Extracellular vesicle separation device, separation method of extracellular vesicle-containing solution, and extracellular vesicle-containing solution
The extracellular vesicle separation device uses dual hollow fiber membranes with specific permeabilities to efficiently and selectively isolate extracellular vesicles from fluids, achieving high recovery rates and preserving essential biological components.
Patent Information
- Application Number
- JP2024045811
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-07
AI Technical Summary
Existing methods for isolating extracellular vesicles from sample fluids, particularly blood, are inefficient due to batch processing limitations, low recovery rates, and non-selective separation, leading to aggregation and loss of essential biological components.
An extracellular vesicle separation device utilizing two types of hollow fiber membranes with different particle permeabilities, where the first membrane allows 50-100% of extracellular vesicles to pass while blocking larger components, and the second membrane further concentrates vesicles, achieving selective separation and purification.
The device enables high recovery rates of extracellular vesicles (40-60%) and proteins (60-90%), while minimizing the loss of essential biological components, facilitating continuous processing and reducing clogging issues.
Smart Images

Figure 2024137885000005 
Figure 2024137885000006 
Figure 2024137885000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an extracellular vesicle separation device, a method for separating an extracellular vesicle-containing solution, and an extracellular vesicle-containing solution. [Background technology]
[0002] It has been discovered that cells release vesicles wrapped in lipid membranes called extracellular vesicles, and the biological effects of extracellular vesicles have been attracting attention in recent years. Extracellular vesicles contain information-bearing substances such as nucleic acids and are used to exchange information between cells (Non-Patent Document 1). This means that extracellular vesicles can be target substances for various purposes. For example, they can be used for research purposes on changes in cell phenotypes in the fields of basic medicine and basic biology, for testing or diagnosis purposes to obtain information about the inside of the body from samples such as blood collected from humans, for removing extracellular vesicles from the human body or administering extracellular vesicles into the human body to improve the body's condition, or for treatment or anti-aging purposes.
[0003] There is a need for an efficient technique for selectively extracting extracellular vesicles from a sample solution, selectively removing them from a patient's body fluid, particularly blood, or purifying them from a raw solution. Separation or purification of extracellular vesicles is generally performed by centrifugation, but centrifugation is not an efficient method. The reasons for this include the fact that continuous processing is not possible because it is a batch process, there is a limit to the amount that can be processed in one batch, and extracellular vesicles aggregate due to centrifugal force, resulting in a low recovery rate.
[0004] Techniques for separating extracellular vesicles without using centrifugation are also known. For example, Patent Document 1 discloses a technique for concentrating body fluids obtained from humans using a nanomembrane ultrafiltration concentrator. Patent Document 2 discloses a technique for filtering a patient's blood and then adsorbing and removing extracellular vesicles in the blood.
[0005] When concentrating extracellular vesicles in a liquid to be treated that contains cells or cell fragments using an ultrafiltration membrane, the ultrafiltration membrane will quickly become clogged with the cells or cell fragments if the liquid is filtered as is. To avoid this, a pretreatment process has been disclosed in which the liquid to be treated is filtered using a flat membrane filter (microfiltration membrane) to remove the cells and cell fragments (Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-91251 A [Patent Document 2] Special Publication No. 2022-542517 [Patent Document 3] JP 2022-182360 A [Non-patent literature]
[0007] [Non-Patent Document 1] Genomics,Proteomics&Bioinformatics,(Netherlands),2018,Vol.16,p.50-62 Summary of the Invention [Problem to be solved by the invention]
[0008] However, concentration using the nanomembrane ultrafiltration concentrator described in Patent Document 1 had the problem that all substances contained in the body fluid that are larger than extracellular vesicles were concentrated, meaning that it was not possible to selectively concentrate the extracellular vesicle fraction.
[0009] Furthermore, in the system for adsorbing and removing extracellular vesicles described in Patent Document 2, the adsorption capacity of the adsorption carrier is limited, making it difficult to completely remove extracellular vesicles, and non-specific adsorption to the adsorption carrier is unavoidable, resulting in the problem that even substances contained in blood that are necessary for physiological functions are adsorbed and removed.
[0010] In the method described in Patent Document 3, in which the liquid to be treated is pretreated with a membrane filter and concentrated with a hollow fiber membrane having a molecular weight cut-off of 100,000 to 1,000,000, objects on the order of several μm such as cells and cell fragments and substances smaller than the molecular weight cut-off of the hollow fiber membrane can be removed, but extracellular vesicles cannot be selectively separated. Further, in the pretreatment with a flat membrane-shaped membrane filter, ultimately the membrane filter becomes clogged immediately, and there is a problem that a large amount of the liquid to be treated cannot be processed or continuously processed for a long time of several hours or more.
[0011] In order to solve the above problems, an object of the present invention is to provide an extracellular vesicle separation device capable of selectively separating, purifying, or removing extracellular vesicles from a specimen, raw material, body fluid, or the like. [Means for Solving the Problems]
[0012] As a result of intensive studies, the present inventors have found that the above problems can be solved by using two types of membranes having different particle permeabilities. That is, the present invention is as follows in [1] to
[16] . [1] A first module containing a first hollow fiber membrane, a second module containing a second hollow fiber membrane, a flow path B for communicating the inside of the first module and the inside of the second module, and the 0.15 μm particle permeability P1 of the first hollow fiber membrane is 50% or more and 100% or less, and the 0.15 μm particle permeability P2 of the second hollow fiber membrane and the P1 satisfy the relationship P2 < P1. An extracellular vesicle separation device. [2] The extracellular vesicle separation device according to [1], wherein the P2 is 15% or less. [3] The extracellular vesicle separation device according to [1] or [2], wherein the 0.02 μm particle permeability of the second hollow fiber membrane is 5% or less. [4] The water permeability of the second hollow fiber membrane is 250 mL / h / mmHg / m 2 or more and 2000 mL / h / mmHg / m 2 or less. The extracellular vesicle separation device according to any one of [1] to [3]. [5] The extracellular vesicle separation device according to any one of [1] to [4], wherein the first hollow fiber membrane or the second hollow fiber membrane contains a hydrophilic polymer. [6] The extracellular vesicle separation device described in [5], wherein the hydrophilic polymer contains a monocarboxylic acid vinyl ester unit as a repeating unit and is present on at least one surface of the first hollow fiber membrane or the second hollow fiber membrane. [7] The extracellular vesicle separation device according to any one of [1] to [6], wherein the main component of the first hollow fiber membrane or the second hollow fiber membrane is a polysulfone-based polymer. [8] The extracellular vesicle separation device according to any one of [1] to [7], wherein the thickness of the dense layer in the cross section of the first hollow fiber membrane is 1.0 μm or more and 10.0 μm or less. [9] The water permeability of the first hollow fiber membrane is 16000 mL / h / mmHg / m 2 More than 30000mL / h / mmHg / m 2 The extracellular vesicle separation device according to any one of [1] to [8], which is as follows:
[10] The extracellular vesicle separation device described in any one of [1] to [9], wherein the space within the flow path B is connected to the outer surface of the first hollow fiber membrane.
[11] The extracellular vesicle separation device according to any one of [1] to
[10] , which is used for removing extracellular vesicles from body fluids of a living organism.
[12] The extracellular vesicle separation device described in
[11] , wherein the body fluid is blood.
[13] The extracellular vesicle separation device according to any one of [1] to
[12] , comprising: a flow path A in which the space within the flow path B is connected to the inner surface of the second hollow fiber membrane, and which introduces the treated liquid discharged from a liquid reservoir into the inside of the first module; and a flow path D in which the permeated liquid discharged from the second module and the non-permeated liquid discharged from the first module are mixed and introduced into the liquid reservoir.
[14] The extracellular vesicle separation device according to any one of [1] to
[13] , which is used for the treatment of sepsis, autoimmune disease, or chronic liver disease.
[15] Using a first hollow fiber membrane with a 0.15-μm particle transmittance P1 of 50% or more and 100% or less, filtering a liquid to be treated containing extracellular vesicles, and separating it into a first non-permeate liquid in which solutes larger than the extracellular vesicles that can permeate the first hollow fiber membrane are concentrated, and a first permeate liquid in which solutes larger than the extracellular vesicles that can permeate the first hollow fiber membrane are removed; a second separation step of filtering the first permeate liquid using a second hollow fiber membrane in which the 0.15-μm particle transmittance P2 and the P1 satisfy the relationship P2 < P1, and separating it into a second non-permeate liquid in which all or part of the extracellular vesicles contained in the first permeate liquid are concentrated, and a second permeate liquid containing solutes smaller than the extracellular vesicles. A method for separating an extracellular vesicle-containing solution having the above steps.
[16] Having at least one surface marker selected from the group consisting of phosphatidylserine, CD9, CD63, CD81, TyA, and Clq, and having an extracellular vesicle number concentration of 6.0×10 9 cells / mL or more and 1.4×10 12 cells / mL or less. An extracellular vesicle-containing solution.
[0013] Further, the present invention is as follows in
[17] to
[30] below.
[17] A first module containing a first hollow fiber membrane, a second module containing a second hollow fiber membrane, and a flow path B communicating the inside of the first module and the inside of the second module. The 0.15-μm particle transmittance P1 of the first hollow fiber membrane is 50% or more and 100% or less, and the 0.15-μm particle transmittance P2 of the second hollow fiber membrane and the P1 satisfy the relationship P2 < P1. An extracellular vesicle separation device.
[18] The extracellular vesicle separation device according to
[17] above, wherein the P2 is 15% or less.
[19] The extracellular vesicle separation device according to
[17] or
[18] above, wherein the 0.02-μm particle transmittance of the second hollow fiber membrane is 5% or less.
[20] The water permeability of the second hollow fiber membrane is 250 mL / h / mmHg / m 2 or more and 2000 mL / h / mmHg / m 2 or less. The extracellular vesicle separation device according to any one of
[17] to
[19] above.
[21] The extracellular vesicle separation device according to any one of
[17] to
[20] above, wherein the first hollow fiber membrane or the second hollow fiber membrane contains a hydrophilic polymer.
[22] The extracellular vesicle separation device according to
[21] , wherein the hydrophilic polymer contains a monocarboxylic acid vinyl ester unit as a repeating unit and is present on at least one surface of the first hollow fiber membrane and / or the second hollow fiber membrane.
[23] The extracellular vesicle separation device according to any one of
[17] to
[22] above, wherein the main component of the first hollow fiber membrane or the second hollow fiber membrane is a polysulfone-based polymer.
[24] The extracellular vesicle separation device according to any one of
[17] to
[23] above, wherein the thickness of the dense layer in the cross section of the first hollow fiber membrane is 1.0 μm or more and 10.0 μm or less.
[25] The water permeability of the first hollow fiber membrane is 16000 mL / h / mmHg / m 2 More than 30000mL / h / mmHg / m 2 The extracellular vesicle separation device according to any one of
[17] to
[24] above, which is as follows:
[26] The extracellular vesicle separation device according to any one of
[17] to
[25] above, wherein the space within the flow path B is connected to the outer surface of the first hollow fiber membrane.
[27] The extracellular vesicle separation device according to any one of
[17] to
[26] above, which is used for removing extracellular vesicles from body fluids of a living organism.
[28] The extracellular vesicle separation device according to
[27] , wherein the body fluid is blood.
[29] The extracellular vesicle separation device according to any one of
[17] to
[28] above, comprising: a flow path A through which a body fluid extracted from a living body is introduced into the first module, and a flow path D through which a permeate extracted from the second module and a non-permeate extracted from the first module are mixed and introduced into the living body, wherein the space within the flow path B is connected to the inner surface of the second hollow fiber membrane.
[30] The extracellular vesicle separation device according to any one of
[17] to
[29] above, for use in the treatment of sepsis, autoimmune disease or chronic liver disease. Effect of the Invention
[0014] According to the extracellular vesicle separation device of the present invention, it is possible to selectively separate, purify or remove extracellular vesicles from a specimen, a raw material, a body fluid, etc. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram of an extracellular vesicle separation device of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a module containing a hollow fiber membrane provided in the extracellular vesicle separation device of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing an example of the configuration of a first module and a second module provided in the extracellular vesicle separation device of the present invention. [Figure 4] FIG. 1 is a schematic diagram showing an example of the configuration of a first module and a second module provided in the extracellular vesicle separation device of the present invention. [Diagram 5] FIG. 1 is a schematic diagram showing an example of the configuration of a first module and a second module provided in the extracellular vesicle separation device of the present invention. [Figure 6] FIG. 1 is a schematic diagram showing an example of the configuration of a first module and a second module provided in the extracellular vesicle separation device of the present invention. [Figure 7] FIG. 1 is a schematic diagram of an extracellular vesicle separation performance evaluation system. [Figure 8] 1 is a cross-sectional image of a first hollow fiber membrane in Example 1 observed at 2000 times using a scanning electron microscope. [Figure 9] This is an image obtained by binarizing the image in FIG. [Figure 10] This is an image obtained by performing image analysis on Figure 9 and deleting pores with a diameter of 0.5 μm or less. [Figure 11] 1 is an image of the inner surface of the first hollow fiber membrane in Example 1 observed at 1500 times using a scanning electron microscope. [Figure 12] 1 is an image of the outer surface of the first hollow fiber membrane in Example 1 observed at 3000 times using a scanning electron microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments of the extracellular vesicle separation device of the present invention will be described in detail below. However, the present invention is not limited to the following embodiments, and can be modified in various ways depending on the purpose and application.
[0017] <Extracellular vesicle separation device> The extracellular vesicle separation device of the present invention comprises a first module containing a first hollow fiber membrane, a second module containing a second hollow fiber membrane, and a flow path B that connects the interior of the first module with the interior of the second module.
[0018] The configuration of the extracellular vesicle separation device of the present invention will be described below with reference to the schematic diagram shown in FIG. 1-A. A liquid to be treated, such as a specimen, a raw material, or a body fluid, is filtered by a first hollow fiber membrane contained in a first module 101. Since the first hollow fiber membrane contained in the first module has a 0.15 μm particle permeability P1 of 50% or more, the permeate of the first module obtained by filtration (hereinafter referred to as the "first permeate") contains extracellular vesicles. Next, the first permeate is led to the second module 102 through a flow path B (103b). Then, the first permeate is filtered again by a second hollow fiber membrane contained in the second module 102 to obtain a permeate of the second module (hereinafter referred to as the "second permeate"). Since the 0.15 μm particle permeability P2 of the second hollow fiber membrane contained in the second module is lower than P1, all or a portion of the extracellular vesicles contained in the first permeate are filtered out or concentrated by the second module and are not contained in the second permeate.
[0019] That is, a first separation step can be performed by filtering with the first module, in which the liquid to be treated is separated into a non-permeated liquid (hereinafter referred to as a "first non-permeated liquid") in which solutes larger than extracellular vesicles that cannot permeate the first hollow fiber membrane are concentrated, and a first permeated liquid in which solutes larger than extracellular vesicles that cannot permeate the first hollow fiber membrane are removed. Also, a second separation step can be performed by filtering with the second module, in which the liquid to be treated is separated into a non-permeated liquid (hereinafter referred to as a "second non-permeated liquid") in which all or a part of extracellular vesicles of a specific size contained in the first permeated liquid are concentrated, and a second permeated liquid containing solutes smaller than extracellular vesicles or extracellular vesicles of a specific size or less and solutes smaller than extracellular vesicles. The "specific size" referred to here will be described in the description of the method for separating a solution containing extracellular vesicles described later.
[0020] The extracellular vesicle separation device of the present invention is equipped with a first module, a second module, and a flow path B in order to separate extracellular vesicles. That is, the extracellular vesicle separation device of the present invention is not necessarily required to be an integrated machine as long as it is equipped with a first module, a second module, and a flow path B. For example, the first module and the second module may be hung on separate racks and communicated with each other through flow path B. In addition, there is no limitation on the liquid delivery method, and any of a liquid delivery method using gravity or a liquid delivery driving force such as a pump may be used. In particular, it is preferable to provide a liquid delivery pump for the purpose of improving the operability of the device.
[0021] As shown in Figure 1-B, the extracellular vesicle separation device of the present invention preferably has a flow path A (103a) for introducing the treated liquid discharged from a liquid reservoir (e.g., a living body or a cell culture tank) into the inside of the first module, and a flow path C (103c) for discharging the second permeate obtained in the second module.
[0022] That is, the separation method of the present invention preferably includes an introduction step A in which the liquid to be treated is introduced into the inside of a first module through flow path A, a transfer step B in which the first permeate is transferred from the first module to the inside of a second module through flow path B, and an extraction step C in which the second permeate is extracted from the second module through flow path C.
[0023] The term "liquid pool" refers to a reservoir in which the liquid to be treated by the extracellular vesicle separation device of the present invention is stored in a retrievable state in the form of a solution. For example, when the extracellular vesicle separation device of the present invention is used for bodily fluids circulating within an animal's body, the liquid pool is the living body (particularly, the human body when used for humans). When the extracellular vesicle separation device of the present invention is used for extracellular vesicles released from cultured cells, the liquid pool may be a tank in which cell culture supernatant is collected and stored, or a tank in which cells are cultured.
[0024] 1-C, in addition to the above-mentioned flow paths, it is more preferable to provide a flow path D (103d) for mixing the second permeate obtained in the second module with the first non-permeate derived from the first module and introducing the mixture into the liquid reservoir. By providing the flow path D, it is possible to obtain a treatment liquid in which all extracellular vesicles or extracellular vesicles of a specific size are selectively separated from the treatment liquid.
[0025] That is, it is preferable that the separation method of the present invention further includes a mixing step D, after the discharge step C in which the second permeate is discharged from the second module through the flow path C, in which the first non-permeate discharged from the first module through the flow path D is mixed with the second permeate discharged from the second module.
[0026] The material of each flow path is preferably a flexible material for ease of handling, and examples thereof include polyvinyl chloride, silicone, and polytetrafluoroethylene.
[0027] When the extracellular vesicle separation device of the present invention is equipped with a pump, it is preferable that flow path A, flow path B, and flow path C each have one pump.
