluble polyimide resin according to claim 1 and a conductive layer formed by plating, the insulating layer comprising: (a) 5% to 50% by weight of the soluble polyimide resin; (b) 50% by weight or more of one or more surface-functionalized crosslinkable organic or inorganic fillers; (c) 15% to 30% by weight of one or more additives selected from the group consisting of additional resins, surface leveling agents, and adhesion promoters; A multilayer printed wiring board comprising:

Citation Information

Patent Citations

  • Printed circuit board

    KR102422883B1

  • Aqueous developable, photosensitive benzocyclobutene-based oligomers and polymers with high moisture resistance

    US7198878B2

  • Aqueous developable benzocyclobutene-based polymer composition and method of use of such compositions

    US8143360B2