Reflection type photomask blank and reflection type photomask
The reflective photomask blank addresses shadowing and hydrogen radical issues in EUV lithography by using a multilayer absorption layer with varying material compositions, enhancing pattern accuracy and longevity.
Patent Information
- Application Number
- JP2024114474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
EUV lithography faces issues with shadowing and decreased contrast at pattern edges due to the use of tantalum-based absorption layers, leading to line edge roughness and inaccurate line widths, along with contamination and reduced throughput from hydrogen radical exposure.
A reflective photomask blank with a multilayer absorption layer composed of materials with varying compositions, where the content of high absorption materials decreases towards the surface and hydrogen radical-resistant materials increase, reducing shadowing and improving pattern rectangularity and hydrogen radical resistance.
The solution enhances the dimensional and shape accuracy of transferred patterns while extending the photomask's lifespan by reducing shadowing and improving resistance to hydrogen radicals, maintaining high reflectance and optical density.
Smart Images

Figure 2024138522000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a reflective photomask for use in lithography using light in the ultraviolet region as a light source, and a reflective photomask blank for use in producing the same. [Background technology]
[0002] In the manufacturing process of semiconductor devices, the demand for miniaturization of photolithography technology is increasing along with the miniaturization of semiconductor devices. The minimum resolution dimension of the transfer pattern in photolithography depends heavily on the wavelength of the exposure light source, and the shorter the wavelength, the smaller the minimum resolution dimension can be. For this reason, the exposure light source is being replaced from the conventional ArF excimer laser light with a wavelength of 193 nm to light in the EUV (Extreme Ultra Violet) region with a wavelength of 13.5 nm.
[0003] Light in the EUV region is absorbed at a high rate by most substances, so a reflective photomask is used as a photomask for EUV exposure (EUV mask) (see, for example, Patent Document 1). Patent Document 1 discloses an EUV photomask obtained by forming a reflective layer made of a multilayer film in which molybdenum (Mo) layers and silicon (Si) layers are alternately laminated on a glass substrate, forming a light absorbing layer mainly composed of tantalum (Ta) thereon, and forming a pattern on this light absorbing layer.
[0004] Furthermore, as mentioned above, EUV lithography cannot use refractive optics that utilize the transmission of light, so the optical components of the exposure machine are reflective (mirrors) rather than lenses. This creates a problem in that the incident light and reflected light on the reflective photomask (EUV mask) cannot be designed to be coaxial, so EUV lithography normally employs a method in which the optical axis is tilted 6 degrees from the vertical direction of the EUV mask, and the reflected light reflected at an angle of minus 6 degrees is guided to the semiconductor substrate.
[0005] As such, in EUV lithography, the optical axis is tilted via a mirror, which can cause a problem known as the "projection effect," in which the EUV light incident on the EUV mask casts a shadow on the mask pattern (patterned light-absorbing layer) of the EUV mask.
[0006] Current EUV mask blanks use a tantalum (Ta)-based film with a thickness of 60 to 90 nm as the light absorption layer. When performing pattern transfer exposure with an EUV mask fabricated using this mask blank, there is a risk of a decrease in contrast at the shadow edge of the mask pattern depending on the relationship between the incident direction of the EUV light and the orientation of the mask pattern. This can lead to problems such as increased line edge roughness of the transferred pattern on the semiconductor substrate and inability to form the line width to the targeted dimension, resulting in a deterioration of transfer performance.
[0007] Therefore, reflective mask blanks in which the material forming the absorption layer is changed from tantalum (Ta) to a material with high absorptivity (extinction coefficient) for EUV light, or reflective mask blanks in which a material with high absorptivity for EUV light is added to tantalum (Ta) are being considered. For example, Patent Document 2 describes a reflective mask blank in which the absorption layer is made of a material containing 50 atomic % (at %) or more of Ta as a main component and further containing at least one element selected from Te, Sb, Pt, I, Bi, Ir, Os, W, Re, Sn, In, Po, Fe, Au, Hg, Ga, and Al. In addition, after the absorption layer is patterned, the cross-sectional sidewall angle is preferably a nearly vertical rectangular shape. If it has a stepped or tapered shape, it may cause unintended attenuation and amplification of the exposure light or the pattern edge. There is a concern that the change in the reflected light intensity at the portion may deteriorate the transfer performance.
[0008] Furthermore, it is known that mirrors are contaminated by by-products of EUV generation (e.g., Sn) and carbon. Accumulation of contaminants on the mirror reduces the reflectivity of the surface, lowering the throughput of the lithography apparatus. In response to this problem, Patent Document 3 discloses a method of generating hydrogen radicals within the apparatus, reacting the contaminants with the hydrogen radicals, and removing the contaminants from the mirror.
[0009] However, in the reflective mask blank described in Patent Document 2, there is no consideration as to whether the absorbing layer has resistance to hydrogen radicals (hydrogen radical resistance). Therefore, when introduced into an EUV exposure tool, the absorbing film pattern cannot be stably maintained, and as a result, there is a possibility that transferability may deteriorate. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2011-176162 A [Patent Document 2] JP 2007-273678 A [Patent Document 3] JP 2011-530823 A Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a reflective photomask blank which reduces shadowing (projection effect) and improves the rectangularity of the mask pattern, thereby improving the dimensional accuracy and shape accuracy of the pattern transferred onto a wafer, and which imparts hydrogen radical resistance, thereby enabling the photomask to be used for a long period of time, and a reflective photomask manufactured using the reflective photomask blank. [Means for solving the problem]
[0012] In order to achieve the above object, a reflective photomask blank according to one embodiment of the present invention is a reflective photomask blank for producing a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, comprising: a substrate; a reflective portion formed on the substrate and reflecting incident light; and a low-reflection portion formed on the reflective portion and absorbing the incident light, wherein the low-reflection portion is a layer containing at least one material selected from a first material group and at least one material selected from a second material group different from the first material group, the content of the at least one material selected from the first material group decreasing from the substrate side toward the outermost surface side of the low-reflection portion, and the content of the at least one material selected from the second material group decreasing from the substrate side toward the outermost surface side of the low-reflection portion. The content of at least one material increases from the substrate side toward the outermost surface side of the low-reflection portion, the first material group being tellurium (Te), cobalt (Co), nickel (Ni), platinum (Pt), silver (Ag), tin (Sn), indium (In), copper (Cu), zinc (Zn), and bismuth (Bi), as well as oxides, nitrides, and oxynitrides thereof, and the second material group being tantalum (Ta), chromium (Cr), aluminum (Al), silicon (Si), ruthenium (Ru), molybdenum (Mo), zirconium (Zr), titanium (Ti), zinc (Zn), indium (In), vanadium (V), hafnium (Hf), and niobium (Nb), as well as oxides, nitrides, and oxynitrides thereof.