[0028] The filtration direction of the liquid to be treated in the module may be either from the inside to the outside or from the outside to the inside of the hollow fiber membrane contained in the module. When the extracellular vesicle separation device of the present invention is used for a liquid to be treated that contains cells, the inner surface is used as the contact surface of the liquid to be treated, and cross-flow filtration is performed while forming a flow parallel to the membrane surface, so that the cells on the membrane surface are easily washed away by the flow of the liquid to be treated, and cell adhesion to the surface of the first hollow fiber membrane can be suppressed. Therefore, in the extracellular vesicle separation device of the present invention, it is preferable that the space in flow path B is connected to the outer surface of the first hollow fiber membrane.
[0029] Furthermore, the extracellular vesicle separation device of the present invention is more preferably provided with a flow path A in which the space in the flow path B is connected to the inner surface of the second hollow fiber membrane, and which introduces the liquid to be treated drawn out from the liquid reservoir into the first module, and a flow path D in which the permeated liquid drawn out from the second module and the non-permeated liquid drawn out from the first module are mixed and introduced into a liquid reservoir such as a living body. With the above-mentioned configuration, it is possible to selectively separate all extracellular vesicles or extracellular vesicles of a specific size from the liquid to be treated drawn out from the liquid reservoir, and to return cellular components or proteins necessary for the living body to the liquid reservoir such as a living body.
[0030] The extracellular vesicle separation device of the present invention can be suitably used for a liquid to be treated that contains cells, and can be suitably used for removing extracellular vesicles contained in human body fluids, particularly blood. In this case, the removal rate of extracellular vesicles is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more. This is because if the removal rate of extracellular vesicles from blood is 40% or more, a significant difference in biological reactions is likely to be observed.
[0031] In addition, from the viewpoint of selectively separating extracellular vesicles in the liquid to be treated from other substances, the protein recovery rate is preferably 60% or more, more preferably 65% or more. It is even more preferably 70% or more, even more preferably 75% or more, and particularly preferably 80% or more. A protein recovery rate of 60% or more leads to a reduction in production costs in the purification of raw materials containing extracellular vesicles. In addition, when separating extracellular vesicles from human body fluids, the amount of proteins useful to the body to be supplemented by plasma preparations, etc. can be reduced by recovering proteins useful to the body.
[0032] Furthermore, when proteins are recovered and returned to the living body as described above, examples of the proteins to be recovered include albumin, which functions to transport nutrients and metabolic substances and maintain osmotic pressure, and immunoglobulin (IgG, etc.), which functions as an antibody. The type of protein to be recovered may be appropriately selected depending on the disease, but albumin is preferred.
[0033] When albumin is the target of recovery, since albumin plays an important role in the living body as described above, the recovery rate is preferably 70% or more, more preferably 75% or more, further preferably 80% or more, even more preferably 85% or more, and particularly preferably 90% or more.
[0034] Conversely, when separating extracellular vesicles from a sample liquid for testing or separating extracellular vesicles as pharmaceutical ingredients or cosmetic additives, it is preferable that proteins such as albumin are not mixed in. In this case, the albumin residual rate, which corresponds to the above-mentioned albumin recovery rate, is preferably 20% or less, more preferably 10% or less, even more preferably 5% or less, even more preferably 3% or less, and particularly preferably 1% or less.
[0035] <Method for isolating extracellular vesicles-containing solution> As a method for separating an extracellular vesicle-containing solution of the present invention, a treatment liquid containing extracellular vesicles is filtered using a first hollow fiber membrane having a 0.15-μm particle transmittance P1 of 50% or more and 100% or less, and a non-permeate liquid in which solutes larger than the extracellular vesicles that cannot permeate the first hollow fiber membrane are concentrated, and a first permeate liquid from which solutes larger than the extracellular vesicles that cannot permeate the first hollow fiber membrane are removed are separated in a first separation step; and a second separation step of filtering the first permeate liquid using a second hollow fiber membrane in which a 0.15-μm particle transmittance P2 and the above P1 are in a relationship of P2 < P1, and separating the second permeate liquid into a second non-permeate liquid in which all or part of the extracellular vesicles contained in the first permeate liquid are concentrated and a second permeate liquid containing solutes smaller than the extracellular vesicles. There is a separation method having the above.
[0036] In addition, the extracellular vesicles may be separated using the above-described first module and the second module, and the flow path structure is not limited to that described in the previous paragraph.
[0037] Further, by the separation method of the present invention, it is also possible to separate extracellular vesicles of a specific size among the extracellular vesicles contained in the treatment liquid. Examples of the extracellular vesicles present in the treatment liquid include exosomes (40 to 150 nm), microvesicles (50 to 1000 nm), apoptotic vesicles (500 to 2000 nm), and the like. Among them, exosomes and microvesicles are said to play important roles in cell-to-cell communication. Therefore, exosomes or microvesicles may be a target for removal in a specific disease.
[0038] As described above, extracellular vesicles are a population classified into at least three or more types, and the size of extracellular vesicles ranges from 40 nm to 2 μm. In the method for separating an extracellular vesicle-containing solution of the present invention, extracellular vesicles of a specific size can be selectively separated by changing the permeability of the first hollow fiber membrane and the permeability of the second hollow fiber membrane.
[0039] More specifically, the separation is performed as follows.
[0040] When it is desired to selectively separate extracellular vesicles (exosomes) with a size of 40 nm to 150 nm, first, in the first separation step, the solution is separated into a first non-permeating solution in which solutes larger than extracellular vesicles that cannot permeate the first hollow fiber membrane and extracellular vesicles larger than 150 nm are concentrated, and a first non-permeating solution containing extracellular vesicles with a size of 150 nm or less. Next, in the second separation step, all of the extracellular vesicles contained in the first permeating solution are concentrated.
[0041] In another embodiment, when it is desired to selectively separate extracellular vesicles of 150 nm to 300 nm (a part of microvesicles) from among the extracellular vesicles, first, in the first separation step, the solution is separated into a first non-permeating liquid in which solutes larger than the extracellular vesicles that cannot permeate the first hollow fiber membrane and extracellular vesicles larger than 300 nm are concentrated, and a first non-permeating liquid containing extracellular vesicles of 300 nm or less in size. Next, in the second separation step, a part of the extracellular vesicles contained in the first permeating liquid, i.e., extracellular vesicles of 150 nm or more in size, may be concentrated.
[0042] In reality, the size selectivity of solutes in hollow fiber membrane filtration is not perfect, but if the ratio of the membrane permeability of the solute that is intended to be permeated to the membrane permeability of the solute that is intended not to be permeated in the permeated liquid is 2 or more, it can be said that selective separation is possible. Note that permeability is a value obtained by dividing the solute concentration after filtration by the solute concentration before filtration.
[0043] The solution obtained by removing extracellular vesicles from the liquid to be treated can be used, for example, as an extracellular vesicle-free culture medium, or as a preparation for treatment in which extracellular vesicles are removed from a patient's blood and returned to the patient. The solution containing extracellular vesicles separated from the liquid to be treated can be used as a sample for testing and diagnosis based on extracellular vesicles, a pharmaceutical ingredient, a cosmetic additive, etc.
[0044] <Hollow fiber membrane> The extracellular vesicle separation device of the present invention requires at least two types of hollow fiber membranes with different permeabilities for particles of 0.15 μm.
[0045] The term "particle transmittance" refers to the percentage of particles having a specific particle size that are transmitted. In this specification, the particle transmittance is measured using polystyrene latex particles as described later in "Measurement of particle transmittance".
[0046] Extracellular vesicles have a diameter distribution of 40 nm to 1 μm, but are flexible due to their lipid membrane structure. Therefore, for example, extracellular vesicles with a diameter of 1 μm can pass through holes smaller than 1 μm. The present inventors have found that a hollow fiber membrane with a certain or higher 0.15 μm particle permeability has the desired extracellular vesicle permeability.
[0047] That is, in order to obtain the desired extracellular vesicle permeability, the 0.15 μm particle permeability (hereinafter referred to as "P1") of the first hollow fiber membrane must be 50% or more and 100% or less. The first hollow fiber membrane with P1 in the above-mentioned range has high permeability to extracellular vesicles and can selectively separate extracellular vesicles from the liquid to be treated (sample liquid, raw material liquid, body fluid, etc.). Examples of extracellular vesicles present in the liquid to be treated include the above-mentioned exosomes (40 to 150 nm), microvesicles (50 to 1000 nm), apoptotic vesicles (500 to 2000 nm), etc. Among them, exosomes and microvesicles are said to play an important role in intercellular communication. Therefore, exosomes or microvesicles may be the target of removal in certain diseases. From this viewpoint, P1 of the first hollow fiber membrane is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more. In addition, since the upper limit of measurement for 0.15 μm particle transmittance is 100%, P1 is 100% or less.
[0048] Furthermore, for the purpose of separating microvesicles, the 0.20 μm particle permeability of the first hollow fiber membrane is preferably 50% or more, more preferably 55% or more, and even more preferably 60% or more.
[0049] The liquid to be treated containing extracellular vesicles usually contains, at the same time, cells that produce extracellular vesicles or blood cell components. The sizes of blood cell components are, respectively, white blood cells (10 μm or more), red blood cells (about 7 μm), and platelets (about 3 μm). Cultured cells are generally larger than platelets. Since blood cell components are soft and deformable, the size of particles that the first hollow fiber membrane can block so that platelets do not permeate is preferably smaller than 2 μm. Further, the 1.00-μm particle permeability of the first hollow fiber membrane is more preferably 5% or less.
[0050] The second hollow fiber membrane of the present invention separates extracellular vesicles that have passed through the first hollow fiber membrane and substances smaller than the extracellular vesicles. Therefore, the 0.15-μm particle permeability of the second hollow fiber membrane (hereinafter referred to as "P2") needs to satisfy the relationship of P2 < P1.
[0051] The preferable specific ranges of P1 and P2 differ depending on the fraction of extracellular vesicles to be separated. For example, when it is intended to selectively separate microvesicles of 100 nm to 1 μm, P1 is preferably 90% or more, more preferably 100%. On the other hand, P2 is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less.
[0052] When almost all of the extracellular vesicles in the liquid to be treated are separated by the extracellular vesicle separation device of the present invention, P2 is preferably 5% or less. Further, in this case, in order to minimize the leakage of extracellular vesicles, the 0.02-μm particle permeability of the second hollow fiber membrane is preferably 5% or less, more preferably 4% or less, and even more preferably 3% or less.
[0053] As a method for setting the particle permeability within the above range, the first hollow fiber membrane and the second hollow fiber membrane can both follow the same design guidelines. For example, methods such as changing the spinning dope composition or spinning conditions of the hollow fiber membrane to adjust the surface pore size, membrane thickness, or thickness of the dense layer can be mentioned.
[0054] The first hollow fiber membrane and the second hollow fiber membrane used in the extracellular vesicle separation device of the present invention preferably have an asymmetric structure.
[0055] The term "asymmetric structure" refers to a structure in which the pore size on one surface side is different from the pore size on the other surface side, and in the case of a hollow fiber membrane, the pore size is different between the inner surface and the outer surface. By having an asymmetric structure, a membrane can be obtained that has both a steep fractionation curve and high water permeability. Having a steep fractionation curve means that the target substance can be separated from other substances with high efficiency.
[0056] The pore size of the inner surface of the first hollow fiber membrane of the present invention is preferably 0.50 μm or more and 3.00 μm or less. By setting the pore size of the inner surface within the above range, the intrusion of cellular components such as cultured cells and platelets into the inside of the hollow fiber membrane can be suppressed. By suppressing the intrusion of blood cell components into the inside of the hollow fiber membrane, irritation to cells, particularly blood cells, is reduced, blood compatibility is improved, and clogging by cellular components and the like is also suppressed, making it possible to efficiently separate extracellular vesicles from the liquid to be treated. From the viewpoint of improving the extracellular vesicle permeability and water permeability, the pore size of the inner surface is more preferably 0.80 μm or more, even more preferably 0.90 μm or more, particularly preferably 1.00 μm or more, and most preferably 1.10 μm or more. On the other hand, from the viewpoint of further suppressing the intrusion of cellular components such as blood cells and further increasing the strength of the hollow fiber membrane, the pore size of the inner surface of the hollow fiber membrane is more preferably 2.50 μm or less, and even more preferably 2.00 μm or less.
[0057] The pore size of the inner surface of the second hollow fiber membrane of the present invention is preferably 0.001 μm or more and 0.050 μm or less. From the viewpoint of suppressing leakage of extracellular vesicles and obtaining a preferable protein recovery rate, the pore size of the inner surface is more preferably 0.005 μm or more, even more preferably 0.010 μm or more, and particularly preferably 0.020 μm or more. Also, it is more preferably 0.040 μm or less, and even more preferably 0.030 μm or less.
[0058] Methods for adjusting the pore size of the inner surface of the hollow fiber membrane to the above range include, for example, a method of adjusting the concentration of the main component constituting the hollow fiber membrane in the spinning dope, or a method of adjusting the coagulation value of the injected liquid for forming the hollow portion (hereinafter referred to as the "core liquid").
[0059] The term "main component" refers to the component that is most abundant by mass among the components constituting the hollow fiber membrane.
[0060] The "coagulation value" refers to the mass of core liquid added at the point when the system becomes cloudy when the core liquid is added in small amounts to 50 g of a solution containing 1% by mass of the main component constituting the hollow fiber membrane.
[0061] In the first hollow fiber membrane of the present invention, the pore size of the outer surface is preferably 0.50 μm or more and 10.00 μm or less. From the viewpoint of improving separation performance and water permeability, the pore size of the outer surface is more preferably 0.60 μm or more. Also, from the viewpoint of maintaining the strength of the hollow fiber membrane, the pore size of the outer surface is more preferably 5.00 μm or less, even more preferably 2.00 μm or less, particularly preferably 1.00 μm or less, and most preferably 0.90 μm or less.
[0062] In the second hollow fiber membrane of the present invention, the pore size of the outer surface is preferably 0.01 μm or more and 1.50 μm or less. From the viewpoint of improving separation performance and water permeability, the pore size of the outer surface is more preferably 0.02 μm or more, and even more preferably 0.03 μm or more. Moreover, from the viewpoint of maintaining the strength of the hollow fiber membrane, the pore size of the outer surface is more preferably 1.00 μm or less, and even more preferably 0.80 μm or less.
[0063] Examples of methods for adjusting the pore size of the outer surface of the hollow fiber membrane to be within the above range include a method of adjusting the concentration of poor solvent vapor relative to the main component constituting the hollow fiber membrane in the dry section during spinning described below, or a method of adjusting the spinneret temperature during spinning.
[0064] In the first hollow fiber membrane of the present invention, from the viewpoint of ease of production of the hollow fiber membrane, the pore size on the outer surface of the hollow fiber membrane is more preferably smaller than the pore size on the inner surface of the hollow fiber membrane.
[0065] On the other hand, in the second hollow fiber membrane of the present invention, since it is preferable to obtain a steep fractionation curve by the pores near the inner surface, it is more preferable that the pore size on the outer surface of the hollow fiber membrane is larger than the pore size on the inner surface of the hollow fiber membrane.
[0066] In the present invention, the pore size on the surface of the hollow fiber membrane can be measured from an image of the surface observed with a scanning electron microscope (hereinafter referred to as "SEM"). Note that the observation magnification may be appropriately changed as long as the pores can be clearly observed.
[0067] For example, for the surface of the first hollow fiber membrane with a smaller pore size, the area of all pores in an arbitrary 20 μm×20 μm range is measured for pores that can be confirmed at a magnification of 3000 times. If the total number of measured pores is less than 50, measurements are repeated in a 20 μm×20 μm range until the total number of measured pores is 50 or more, and data is added. For the surface of the first hollow fiber membrane with a larger pore size, the area of all pores in an arbitrary 40 μm×40 μm range is measured for pores that can be confirmed at a magnification of 1500 times. If the total number of measured pores is less than 50, measurements are repeated in a 40 μm×40 μm range until the total number of measured pores is 50 or more, and data is added.
[0068] For the second hollow fiber membrane, for example, for the surface with smaller pores, calculate the area of all pores in any 1.2 μm × 1.2 μm range for pores that can be observed at a magnification of 50,000 times. For the surface with larger pores, calculate the area of all pores in any 20 μm × 20 μm range for pores that can be observed at a magnification of 3,000 times. Measure until the total number of measured pores is 50 or more.
[0069] The position of the dense layer within the hollow fiber membrane provided in the extracellular vesicle separation device of the present invention is arbitrary, and may be located closer to either the inner surface or the outer surface.
[0070] The "dense layer" refers to a region in which no pores with a pore size of 0.50 μm or more exist when the cross section of the first hollow fiber membrane is observed by the method described below in "Measurement of the thickness of the dense layer in the first hollow fiber membrane", and refers to a region in which no pores with a pore size of 0.50 μm or more exist when the cross section of the second hollow fiber membrane is observed by the method described below in "Measurement of the thickness of the dense layer in the second hollow fiber membrane". 2It should be noted that one of the factors that influence the separation performance of a hollow fiber membrane is the thickness of the dense layer.
[0071] The first and second hollow fiber membranes of the extracellular vesicle separation device of the present invention preferably have a dense layer. By having a dense layer, a dense region (dense layer) that contributes to the separation of the separation target substance and a coarse region (coarse layer) with a large pore size that has low water permeation resistance are present, so that it is easy to achieve both separation performance and water permeability. The dense layer may be present at any position on the cross section of the hollow fiber membrane. For example, the dense layer may be present near the inner surface of the hollow fiber membrane, near the outer surface, or in the center of the cross section. In addition, the dense layer may be present continuously from the inner surface or outer surface, or multiple dense layers may be present as described above.
[0072] Although not particularly limited, when a polysulfone-based polymer is used as the material for the first hollow fiber membrane, it is preferable that the first hollow fiber membrane has a dense layer on the outer surface side from the viewpoint of ease of controlling the membrane structure and ease of production. Also, when a polysulfone-based polymer is used as the material for the second hollow fiber membrane, it is preferable that the second hollow fiber membrane has a dense layer on the inner surface side from the viewpoint of preventing leakage of extracellular vesicles due to fine scratches on the outer surface of the hollow fiber membrane.
[0073] The thickness of the dense layer in the first hollow fiber membrane of the present invention is preferably 1.0 μm or more and 10.0 μm or less. By having the thickness of the dense layer in the above range, it is possible to achieve both high permeability and high separation function, and the increase in filtration pressure when the amount of the liquid to be treated is increased can be suppressed. From the viewpoint of reducing the permeation resistance of the substance, the thickness of the dense layer is preferably 7.0 μm or less, more preferably 6.5 μm or less, even more preferably 6.0 μm or less, and particularly preferably 5.5 μm or less. On the other hand, since the dense layer has the effect of improving the separation function of the hollow fiber membrane, it is preferable that it has a certain thickness or more. Therefore, the thickness of the dense layer is more preferably 1.5 μm or more, more preferably 2.0 μm or more, and particularly preferably 2.5 μm or more.
[0074] The second hollow fiber membrane of the present invention has a smaller separation target than the first hollow fiber membrane, so that the dense layer is preferably thinner than the first hollow fiber membrane from the viewpoint of water permeability. On the other hand, since the dense layer is a layer that has the effect of improving the separation function of the hollow fiber membrane, it is preferable that it has a certain thickness or more. Therefore, the thickness of the dense layer in the second hollow fiber membrane is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. In addition, it is preferably 5.0 μm or less, more preferably 3.0 μm or less, even more preferably 2.0 μm or less, and particularly preferably 1.0 μm or less.
[0075] The thickness of the dense layer in the present invention can be calculated by observing a cross section perpendicular to the longitudinal direction of the hollow fiber membrane using a SEM and analyzing the captured image using image processing software. The observation magnification is 2000 times for the first hollow fiber membrane and 5000 times for the second hollow fiber membrane.
[0076] The analysis procedure using the image processing software is as follows. First, the captured image is binarized by determining a threshold value so that the structural parts are bright and the other parts are dark. Next, a perpendicular line is drawn to the tangent of the inner or outer surface of the hollow fiber membrane. Then, for the first hollow fiber membrane, a line with an area of 0.2 μm2 is drawn. 2 In the second hollow fiber membrane, the area is 0.10 μm 2 The areas where the above dark and bright areas are not observed are considered to be dense layers. 2 The area where no dark brightness parts of 0.5 μm or more are observed is defined as an area of 0.10 μm2 where no pores with a diameter of 0.5 μm or more are observed. 2 The regions where the above dark brightness parts are not observed mean regions where pores with a pore size of 0.36 μm or more are not observed. Finally, the average thickness of the dense layer in the observed cross section is calculated.
[0077] More specifically, the thickness is measured by the method described in "Measurement of thickness of dense layer in first hollow fiber membrane" or "Measurement of thickness of dense layer in second hollow fiber membrane" in the Examples described later.
[0078] Examples of methods for controlling the thickness of the dense layer within the above range include a method of controlling the composition of the spinning dope or the spinneret temperature during spinning, etc. More specifically, examples of the method include a method of increasing the content of the main component constituting the hollow fiber membrane in the spinning dope or a method of increasing the amount of a high molecular weight polymer added to increase the viscosity.
[0079] From the viewpoint that the higher the surface porosity of the first hollow fiber membrane, the lower the permeation resistance and the higher the water permeability, the surface porosity of the smaller pore size is preferably 20% or more, more preferably 25% or more, and the surface porosity of the larger pore size is preferably 20% or more. On the other hand, from the viewpoint of maintaining the strength of the hollow fiber membrane, the surface porosity of the smaller pore size is preferably 50% or less, more preferably 40% or less, and the surface porosity of the larger pore size is preferably 40% or less, more preferably 35% or less.
[0080] The porosity of the surface of the second hollow fiber membrane having a smaller pore size is preferably 0.5% to 10% from the viewpoint of preventing the permeation of extracellular vesicles. From the viewpoint of achieving both permeability and water permeability, it is more preferably 1% to 9% and even more preferably 2% to 8%. From the viewpoint of improving water permeability, the porosity of the surface of the second hollow fiber membrane having a larger pore size is preferably 1% to 25%, more preferably 2% to 22%, and even more preferably 3% to 20%.
[0081] The pore ratio of the hollow fiber membrane surface can be calculated by the methods described below in "Measurement of pore ratio of the first hollow fiber membrane surface" and "Measurement of pore ratio of the second hollow fiber membrane surface".
[0082] The inner diameters of the first hollow fiber membrane and the second hollow fiber membrane provided in the extracellular vesicles separation device of the present invention are preferably 150 μm or more and 500 μm or less. The liquid to be treated is often viscous, and when the liquid to be treated is introduced inside the hollow fiber membrane, the pressure loss is large, so the inner diameter of the first hollow fiber membrane is preferably larger than the inner diameter of the second hollow fiber membrane. More specifically, from the viewpoint of increasing a certain effective hollow fiber membrane area without increasing the number of hollow fiber membranes and from the viewpoint of reducing pressure loss during use, the inner diameter of the first hollow fiber membrane is more preferably 200 μm or more, even more preferably 240 μm or more, and particularly preferably 280 μm or more. On the other hand, from the viewpoint of reducing the internal volume of the hollow fiber and reducing the module size, the inner diameter of the first hollow fiber membrane is more preferably 450 μm or less, even more preferably 410 μm or less, and particularly preferably 370 μm or less.
[0083] The second hollow fiber membrane is less affected by pressure loss than the first hollow fiber membrane, so the inner diameter is more preferably 150 μm or more, even more preferably 170 μm or more, and particularly preferably 180 μm or more. From the viewpoint of making the entire device more compact, the inner diameter is more preferably 400 μm or less, even more preferably 350 μm or less, and particularly preferably 300 μm or less.
[0084] An example of a method for adjusting the inner diameter of the hollow fiber membrane within the above range is to adjust the amount of core liquid discharged during spinning.
[0085] The membrane thickness of the first hollow fiber membrane and the second hollow fiber membrane provided in the extracellular vesicle separation device of the present invention is preferably 20 μm or more and 100 μm or less. The membrane thickness can be calculated by the method described in "Inner diameter and membrane thickness measurement" below. From the viewpoint of improving the strength of the hollow fiber membrane, the membrane thickness of the hollow fiber membrane is more preferably 30 μm or more, even more preferably 40 μm or more, and particularly preferably 50 μm or more. On the other hand, from the viewpoint of reducing the permeation resistance of the substance, the membrane thickness of the hollow fiber membrane is more preferably 90 μm or less, even more preferably 80 μm or less, and particularly preferably 70 μm or less.
[0086] An example of a method for adjusting the thickness of the hollow fiber membrane to the above range is to adjust the amount of the spinning dope discharged during spinning.
[0087] The first hollow fiber membrane and the second hollow fiber membrane provided in the extracellular vesicle separation device of the present invention preferably have a three-dimensional mesh structure.
[0088] The term "three-dimensional network structure" refers to a structure in which solid components are spread three-dimensionally in a network shape. The three-dimensional network structure has pores partitioned by the solid components forming the network.
[0089] When treating a liquid containing cells, particularly blood, using the extracellular vesicle separation device of the present invention, it is preferable that the first hollow fiber membrane has high water permeability in order to suppress hemolysis and activation of platelets, etc., due to the load on blood cell components. By using a hollow fiber membrane with high water permeability, the pressure required for filtering the liquid can be reduced, the load on blood components is reduced, and treatment in a short time is also possible. The water permeability can be calculated by the method described below in "Water Permeability Measurement".
[0090] From the above viewpoint, the water permeability of the first hollow fiber membrane is 16000 mL / h / mmHg / m 2 More than 17000mL / h / mmHg / m is preferable. 2 More preferably, the water permeability is 30,000 mL / h / mmHg / m from the viewpoint of suppressing stimulation of blood cells. 2 Less than 25,000 mL / h / mmHg / m is preferable. 2 The following is more preferred:
[0091] The water permeability of the second hollow fiber membrane is 250 mL / h / mmHg / m 2 More than 2000mL / h / mmHg / m 2 From the viewpoint of efficiently separating the extracellular vesicles contained in the first permeate and from the viewpoint of reducing physical stimulation to the extracellular vesicles, the water permeability of the second hollow fiber membrane is preferably 270 mL / h / mmHg / m 2 More preferably, 290 mL / h / mmHg / m 2 More preferably, 1700 mL / h / mmHg / m 2 Less than 1500mL / h / mmHg / m is more preferable. 2More preferably, 1200 mL / h / mmHg / m 2 Even more preferably, 1000 mL / h / mmHg / m 2 The following are particularly preferred:
[0092] The extracellular vesicle separation device of the present invention is equipped with a hollow fiber membrane as a separation membrane. Compared with a flat membrane, a hollow fiber membrane can increase the effective membrane area for filtration even in a module with a small volume, that is, the module can be made smaller. From the viewpoint of increasing the effective membrane area, the cross-sectional shape of the hollow fiber membrane may be a circle, a cross, a star, or the like, and among them, a circle is preferable from the viewpoint of ease of manufacture.
[0093] From the standpoint of strength, it is preferable that the hollow fiber membrane provided in the extracellular vesicle separation device of the present invention does not have any macrovoids, which are oval or teardrop-shaped void regions where a solid portion of the membrane is missing, observed in the cross section of the hollow fiber membrane.
[0094] When the extracellular vesicle separation device of the present invention is used, for example, for blood purification, from the viewpoint of preventing platelet activation, the average depth of the pores on the inner surface of the first hollow fiber membrane is preferably 0.15 μm or more and 7.00 μm or less. In general, when the pore size of the inner surface of the hollow fiber membrane is increased, the depth of the pores on the inner surface tends to become deeper and the surface tends to become rough, so that the stimulation to blood cells increases and platelets are easily activated. Therefore, from the viewpoint of suppressing platelet activation, the average depth of the pores on the inner surface is more preferably 6.00 μm or less, even more preferably 5.00 μm or less, and particularly preferably 4.00 μm or less. On the other hand, from the viewpoint of improving extracellular vesicle permeability, the average depth of the pores on the inner surface is more preferably 0.50 μm or more, even more preferably 1.00 μm or more, and particularly preferably 1.50 μm or more. Examples of methods for controlling the average depth of the pores on the inner surface include a method of adjusting the coagulation value and viscosity of the core liquid.
[0095] <Hydrophilic polymer> The first hollow fiber membrane or the second hollow fiber membrane provided in the extracellular vesicle separation device of the present invention preferably contains a hydrophilic polymer. Examples of the manner in which the hollow fiber membrane contains a hydrophilic polymer include a state in which the hydrophilic polymer is kneaded with the main component of the hollow fiber membrane, inclusion in a closed vesicle structure, attachment (physical adsorption) or chemical fixation. Among these, attachment or chemical fixation is preferable. By containing a hydrophilic polymer in the hollow fiber membrane, adsorption of proteins in a cell-containing solution, particularly blood, and clogging due to adsorption are suppressed, and extracellular vesicle or protein permeability can be improved or blood coagulation can be suppressed.
[0096] "Hydrophilic" refers to the property of interacting with water molecules through electrostatic interaction or hydrogen bonding, and a polymer that interacts with water molecules in this manner, whether it is water-soluble or water-insoluble, is called a hydrophilic polymer.
[0097] "Water-soluble" means a property of dissolving at a rate of 1000 ppm (0.1 g / L) or more in pure water at 25°C, and a hydrophilic polymer having the above property is called a water-soluble hydrophilic polymer. Specific examples of water-soluble hydrophilic polymers include polyalkylene glycols such as polyethylene glycol or polypropylene glycol, polyvinyl alcohol, polyvinylpyrrolidone (hereinafter referred to as "PVP"), dextran sulfate, polyacrylic acid, or ionic hydrophilic polymers such as polyethyleneimine or polyallylamine.
[0098] Examples of hydrophilic polymers that are water-insoluble but interact with water molecules through electrostatic interactions or hydrogen bonds include nonionic hydrophilic polymers such as polyvinyl acetate, polyvinyl propanoate, polyvinyl caprolactam, hydroxyethyl methacrylate, and methyl methacrylate. The above-mentioned hydrophilic polymers may be copolymerized with other monomers.
[0099] The hydrophilic polymer content of the first hollow fiber membrane provided in the extracellular vesicle separation device of the present invention is preferably 5.0% by mass or more and 15.0% by mass or less. From the viewpoint that the presence of the hydrophilic polymer in the hollow fiber membrane improves the wettability of the hollow fiber membrane and improves the water permeability and permeability, the hydrophilic polymer content of the first hollow fiber membrane is more preferably 6.0% by mass or more, even more preferably 7.0% by mass or more, even more preferably 8.0% by mass or more, and particularly preferably 9.0% by mass or more. On the other hand, the lower the hydrophilic polymer content in the hollow fiber membrane, the more the elution during use can be suppressed and the performance change of the hollow fiber membrane can be suppressed, so the hydrophilic polymer content is more preferably 14.5% by mass or less, and particularly preferably 14.0% by mass or less.
[0100] The second hollow fiber membrane may have a hydrophilic polymer content less than that of the first hollow fiber membrane, since the second hollow fiber membrane filters the first permeate filtered by the first hollow fiber membrane. Rather, from the viewpoint of reducing the permeation resistance during filtration, the hydrophilic polymer content is preferably less than that of the first hollow fiber membrane. From these viewpoints, the hydrophilic polymer content of the second hollow fiber membrane is preferably 0.5% by mass or more and 6.5% by mass or less. More preferably, it is 1.0% by mass or more, and even more preferably, it is 1.5% by mass or more. More preferably, it is 6.0% by mass or less, and even more preferably, it is 5.5% by mass or less.
[0101] The method for measuring the hydrophilic polymer content in the hollow fiber membrane must be selected depending on the type of polymer, but in this specification, the value determined by elemental analysis is used.
[0102] In the first hollow fiber membrane, a part of the hydrophilic polymer is preferably insolubilized in the hollow fiber membrane. Examples of a method for insolubilizing the hydrophilic polymer include a method of crosslinking by heat or radiation.
[0103] The "insoluble component" refers to a component that does not dissolve in a good solvent for the main component of the hollow fiber membrane. For example, the insoluble component in the first hollow fiber membrane, which has a polysulfone-based polymer as the main component and contains a hydrophilic polymer, is a component that remains undissolved when dissolved in N,N-dimethylacetamide (hereinafter referred to as "DMAc"), which is a good solvent. The insoluble component also contains a hydrophilic unit that constitutes the hydrophilic polymer.
[0104] The term "unit" refers to a repeating unit in a homopolymer or copolymer obtained by polymerizing a monomer. A unit that has the property of interacting with water molecules through electrostatic interaction or hydrogen bonding is called a hydrophilic unit. For example, when the hydrophilic polymer is PVP, the hydrophilic unit refers to the vinylpyrrolidone portion, which is a repeating unit of PVP.
[0105] The ratio of the mass of the insoluble components to the dry mass of the hollow fiber membrane is preferably 1% by mass or more and 45% by mass or less. From the viewpoint of suppressing elution of the hydrophilic polymer, the ratio of the insoluble components in the first hollow fiber membrane is more preferably 3% by mass or more, even more preferably 5% by mass or more, particularly preferably 6% by mass or more, and most preferably 7% by mass or more. On the other hand, since the lower the degree of crosslinking of the hydrophilic polymer, the higher the effect of suppressing adhesion of proteins and cellular components, it is more preferably 35% by mass or less, even more preferably 25% by mass or less, particularly preferably 20% by mass or less, and most preferably 15% by mass or less.
[0106] The hydrophilic polymer may be appropriately selected depending on the material of the hollow fiber membrane and its affinity with the solvent. Although there is no particular limitation, in the case of polysulfone-based polymers, PVP is preferably used because of its high compatibility.
[0107] It is preferable that a hydrophilic polymer is present on at least one surface of the first hollow fiber membrane or the second hollow fiber membrane included in the extracellular vesicle separation device of the present invention. In particular, as described above, it is preferable to filter the inner surface of the hollow fiber membrane as the contact surface with the treatment liquid, so it is more preferable that a hydrophilic polymer is present at least on the inner surface of the hollow fiber membrane.
[0108] The presence of a hydrophilic polymer on the hollow fiber membrane surface exerts a higher effect of inhibiting adhesion of proteins and cellular components, and reduces the occurrence of clogging of the membrane and blood coagulation such as platelet aggregation. Therefore, the ratio of the hydrophilic polymer on the first hollow fiber membrane surface is preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more. On the other hand, it is preferable that the ratio of the hydrophilic polymer is not too high, because the arrangement of the polymer changes on the membrane surface during use, and changes in the performance of the hollow fiber membrane during use are suppressed. For these reasons, the ratio of the hydrophilic polymer on the hollow fiber membrane surface is preferably 70% by mass or less, and more preferably 60% by mass or less.
[0109] The proportion of hydrophilic polymers on the surface of the hollow fiber membrane can be measured using X-ray photoelectron spectroscopy (hereinafter referred to as "XPS"). The measurement angle is 45°. A measurement angle of 45° detects an area up to a depth of several nm from the surface. The value is the average value of three points. For example, if the main component of the hollow fiber membrane is polysulfone and the hydrophilic polymer is PVP, the proportion of PVP on the surface of the hollow fiber membrane can be calculated from the measured values of the nitrogen amount (d (atomic number %)) and sulfur amount (e (atomic number %)) using the following formula (1). PVP ratio (%) = 100 × (d × 111) / (d × 111 + e × 442) Equation (1)
[0110] The hydrophilic polymer contained in the first hollow fiber membrane or the second hollow fiber membrane of the extracellular vesicle separation device of the present invention preferably has an effect of suppressing adhesion of biological components, particularly proteins, contained in blood, plasma, urine, etc. (hereinafter referred to as "biocompatibility"). In addition, the first hollow fiber membrane or the second hollow fiber membrane may contain multiple types of hydrophilic polymers.
[0111] A biocompatible polymer is one that has a platelet adhesion rate of 50 / 10 3 μm 2 The platelet adhesion test can be performed using a polymer resin or a polymer film whose surface is modified with a polymer, by the method described in the "Platelet Adhesion Test" in the Examples below.