[0013] Furthermore, the reflective photomask blank according to one embodiment of the present invention may be a structure in which, even when the low-reflection portion is divided into multiple layers, the total thickness of the entire low-reflection portion is at least 33 nm or more, and the low-reflection portion contains at least one material selected from the first material group in a total amount of 20 atomic % or more. In addition, in the reflective photomask blank according to one embodiment of the present invention, the low reflection portion is formed in a plurality of layers. Even if divided, the low-reflection portion may have a total thickness of at least 26 nm and may contain at least one material selected from the first material group in a total amount of 55 atomic % or more in the low-reflection portion.
[0014] Furthermore, the reflective photomask blank according to one embodiment of the present invention may be a structure in which, even when the low-reflection portion is divided into multiple layers, the total thickness of the entire low-reflection portion is at least 17 nm or more, and the entire low-reflection portion contains at least one material selected from the first material group in a total amount of 95 atomic % or more. Furthermore, the reflective photomask blank according to one embodiment of the present invention may be a structure in which the outermost surface layer of the low reflection portion contains at least one material selected from the second material group in a total amount of 80 atomic % or more.
[0015] Furthermore, in the reflective photomask blank of one embodiment of the present invention, when the thickness dimension of the low-reflection portion is taken as 100%, and the outermost layer of the low-reflection portion is defined as a region at a depth of 50% or less from the surface of the low-reflection portion, the outermost layer of the low-reflection portion may be a structure containing a total of 80 atomic % or more of at least one material selected from the second material group. In the reflective photomask blank according to one embodiment of the present invention, the outermost surface layer of the low reflection portion may have a film thickness of 0.5 nm or more and 30 nm or less.
[0016] A reflective photomask according to one aspect of the present invention includes a substrate, a reflective portion formed on the substrate to reflect incident light, and a low-reflective portion formed on the reflective portion to absorb incident light, the low-reflective portion being a layer including at least one material selected from a first material group and at least one material selected from a second material group different from the first material group, the content of the at least one material selected from the first material group decreasing from the substrate side toward the outermost surface side of the low-reflective portion, and the content of the at least one material selected from the second material group decreasing from the substrate side toward the outermost surface side of the low-reflective portion. The first material group is tellurium (Te), cobalt (Co), nickel (Ni), platinum (Pt), silver (Ag), tin (Sn), indium (In), copper (Cu), zinc (Zn), and bismuth (Bi), as well as oxides, nitrides, and oxynitrides thereof, and the second material group is tantalum (Ta), chromium (Cr), aluminum (Al), silicon (Si), ruthenium (Ru), molybdenum (Mo), zirconium (Zr), titanium (Ti), zinc (Zn), indium (In), vanadium (V), hafnium (Hf), and niobium (Nb), as well as oxides, nitrides, and oxynitrides thereof. Effect of the Invention
[0017] According to one aspect of the present invention, by forming a low-reflection portion in which the content of a compound material having high absorbency for EUV light is decreased from the substrate side toward the outermost surface side and the content of a compound material having high hydrogen radical resistance is increased from the substrate side toward the outermost surface side, shadowing is reduced and the rectangularity of the mask pattern is improved, thereby improving the dimensional accuracy and shape accuracy of the pattern transferred onto the wafer and imparting hydrogen radical resistance, making it possible to use the photomask for a long period of time. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment of the present invention. [Diagram 3] 1 is a graph showing the optical constants of each metal material at the wavelength of EUV light. [Figure 4] FIG. 1 is a conceptual diagram showing an example of the content (concentration) distribution of a first material group and the content (concentration) distribution of a second material group in an absorption layer (low reflection portion) provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Diagram 5] 3A to 3C are conceptual diagrams showing examples of the content distribution of a first material group and the content distribution of a second material group in an absorber layer provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Figure 6] 3A to 3C are conceptual diagrams showing examples of the content distribution of a first material group and the content distribution of a second material group in an absorber layer provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Figure 7] 3A to 3C are conceptual diagrams showing examples of the content distribution of a first material group and the content distribution of a second material group in an absorber layer provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Figure 8] FIG. 1 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to an embodiment of the present invention. [Figure 9] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 10] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 11] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 12] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment of the present invention. [Figure 13] 1 is a schematic plan view showing a design pattern of a reflective photomask according to an embodiment of the present invention. [Figure 14]FIG. 2 is a schematic cross-sectional view showing the structure of an existing reflective photomask blank according to a comparative example of the present invention, which has an absorption layer with a two-layer structure. [Figure 15] FIG. 1 is a schematic cross-sectional view showing the structure of an existing reflective photomask according to a comparative example of the present invention, which has an absorption layer with a two-layer structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the embodiments of the present invention will be described, but the present invention is not limited to the embodiments shown below. In the embodiments shown below, technically preferable limitations are imposed for carrying out the present invention, but these limitations are not essential requirements of the present invention. Fig. 1 is a schematic cross-sectional view showing the structure of a reflective photomask blank 10 according to an embodiment of the present invention. Also, Fig. 2 is a schematic cross-sectional view showing the structure of a reflective photomask 20 according to an embodiment of the present invention. Here, the reflective photomask 20 according to the embodiment of the present invention shown in Fig. 2 is formed by patterning the absorption layer 4 of the reflective photomask blank 10 according to the embodiment of the present invention shown in Fig. 1.