[0112] Examples of biocompatible hydrophilic polymers include hydrophilic polymers such as polyethylene glycol, polyethyleneimine, polyvinyl alcohol, PVP, or derivatives thereof, 2-methacryloyloxyethyl phosphorylcholine (MPC) or derivatives thereof, 2-methoxyethyl acrylate (PMEA) or derivatives thereof, or polymers containing an ester group as described below. Among these, hydrophilic polymers containing an ester group are particularly preferred because they are chemically stable and have little effect on pH. Furthermore, among hydrophilic polymers containing an ester group, hydrophilic polymers containing a monocarboxylic acid vinyl ester unit are particularly preferred. That is, it is particularly preferred that the first hollow fiber membrane or the second hollow fiber membrane provided in the extracellular vesicle separation device of the present invention has a hydrophilic polymer containing a monocarboxylic acid vinyl ester unit as a repeating unit on at least one surface.
[0113] The term "monocarboxylic acid" refers to a compound consisting of one carboxy group and a hydrocarbon group bonded to the carbon atom of the carboxy group, that is, a compound represented by "R-COOH" (R is a hydrocarbon group). The hydrocarbon group R may be either an aliphatic hydrocarbon group or an aromatic hydrocarbon group, but from the viewpoint of ease of synthesis, an aliphatic hydrocarbon group is preferred, and a saturated aliphatic hydrocarbon group is more preferred. Examples of the saturated aliphatic hydrocarbon group include those having a straight chain structure such as an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, or an n-hexyl group, those having a branched structure such as an isopropyl group or a tertiary butyl group, or those having a cyclic structure such as a cyclopropyl group or a cyclobutyl group. The aliphatic chain may contain an ether bond, an ester bond, or the like. Among these, from the viewpoint of the production cost of the carboxylic acid, the saturated aliphatic hydrocarbon group preferably has a straight chain structure or a branched structure, and more preferably has a straight chain structure.
[0114] Examples of monocarboxylic acids in which the hydrocarbon group R is an aromatic hydrocarbon group include benzoic acid and its derivatives, etc. Examples of monocarboxylic acids in which the hydrocarbon group R is a saturated aliphatic hydrocarbon group include acetic acid, propanoic acid, and butyric acid, etc.
[0115] In addition, at least a portion of the hydrogen atoms of the hydrocarbon group R may be optionally substituted. In this case, the substituent is preferably a nonpolar group or a cationic functional group, since this makes it difficult for the protein to be denatured by contact and the associated protein to be adsorbed onto the surface of the hollow fiber membrane to occur.
[0116] A smaller number of carbon atoms in the hydrocarbon group R is preferable in terms of lowering the hydrophobicity of the monocarboxylic acid, reducing the hydrophobic interaction with proteins, and preventing adhesion. Therefore, when R is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, the number of carbon atoms is preferably 20 or less, more preferably 9 or less, and even more preferably 5 or less. On the other hand, when R is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, the number of carbon atoms is 1 or more, but from the viewpoint of improving the mobility of the monocarboxylic acid and further suppressing protein adhesion, 2 or more is preferable. When R is a saturated aliphatic hydrocarbon group, the compound with 1 carbon atom is acetic acid, and the compound with 2 carbon atoms is propanoic acid.
[0117] The term "vinyl carboxylate unit" refers to a repeating unit obtained by polymerizing a vinyl carboxylate monomer, i.e., a repeating unit represented by "-CH(OCO-R)-CH-" (R is a hydrocarbon group). R is the same as described above for monocarboxylic acid, and preferred examples are also as described above.
[0118] Furthermore, from the viewpoint of the balance between hydrophilicity and hydrophobicity, the "vinyl carboxylate unit" is preferably a "monocarboxylate vinyl ester unit" obtained by polymerizing a monocarboxylate vinyl ester monomer.
[0119] Specific examples of the monocarboxylic acid vinyl ester unit in which the hydrocarbon group R is saturated aliphatic include vinyl acetate unit, vinyl propanoate unit, vinyl pivalate unit, vinyl decanoate unit, and vinyl methoxyacetate unit. Since it is preferable that the hydrophobicity is not too strong, preferred examples include vinyl acetate unit (R:CH3), vinyl propanoate unit (R:CH2CH3), vinyl butyrate unit (R:CH2CH2CH3), vinyl pentanoate unit (R:CH2CH2CH2CH3), vinyl pivalate unit (R:C(CH3)3), and vinyl hexanoate unit (R:CH2CH2CH2CH2CH3). Specific examples of the monocarboxylic acid vinyl ester unit in which R is aromatic include vinyl benzoate unit and its substitutes.
[0120] As a method for confirming the structure of the hydrophilic polymer present on the surface of the hollow fiber membrane, the case where the hydrophilic polymer is a monocarboxylate vinyl ester unit is shown as an example. When other polymers are used as the hydrophilic polymer, ion signals derived from the molecular structure specific to the hydrophilic polymer used are measured by appropriately combining time-of-flight secondary ion mass spectrometry (hereinafter referred to as "TOF-SIMS") and other measurement methods.
[0121] The presence of a hydrophilic polymer containing a vinyl monocarboxylate unit on the surface of the hollow fiber membrane can be confirmed by TOF-SIMS measurement. Specifically, first, a peak derived from the carboxylate ion of the saturated aliphatic monocarboxylate is detected by TOF-SIMS measurement, and the structure of the monocarboxylate is clarified by analyzing the mass (m / z) of the peak.
[0122] In TOF-SIMS measurements, for example, Bi was used as the primary ion species. 3++ When using a fluorine atom detector to detect secondary positive ions, the peak at m / z=43.01 is C2H3O + That is, it corresponds to acetic acid (aliphatic chain carbon number: 1). Also, the peak at m / z = 57.03 corresponds to C3H5O +That is, it corresponds to propanoic acid (number of aliphatic chain carbon atoms: 2). Specifically, it can be measured by the method described in "TOF-SIMS measurement" below.
[0123] Furthermore, the proportion of monocarboxylic acid vinyl esters present on the surface of the hollow fiber membrane can be calculated by XPS measurement. When XPS measurement is performed, the peak of carbon derived from the ester group (COO) appears at +4.0 to +4.2 eV from the main peak (around 285 eV) of CHx and CC, which indicates that the above carboxylic acid forms an ester bond. The measurement angle used for XPS is 45°. When measured at a measurement angle of 45°, an area up to a depth of several nm from the surface can be detected.
[0124] The carbon peak derived from the ester group (COO) can be obtained by peak division of the peak appearing at +4.0 to 4.2 eV from the main peak derived from CH or CC of C1s. More specifically, the C1s peak is composed of five components, namely, components derived mainly from CHx, CC, C=C, and CS, components derived mainly from CO and CN, components derived from π-π* satellites, components derived from C=O, and components derived from COO. The amount of carbon derived from the ester group (atomic number %) can be obtained by dividing the peak into the above five components and calculating the ratio of the peak area derived from the ester group to the total peak area derived from carbon. In this case, if the ratio of the peak area derived from the ester group to the total peak area derived from carbon is 0.4% or less, it is judged to be noise and no ester group is present.
[0125] When the extracellular vesicle separation device of the present invention is used for a liquid to be treated that contains cells, particularly blood, proteins in the blood pass through the inside of the first hollow fiber membrane and are separated from blood cell components. In addition, in the second hollow fiber membrane, the first permeate containing proteins sent through flow path B also passes through the inside of the second hollow fiber membrane and is separated from extracellular vesicles. For this reason, it is preferable to suppress protein adhesion to the entire hollow fiber membrane.
[0126] Therefore, it is preferable that the hydrophilic polymer is present throughout the first or second hollow fiber membrane, and it is more preferable that the hydrophilic polymer is a biocompatible hydrophilic polymer. From the above viewpoint, the amount of carbon (atomic percentage) derived from ester groups is preferably 1% or more and 10% or less on both the blood contact surface and the opposite surface. Furthermore, the presence of the hydrophilic polymer throughout the entire hollow fiber membrane can be confirmed by carrying out the above-mentioned TOF-SIMS measurement on the cross section of the hollow fiber membrane.
[0127] From the viewpoint of sufficiently suppressing protein adhesion and further improving protein permeability, the weight-average molecular weight of the biocompatible hydrophilic polymer is preferably 1000 or more, more preferably 5000 or more, even more preferably 10000 or more, and even more preferably 15000 or more. On the other hand, from the viewpoint of the efficiency of introducing the biocompatible hydrophilic polymer into the hollow fiber membrane, the weight-average molecular weight is preferably 1000000 or less, more preferably 500000 or less, and even more preferably 100000 or less. The weight-average molecular weight of the biocompatible hydrophilic polymer can be measured by gel permeation chromatography (hereinafter referred to as "GPC").
[0128] The GPC measurement conditions in the present invention are as follows. Developing solvent: 0.1M LiNO3H2O / MeOH=1 / 1 Column: Tosoh Corporation "TSK-GEL GMPWXL" Flow rate: 0.5mL / mL Column temperature: 40℃ Detection: RI-8010 The calibration curve used is prepared using polyethylene oxide standard samples (0.1 to 1258 kDa) manufactured by Agilent.
[0129] In particular, when a biocompatible hydrophilic polymer is applied to the entire hollow fiber membrane after membrane formation, it is preferable that the molecular weight of the polymer is smaller than the pore size of the hollow fiber membrane and easily passes through.
[0130] A biocompatible hydrophilic polymer, particularly a polymer containing a monocarboxylic acid vinyl ester unit, is preferably a copolymer consisting of a water-soluble hydrophilic unit and a water-insoluble hydrophilic unit, and more preferably the water-insoluble hydrophilic unit contains a monocarboxylic acid vinyl ester unit. When the surface of a hollow fiber membrane is coated with a hydrophilic polymer consisting only of a water-soluble hydrophilic unit such as polyethylene glycol or polyvinyl alcohol, the adhesion suppression effect of proteins and the like may be insufficient. This is thought to be because if the hydrophilicity of the hollow fiber membrane surface is too high, the protein structure becomes unstable, and the adhesion of proteins cannot be sufficiently suppressed.
[0131] In particular, in recent years, attention has been focused on the water surrounding the polymer. Highly hydrophilic polymers have strong interactions with water, and the mobility of the water around the polymer decreases. On the other hand, it is believed that the structure of proteins is stabilized by water called adsorbed water. Adsorbed water is a general term for water in a state also called "unfrozen water" or "intermediate water" (see, for example, p. 542 of Vol. 63, August 2014, Journal of Polymer Science). Therefore, if the state of the adsorbed water of the protein is similar to that of the adsorbed water around the polymer, the structure of the protein is not destabilized, and it is believed that the adhesion of the protein to the hollow fiber membrane surface can be suppressed. In the case of a copolymer consisting of a water-soluble hydrophilic unit and a water-insoluble hydrophilic unit, it is possible to control the state of the adsorbed water around the polymer by selecting the hydrophilic group, the water-insoluble hydrophilic group, and the copolymerization ratio used, and it is believed that the effect of suppressing the adhesion of proteins can be further improved.
[0132] The term "water-soluble hydrophilic unit" refers to a hydrophilic unit in which a polymer of the monomer constituting the unit alone and having a weight average molecular weight of 10,000 to 1,000,000 dissolves in pure water at 25°C at a rate of 1,000 ppm (0.1 g / L) or more.
[0133] The monomer constituting the water-soluble hydrophilic unit is preferably a monomer having a solubility of more than 10 g. Examples of such monomers include vinyl alcohol monomers, acryloylmorpholine monomers, vinylpyridine monomers, vinylimidazole monomers, and vinylpyrrolidone monomers.
[0134] The monomer constituting the water-soluble hydrophilic unit may be two or more of these. Among them, monomers having an amide bond, an ether bond, or an ester bond are preferred because they are not too hydrophilic compared to monomers having a carboxy group or a sulfonic acid group, and are easily balanced with more hydrophobic monomers. In particular, vinylacetamide monomers, vinylpyrrolidone monomers, or vinylcaprolactam monomers having an amide bond are more preferred. Among them, vinylpyrrolidone monomers are even more preferred because the toxicity of the polymer is low. Therefore, it is preferred that the biocompatible hydrophilic polymer present on the surface of the hollow fiber membrane of the present invention further contains a vinylpyrrolidone unit as a hydrophilic unit.
[0135] The monomers constituting the water-insoluble hydrophilic unit include at least monocarboxylic acid vinyl esters, and other monomers include acrylic acid esters, methacrylic acid esters, vinyl-ε-caprolactam, and the like.
[0136] From the viewpoint of further suppressing protein adhesion, the molar fraction of the water-insoluble hydrophilic units in the entire copolymer consisting of the water-soluble hydrophilic units and the water-insoluble hydrophilic units is preferably 10% to 90%, more preferably 20% to 80%, and even more preferably 30% to 70%. In this case, the water-insoluble hydrophilic units may be only monocarboxylic acid vinyl ester units, or may contain other water-insoluble hydrophilic units.
[0137] By setting the molar fraction of the water-insoluble hydrophilic units to 90% or less, the increase in hydrophobicity of the entire copolymer can be suppressed, and protein adhesion can be further suppressed. On the other hand, by setting the molar fraction of the water-insoluble hydrophilic units to 10% or more, the increase in hydrophilicity of the entire copolymer can be suppressed, structural instability and denaturation of proteins can be avoided, and adhesion can be further suppressed.
[0138] The molar fraction can be calculated from the peak area by performing nuclear magnetic resonance (hereinafter referred to as "NMR") measurement. When the molar fraction cannot be calculated by NMR measurement due to overlapping of peaks, the molar fraction may be calculated by elemental analysis.
[0139] As the biocompatible hydrophilic polymer, a copolymer consisting of a vinyl monocarboxylate unit and a vinylpyrrolidone unit is particularly preferred. In this case, the molar ratio of the vinylpyrrolidone unit to the vinyl monocarboxylate unit is preferably 30:70 to 90:10, more preferably 40:60 to 80:20, and further preferably 50:50 to 70:30.
[0140] The arrangement of the units in the copolymer may be, for example, a block copolymer, an alternating copolymer, or a random copolymer. Of these, an alternating copolymer or a random copolymer is preferred because the distribution of hydrophilicity and hydrophobicity in the entire copolymer is small. Among these, a random copolymer is more preferred because it is easy to synthesize.
[0141] Although not essential, in order to prevent the hydrophilic polymer from eluting from the hollow fiber membrane during use for filtration, the hydrophilic polymer is preferably immobilized on the hollow fiber membrane by chemical bonding. The method of immobilization will be described later.
[0142] In the extracellular vesicle separation device of the present invention, the hydrophilic polymer present on the surface of the second hollow fiber membrane that comes into contact with the first permeate also contributes to preventing clogging of the hollow fiber membrane and improving the recovery rate of extracellular vesicles. When filtering the first permeate through the second hollow fiber membrane, it is preferable that the hydrophilic polymer is present on the surface of the second hollow fiber membrane in order to prevent the extracellular vesicles contained in the first permeate from denaturing or adhering to the surface of the second hollow fiber membrane.
[0143] As such a hydrophilic polymer, the above-mentioned hydrophilic polymer having biocompatibility, particularly a hydrophilic polymer containing a monocarboxylic acid vinyl ester unit as a repeating unit, is preferred. That is, it is preferred that the extracellular vesicle separation device has a hydrophilic polymer containing a monocarboxylic acid vinyl ester unit as a repeating unit present on the surface of the second hollow fiber membrane. This is thought to be because the hydrophilic polymer containing a monocarboxylic acid vinyl ester unit as a repeating unit has a weak physicochemical interaction with extracellular vesicles and can suppress the denaturation of extracellular vesicles.
[0144] Since the first hollow fiber membrane and the second hollow fiber membrane have different separation targets, hydrophilic polymers having different biocompatibility may be present on the surfaces of the respective hollow fiber membranes. Since the extracellular vesicle separation device of the present invention is suitably used for a treatment liquid containing cell components (including cell fragments), extracellular vesicles, proteins, etc., it is more preferable that the biocompatible hydrophilic polymers present on the surfaces of the first hollow fiber membrane and the second hollow fiber membrane contain vinyl propanoate units or vinyl acetate units as monocarboxylic acid vinyl ester units.
[0145] As the main component material constituting the hollow fiber membrane, a non-crystalline polymer is preferably used.
[0146] A "non-crystalline polymer" is a polymer that does not crystallize and does not have a heat generation peak due to crystallization in the measurement of a differential scanning calorimeter. Since non-crystalline polymers are prone to structural deformation, it is easy to control the structure in the film thickness direction. A hollow fiber membrane made of a non-crystalline polymer is obtained by inducing phase separation of a membrane-making solution prepared by dissolving the non-crystalline polymer in a solvent using heat or a poor solvent, and removing the solvent components. The non-crystalline polymer dissolved in the solvent has high mobility and aggregates during phase separation, increasing the concentration and forming a dense structure. By changing the speed of phase separation in the film thickness direction, it is possible to obtain a membrane with an asymmetric structure with different pore sizes in the film thickness direction.
[0147] Examples of polymers that can be used as the material for hollow fiber membranes include polyacrylic polymers, polyvinyl acetate polymers, polysulfone polymers, polyethylene polymers, cellulose polymers, and acetylcellulose polymers. Among these, from the viewpoint of membrane formability, etc., amorphous polymers such as polyacrylic polymers, polyvinyl acetate polymers, and polysulfone polymers are preferred. Among these, polysulfone polymers are more preferred because they have high strength and are easy to control the pore size.
[0148] The "polysulfone polymer" has an aromatic ring, a sulfonyl group, and an ether group in the main chain, and for example, a polysulfone polymer represented by the following general formula (I) or (II) is preferably used, but is not limited to these in the present invention. For example, a molecule or polymer may be grafted by introducing a sulfonic acid group into a part of the aromatic ring. In the general formula, n is an integer such as 50 to 80.
[0149] [ka]
[0150] Specific examples of polysulfone include polysulfones such as "Udel" (registered trademark) polysulfone P-1700 and P-3500 (manufactured by Solvay), and "Ultrason" (registered trademark) S3010 and S6010 (manufactured by BASF). The polysulfone used in the present invention is preferably a polymer consisting of only repeating units represented by the above general formula (I) or (II), but may be copolymerized with other monomers as long as the effects of the present invention are not hindered. Although there are no particular limitations, it is preferable that the amount of other copolymerized monomers is 10 mass % or less.
[0151] In addition, by adding a hydrophilic polymer to the membrane-forming solution, the hollow fiber membrane contains the hydrophilic polymer, which improves water wettability and water permeability. Furthermore, it is possible to adjust the viscosity of the membrane-forming solution, i.e., the pore size.