[0020] (Overall composition) As shown in Fig. 1, a reflective photomask blank 10 according to an embodiment of the present invention includes a substrate 1, a reflective layer 2 formed on the substrate 1, a capping layer 3 formed on the reflective layer 2, and an absorbing layer 4 formed on the capping layer 3. More specifically, the reflective photomask blank 10 according to an embodiment of the present invention is a reflective photomask blank for producing a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, and includes a substrate 1, a reflective layer 2 and a capping layer 3 formed on the substrate 1 and functioning as a reflective portion that reflects incident light, and an absorbing layer 4 formed on the reflective portion and functioning as a low-reflecting portion that absorbs incident light. The configuration of each of the above-mentioned layers will be described below.
[0021] (substrate) The substrate 1 according to the embodiment of the present invention may be a flat Si substrate, a synthetic quartz substrate, etc. The substrate 1 may be made of low thermal expansion glass containing titanium, but the present embodiment is not limited to these as long as the material has a small thermal expansion coefficient.
[0022] (reflective layer) The reflective layer 2 according to the embodiment of the present invention is a layer that constitutes a part of the reflective section. The reflective layer 2 according to the embodiment of the present invention reflects EUV light (extreme ultraviolet light) which is the exposure light, and is composed of, for example, a multilayer reflective film made of a combination of materials having significantly different refractive indices for EUV light. An example of a multilayer reflective film is one formed by repeatedly stacking layers of a combination of Mo (molybdenum) and Si (silicon), or Mo (molybdenum) and Be (beryllium), for example, for about 40 periods.
[0023] (capping layer) The capping layer 3 according to the embodiment of the present invention is a layer that constitutes a part of the reflective portion. The capping layer 3 according to the embodiment of the present invention is made of a material that is resistant to dry etching performed when forming a transfer pattern in the absorbing layer 4, and functions as an etching stopper that prevents damage to the reflective layer 2 when etching the absorbing layer 4. The capping layer 3 is made of, for example, Ru (ruthenium). Here, depending on the material of the reflective layer 2 and the etching conditions, the capping layer 3 may not be necessary. Although not shown, a back conductive film can be formed on the surface of the substrate 1 on which the reflective layer 2 is not formed. The back conductive film is a film for fixing the reflective photomask 20 by utilizing the principle of an electrostatic chuck when the reflective photomask 20 is placed in an exposure machine.
[0024] (Absorption layer) The absorbing layer 4 of the reflective photomask blank 10 is a layer that becomes the absorbing pattern layer 41 (see FIG. 2) of the reflective photomask 20 by removing a part of it. In EUV lithography, EUV light is incident obliquely on the horizontal surface of the substrate of the reflective photomask 20 and is reflected by the reflective layer 2, but due to a projection effect in which the absorbing pattern layer 41 obstructs the optical path, the transfer performance onto the wafer may deteriorate. This deterioration in transfer performance can be reduced by reducing the thickness of the absorbing layer 4 that absorbs EUV light. The thickness of the absorbing layer 4 can be reduced by applying a material that is more absorbent to EUV light than conventional materials, that is, a material with a high extinction coefficient k at a wavelength of 13.5 nm.
[0025] Figure 3 is a graph showing the optical coefficients of each metal material for EUV light with a wavelength of 13.5 nm. The horizontal axis of Figure 3 represents the refractive index n, and the vertical axis represents the extinction coefficient k. The extinction coefficient k of tantalum (Ta), which is the main material of the conventional absorption layer 4, is 0.041. If a compound material has a larger extinction coefficient k than this, it is possible to reduce the thickness of the absorption layer 4. If the extinction coefficient k is 0.06 or more, it is possible to sufficiently reduce the thickness of the absorption layer 4, and therefore the projection effect can be sufficiently reduced. Materials that satisfy the above combination of optical constants (nk value) include, for example, silver (Ag), platinum (Pt), indium (In), cobalt (Co), tin (Sn), nickel (Ni), and tellurium (Te), as shown in FIG. 3.
[0026] The materials (elements) that can be added to the absorbing layer 4 will be described in detail below. The absorbent layer 4 is a layer containing at least one material selected from a first material group described below, and at least one material selected from a second material group different from the first material group described below. In the absorbent layer 4, the content of at least one material selected from the first material group decreases from the substrate 1 side toward the outermost surface 4a side of the absorbent layer 4, and the content of at least one material selected from the second material group decreases from the substrate 1 side toward the outermost surface 4a side of the absorbent layer 4. The number of such cases is increasing.
[0027] Here, the first material group includes tellurium (Te), cobalt (Co), nickel (Ni), platinum (Pt), silver (Ag), tin (Sn), indium (In), copper (Cu), zinc (Zn), and bismuth (Bi), as well as their oxides, nitrides, and oxynitrides. The second material group includes tantalum (Ta), chromium (Cr), aluminum (Al), silicon (Si), ruthenium (Ru), molybdenum (Mo), zirconium (Zr), titanium (Ti), zinc (Zn), indium (In), vanadium (V), hafnium (Hf), and niobium (Nb), as well as their oxides, nitrides, and oxynitrides.
[0028] Even when the absorption layer 4 is divided into multiple layers, it is preferable that the total thickness of the entire absorption layer 4 is at least 33 nm, and that the absorption layer 4 has a structure containing at least one material selected from the first material group in a total amount of 20 atomic % or more in the entire absorption layer 4. Furthermore, even when the absorption layer 4 is divided into a plurality of layers, it is more preferable that the total thickness of the entire absorption layer 4 is at least 26 nm, and the entire absorption layer 4 contains at least one material selected from the first material group in a total amount of 55 atomic % or more.
[0029] Furthermore, even when the absorption layer 4 is divided into a plurality of layers, it is more preferable that the total thickness of the entire absorption layer 4 is at least 17 nm, and the entire absorption layer 4 has a structure containing at least one material selected from the first material group in a total amount of 95 atomic % or more. Moreover, the outermost layer of the absorbing layer 4 is preferably a structure containing at least one material selected from the second material group in a total amount of 80 atomic % or more.
[0030] Furthermore, when the thickness dimension of the absorption layer 4 is taken as 100%, and a region within 50% of the depth from the surface of the absorption layer 4 is defined as the "outermost layer of the absorption layer 4", the outermost layer of the absorption layer 4 is preferably a structure containing at least one material selected from the second material group, in a total amount of 80 atomic % or more. In addition, the outermost layer of the absorbing layer 4 preferably has a thickness of 0.5 nm to 30 nm. The film thickness of the outermost layer of the absorbing layer 4 is limited to 0.5 nm, and it is extremely difficult to form a film with a thickness of less than 0.5 nm. In addition, when the film thickness of the outermost layer of the absorbing layer 4 exceeds 30 nm, the effect of shadowing tends to become significant.
[0031] Hereinafter, the distribution of the contents (concentrations) of the materials contained in the first material group and the contents (concentrations) of the materials contained in the second material group in the absorbent layer 4 will be described. In this embodiment, it is preferable that the content of the material contained in the first material group decreases linearly (linearly), curvedly (e.g., S-curve), or exponentially from the substrate 1 side toward the outermost surface 4a side of the absorbent layer 4. In addition, in this embodiment, it is preferable that the content of the material contained in the second material group increases linearly (linearly), curvedly (e.g., S-curve), or exponentially from the substrate 1 side toward the outermost surface 4a side of the absorbent layer 4.
[0032] At least one of the first material group and the second material group preferably has a uniform composition in at least one of the regions on the substrate 1 side and the outermost surface 4a side of the absorbent layer 4. In this embodiment, the "region on the substrate 1 side" refers to the lower 10% of the entire absorbent layer 4, and the "region on the outermost surface 4a side" refers to the upper 10% of the entire absorbent layer 4. In addition, the point (location) where the content (concentration) of the first material group and the content (concentration) of the second material group become the same may be located on the substrate 1 side when the absorption layer 4 is divided into two equal parts in the thickness direction. Alternatively, it may be located on the outermost surface 4 a side of the absorbent layer 4 .
[0033] Furthermore, the region on the substrate 1 side (the lower 10% of the entire absorbent layer 4) does not have to be made up of only materials included in the first material group, and the region on the outermost surface 4a side (the upper 10% of the entire absorbent layer 4) does not have to be made up of only materials included in the second material group. In other words, the region on the substrate 1 side may contain a material included in the second material group, and the region on the outermost surface 4a side may contain a material included in the first material group. Hereinafter, the distribution of the contents (concentrations) of the materials contained in the first material group and the contents (concentrations) of the materials contained in the second material group in the absorbent layer 4 will be described with reference to the drawings.
[0034] 4 to 7 are conceptual diagrams showing the content distribution (concentration distribution) of the material contained in the first material group and the content distribution (concentration distribution) of the material contained in the second material group. In each of Figs. 4 to 7, the vertical axis indicates the content (%) of the first material group and the second material group in the entire absorbent layer 4, respectively, and the horizontal axis indicates the depth direction of the entire absorbent layer 4. FIG. 4 shows a configuration in which the content of the material included in the first material group (solid line) decreases linearly from the substrate 1 side toward the outermost surface 4a of the absorbent layer 4, and the content of the material included in the second material group (dashed line) increases linearly from the substrate 1 side toward the outermost surface 4a of the absorbent layer 4.
[0035] FIG. 5 shows a configuration in which the content of the material included in the first material group (solid line) decreases linearly from the substrate 1 side toward the outermost surface 4a of the absorbent layer 4, and the content of the material included in the second material group (dashed line) increases linearly from the substrate 1 side toward the outermost surface 4a of the absorbent layer 4, and the point (location) where the content (concentration) of the first material group and the content (concentration) of the second material group are the same is located on the substrate 1 side when the absorbent layer 4 is divided into two equal parts in the thickness direction, and the region on the substrate 1 side contains the material included in the second material group, and the region on the outermost surface 4a side contains the material included in the first material group.
[0036] FIG. 6 shows a configuration in which the content of the material included in the first material group (solid line) exponentially decreases from the substrate 1 side toward the outermost surface 4a side of the absorbent layer 4, and the content of the material included in the second material group (dashed line) exponentially increases from the substrate 1 side toward the outermost surface 4a side of the absorbent layer 4, in which the region on the substrate 1 side and the region on the outermost surface 4a side each have a uniform composition, and the point (location) where the content (concentration) of the first material group and the content (concentration) of the second material group are the same is located on the outermost surface 4a side when the absorbent layer 4 is divided into two equal parts in the thickness direction.
[0037] FIG. 7 shows a configuration in which the content of the material included in the first material group (solid line) decreases in a curved manner (like an S-shaped curve) from the substrate 1 side toward the outermost surface 4a of the absorbent layer 4, and the content of the material included in the second material group (dashed line) increases in a curved manner (like an S-shaped curve) from the substrate 1 side toward the outermost surface 4a of the absorbent layer 4, with the substrate 1 side region and the outermost surface 4a side region each having a uniform composition.