[0152] Methods for incorporating a biocompatible hydrophilic polymer into a hollow fiber membrane include, for example, a method of adding a biocompatible hydrophilic polymer to the raw solution or core liquid during membrane formation, or a method of contacting the surface of the membrane with a biocompatible hydrophilic polymer solution after membrane formation.
[0153] Among these, the method of contacting the membrane with a biocompatible hydrophilic polymer solution after membrane formation is preferred in terms of not affecting the membrane formation conditions. Examples of such methods include a method of immersing the hollow fiber membrane in the biocompatible hydrophilic polymer solution, a method of passing the solution through the membrane, or a method of spraying the solution with a spray or the like. Among these, the method of passing the biocompatible hydrophilic polymer solution through the hollow fiber membrane is preferred because it can impart the biocompatible hydrophilic polymer to the inside of the hollow fiber membrane.
[0154] When a biocompatible hydrophilic polymer solution is passed through a hollow fiber membrane, the concentration of the biocompatible hydrophilic polymer in the solution is preferably 10 ppm or more, more preferably 100 ppm or more, and even more preferably 300 ppm or more, from the viewpoint of more efficiently introducing the biocompatible hydrophilic polymer, while the concentration of the biocompatible hydrophilic polymer in the solution is preferably 100,000 ppm or less, more preferably 10,000 ppm or less, from the viewpoint of suppressing elution from the module.
[0155] The solvent used for preparing the biocompatible hydrophilic polymer solution is preferably water. However, if the desired concentration is not dissolved in water, the biocompatible hydrophilic polymer may be dissolved in an organic solvent that does not dissolve the hollow fiber membrane or a mixed solvent of an organic solvent that does not dissolve the hollow fiber membrane and water. The organic solvent used in the organic solvent or mixed solvent may be, for example, an alcohol solvent such as methanol, ethanol, or propanol, but is not limited thereto.
[0156] The direction of passing the biocompatible hydrophilic polymer solution through the hollow fiber membrane may be from the dense layer side to the coarse layer side of the hollow fiber membrane or from the coarse layer side to the dense layer side. In particular, from the viewpoint of efficiently imparting the biocompatible hydrophilic polymer to the inside of the hollow fiber membrane, passing the solution from the coarse layer side to the dense layer side is preferred. When the hydrodynamic radius of the biocompatible hydrophilic polymer used is larger than the pore size of the dense layer, passing the solution from the coarse layer side to the dense layer side is particularly preferred.
[0157] As described above, the biocompatible hydrophilic polymer is preferably immobilized on the hollow fiber membrane by chemical bonding. Examples of the immobilization method by chemical bonding include a method of contacting the biocompatible hydrophilic polymer with the hollow fiber membrane and then irradiating the membrane with radiation, and a method of introducing reactive groups such as amino groups and carboxy groups into the biocompatible hydrophilic polymer and the hollow fiber membrane surface to be immobilized, followed by condensation.
[0158] <Manufacturing method of hollow fiber membrane> A method for producing a hollow fiber membrane provided in the extracellular vesicle separation device of the present invention includes, for example, a method in which a core liquid or injected gas is flowed through an inner circular tube of a double-tube nozzle and a membrane forming solution is discharged from an outer slit. In this case, the structure of the inner surface of the hollow fiber membrane can be controlled by changing the poor solvent concentration and temperature of the core liquid or adding an additive. On the other hand, the structure of the outer surface side can be controlled by the atmospheric conditions of the dry section from when it is discharged from the nozzle until it enters the coagulation bath, or the temperature and composition of the coagulation bath. Since it is easier to control the structure of the inner surface of the hollow fiber membrane than the outer surface, it is preferable to use a hollow fiber membrane with an asymmetric structure in which the pore size on the inner surface side is larger.
[0159] As the hollow fiber membrane provided in the extracellular vesicle separation device of the present invention, an example of a method for manufacturing a hollow fiber membrane mainly composed of a polysulfone polymer is shown below. As a method for producing a hollow fiber membrane, a non-solvent induced separation method (hereinafter referred to as "NIPS") in which phase separation is induced by a poor solvent, or a thermally induced phase separation method (TIPS) in which phase separation is induced by cooling a high-temperature membrane-forming solution using a solvent with relatively low solubility, etc. can be used. Among them, membrane production by NIPS is particularly preferable.
[0160] One example of a membrane production process using NIPS is a process in which an orifice-type double-cylinder nozzle is used to simultaneously extrude a membrane-producing solution containing a polysulfone polymer from an outer cylinder and a core solution from an inner cylinder, and the two are passed through a dry section, then immersed in a coagulation bath containing a coagulation solution to coagulate the solution, and then washed with warm water.
[0161] The concentration of the polysulfone-based polymer contained in the membrane-forming solution is preferably 10% by mass or more and 25% by mass or less, more preferably 10% by mass or more and 20% by mass or less. If the polysulfone-based polymer concentration is 25% by mass or less, the cohesive force between the polysulfone-based polymers is weakened, the pressure in the membrane-forming process is less likely to increase, and the porosity of the separation membrane surface is more likely to improve. On the other hand, if the polysulfone-based polymer concentration is 10% by mass or more, the strength of the hollow fiber membrane is improved and fiber breakage is less likely to occur.
[0162] By adding a hydrophilic polymer with a relatively low molecular weight (weight average molecular weight 1000 to 200000) to the membrane forming solution, the pore-forming effect is strengthened, the pore rate is improved, and the water permeability of the hollow fiber membrane can be improved. On the other hand, the pore size becomes relatively small.
[0163] In addition, when a hydrophilic polymer with a relatively high molecular weight (weight average molecular weight 200,000 to 1,200,000) is added, the molecular chain is long and the interaction with the polysulfone polymer is large, so that the polymer is likely to remain in the hollow fiber membrane and contributes to improving the hydrophilicity of the hollow fiber membrane. Furthermore, the pore size also becomes relatively large.
[0164] The hydrophilic polymer to be added to the membrane-forming solution may be one type, or two or more types may be mixed, or hydrophilic polymers having different molecular weights may be blended.
[0165] The dissolution temperature for preparing the film-forming solution is preferably 30° C. or higher and 120° C. or lower from the viewpoint of improving solubility and suppressing changes in composition due to thermal denaturation of the polymer and evaporation of the solvent. However, the optimal range may vary depending on the types of polymer and additives used.
[0166] The core liquid in the above membrane-forming process is a liquid present in the hollow portion formed by the hollow fiber membrane during the manufacturing process, and is a solution containing a good solvent for polysulfone-based polymers, such as DMAc, dimethylformamide, N-methylpyrrolidone, dimethylsulfoxide, glycerin, or a mixture thereof. In order to increase the stability of the membrane formation, PVP, a copolymer containing vinylpyrrolidone, polyethylene glycol, polyvinyl alcohol, polyacrylic acid, polyethyleneimine, or the like may be added to the core liquid.
[0167] The composition of the core liquid greatly affects the porosity, pore size, pore shape, and hydrophilic polymer content on the surface of the hollow fiber membrane. Increasing the concentration of the good solvent contained in the core liquid can reduce the aggregation of polysulfone-based polymers, resulting in a hollow fiber membrane with a high porosity and large pore size on the surface of the hollow fiber membrane. Adding a hydrophilic polymer to the core liquid not only makes it possible to localize the hydrophilic polymer on the inner surface of the hollow fiber membrane, but also induces phase separation as a nucleus, resulting in a hollow fiber membrane with a high hydrophilic high molecular weight on the inner surface of the hollow fiber membrane and a high porosity.
[0168] In the membrane-forming process, when the surface that comes into contact with the treated liquid is the inner surface, the temperature of the core liquid is preferably the same as or 5° C. or more lower than the temperature of the membrane-forming raw liquid, and more preferably 10° C. or more lower.
[0169] The dew point temperature of the dry section in the membrane production process can control the phase separation reaction of the membrane-forming solution by controlling the dew point temperature, and it has a large effect on the outer surface of the hollow fiber membrane in particular. For example, a dense layer can be formed by supplying moisture to the outer surface of the hollow fiber membrane. When the purpose is to separate extracellular vesicles as in the device of the present invention, the dew point temperature is preferably adjusted to 20°C or higher and 40°C or lower.
[0170] The length of the dry section in the membrane production process determines the time from the formation of holes on the surface of the hollow fiber membrane to solidification, and is preferably 10 mm or more and 400 mm or less. If the length of the dry section is 10 mm or more, the pore size on the surface of the hollow fiber membrane becomes large. On the other hand, if the length of the dry section is 400 mm or less, thread shaking is less likely to occur in the membrane production process, and the occurrence of thread breakage can be suppressed.
[0171] The coagulation solution in the membrane-forming process refers to a poor solvent for the polysulfone-based polymer, and examples thereof include alcohol, water, and glycerin, with water being preferred.
[0172] The coagulation bath temperature in the membrane production process is preferably 30°C or higher and 100°C or lower, more preferably 60°C or higher and 90°C or lower. The coagulation bath temperature greatly affects the pore size on the surface of the hollow fiber membrane and the water permeability of the hollow fiber membrane. If the coagulation bath temperature is 30°C or higher, the pore size on the outer surface of the hollow fiber membrane becomes large, the permeable particle size becomes large, and the water permeability improves. On the other hand, if the coagulation bath temperature is 100°C or lower, the pore ratio on the surface of the hollow fiber membrane becomes low, and the strength of the hollow fiber membrane is easily improved.
[0173] In addition to the coagulation solution such as water, a good solvent for the polysulfone polymer may be added to the coagulation bath in the membrane production process at a ratio of 1% by mass to 10% by mass. By adding the good solvent, the diffusion speed of the coagulation solution during desolvation can be reduced, and the structure of the outer surface side of the hollow fiber membrane can be made suitable. When the concentration of the good solvent is 1% by mass or more, it becomes easy to control the pore size and dense layer thickness of the outer surface of the hollow fiber membrane. On the other hand, when the concentration of the good solvent is 10% by mass or less, desolvation of the hydrophilic polymer is moderately promoted, and the strength of the hollow fiber membrane is likely to be improved.
[0174] In the membrane production process, hot water washing means exposing the hollow fiber membrane after immersion in the coagulation bath to hot water of 60°C or higher for 1 minute or more. Examples of methods for exposing the hollow fiber membrane to hot water include immersion and shower spraying. Hot water washing can remove excess solvent and hydrophilic polymer remaining in the hollow fiber membrane. When a hydrophilic polymer is added to the core liquid, it is preferable to cut the hollow fiber membrane to a certain length and divide it into small portions before additional hot water washing in order to effectively remove excess hydrophilic polymer and improve the water permeability of the hollow fiber membrane.
[0175] As a specific example, it is preferable to wind up the hollow fiber membrane after hot water washing, cut it into 400 mm pieces, and divide the hollow fiber membrane bundle into smaller pieces, wrap them in gauze, and perform additional hot water washing for 1 hour to 5 hours in hot water of 70° C. or higher. If hot water washing is performed with hot water of 90° C. or higher, excess hydrophilic polymer that is not supported or chemically fixed on the hollow fiber membrane and hydrophilic polymer that filled the pores of the hollow fiber surface membrane are dissolved in the hot water, and therefore these can be removed.
[0176] Although the hollow fiber membrane after the above-mentioned hot water washing is in a wet state, it is preferable to carry out a drying step from the viewpoint of further stabilizing the water permeability of the hollow fiber membrane. The temperature of the drying step is preferably 100°C or higher in order to evaporate water. When drying a hollow fiber membrane mainly composed of a polysulfone-based polymer, the temperature of the drying step is preferably 180°C or lower so as not to exceed the glass transition point of the polysulfone-based polymer.
[0177] In the extracellular vesicle separation device of the present invention, it is preferable to suppress the elution of hydrophilic polymers from the hollow fiber membrane into the permeate and non-permeate liquids. In order to suppress the elution of hydrophilic polymers, it is preferable to crosslink the obtained hollow fiber membrane by heating or irradiating it with radiation.
[0178] In the thermal crosslinking in which the hollow fiber membrane is heated, the hydrophilic polymers present in the hollow fiber membrane are crosslinked with each other. From the viewpoint of crosslinking the hydrophilic polymers with each other and preventing decomposition reactions, the temperature of the thermal crosslinking is preferably 120° C. or more and 250° C. or less, and more preferably 130° C. or more and 200° C. or less. The time of the thermal crosslinking is preferably 1 hour or more and 10 hours or less, and more preferably 3 hours or more and 8 hours or less.
[0179] In radiation crosslinking in which radiation is irradiated to the hollow fiber membrane, a hydrophilic polymer or the above-mentioned hydrophilic polymer having biocompatibility is crosslinked with a polysulfone-based polymer. From the viewpoint of promoting the crosslinking reaction and making it difficult for a decomposition reaction to occur, the radiation exposure dose is preferably 5 kGy to 75 kGy, more preferably 10 kGy to 50 kGy. For example, α-rays, β-rays, γ-rays, X-rays, ultraviolet rays, electron beams, etc. can be used as the radiation to be irradiated.
[0180] When crosslinking a biocompatible hydrophilic polymer to a hollow fiber membrane by radiation, radiation is applied to the hollow fiber membrane in the module in a state where the hollow fiber membrane is in contact with a solution in which a biocompatible hydrophilic polymer is dissolved, or in a state where the solution in the hollow fiber membrane module is removed after the biocompatible hydrophilic polymer is introduced to the surface, or in a state where the hollow fiber membrane is dried. Radiation crosslinking is preferred because it can achieve sterilization of the hollow fiber membrane module at the same time as immobilizing the biocompatible hydrophilic polymer. For sterilization, it is preferable for the radiation to have a certain degree of material permeability, and therefore, among the above-mentioned radiations, β-rays, γ-rays, X-rays, or electron beams are more preferred.
[0181] In addition, an antioxidant may be used to suppress crosslinking reactions of biocompatible hydrophilic polymers caused by radiation exposure. An antioxidant is a substance that has the property of easily donating electrons to other molecules.
[0182] Examples of antioxidants include, but are not limited to, water-soluble vitamins such as vitamin C, polyphenols, and alcohol solvents such as methanol, ethanol, or propanol. These antioxidants may be used alone or in combination of two or more. When safety is a consideration, antioxidants with low toxicity such as ethanol or propanol are preferably used.
[0183] <Hollow fiber membrane module> The first module of the extracellular vesicle separation device of the present invention contains a first hollow fiber membrane, and the second module contains a second hollow fiber membrane.
[0184] Methods for producing a hollow fiber membrane module include, for example, a method in which the hollow fiber membrane is fixed to a case while being centrifuged, or a method in which the hollow fiber membrane is formed into a U-shape and only the opening side of the hollow fiber membrane is fixed to the case.
[0185] As an example, a method for manufacturing a hollow fiber membrane module 201 shown in Fig. 2 will be described. First, the hollow fiber membranes are cut to the required length, and the required number are bundled together and placed in a cylindrical case 202 equipped with a nozzle 205. Then, both ends are temporarily capped, and potting material 203 is placed on both ends of the hollow fiber membranes. In this case, the potting material is placed while rotating the module with a centrifuge, which is a preferred method because the potting material can be filled evenly. After the potting material has solidified, both ends of the hollow fiber membranes are cut so that both ends are open. A hollow fiber membrane module is obtained by attaching headers 204 equipped with ports for inflow and outflow of the liquid to be treated to both ends of the case.
[0186] The hollow fiber membranes may be provided with crimps or spacer fibers, since this facilitates uniform filling of the potting material into the hollow fiber membrane bundle. When the liquid to be treated is brought into contact with the outer surface side, the hollow fiber membranes may be provided with crimps or spacer fibers, so that the liquid to be treated can be brought into contact with the entire hollow fiber membrane bundle.
[0187] The membrane area of the hollow fiber membrane contained in the module is 0.1 m 2 More than 3.0m 2 From the viewpoint of processing capacity, the membrane area is preferably 0.15 m 2 More preferably, 0.2m or more 2 More preferably, 0.25m or more 2 On the other hand, the membrane area is preferably 3.0 m or less because the module size can be reduced and handling is easy. 2 Less than 2.5m is preferable. 2 Less than 2.0m is more preferable. 2 The following is particularly preferred. In addition, since clogging is likely to occur in the second module that separates extracellular vesicles, it is preferred that the membrane area of the second module is larger than the membrane area of the first module.
[0188] There is no particular limitation on the inner diameter of the module, but in order to easily achieve the above-mentioned preferred membrane area range and to facilitate easy handling of the module, the inner diameter is preferably 1.0 cm or more and 9.0 cm or less, more preferably 1.5 cm or more and 7.0 cm or less, and even more preferably 2.0 cm or more and 5.5 cm or less.
[0189] From the viewpoint of ease of handling of the module, the length of the module is preferably 10.0 cm or more and 40.0 cm or less, more preferably 15.0 cm or more and 35.0 cm or less, and even more preferably 20.0 cm or more and 30.0 cm or less.
[0190] Furthermore, the ratio of the volume of the hollow fiber membrane to the internal volume of the module, i.e., the filling rate, is preferably 30% or more and 70% or less, more preferably 35% or more and 65% or less, even more preferably 40% or more and 60% or less, and particularly preferably 45% or more and 55% or less, from the viewpoints of the ease of flow of the treated liquid within the module and effective utilization of the module volume.
[0191] The above-mentioned packing ratio can be calculated by the following formulas (2) to (4). Filling rate (%) = (cross-sectional area of hollow fiber membrane) × (number of hollow fiber membranes) / (cross-sectional area of module) × 100 Formula (2) Cross-sectional area of hollow fiber membrane (cm 2 )={(hollow fiber membrane outer diameter) / 2} 2 × Pi Equation (3) Module cross-sectional area (cm 2 )={(module inner diameter) / 2} 2 × Pi Equation (4)
[0192] The first module and the second module of the extracellular vesicle separation device of the present invention may be integrated. In this case, an opening communicating the inside of the first module with the inside of the second module becomes flow path B. In addition, a state in which the first hollow fiber membrane and the second hollow fiber membrane are housed in the same case separated by a partition is also included in the shape in which the first module and the second module are integrated.