[0038] In the above-described embodiment, the absorption layer 4 has a content of compound material (material included in the first material group) having high absorbency for EUV light that decreases from the substrate 1 side toward the outermost surface 4a side, and a content of compound material (material included in the second material group) having high hydrogen radical resistance that increases from the substrate 1 side toward the outermost surface 4a side. This reduces shadowing and improves the rectangularity of the mask pattern, thereby improving the dimensional accuracy and shape accuracy of the pattern transferred onto the wafer and imparting hydrogen radical resistance, thereby making it possible to manufacture a photomask that can be used for a long period of time. In addition, the distribution of the content of each of the first material group and the second material group in this embodiment is not limited to the above-mentioned distribution, and may be a distribution that combines each of them.
[0039] In general, a reflective photomask blank needs to be processable for patterning. Among the above materials, it is known that tin oxide can be dry-etched with chlorine-based gas. Therefore, it is more preferable that the absorption layer 4 contains a material containing tin (Sn) and oxygen (O).
[0040] Furthermore, since the reflective photomask is exposed to a hydrogen radical environment, the reflective photomask cannot withstand long-term use unless the absorbing layer 4 contains an absorbing material (second material group) that is highly resistant to hydrogen radicals. In this embodiment, a material with a film reduction rate of 0.1 nm / s or less in a hydrogen radical environment with a power of 1 kW and a hydrogen pressure of 0.36 mbar or less using microwave plasma is defined as a material with high hydrogen radical resistance. Of the above materials, tin (Sn) alone is known to have low resistance to hydrogen radicals, but adding oxygen (O) increases the resistance to hydrogen radicals. As shown in Table 1, hydrogen radical resistance was confirmed in materials with an atomic ratio of tin (Sn) to oxygen (O) exceeding 1:2. This is because when the atomic ratio of tin (Sn) to oxygen (O) is 1:2 or less, not all of the tin (Sn) bonds become tin oxide (SnO2), and it is believed that an atomic ratio of more than 1:2 is necessary to turn the entire film into tin oxide (SnO2).
[0041] Table 1 shows hydrogen radical resistance according to the element ratio of Sn and O according to the embodiment of the present invention. The atomic ratio shown in Table 1 is the result of measuring a material formed into a film having a thickness of 1 μm by EDX (energy dispersive X-ray analysis). Here, when the atomic ratio of tin (Sn) and oxygen (O) is 1:2, variation was confirmed in repeated evaluations, and therefore it is indicated as "△" in Table 1. In this embodiment, "△" and "◯" are deemed to be acceptable since there is no problem in use.
[0042] [Table 1]
[0043] A material containing tin (Sn) and oxygen (O) that can be used to form the absorbing layer 4 preferably contains more oxygen than tin oxide of a stoichiometric composition. That is, the atomic ratio of tin (Sn) to oxygen (O) in the material of the absorbing layer 4 preferably exceeds 1:2. Furthermore, when the atomic ratio of tin (Sn) to oxygen (O) exceeds 1:3.5, the absorbency to EUV light decreases, so the atomic ratio of tin (Sn) to oxygen (O) is preferably 1:3.5 or less, and more preferably 1:3 or less. In other words, when the absorption layer 4 is formed of a material containing tin (Sn) and oxygen (O), the content of oxygen (O) is preferably within a range of 2 to 3.5 times the content of tin (Sn) in terms of atomic ratio.
[0044] Moreover, the absorbing layer 4 preferably contains tin (Sn) and oxygen (O) in total at 50 atomic % or more based on the entire absorbing layer 4. This is because, although there is a possibility that both the EUV light absorbency and the hydrogen radical resistance may decrease if the absorber layer 4 contains components other than tin (Sn) and oxygen (O), if the components are less than 50 atomic %, the decrease in both the EUV light absorbency and the hydrogen radical resistance is very slight, and there is almost no decrease in performance as the absorber layer 4 of an EUV mask (reflective photomask). In this embodiment, the absorbing layer 4 may contain 50 atomic % or more of the materials included in the first material group and the materials included in the second material group in total relative to the entire absorbing layer 4.
[0045] Materials other than tin (Sn) and oxygen (O) include, for example, Ta, Pt, Te, Zr, Hf, The absorption layer 4 may contain Ti, W, Si, Cr, In, Pd, Ni, Al, Ni, F, N, C, or H. For example, by mixing In within a range of, for example, 10 atomic % or more and less than 50 atomic %, it is possible to provide electrical conductivity to the film (absorption layer 4) while ensuring high absorption of EUV light, and therefore it is possible to improve the inspectability in mask pattern inspection using EUV light with a wavelength of 190 nm to 260 nm. Alternatively, when N or Hf is mixed within a range of, for example, 10 atomic % or more and less than 50 atomic %, it is possible to make the film quality of the absorption layer 4 more amorphous, and therefore the roughness and in-plane dimensional uniformity of the absorption pattern layer 41 after dry etching and the in-plane uniformity of the transferred image are improved.
[0046] As mentioned above, compound materials mainly composed of Ta have been used for the absorption layer of conventional EUV reflective photomasks. In this case, in order to obtain an optical density OD (Equation 1), which is an index showing the contrast of light intensity between the absorption layer and the reflection layer, of 1 or more, the film thickness needs to be 40 nm or more, and in order to obtain an OD of 2 or more, the film thickness needs to be 70 nm or more. The extinction coefficient k of Ta is 0.041, but by applying a compound material containing tin (Sn) and oxygen (O), which has an extinction coefficient k of 0.06 or more, to the absorption layer, according to Beer's law, it is possible to make the film thickness 17 nm or less even when obtaining an OD of 1 or more, and to make the film thickness 45 nm or less even when obtaining an OD of 2 or more. However, if the film thickness is 45 nm or more, the projection effect will be about the same as that of a conventional compound material mainly composed of Ta and having a film thickness of 60 nm. OD = -log(Ra / Rm) (Equation 1) Therefore, the thickness of the absorbing layer 4 is preferably 17 nm or more and 45 nm or less.