[0193] The first module and the second module in the extracellular vesicles separation device of the present invention may be U-shaped modules as described above. The U-shaped module is a module in which the hollow fiber membrane is folded back into a U shape, both ends of the hollow fiber membrane bundle are bonded to a case with resin, and both ends of the hollow fiber membrane are open. The U-shaped module is easy to handle and is suitable for research, testing, and inspection purposes. When the U-shaped module is used to separate extracellular vesicles from the liquid to be treated, full-flow filtration is performed.
[0194] For example, dead end filtration is performed in a U-shaped first module, and the first permeate is led to a second module that is not U-shaped through flow path B. Then, cross-flow filtration is performed in the second module, whereby the first permeate can be separated into a second retentate containing extracellular vesicles of a specific size and a second permeate not containing extracellular vesicles of a specific size.
[0195] In addition, by performing cross-flow filtration in a first module that is not U-shaped, directing the first permeate through flow path B to a second module that is U-shaped, performing total filtration in the second module, and mixing the resulting first non-permeate and second permeate, it is possible to separate only extracellular vesicles of a specific size from the treatment liquid.
[0196] By using the module having the structure shown in Fig. 2, the first module and the second module can be connected in various ways. Below, configuration examples of the extracellular vesicle separation device of the present invention will be described with reference to Figs. 3 to 6.
[0197] 3, the first permeated liquid is guided to flow path B (103b) from a nozzle on the side closer to the connection with flow path A (103a) of the first module 101, and connected to the second module 102. In the second module 102, the second permeated liquid is guided to flow path C (103c) from a nozzle on the side farther from flow path B (103b), and is then guided to flow path D (103d) and mixed with the first non-permeated liquid.
[0198] 4, the first permeated liquid is guided to flow path B (103b) from a nozzle on the side farther from the connection to flow path A (103a) of the first module 101, and is connected to the second module 102. In the second module 102, the second permeated liquid is guided to flow path C (103c) from a nozzle on the side farther from flow path B (103b), and is then guided to flow path D (103d) and mixed with the first non-permeated liquid.
[0199] 5, the first permeated liquid is guided from two nozzles of the first module 101 to flow path B (103b) and connected to the second module 102. In the second module 102, the second permeated liquid is guided from the nozzle farther from flow path B (103b) to flow path C (103c), and then guided to flow path D to be mixed with the first non-permeated liquid.
[0200] 6, the first permeated liquid is guided from two nozzles of the first module 101 to flow path B (103b) and connected to the second module 102. In the second module 102, the second permeated liquid is guided from the nozzle closer to flow path B (103b) to flow path C (103c), and then guided to flow path D to be mixed with the first non-permeated liquid.
[0201] <Extracellular vesicles and solutions containing extracellular vesicles> The type of extracellular vesicles in the present invention is not particularly limited, but it is preferable that the extracellular vesicles have at least one surface marker selected from the group consisting of phosphatidylserine, CD9, CD63, CD81, TyA and Clq as a surface marker. Among the above markers, phosphatidylserine and CD9 are preferred surface markers for extracellular vesicles. Phosphatidylserine is a type of phospholipid, and is present only on the inside of the cell membrane, but is also present on the outside of the extracellular vesicles. CD9 is a type of four-transmembrane protein called tetraspanin.
[0202] Extracellular vesicles in a measurement sample solution can be detected and quantified by ELISA (Enzyme-Linked Immuno-Sorbent Assay) using phosphatidylserine and CD9 as markers. In this case, it is preferable to use an antibody that binds to phosphatidylserine as the capture antibody on the plate side and an antibody that binds to CD9 as the labeled detection antibody.
[0203] The extracellular vesicle separation device of the present invention can be suitably used for the treatment of diseases. The target disease is not particularly limited, but the device can be suitably used for a treatment method for removing extracellular vesicles from the blood of a patient with sepsis, an autoimmune disease, a chronic liver disease, or the like.
[0204] The size and type (surface marker) of extracellular vesicles to be removed from the patient's blood vary depending on the disease. In the case of sepsis, since there are a large amount of extracellular vesicles with an inflammatory enhancing effect in the blood, it is preferable to remove them without limiting the surface marker or size. In the case of autoimmune diseases, since removing all extracellular vesicles in the blood may affect the homeostasis of the human body, it is preferable to remove extracellular vesicles with a size of 50 nm to 150 nm. In the case of chronic liver diseases, it is preferable to remove extracellular vesicles with a size of 150 nm to 300 nm, which mainly contribute to the deterioration of the pathology.
[0205] The size of extracellular vesicles can be measured by a nanoparticle tracking method. An example of a device capable of measuring by the nanoparticle tracking method is the "NanoSight" manufactured by Quantum Design.
[0206] The extracellular vesicle separation device and the method for separating extracellular vesicles of the present invention can be suitably used for purifying a liquid to be treated that contains extracellular vesicles, and a solution containing extracellular vesicles with higher purity and concentration can be obtained. If the second non-permeated liquid is collected without being discarded, the extracellular vesicles can be collected. In other words, the solution containing extracellular vesicles of the present invention is preferably a solution containing extracellular vesicles obtained by the device for separating extracellular vesicles or the method for separating extracellular vesicles of the present invention.
[0207] The solvent of the extracellular vesicle-containing solution is not particularly limited, and examples thereof include water, ethanol, and dimethyl sulfoxide. These solvents may also be used in combination. Since the extracellular vesicles are samples derived from living organisms, it is more preferable to use a buffer solution whose main component is water. Examples of the buffer solution include phosphate buffer, phosphate buffered saline, acetate buffer, Tris buffer, and citrate buffer.
[0208] The second non-permeated liquid obtained by the extracellular vesicle separation device of the present invention contains only extracellular vesicles of a specific size. In other words, it is a purified solution of extracellular vesicles. The purified solution can be suitably used for, for example, examination, treatment, beauty, or anti-aging. Since extracellular vesicles contain information transmitters such as proteins and nucleic acids, a lot of information about the state inside the body can be obtained, and they can be an effective subject for examination. For example, cancer cells are known to release extracellular vesicles that act to weaken the attack of immune cells that try to attack them, and the presence or absence of cancer can be examined using an extracellular vesicle-containing solution obtained by purifying body fluid collected from a subject.
[0209] In addition, since the activity of cells can be changed by the signaling substances in the extracellular vesicles, the extracellular vesicles can also be used for treatment. For example, in contrast to the previous example, a method can be considered in which the extracellular vesicles act to instruct immune cells to attack cancer cells. Furthermore, beauty and anti-aging effects can be expected by promoting the breakdown of waste products and metabolism in cells. As a method for administering the extracellular vesicle-containing solution, injection or drip infusion is suitable for treatment and anti-aging purposes, and application as a cosmetic product is suitable for beauty purposes.
[0210] As described above, solutions containing extracellular vesicles have a variety of applications, and when preparing solutions containing extracellular vesicles as pharmaceutical or cosmetic raw materials, it is preferable that the concentration of extracellular vesicles in the solution is high in order to obtain the desired effect and to reduce production costs by reducing the production scale. By using the method for separating extracellular vesicles of the present invention, a solution containing extracellular vesicles at a high concentration can be obtained. On the other hand, if the concentration of extracellular vesicles is too high, the extracellular vesicles tend to aggregate.
[0211] From these viewpoints, the number concentration of extracellular vesicles in the extracellular vesicle-containing solution obtained by the extracellular vesicle separation method of the present invention is 6.0 × 10 9 pcs / mL or more, 1.4×10 12 The number of cells / mL or less is preferably 1.5×10 10 pcs / mL or more, 1.2×10 12 More preferably, the number is 3.0×10 10 pcs / mL or more, 1.0×10 12 It is particularly preferable that the number is less than or equal to 1 / mL.
[0212] In addition, from the viewpoint of preventing deterioration, the extracellular vesicle-containing solution of the present invention preferably contains an extracellular vesicle stabilizer having a weight-average molecular weight of 10,000 or more and 1,000,000 or less. In this case, the extracellular vesicle stabilizer is preferably a polymer containing at least one repeating unit selected from the group consisting of 2-methacryloyloxyethyl phosphorylcholine, vinyl alcohol, vinylpyrrolidone, methoxyalkylene glycol monomethacrylate, and 2-hydroxyethyl methacrylate. Among these, a polymer of 2-methacryloyloxyethyl phosphorylcholine is particularly preferred.
[0213] The storage form of the collected extracellular vesicles is not limited to the above-mentioned solution state. For example, they may be in a state in which water has been removed by freeze-drying. The form of the extracellular vesicles in the state in which water has been removed may be in the form of a powder, or may be in the form of a tablet in combination with other substances. EXAMPLES
[0214] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0215] <Preparation of hollow fiber membrane module> Ten hollow fiber membranes were packed into a case with a diameter of about 5 mm and a length of about 17 cm. Both ends were potted with Konishi Co., Ltd.'s epoxy resin-based chemical reaction adhesive "QuickMender" (registered trademark), and the ends were cut to open, producing a hollow fiber membrane module with an effective length of 12 cm.
[0216] <Particle transmittance measurement> The particle transmittance of the hollow fiber membrane was measured using commercially available polystyrene latex beads (hereinafter referred to as "LB") with average particle sizes of 0.02 μm, 0.15 μm, 0.20 μm, and 1.00 μm. The LB with an average particle size of 0.15 μm was purchased from the National Institute of Advanced Industrial Science and Technology's Reference Materials Center, and the LB with average particle sizes of 0.02 μm, 0.20 μm, and 1.00 μm was "Sulfate Latex Beads" manufactured by Thermo Fisher. The relationship between the concentration of the LB suspension and the turbidity was calculated in advance from the absorbance at a wavelength of 260 nm measured by ultraviolet-visible spectroscopy.
[0217] The turbidity of the filtrate filtered through the hollow fiber membrane was measured, and the particle transmittance was calculated by the following formula (5). The liquid to be treated was diluted with pure water to an LB concentration of 0.02 mass% (200 ppm). The measurement was performed by flowing the treatment liquid from the inside to the outside of the hollow fiber membrane at a pressure of 13.3 kPa, calculating the average value of the values measured for two different hollow fiber membrane modules, and rounding off the value to the nearest whole number. Particle transmittance (%) = {(turbidity of filtrate) / (turbidity before treatment)} × 100 Equation (5)
[0218] <Water permeability measurement> The inside of the hollow fiber membrane module prepared by the method described in "Preparation of hollow fiber membrane module" was washed with distilled water for 30 minutes. A water pressure of 150 mmHg was applied to the inside of the hollow fiber membrane, and the filtration amount per unit time flowing out to the outside of the hollow fiber membrane was measured. The water permeability (UFR) was calculated using the following formula (6), and the value was rounded off to the first decimal place. Water permeability (mL / h / mmHg / m 2 )=Qw / (P×T×A) Equation (6) where Qw is the filtration volume (mL), T is the outflow time (h), P is the pressure (mmHg), and A is the inner surface area of the hollow fiber membrane (m 2 ),.
[0219] The inner surface area A of the hollow fiber membrane was calculated by multiplying the inner diameter of the hollow fiber by pi and the length of the part of the hollow fiber used in the water permeability measurement that was effective for the measurement.
[0220] <Hydrophilic polymer content measurement> The nitrogen atom content of the hollow fiber membrane was measured by elemental analysis to calculate the hydrophilic polymer content in the hollow fiber membrane. The hollow fiber membrane was freeze-pulverized and then dried under reduced pressure at room temperature (25°C) for 2 hours to prepare a measurement sample. The measurement device and measurement conditions are as follows. The measurement was performed three times, and the average value was used as the measured value.
[0221] Measuring device: Trace nitrogen analyzer ND-100 type (manufactured by Mitsubishi Chemical Corporation) Electric furnace temperature (horizontal reactor) Pyrolysis part: 800℃ Catalyst part: 900℃ Main O2 flow rate: 300mL / min Sub-O2 flow rate: 300mL / min Ar flow rate: 400mL / min Sens.: Low
[0222] The molar mass of the nitrogen atom is 14 g / mol, and the molar mass of the repeating unit of PVP is 111 g / mol. Therefore, the hydrophilic polymer content (mass%) was calculated from the amount of nitrogen atoms (μg / g) contained in the hollow fiber membrane per unit mass determined by elemental analysis using the following formula (7), and the value was rounded off to one decimal place. Hydrophilic polymer content (mass%) = nitrogen atom amount contained in hollow fiber membrane × 111 / 14 × 100 Equation (7)
[0223] In this example, the main component of the hollow fiber membrane is polysulfone, and the hydrophilic polymer is PVP only, PVP and vinyl acetate / vinylpyrrolidone copolymer, or PVP and vinyl propanoate / vinylpyrrolidone copolymer. However, the hydrophilic polymer content can be determined in a similar manner by appropriately changing the elements quantified by elemental analysis and the calculation formula according to the type of polymer used.
[0224] <Measurement of the proportion of insoluble components> Approximately 1 g of dried hollow fiber membrane was weighed out and placed in an Erlenmeyer flask, and 40 mL of DMAc was added as a good solvent for the hollow fiber membrane, followed by stirring with a stirrer at room temperature (25°C) for 2 hours. Next, centrifugation was performed at 2500 rpm to precipitate the insoluble components, and the supernatant was removed. 10 mL of DMAc was added to the insoluble components obtained, and the insoluble components were washed by stirring again with a stirrer, centrifuged, and the supernatant was removed. This series of operations was repeated three times. Finally, the supernatant was removed, and the insoluble components obtained were freeze-dried.
[0225] The mass of the insoluble components was measured, and the ratio of the insoluble components to the total mass of the hollow fiber membrane was calculated according to the following formula (8). The ratio of the insoluble components was calculated by rounding off to one decimal place. Percentage of insoluble components (mass%) = mass of insoluble components / mass of hollow fiber membrane × 100 Equation (8)
[0226] In this example, although the case where the main component of the hollow fiber membrane is polysulfone and the hydrophilic polymer is only PVP, PVP and vinyl acetate / vinyl pyrrolidone copolymer, or PVP and vinyl propionate / vinyl pyrrolidone copolymer has been described, depending on the type of polymer used, by appropriately changing the good solvent for dissolving the hollow fiber membrane, the ratio of the insoluble component can be similarly determined.
[0227] <TOF-SIMS measurement> The hollow fiber membrane was cut into a semi-cylindrical shape with a single-edge blade, and three points on different locations of the inner surface or outer surface of the hollow fiber membrane were measured. The measurement sample was rinsed with ultrapure water, dried at room temperature and 0.5 Torr for 10 hours, and then used for measurement. The measurement apparatus and conditions are as follows.
[0228] Measurement apparatus: TOF.SIMS 5 (manufactured by ION-TOF) Primary ion: Bi 3++ Primary ion acceleration voltage: 30 kV Pulse width: 5.9 ns Secondary ion polarity: negative Number of scans: 64 scan / cycle Cycle Time: 140 μs Measurement range: 200 μm × 200 μm Mass range (m / z): 0 - 1500.
[0229] From the obtained spectrum of mass m / z, the presence or absence of carboxylic acid ions on the surface of the hollow fiber membrane was confirmed. However, when the intensity of carboxylic acid ions relative to the total secondary ion intensity was 0.4% or less, it was judged as noise and it was considered that carboxylic acid was absent.
[0230] <Measurement of the ratio of hydrophilic polymer on the surface of the hollow fiber membrane> When measuring the inner surface of the hollow fiber membrane, the hollow fiber membrane was fixed on double-sided tape, and the attached hollow fiber membrane was cut into a semi-cylindrical shape with a single-edged blade to expose the inner surface and measure it. When measuring the outer surface of the hollow fiber membrane, the outer surface of the hollow fiber membrane fixed on the double-sided tape was measured as it was. XPS measurement was performed on the surface of the hollow fiber membrane under the following conditions, and the integrated value of the peak intensity was obtained.
[0231] Equipment: PHI Quantera SXM (ULVAC-PHI, Inc.) Excitation X-ray: Monochromatic Al Kα 1.2 Rays (1486.6 eV) X-ray diameter: 100μm Photoelectron detection angle: 45° Horizontal axis correction: C1s main peak (CHx, CC) is corrected to 284.6 eV Smoothing: 9-point smoothing
[0232] When the main component of the hollow fiber membrane is polysulfone and the hydrophilic polymer is PVP, the proportion of vinylpyrrolidone units on the hollow fiber membrane surface was calculated using the following formula (9). In this case, when the only hydrophilic polymer present on the hollow fiber membrane surface is PVP, the proportion of the vinylpyrrolidone units is the proportion of PVP. Proportion of vinylpyrrolidone units (%) = 100 × (d × 111) / (d × 111 + e × 442 + c × 86) Formula (9) Here, d is the number of nitrogen atoms in %, e is the number of sulfur atoms in %, and c is the number of carbon atoms derived from ester groups in %.
[0233] On the other hand, when a hydrophilic polymer containing a vinyl acetate unit, for example, is present as a hydrophilic polymer containing a monocarboxylate vinyl ester unit on the surface of the hollow fiber membrane, the proportion of the vinyl acetate unit on the surface of the hollow fiber membrane was calculated using the following formula (10). Percentage of vinyl acetate units (%) = 100 × (c × 86) / (d × 111 + e × 442 + c × 86) Equation (10)
[0234] Therefore, when the hydrophilic polymer is a copolymer of vinylpyrrolidone and vinyl acetate, the proportion of the hydrophilic polymer present on the surface of the hollow fiber membrane can be expressed by the sum of the above formula (9) and formula (10).
[0235] <Inner diameter and film thickness measurement> The membrane thickness of 16 randomly selected hollow fiber membranes was measured at 1000x magnification using a microwatcher (digital microscope RH-2000, manufactured by Hirox Corporation), and the average value was taken as the membrane thickness.
[0236] The inner diameter of the hollow fiber membrane was calculated by the following formula (11). The outer diameter of the hollow fiber membrane was determined by measuring the outer diameters of 16 randomly selected hollow fiber membranes with a laser displacement meter (e.g., LS5040T; KEYENCE Corporation) and using the average value. Inner diameter of hollow fiber membrane (μm) = outer diameter of hollow fiber membrane - (2 × membrane thickness) Equation (11)
[0237] <Measurement of surface pore size in the first hollow fiber membrane> The first hollow fiber membrane was immersed in water for 5 minutes to wet it, then frozen with liquid nitrogen and freeze-dried to use as a measurement sample. The hollow fiber membrane was cut into a semi-cylindrical shape so that the inner surface was exposed. The inner surface of the hollow fiber membrane was observed at a magnification of 1500 times and the outer surface at a magnification of 3000 times using an SEM (S-5500, Hitachi High-Technologies Corporation), and the images were imported into a computer. The size of the imported image was 640 pixels x 480 pixels.