[0047] In addition, the absorption layer of conventional EUV reflective photomasks often uses an oxide film mainly composed of Ta for the top layer, which is the outermost surface, and a nitride film mainly composed of Ta for the bottom layer, and the absorption layer often has a boundary (interface) between the upper and lower layers. Therefore, when the cross-sectional shape of the absorption layer of a conventional EUV reflective photomask is observed after patterning by dry etching, a step may be generated at the boundary (interface) between the upper and lower layers. Since such a step in the absorption layer leads to a decrease in the dimensional accuracy and shape accuracy of the pattern transferred onto the wafer, it is desirable for the absorption layer to have no step after patterning.
[0048] [Example 1] Examples of the reflective photomask blank and the reflective photomask according to the present invention will be described below. 8, a reflective layer 12 was formed by stacking 40 layers of a laminated film made of a pair of silicon (Si) and molybdenum (Mo) on a synthetic quartz substrate 11 having low thermal expansion characteristics. The thickness of the reflective layer 12 was 280 nm. Next, on the reflective layer 12, a capping layer 13 made of ruthenium (Ru) was formed as an intermediate film to a thickness of 3.5 nm. Next, an absorption layer 14 having a region (layer) containing tin (Sn) and oxygen (O) and a region (layer) containing tantalum (Ta) and oxygen (O) was formed on the capping layer 13 to a thickness of 26 nm and 7 nm, respectively. Sputtering was performed continuously so as to prevent the formation of a boundary (interface). This point will be described in detail below.
[0049] In this embodiment, a film (layer) containing tin (Sn) and oxygen (O) was first formed on the capping layer 13 as the absorbing layer 14 to a thickness of 26 nm. Then, when the thickness of the film (layer) containing tin (Sn) and oxygen (O) reached 26 nm, the film (layer) containing tin (Sn) and oxygen (O) and the film (layer) containing tantalum (Ta) and oxygen (O) were simultaneously formed. In this way, the film (layer) containing SnO and TaO was formed to a thickness of about 0.5 nm. The film was formed to a thickness of 7 nm. Thereafter, the film (layer) containing tin (Sn) and oxygen (O) was completed, and the film (layer) containing tantalum (Ta) and oxygen (O) was formed to a thickness of 7 nm. In this way, the absorption layer 14 was formed so that no boundary (interface) would be generated between the region containing tin (Sn) and oxygen (O) and the region containing tantalum (Ta) and oxygen (O).
[0050] In the absorption layer 14 thus formed, the atomic ratio of tin (Sn) to oxygen (O) was 1:2.5 as measured by EDX (energy dispersive X-ray analysis), and the atomic ratio of tantalum (Ta) to oxygen (O) was 1:1.9 as measured by EDX (energy dispersive X-ray analysis). Furthermore, when measured by an XRD (X-ray diffraction device), the film quality of the absorbing layer 14 was amorphous, although slight crystallinity was observed.
[0051] Next, a back conductive film 15 made of chromium nitride (CrN) was formed to a thickness of 100 nm on the side of the substrate 11 on which the reflective layer 12 was not formed, thereby producing the reflective photomask blank 100 of Example 1. In Example 1, a multi-target sputtering device was used to deposit each film on the substrate 11. The thickness of each film was controlled by the sputtering time. The absorption layer 14 was deposited by reactive sputtering, with the O / Sn ratio being 2.5 and the O / Ta ratio being 1.9, by controlling the amount of oxygen introduced into the chamber during sputtering.
[0052] Next, a method for producing the reflective photomask 200 of the first embodiment will be described with reference to FIGS. As shown in FIG. 9, a positive chemically amplified resist (SEBP9012: manufactured by Shin-Etsu Chemical Co., Ltd.) was spin-coated on the absorption layer 14 of the reflective photomask blank 100 to a thickness of 120 nm, and baked at 110° C. for 10 minutes to form a resist film 16. Next, a predetermined pattern was drawn on the resist film 16 using an electron beam drawing machine (JBX3030: manufactured by JEOL Ltd.). Thereafter, a pre-baking treatment was carried out at 110° C. for 10 minutes, and then a development treatment was carried out using a spray developer (SFG3000: manufactured by Sigma Meltec Co., Ltd.). In this way, a resist pattern 16a was formed as shown in FIG.
[0053] Next, the absorbing layer 14 was patterned by dry etching using the resist pattern 16a as an etching mask and mainly using a chlorine-based gas. Thus, an absorbing pattern layer 141 was formed on the capping layer 13 as shown in FIG. Next, the resist pattern 16a was peeled off to produce a reflective photomask 200 of this example as shown in FIG.
[0054] In this embodiment, the transfer pattern (shape of the absorption pattern layer 141) formed on the absorption layer 14 was a pattern including a LS (line and space) pattern with a line width of 64 nm, an LS pattern with a line width of 200 nm for measuring the film thickness of the absorption layer using an AFM, and an absorption layer removed portion of 4 mm square for measuring the EUV reflectance, on a reflective photomask 200 for transfer evaluation. The LS pattern with a line width of 64 nm was designed in each of the x direction and the y direction as shown in FIG. 13 so that the influence of the projection effect due to EUV irradiation can be easily seen.
[0055] [Comparative Example 1] As Comparative Example 1, a conventional EUV reflective photomask blank was prepared as follows. As shown in FIG. 14, the lower layer 5 constituting the absorption layer is formed so that the atomic ratio of tantalum (Ta) and nitrogen (N) is 1:0.25 and the film thickness is 58 nm, and then the upper layer 6 constituting the absorption layer is formed so that the atomic ratio of tantalum (Ta) and oxygen (O) is 1:1.9. The lower layer 5 and the upper layer 6 were formed so as to have a thickness of 2 nm. Thus, a reflective photomask blank 30 of Comparative Example 1 was produced. A boundary (interface) was formed between the lower layer 5 and the upper layer 6 thus formed. Next, as shown in Fig. 15, a reflective photomask 300 of Comparative Example 1 was produced in the same manner as in Example 1. As shown in Fig. 15, the reflective photomask 300 of Comparative Example 1 includes an absorbing pattern layer (lower layer) 51 and an absorbing pattern layer (upper layer) 61 as the absorbing pattern layer 142. However, with respect to the absorbing pattern layer 142, TaN and TaO are separated into an upper layer and a lower layer, and the film is not one in which the composition changes continuously.
[0056] [Example 2] The absorbing layer 14 was formed so that the atomic ratio of tin (Sn) to oxygen (O) was 1:2.5. The total content of tin (Sn) and oxygen (O) was 55 atomic % of the entire absorbing layer 14, and the remaining 45 atomic % was Ta, and the absorbing layer 14 was formed so that the film thickness was 26 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 2 were produced in the same manner as in Example 1.
[0057] [Example 3] The absorbing layer 14 was formed so that the atomic ratio of tin (Sn) to oxygen (O) was 1:2.5. The total content of tin (Sn) and oxygen (O) was 95 atomic % of the entire absorbing layer 14, and the remaining 5 atomic % was Ta, and the absorbing layer 14 was formed so that the film thickness was 26 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 3 were produced in the same manner as in Example 1.
[0058] [Example 4] The absorbing layer 14 was formed so that the atomic ratio of tin (Sn) to oxygen (O) was 1:2.5. The total content of tin (Sn) and oxygen (O) was 95 atomic % of the entire absorbing layer 14, and the remaining 5 atomic % was Ta, and the absorbing layer 14 was formed so that the film thickness was 17 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 4 were produced in the same manner as in Example 1.
[0059] [Example 5] The absorbing layer 14 was formed so that the atomic ratio of tin (Sn) to oxygen (O) was 1:2.5. The total content of tin (Sn) and oxygen (O) was 60 atomic % of the entire absorbing layer 14, and the remaining 40 atomic % was Si, and the absorbing layer 14 was formed so that the film thickness was 33 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 5 were produced in the same manner as in Example 1.
[0060] [Example 6] The absorbing layer 14 was formed so that the atomic ratio of tin (Sn) to oxygen (O) was 1:2.5. The total content of tin (Sn) and oxygen (O) was 78 atomic % of the entire absorbing layer 14, and the remaining 22 atomic % was Si, and the absorbing layer 14 was formed so that the film thickness was 26 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 6 were produced in the same manner as in Example 1.
[0061] [Example 7] The absorbing layer 14 was formed so that the atomic ratio of tin (Sn) to oxygen (O) was 1:2.5. The total content of tin (Sn) and oxygen (O) was 95 atomic % of the entire absorbing layer 14, and the remaining 5 atomic % was Si, and the absorbing layer 14 was formed to a thickness of 17 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 7 were produced in the same manner as in Example 1.
[0062] (film thickness measurement) In each of the above-mentioned examples and comparative examples, the film thickness of the absorbing layer 14 was measured by a transmission electron microscope. (reflectance measurement) In each of the above-mentioned Examples and Comparative Examples, the reflectance Ra of the absorption pattern layer 141 region of the fabricated reflective photomask was measured by a reflectance measuring device using EUV light. In each of the above-mentioned examples and comparative examples, the reflectance Rm of the region other than the absorption pattern layer 141 region of the produced reflective photomask was measured by a reflectance measuring device using EUV light.
[0063] (Hydrogen radical resistance measurement) The reflective photomasks produced in each of the examples and comparative examples were placed in a hydrogen radical environment with a hydrogen pressure of 0.36 mbar or less at a power of 1 kW using microwave plasma. The change in film thickness of the absorption layer 14 after the hydrogen radical treatment was confirmed using an atomic force microscope (AFM). The measurement was performed using an LS pattern with a line width of 200 nm.
[0064] (Wafer exposure evaluation) Using an EUV exposure tool (NXE3300B, manufactured by ASML), the transfer patterns of the reflective photomasks prepared in each of the Examples and Comparative Examples were transferred and exposed onto a semiconductor wafer coated with an EUV positive chemically amplified resist. At this time, the exposure dose was adjusted so that the LS pattern in the x direction in FIG. 13 was transferred as designed. The transferred resist pattern was observed and line width was measured using an electron beam dimension measuring device to confirm the resolution. The evaluation results are shown in Table 2.
[0065] [Table 2]
[0066] The reflectance of a conventional tantalum (Ta)-based absorption layer having a thickness of 60 nm was 0.019 (OD=1.54), whereas in Example 3 in which the SnO mixing ratio was as high as 95%, the reflectance was good at 0.007 (OD=1.97). In contrast, in Example 4 in which the SnO mixing ratio was as high as 95% but the absorption layer 14 was made very thin at 17 nm, the reflectance was 0.059 (OD=1.05), and in Example 7, the reflectance was 0.061 (OD=1.03), which was lower. In addition, OD of 1.5 or more is represented as "◎", and OD of 1.0 or more and less than 1.5 is represented as "◯". If the OD is "◎" or "◯", there is no problem in use, so this example was passed.
[0067] Next, the hydrogen radical resistance of each Example and Comparative Example is shown. Here, materials with a film reduction rate of 0.1 nm / s or less are represented by "◎", and those with a film reduction rate of over 0.1 nm / s are represented by "×". In all of Comparative Example 1 and Examples 1 to 7, which are existing EUV reflective photomasks, the film reduction rate was 0.1 nm / s or less, and it was found that they had sufficient resistance. Next, the results of the evaluation of the cross-sectional shape after patterning of the absorption layer are shown. Here, the cross-section of the patterned absorption layer was visually observed with an SEM, and the presence of a step on the cross-section was marked with "x", and the absence of a step was marked with "◎".