[0238] The number of holes and the area of each hole were measured using image processing software (ImageJ (version 1.52), developed by the National Institutes of Health, USA) for holes in the range of 40 μm × 40 μm on the inner surface of the hollow fiber membrane and holes in the range of 20 μm × 20 μm on the outer surface. Measurements were repeated in the range of 40 μm × 40 μm or 20 μm × 20 μm until the total number of measured holes reached 50 or more, and data was added. If holes were observed twice in the depth direction, the exposed part of the deeper hole was measured. If a part of a hole was outside the measurement range (field of view of the SEM image), that hole was excluded. The SEM image was binarized to obtain an image in which the pores were black and the structure part was white. If the pores and structure part could not be clearly binarized due to the difference in contrast in the analysis image, the pores were painted black before image processing, and the sum of the pore number and hole area was calculated. At this time, in order to reduce noise, holes with an area of 5 or less consecutive pixels were excluded from the data.
[0239] The pore size was calculated from the sum of the calculated areas of each pore using the following formula (12), and was rounded off to two decimal places. Pore diameter (μm)={(S / a) / pi} 1 / 2 ×2...Equation (12) where a is the number of measured holes, S is the sum of the measured hole areas (μm 2 ),.
[0240] <Measurement of surface pore size in the second hollow fiber membrane> As with the first hollow fiber membrane, a hollow fiber membrane that had been immersed in water and then freeze-dried with liquid nitrogen was used as the measurement sample. After cutting the hollow fiber membrane into a semi-cylindrical shape, the inner surface of the hollow fiber membrane was observed at 50,000 times magnification using an SEM, and the outer surface was observed at 3,000 times magnification, and the images were imported into a computer. The size of the imported image was 640 pixels x 480 pixels. As with the first hollow fiber membrane, the number of holes and the area of each hole were measured using image processing software for holes in the range of 1.2 μm x 1.2 μm on the inner surface of the hollow fiber membrane and for holes in the range of 20 μm x 20 μm on the outer surface, and the area was calculated using the above formula (12).
[0241] <Measurement of the average depth of pores in the first hollow fiber membrane> As in the above-mentioned "Surface pore size measurement of the first hollow fiber membrane," the hollow fiber membrane was cut into a semi-cylindrical shape, and the inner surface of the exposed hollow fiber membrane was observed at a magnification of 150x using a laser microscope (Keyence Corporation, VK-9710).
[0242] The results were analyzed using the shape analysis software "VK ANALYZER" mounted on a laser microscope to calculate the average depth of the holes on the inner surface. The analysis was performed in "line roughness measurement" mode, by specifying a measurement line that crossed the center of the observation screen from left to right, and calculating the average height (depth) according to the measurement method standard "JIS B0601:2001 (ISO 4287:1997)". Analysis was performed on 10 images, and the average of the obtained values was taken as the average hole depth.
[0243] <Measurement of pore ratio on the surface of the first hollow fiber membrane> As in the above-mentioned "Surface pore size measurement in the first hollow fiber membrane", the inner surface of the first hollow fiber membrane was observed at a magnification of 1500x and the outer surface at a magnification of 3000x using an SEM (S-5500, Hitachi High-Technologies Corporation), and the images were imported into a computer. The size of the imported image was 640 pixels x 480 pixels.
[0244] The SEM image was cut into a range of 40 μm × 40 μm for the inner surface and 20 μm × 20 μm for the outer surface, and image analysis was performed using image processing software. A threshold was determined by binarization processing so that the structural part was bright and the other parts were dark, and an image was obtained in which the bright parts were white and the dark parts were black. If the structural part and the other parts could not be separated due to the difference in contrast within the image, the image was cut into parts with the same contrast, binarized, and then joined together as before to return to a single image. As another method of binarization processing, the image analysis may be performed by painting the parts other than the structural part black. The image contains noise, and dark parts with five or fewer consecutive pixels cannot be distinguished from noise and holes, so they were treated as bright parts of the structure. As a method of eliminating noise, dark parts with five or fewer consecutive pixels were excluded when measuring the number of pixels. As another method of eliminating noise, the noise parts may be painted white.
[0245] The number of pixels in the dark luminance portion was counted, and the percentage of the number of pixels in the dark luminance portion to the total number of pixels forming the analysis image was calculated using the following formula (13) to determine the aperture ratio. The same measurement was performed on five images, and the average value was calculated and rounded off to one decimal place. Open area ratio (%)=S / A×100...Formula (13) Where A: Area of measurement range (μm 2 ), S: sum of the measured pore areas (μm 2 ),.
[0246] <Measurement of pore ratio on the surface of the second hollow fiber membrane> As in the above-mentioned "Surface pore size measurement in the second hollow fiber membrane", the inner surface of the second hollow fiber membrane was observed at a magnification of 50,000 times using an SEM, and the outer surface was observed at a magnification of 3,000 times. The images were imported into a computer and analyzed using image processing software. The pore ratio of the five images was calculated in the same manner as in "Measurement of the pore ratio of the first hollow fiber membrane".
[0247] <Measurement of thickness of dense layer in first hollow fiber membrane> The first hollow fiber membrane was immersed in water for 5 minutes to wet it, then frozen in liquid nitrogen, quickly folded, and freeze-dried to obtain a hollow fiber membrane to be observed as a sample. The cross section of the hollow fiber membrane was observed at a magnification of 2000 times using an SEM (S-5500, Hitachi High-Technologies Corporation), and the image was imported into a computer. The size of the imported image was 640 pixels x 480 pixels. If the pores in the cross section were blocked when observed with the SEM, the sample was prepared again. Pore blockage may occur when the hollow fiber membrane is deformed in the direction of stress during the cutting process.
[0248] The obtained SEM images were analyzed using image processing software. The analysis range should be long enough to cover the entire film thickness. If the entire film thickness does not fit within the observation field of the measurement magnification, two or more SEM images were combined. A threshold was determined by binarization processing so that the structural parts were bright and the other parts were dark, and an image was obtained in which the bright parts were white and the dark parts were black. If the structural parts and other parts could not be separated due to the difference in contrast within the image, the image was cut at the parts with the same contrast, binarized, and then joined together as before to return to a single image. As a method for separating other structural parts from other parts, image analysis may be performed by filling in the parts other than the structural parts with black. If holes were observed in double in the depth direction, the shallower hole was measured. If part of the hole was outside the measurement range, that hole was excluded. The image contained noise, and dark parts with five or fewer consecutive pixels were treated as bright parts of the structure because it was impossible to distinguish between noise and holes.
[0249] To eliminate noise, dark areas with 5 or fewer consecutive pixels were excluded when counting the number of pixels. Another method to eliminate noise is to paint the noisy areas white. The number of pixels on a scale bar showing a known length in the image was counted, and the length per pixel was calculated.
[0250] The number of pixels of the detected holes was counted, and the hole area was calculated by multiplying the number of pixels of the holes by the square of the length per pixel. The diameter of the circle corresponding to the hole area was calculated using the following formula (14) to determine the hole diameter. The hole area corresponding to a hole diameter of 0.5 μm is 0.2 μm. 2 It is. Pore diameter (μm) = 2 × (pore area / pi) 1 / 2 ...Equation (14)
[0251] In the binarized image, pores with a diameter of 0.5 μm or more, i.e., a pore area of 0.2 μm 2 Identify the pores with an area of 0.2 μm or more, draw a perpendicular line from the outer surface to the inner surface of the hollow fiber membrane, and 2 Among the layers where no holes were observed, the thickest area was taken as the dense layer, and the thickness of the dense layer was measured. Measurements were taken at 10 locations in the same image. The same measurement was taken on three more images, and the average of a total of 30 measurement data was calculated, and the value rounded off to one decimal place was taken as the dense layer thickness.
[0252] <Measurement of the thickness of the dense layer in the second hollow fiber membrane> As in the above-mentioned "measurement of the thickness of the dense layer in the first hollow fiber membrane", the second hollow fiber membrane was immersed in water, frozen with liquid nitrogen, cut, and then freeze-dried to prepare an observation sample. The cross section of the hollow fiber membrane was observed at a magnification of 5000 times using an SEM. The image was imported into a computer and analyzed using image processing software. Area 0.10 μm 2 The region in which the above dark luminance parts were not observed was determined to be a dense layer, and the thickness of the dense layer was calculated using the same procedure as in "Measurement of thickness of dense layer in first hollow fiber membrane".
[0253] <Extracellular vesicle separation performance evaluation> For the test, a hollow fiber membrane module prepared by the method described in the above "Preparation of hollow fiber membrane module" was used. An outline of the extracellular vesicle separation performance evaluation system is shown in Figure 7.
[0254] 20 mL of commercially available human serum (manufactured by Cosmo Bio Co., Ltd., product code: 12181450) was placed in a container to form a human serum pool 301, which was then kept at 37°C using a thermostatic bath 302. The human serum pool 301 was a liquid reservoir. The liquid was passed through the inside of the hollow fiber membrane of the first module 101 at a rate of 0.5 mL / min using a circulation pump 303a, creating a circulating state (introduction step A). The liquid to be treated drawn off from the human serum pool was introduced into the first module through flow path A (103a).
[0255] At the same time, filtration was performed from the outside of the hollow fiber membrane using the first filtration pump 303b at a rate of 0.15 mL / min to obtain a first permeate. This filtration removes solutes larger than extracellular vesicles that cannot permeate the first hollow fiber membrane from the first permeate, and this filtration is the first separation step.
[0256] The first permeate discharged from the first module 101 was introduced to the inside of the hollow fiber membrane of the second module 102 via flow path B (103b) (liquid transfer process B), and filtered from the outside of the second hollow fiber membrane at a rate of 0.135 mL / min using the second filtration pump 303c to obtain a second permeate and a second non-permeate. As a result of this filtration, extracellular vesicles were concentrated in the second non-permeate, and solutes smaller than extracellular vesicles were contained in the second permeate, and this filtration is the second separation process. The second permeate was discharged from the second module via flow path C (103c) (discharge process C).
[0257] 7, in the evaluation of extracellular vesicles separation performance, the liquid to be treated was introduced into the inside of the first hollow fiber membrane, filtered toward the outside of the first hollow fiber membrane, and introduced into flow path B, and the space in flow path B was connected to the outer surface of the first hollow fiber membrane. Also, the first permeated liquid was introduced into the inside of the second hollow fiber membrane, filtered toward the outside of the second hollow fiber membrane, and the space in flow path B was connected to the inner surface of the second hollow fiber membrane.
[0258] The first non-permeated liquid discharged from the first module 101 and the second permeated liquid discharged from the second module 102 to flow path C (103c) were returned to the human serum pool 301 and mixed (mixing step D). The portion where the first non-permeated liquid and the second permeated liquid are mixed is flow path D. The second non-permeated liquid that passed through the inside of the hollow fiber membrane without being filtered was discarded or collected from flow path E (103e).
[0259] The circulation time was 180 minutes, and the human serum and permeate in the container were sampled at appropriate times, and the extracellular vesicle concentration was measured by the sandwich ELISA method described below. The extracellular vesicle removal rate was calculated using the following formula (15), and the value rounded off to the nearest whole number was used as the extracellular vesicle removal rate. Extracellular vesicle removal rate (%) = 100 × (C1 - C2) / C1 Equation (15) Here, C1 is the concentration of extracellular vesicles in the human serum in the container before the start of the experiment, and C2 is the concentration of extracellular vesicles in the human serum in the container after the end of the experiment.
[0260] To measure the concentration of extracellular vesicles in human serum in solution, a "CD9 / CD63 Exosome ELISA Kit" (Cosmo Bio Co., Ltd.) was used to measure extracellular vesicles with surface markers CD9 and CD63. First, the sample solution was placed on a plate immobilized with the anti-CD9 antibody of this kit, and the plate was left to react for 2 hours to immobilize CD9-positive extracellular vesicles on the plate.
[0261] After washing each well, HRP-labeled anti-CD63 antibody (detection antibody) was added to each well and allowed to react for 2 hours to bind the detection antibody to CD63-positive extracellular vesicles. After washing each well again, substrate solution was added to each well and allowed to react for 20 minutes to develop color. After adding a reaction stop solution to stop the color reaction, the absorbance of each well at a wavelength of 450 nm was measured using a plate reader to determine the extracellular vesicle concentration.
[0262] In this case, the CD9 / CD63 fusion protein provided with the kit was used as a standard substance to create a calibration curve. When measuring extracellular vesicles with surface markers PS and CD9, quantification was performed using a similar sandwich ELISA.
[0263] A plate with immobilized anti-phosphatidylserine antibody ("PS Capture" (registered trademark) Exosome ELISA Kit (Streptavidin HRP), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used to react with shaking at 500 rpm for 2 hours. After washing, a biotin-conjugated anti-CD9 antibody (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as a detection antibody and reacted with shaking for 1 hour. After washing, HRP-labeled streptavidin was reacted with shaking for 2 hours. After washing, a substrate solution was added and left to react for 20 minutes, after which the absorbance at a main wavelength of 450 nm and a secondary wavelength of 620 nm were measured, and the concentration was calculated using the value obtained by subtracting the absorbance at 620 nm from the absorbance at 450 nm.
[0264] In this case, a calibration curve was prepared using a solution containing extracellular vesicles purified from fresh human volunteer plasma using magnetic beads ("MagCapture" (registered trademark) Exosome Isolation Kit PS, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0265] The albumin recovery rate of the purified solution obtained by treatment using the extracellular vesicle separation device was calculated using the following formula (16). The albumin concentration was measured using a kit using the BCG method (A / G B-Test Wako, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). Albumin recovery rate (%) = 100 × (C3 / C4) Equation (16) Here, C3 is the albumin concentration in the human serum in the container after the experiment is completed, and C4 is the albumin concentration in the human serum in the container before the experiment is started.
[0266] The number and concentration of extracellular vesicles in the extracellular vesicle-containing solution collected from 103e in FIG. 7 was determined by a nanoparticle tracking method using Quantum Design's NanoSight (analysis software: NanoSight NTA3.2).
[0267] <Platelet adhesion test> Double-sided tape was attached to a circular polystyrene plate with a diameter of 18 mm, and the hollow fiber membrane was fixed onto the double-sided tape. The attached hollow fiber membrane was cut into a semi-cylindrical shape with a single blade to expose the inner surface of the hollow fiber membrane. If there was dirt, scratches, or creases on the inner surface of the hollow fiber membrane, these areas were excluded from the measurement because platelets may adhere to these areas and an accurate evaluation may not be possible.
[0268] The circular plate was attached to a cylindrical polypropylene tube with a diameter of 18 mm so that the surface with the hollow fiber membrane attached was facing the inside of the cylinder, and the gap was filled with parafilm. The inside of the cylindrical tube was washed with physiological saline and then filled with physiological saline.
[0269] Venous blood collected from healthy subjects (red blood cell count: 4.5 to 5 million / mm 3 , white blood cell count 5000~8000 cells / mm 3 , platelets 200,000 to 500,000 / mm 3 ) and heparin sodium was added to the tube at a concentration of 50 U / mL to prepare a test solution. After discarding the saline solution in the cylindrical tube, 1.0 mL of the test solution was added to the cylindrical tube within 30 minutes after blood collection, and the tube was shaken at 37°C for 1 hour at 700 rpm. The hollow fiber membrane was then washed with 10 mL of saline, and 2.5% by volume of glutaraldehyde / saline was added to immobilize the attached platelets on the hollow fiber membrane.
[0270] After 1 hour or more, the hollow fiber membrane was washed with 20 mL of distilled water. The washed hollow fiber membrane was dried at room temperature (25°C) and reduced pressure of 0.5 Torr for 10 hours. The hollow fiber membrane was attached to the sample stage of the SEM with double-sided tape. After that, a thin film of Pt-Pd was formed on the inner surface of the hollow fiber membrane by sputtering to prepare a platelet-attached sample.
[0271] The images of the inner surface of the obtained platelet-adhered sample were observed with a SEM (S-3000 Type H, Hitachi Science Co., Ltd.) at a magnification of 1500 times, and the number of particles per field of view (5.2 × 10 3 μm 2 ) were counted. The number of observation fields was 20 per sample, and the average was calculated. 3 μm 2 If it exceeded this, it was deemed impossible to measure.
[0272] In addition, the ends of the hollow fibers in the longitudinal direction were excluded from the measurement of the platelet adhesion number because blood accumulates there and the platelet adhesion number is unstable. This test procedure was performed using test solutions derived from three different people, and the results were averaged and rounded off to one decimal place to determine the platelet adhesion number.
[0273] [Example 1] (First module) 13% by mass of polysulfone (SOLVAY's "Udel" (registered trademark) P-3500) and 7.4% by mass of PVP (ASHLAND LCC's Povidone (PLASDONE) K90) were added to a solvent consisting of 76.6% by mass of DMAc and 3% by mass of water, and dissolved by heating at 90°C for 14 hours to obtain a film-forming solution.
[0274] This membrane forming solution was discharged from an orifice-type double cylindrical nozzle with an outer diameter of 1.0 mm and an inner diameter of 0.7 mm, which had been adjusted to 37°C. At the same time, a liquid consisting of 92% by mass of DMAc and 8% by mass of water was discharged from the inner tube as a core liquid. After passing through a 70 mm long dry section set at a dew point of 28°C, the membrane was immersed in a coagulation bath at 80°C and coagulated. It was further washed with warm water in a water washing bath at 80°C, and then wound around a winding frame at a speed of 30 m / min to obtain a wet hollow fiber membrane.
[0275] The inner diameter of the obtained hollow fiber membrane was 317 μm and the membrane thickness was 50 μm. The obtained wet hollow fiber membrane was cut into 0.4 m lengths and divided into small pieces, immersed in a 90° C. hot water bath for 3 hours and washed with hot water, then dried at 100° C. for 10 hours, and further subjected to a heat crosslinking treatment at 170° C. for 5 hours in a dry heat dryer to obtain a hollow fiber membrane 1. The average pore depth of the inner surface of the obtained hollow fiber membrane 1 was 1.63 μm.