[0068] As described above, the reflective photomask blanks and reflective photomasks of the respective Examples have a sufficient OD value, sufficient hydrogen radical resistance, and no steps are formed in the cross-sectional shape of the patterned absorption layer. Therefore, the reflective photomask blanks and reflective photomasks of the respective Examples improve the dimensional accuracy and shape accuracy of the pattern transferred onto the wafer, and are endowed with hydrogen radical resistance, making it possible to use the photomask for a long period of time. [Industrial Applicability]
[0069] The reflective photomask blank and reflective photomask according to the present invention can be suitably used for forming fine patterns by EUV exposure in the manufacturing process of semiconductor integrated circuits and the like. [Explanation of symbols]
[0070] 1...Substrate 2...Reflection layer 3…Capping layer 4…Absorption layer 4a...Top surface 5...Absorption layer (lower layer) 6...Absorption layer (upper layer) 41...Absorption pattern layer 51...Absorption pattern layer (lower layer) 61...Absorption pattern layer (upper layer) 10...Reflective photomask blank 20...Reflective photomask 30...Reflective photomask blank 11...Substrate 12...Reflection layer 13…Capping layer 14...Absorption layer 141...Absorption pattern layer 142...Absorption pattern layer (two-layer film) 15…Back conductive film 16...Resist film 16a...Resist pattern 17...Reflector 18…Low reflective part 100...Reflective photomask blank 200...Reflective photomask 300...Reflective photomask
Claims
1. A reflective photomask blank for producing a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, comprising: A substrate; A reflecting portion formed on the substrate for reflecting incident light; a low-reflection portion formed on the reflection portion and absorbing incident light, the low-reflection portion is a layer including at least one material selected from a first material group and at least one material selected from a second material group different from the first material group, the content of at least one material selected from the first material group decreases from the substrate side toward the outermost surface side of the low-reflection portion, the content of at least one material selected from the second material group increases from the substrate side toward the outermost surface side of the low-reflection portion, the first group of materials being tellurium (Te), cobalt (Co), nickel (Ni), platinum (Pt), silver (Ag), tin (Sn), indium (In), copper (Cu), zinc (Zn), and bismuth (Bi), and oxides, nitrides, and oxynitrides thereof; The second material group is tantalum (Ta), chromium (Cr), aluminum (Al), silicon (Si), ruthenium (Ru), molybdenum (Mo), zirconium (Zr), titanium (Ti), zinc (Zn), indium (In), vanadium (V), hafnium (Hf), and niobium (Nb), as well as oxides, nitrides, and oxynitrides thereof.
2. The reflective photomask blank according to claim 1, wherein the low-reflection portion has a total film thickness of at least 33 nm even when divided into multiple layers, and is a structure containing at least one material selected from the first material group in a total amount of 20 atomic % or more in the entire low-reflection portion.
3. The reflective photomask blank according to claim 1, wherein the low-reflection portion has a total film thickness of at least 26 nm even when divided into multiple layers, and is a structure containing at least one material selected from the first material group in a total amount of 55 atomic % or more in the entire low-reflection portion.
4. The reflective photomask blank according to claim 1, wherein the low-reflection portion has a total thickness of at least 17 nm even when divided into multiple layers, and is a structure containing at least one material selected from the first material group in a total amount of 95 atomic % or more in the entire low-reflection portion.
5. 5. The reflective photomask blank according to claim 2, wherein the outermost surface layer of the low-reflection portion is a structure containing at least one material selected from the second material group in a total amount of 80 atomic % or more.
6. When the thickness dimension of the low reflection portion is taken as 100%, and a region within 50% of the depth from the surface of the low reflection portion is taken as the outermost surface layer of the low reflection portion, 6. The reflective photomask blank according to claim 1 , wherein the outermost surface layer of the low-reflection portion is a structure containing at least one material selected from the second material group in a total amount of 80 atomic % or more.
7. 7. The reflective photomask blank according to claim 2, wherein the outermost surface layer of the low reflection portion has a film thickness of 0.5 nm or more and 30 nm or less.
8. A substrate; A reflecting portion formed on the substrate for reflecting incident light; a low-reflection portion formed on the reflection portion and absorbing incident light, the low-reflection portion is a layer including at least one material selected from a first material group and at least one material selected from a second material group different from the first material group, the content of at least one material selected from the first material group decreases from the substrate side toward the outermost surface side of the low-reflection portion, the content of at least one material selected from the second material group increases from the substrate side toward the outermost surface side of the low-reflection portion, the first group of materials being tellurium (Te), cobalt (Co), nickel (Ni), platinum (Pt), silver (Ag), tin (Sn), indium (In), copper (Cu), zinc (Zn), and bismuth (Bi), and oxides, nitrides, and oxynitrides thereof; The second material group is a reflective photomask that is made of tantalum (Ta), chromium (Cr), aluminum (Al), silicon (Si), ruthenium (Ru), molybdenum (Mo), zirconium (Zr), titanium (Ti), zinc (Zn), indium (In), vanadium (V), hafnium (Hf), and niobium (Nb), as well as oxides, nitrides, and oxynitrides thereof.
Citation Information
Patent Citations
Reflective mask blank, reflective mask, method for manufacturing the same and method for manufacturing semiconductor
JP2004006798A
Reflective mask blank, reflective mask, and exposure method of extremely short ultraviolet ray
JP2007250613A
Reflective mask blanks, reflective mask, and manufacturing method of semiconductor device
JP2007273678A
Reflection type photomask, reflection type photomask blank, and method of manufacturing the same
JP2011176162A
Radiation source, lithography apparatus, and device manufacturing method
JP2011530823A