[0276] A cross-sectional SEM image of the first hollow fiber membrane is shown in Figure 8, an SEM image of the inner surface is shown in Figure 11, and an SEM image of the outer surface is shown in Figure 12. As shown in Figure 8, it had an asymmetric three-dimensional mesh structure with a dense layer near the outer surface.
[0277] An example of the method described in "Measuring the thickness of the dense layer in the first hollow fiber membrane" above will be described in detail with reference to Figs. 8 to 10. Fig. 9 shows a cross-sectional binarized image obtained when analyzing the cross-sectional SEM image shown in Fig. 8, and Fig. 10 shows an image in which pores with a pore size of 0.5 µm or less have been removed. In Fig. 10, the vertical line on the left side is a tangent line 404 drawn to the outer surface of the hollow fiber membrane. The dotted line in Fig. 10 is a perpendicular line 405 to the tangent line drawn to the outer surface. On this perpendicular line 405, the portion where the distance between the recognized pores is long was determined as the dense layer thickness 403.
[0278] In addition, in Figs. 8 to 10, the left side of the image is the outer surface side 401 of the hollow fiber membrane, and the right side is the inner surface side 402. The dense layer thickness obtained from the SEM image of the cross section of the first hollow fiber membrane obtained by the above method was 4.5 µm. Furthermore, a hollow fiber membrane module 1 was produced by the method described in "Preparation of a hollow fiber membrane module". The results of each measurement of the hollow fiber membrane 1 are shown in Table 1.
[0279] A platelet adhesion test was performed on the inner surface of the first hollow fiber membrane, and the number of platelets attached was 50 / 5.2×10 3 μm 2 The number was nearly impossible to count, but there were 82 pieces / 5.2×10 3 μm 2 It was.
[0280] (Second module) 19% by mass of polysulfone (“Udel” (registered trademark) P-3500, manufactured by SOLVAY), 3% by mass of PVP (Povidone (PLASDONE) K90, manufactured by ASHLAND LCC), and 6% by mass of PVP (Povidone (PLASDONE) K30, manufactured by ASHLAND LCC) were added to a solvent composed of 67% by mass of DMAc and 1% by mass of water, and heated and dissolved at 90 °C for 14 hours to obtain a casting dope solution.
[0281] This casting dope solution was discharged from an orifice-type double cylindrical die with an outer diameter of 0.35 mm / inner diameter of 0.25 mm adjusted to 50 °C. At the same time, a liquid composed of 72% by mass of DMAc and 28% by mass of water was discharged as the core liquid from the inner tube. After passing through a dry section with a length of 350 mm set at a dew point of 28 °C, it was immersed in a coagulation bath at 40 °C containing water for coagulation. Further, it was washed with warm water in a water washing bath at 80 °C and then wound up on a winding frame at a speed of 30 m / min to obtain a wet hollow fiber membrane 2.
[0282] A hollow fiber membrane module 2 was obtained by the method described in “Fabrication of Hollow Fiber Membrane Module” except that 150 hollow fiber membranes 2 were used. The measurement results for the second hollow fiber membrane used in the hollow fiber membrane module 2 are shown in Table 1.
[0283] P2 was 0% and P2 < P1. As a result of measuring the inner surface of the hollow fiber membrane 2 by the method described in “Measurement of the Ratio of Hydrophilic Polymer on the Surface of Hollow Fiber Membrane”, the ratio of the hydrophilic polymer on the inner surface was 32% by mass.
[0284] (Extracellular Vesicle Separation Device) Using the hollow fiber membrane module 1 as the first module and the hollow fiber membrane module 2 as the second module, the extracellular vesicle separation performance was evaluated. As a result, the removal rate of extracellular vesicles was 82%, indicating high separation performance. Also, the albumin recovery rate was 75%, confirming that most of the albumin remained without being lost.
[0285] [Example 2] An aqueous solution containing vinyl acetate / vinylpyrrolidone copolymer ("Kollidon" (registered trademark), manufactured by BASF, weight average molecular weight 45000 to 70000) at a concentration of 100 ppm and ethanol at a concentration of 1000 ppm was passed through the hollow fiber membrane module 2 obtained in Example 1 from the inside to the outside, thereby coating the entire membrane. Subsequently, the hollow fiber membrane module 2 was irradiated with 25 kGy of gamma rays to obtain a hollow fiber membrane module 3.
[0286] Measurements and evaluation of extracellular vesicle separation performance were performed in the same manner as in Example 1, except that hollow fiber membrane module 3 was used instead of hollow fiber membrane module 2. The measurement results are shown in Table 1. It can be seen that the albumin recovery rate is excellent because a hydrophilic polymer containing a monocarboxylic acid vinyl ester unit as a repeating unit is present on the surface of the second hollow fiber membrane. This is thought to be because adhesion of albumin to the surface of the second hollow fiber membrane is suppressed.
[0287] [Example 3] An aqueous solution of vinylpyrrolidone / vinyl propanoate random copolymer (vinyl propanoate unit molar fraction 40%, weight average molecular weight 16500) at a concentration of 100 ppm and ethanol at a concentration of 1000 ppm was passed from the inside to the outside of the hollow fiber membrane to coat the entire membrane of the hollow fiber membrane module 1 obtained in Example 1. Subsequently, the hollow fiber membrane module 4 was irradiated with 25 kGy of gamma rays to obtain a hollow fiber membrane module 4.
[0288] Measurements and evaluation of extracellular vesicle separation performance were performed in the same manner as in Example 2, except that hollow fiber membrane module 4 was used instead of hollow fiber membrane module 1. The measurement results are shown in Table 1.
[0289] It can be seen that the presence of a hydrophilic polymer containing a monocarboxylate vinyl ester unit as a repeating unit on the surface of the first hollow fiber membrane and the surface of the second hollow fiber membrane results in a superior albumin recovery rate compared to Examples 1 and 2. This is believed to be because adhesion of albumin to the surfaces of the first hollow fiber membrane and the second hollow fiber membrane is suppressed. A platelet adhesion test was performed on the surface of the first hollow fiber membrane, and the number of adherent platelets was 7 / 5.2×10 3 μm 2 It was.
[0290] The second non-permeated liquid that passed through the inside of the hollow fiber membrane without being filtered in the second module 102 was collected from flow path E (103e). The obtained second non-permeated liquid was extracellular vesicle-containing solution A, and the amount of extracellular vesicles in the extracellular vesicle-containing solution A was quantified by the above-mentioned phosphatidylserine / CD9 sandwich ELISA method, and the concentration was 340 μg / mL. In addition, the number concentration of extracellular vesicles was measured by NanoSight and was found to be 6.0 × 10 9 The number of cells / mL.
[0291] [Comparative Example 1] A hollow fiber membrane taken out of a plasma separator "Plasma Flow" (registered trademark) manufactured by Asahi Kasei Medical Corporation was used as the first hollow fiber membrane, and a hollow fiber membrane module 5 was obtained by the same operation as in Example 1. An extracellular vesicle separation experiment was performed in the same manner as in Example 2, except that the obtained hollow fiber membrane module 5 was used as the first module. The measurement results are shown in Table 2. In this case, P1 was 30%, and the removal rate of extracellular vesicles was 23%, which was far inferior to the separation performance of Examples 1 to 3.
[0292] [Comparative Example 2] An extracellular vesicle separation experiment was carried out in the same manner as in Example 1, except that hollow fiber membrane module 1 was used as the second module instead of hollow fiber membrane module 2. The measurement results are shown in Table 2. In this case, P1=P2, and the extracellular vesicles permeated the second hollow fiber membrane and were returned to the human serum pool, indicating that almost no extracellular vesicles were removed.
[0293] [Example 4] (First module) A hollow fiber membrane module 4 obtained in the same manner as in Example 3 was used as the first module.
[0294] (Second module) 15.5% by mass of polysulfone, 4.5% by mass of PVP (povidone (PLASDONE) K90), and 2% by mass of PVP (povidone (PLASDONE) K30) were added to a solvent consisting of 77% by mass of DMAc and 1% by mass of water, and dissolved by heating at 90°C for 14 hours to obtain a film-forming solution.
[0295] This membrane forming solution was discharged from an orifice-type double cylindrical nozzle with an outer diameter of 0.58 mm / inner diameter of 0.33 mm adjusted to 35° C. At the same time, a liquid consisting of 70% by mass of DMAc and 30% by mass of water was discharged from the inner tube as a core liquid. After passing through a 350 mm long dry section set at a dew point of 28° C., the membrane was immersed in a coagulation bath of 50° C. containing water to be coagulated. It was further washed with warm water in a water washing bath at 60° C., and then wound around a winding frame at a speed of 30 m / min to obtain a wet hollow fiber membrane 3.
[0296] The inner diameter of the obtained hollow fiber membrane was 247 μm and the membrane thickness was 62 μm. A hollow fiber membrane module 6 was obtained by the method described in "Preparation of a hollow fiber membrane module" except that 150 hollow fiber membranes 3 were used. The evaluation results are shown in Table 3.
[0297] [Example 5] (First module) 15% by mass of polysulfone and 7% by mass of PVP (povidone (PLASDONE) K90) were added to a solvent consisting of 75.3% by mass of DMAc and 2.7% by mass of water, and dissolved by heating at 90° C. for 14 hours to obtain a film-forming solution.
[0298] This membrane forming solution was discharged from an orifice-type double cylindrical nozzle with an outer diameter of 0.7 mm and an inner diameter of 0.5 mm, which had been adjusted to 37°C. At the same time, a liquid consisting of 55% by mass of DMAc, 30% by mass of PVP (povidone (PLASDONE) K30), and 15% by mass of glycerin was discharged from the inner tube as a core liquid. After passing through a 75 mm long dry section set at a dew point of 30°C, the membrane was immersed in a coagulation bath at 80°C containing water to be coagulated. It was then washed with warm water in a water washing bath at 80°C, and wound around a winding frame at a speed of 40 m / min to obtain a wet hollow fiber membrane.
[0299] The obtained hollow fiber membrane had an inner diameter of 178 μm and a membrane thickness of 64 μm. The obtained wet hollow fiber membrane was cut into 0.4 m lengths and divided into small pieces, immersed in a 90° C. hot water bath for 3 hours and washed with hot water, then dried at 100° C. for 10 hours, and further subjected to thermal crosslinking treatment at 170° C. for 5 hours in a dry heat dryer to obtain hollow fiber membrane 4. A hollow fiber membrane module 7 was obtained by the method described in “Preparation of hollow fiber membrane module” except that hollow fiber membrane 4 was used.
[0300] (Second module) The hollow fiber membrane module 3 obtained in the same manner as in Example 2 was used as the second module. The evaluation results are shown in Table 3.
[0301] [Example 6] (First module) A hollow fiber membrane module 4 obtained in the same manner as in Example 3 was used as the first module.
[0302] (Second module) 20% by mass of polysulfone, 6% by mass of PVP (povidone (PLASDONE) K90), and 5% by mass of PVP (povidone (PLASDONE) K30) were added to a solvent consisting of 68% by mass of DMAc and 1% by mass of water, and dissolved by heating at 90°C for 14 hours to obtain a film-forming solution.
[0303] This membrane forming solution was discharged from an orifice-type double cylindrical nozzle with an outer diameter of 0.58 mm and an inner diameter of 0.33 mm, which had been adjusted to 35° C. At the same time, a liquid consisting of 72% by mass of DMAc and 28% by mass of water was discharged from the inner tube as a core liquid. After passing through a 350 mm long dry section set at a dew point of 28° C., the membrane was immersed in a coagulation bath at 40° C. containing water to be coagulated. It was then washed with warm water in a water washing bath at 60° C., and then wound around a winding frame at a speed of 30 m / min to obtain a wet hollow fiber membrane 5.
[0304] The obtained hollow fiber membrane had an inner diameter of 276 μm and a membrane thickness of 52 μm. A hollow fiber membrane module 8 was obtained by the method described in "Preparation of a hollow fiber membrane module" except that 150 hollow fiber membranes 5 were used.
[0305] The evaluation results are shown in Table 3. The test was carried out without any problems and showed a good extracellular vesicle removal rate. However, when the pressure on the filtration side of the second module (103c in FIG. 7) was measured during the evaluation test, it was found to be negative at -10 kPa due to clogging of the second module. From this, it was concluded that the water permeability of the second hollow fiber membrane in the device of the present invention was 250 mL / h / mmHg / m 2 It is understood that the above is preferable.
[0306] [Example 7] An extracellular vesicle separation performance evaluation test was performed in the same manner as in Example 3, except that the amount of human serum used in the evaluation of extracellular vesicle separation performance was 60 mL instead of 20 mL, and the circulation time was 540 minutes. The second non-permeated liquid that passed through the inside of the hollow fiber membrane without being filtered in the second module 102 was collected from flow path E (103e).
[0307] The obtained second non-permeated liquid was extracellular vesicle-containing solution B. The amount of extracellular vesicles in extracellular vesicle-containing solution B was quantified by the above-mentioned phosphatidylserine / CD9 sandwich ELISA method, and the concentration was 910 μg / mL. In addition, the number concentration of extracellular vesicles was measured by NanoSight and was 1.6 × 10 10 The number of cells / mL.
[0308] [Table 1]
[0309] [Table 2]
[0310] [Table 3] [Explanation of symbols]
[0311] 101...first module, 102...second module, 103a...flow path A, 103b...flow path B, 103c...flow path C, 103d...flow path D, 103e...flow path E, 201...hollow fiber membrane module, 202...case, 203...potting material, 204...header, 205...nozzle, 206...module inner diameter, 301...human serum pool, 302...thermostatic bath, 303a...circulation pump, 303b...first filtration pump, 303c...second filtration pump, 401...outer surface side, 402...inner surface side, 403...example of dense layer thickness, 404...tangent line drawn to outer surface, 405...perpendicular line to tangent line drawn to outer surface
Claims
1. A first module containing a first hollow fiber membrane; a second module containing a second hollow fiber membrane; and a flow path B that communicates an interior of the first module with an interior of the second module, The 0.15 μm particle permeability P1 of the first hollow fiber membrane is 50% or more and 100% or less, An extracellular vesicle separation device, wherein P2, which is the 0.15 μm particle permeability of the second hollow fiber membrane, and P1 satisfy the relationship P2 < P1.
2. The extracellular vesicle separation device according to claim 1 , wherein P2 is 15% or less.
3. The extracellular vesicle separation device according to claim 1 or 2, wherein the second hollow fiber membrane has a 0.02 μm particle permeability of 5% or less.
4. The water permeability of the second hollow fiber membrane is 250 mL / h / mmHg / m 2 More than 2000mL / h / mmHg / m 2 The extracellular vesicle separation device according to claim 1 or 2, wherein:
5. The extracellular vesicle separation device according to claim 1 or 2, wherein the first hollow fiber membrane or the second hollow fiber membrane contains a hydrophilic polymer.
6. The extracellular vesicle separation device according to claim 5 , wherein the hydrophilic polymer contains a monocarboxylic acid vinyl ester unit as a repeating unit and is present on at least one surface of the first hollow fiber membrane or the second hollow fiber membrane.
7. The extracellular vesicle separation device according to claim 1 or 2, wherein a main component of the first hollow fiber membrane or the second hollow fiber membrane is a polysulfone-based polymer.
8. The extracellular vesicle separation device according to claim 1 or 2, wherein the thickness of the dense layer in the cross section of the first hollow fiber membrane is 1.0 μm or more and 10.0 μm or less.
9. The water permeability of the first hollow fiber membrane is 16000 mL / h / mmHg / m 2 More than 30000mL / h / mmHg / m 2 The extracellular vesicle separation device according to claim 1 or 2, wherein:
10. The extracellular vesicle separation device according to claim 1 or 2, wherein the space within the flow path B is connected to the outer surface of the first hollow fiber membrane.
11. The extracellular vesicle separation device according to claim 1 or 2, which is used for removing extracellular vesicles from body fluids of a living organism.
12. The extracellular vesicle separation device according to claim 11 , wherein the body fluid is blood.
13. The space in the flow path B is in communication with the inner surface of the second hollow fiber membrane, a flow path A for introducing the liquid to be treated led out from the liquid reservoir into the first module; The extracellular vesicle separation device according to claim 1 or 2, further comprising a flow path D for mixing the permeate discharged from the second module and the non-permeate discharged from the first module and introducing the mixture into the liquid reservoir.
14. The extracellular vesicle separation device according to claim 1 or 2, which is used for the treatment of sepsis, autoimmune diseases or chronic liver diseases.
15. a first separation step of filtering a liquid to be treated containing extracellular vesicles using a first hollow fiber membrane having a 0.15 μm particle permeability P1 of 50% to 100%, and separating the liquid into a first non-permeated liquid in which solutes larger than extracellular vesicles capable of permeating the first hollow fiber membrane are concentrated, and a first permeated liquid in which solutes larger than extracellular vesicles capable of permeating the first hollow fiber membrane are removed; A method for separating a solution containing extracellular vesicles, comprising a second separation step of filtering the first permeate using a second hollow fiber membrane having a 0.15 μm particle permeability P2 and the P1 such that P2 < P1, and separating the first permeate into a second non-permeate in which all or a part of the extracellular vesicles contained in the first permeate are concentrated, and a second permeate containing solutes smaller than the extracellular vesicles.
16. having at least one surface marker selected from the group consisting of phosphatidylserine, CD9, CD63, CD81, TyA and Clq; The number concentration of extracellular vesicles is 6.0 × 10 9 pcs / mL or more, 1.4 x 10 12 An extracellular vesicle-containing solution having an extracellular vesicle content of vesicles / mL or less.
Citation Information
Patent Citations
Use of microvesicles in diagnosis, prognosis and treatment of medical diseases and conditions
JP2015091251A
Separating / purifying method of extracellular vesicles
JP2022182360A
Devices, systems and methods for widespread reduction of pro-inflammatory cytokines in the blood
JP2022542517A
Cited By
Combination of bilberry, emblic leafflower fruit and roselle
CN122028925A
Method for producing extracellular vesicles, and extracellular vesicle composition
JP2026151512A
Exosome manufacturing method
JP2026151537A
Method for producing an anion exchange membrane, membrane for capturing extracellular vesicles, and method for producing extracellular vesicles