Powdery ground improver and producing method thereof

A powdery ground improvement material with a powdery cement-based solidifying agent and thiosulfate additive addresses caking and chromium leaching issues, ensuring effective ground improvement under high humidity and environmental safety.

JP2024138693APending Publication Date: 2024-10-09TAIHEIYO CEMENT CORP

Patent Information

Application Number
JP2023049295
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Cement-based solidifying materials used for ground improvement can cause caking under high humidity conditions and may contaminate soil with hexavalent chromium, leading to leaching issues.

Method used

A powdery ground improvement material comprising a powdery cement-based solidifying agent and a powdery thiosulfate-containing additive with a water content of 3.0% or less, and a specific ratio of 0.5 to 10 parts by mass of the additive per 100 parts of the solidifying agent, which suppresses caking and hexavalent chromium elution.

Benefits of technology

The material prevents caking under high humidity and effectively reduces hexavalent chromium leaching, ensuring effective ground improvement without clumping or environmental contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138693000001
    Figure 2024138693000001
Patent Text Reader

Abstract

To provide a powdery ground improver that is a powdery ground improver containing a powdery cement-based solidifying material, even when relative humidity is such high as exceeding 60%, for instance, solidification (agglomeration) due to moisture absorption is difficult to occur, and, hexa-valent chromium can be suppressed from eluting.SOLUTION: A powdery ground improver comprising a powdery cement-based solidification material and a powdery thiosulfate-containing additive, wherein the powdery thiosulfate-containing additive has a water content of 3.0% or less, and an amount of the powdery thiosulfate-containing additive is 0.5 to 10 pts.mass per 100 pts.mass of the powdery cement-based solidification material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powdery ground improvement material and a method for producing the same. [Background technology]

[0002] As a method for improving soft ground, a method is known in which a slurry containing a cement-based solidification material (cement milk) is injected into the ground and mixed and stirred to increase the strength of the ground after improvement (solidification) (e.g., uniaxial compressive strength). On the other hand, when ground improvement (solidification) is carried out using cement-based solidification materials, there is a problem that hexavalent chromium (a harmful heavy metal) may leach from the improved ground because the cement may contain trace amounts of hexavalent chromium compounds. To solve this problem, various techniques have been proposed. For example, Patent Document 1 describes a hexavalent chromium elution-reducing agent for hydraulic substances, the main component of which is a reducing substance for hexavalent chromium (for example, blast furnace slag, thiosulfate, etc.). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-86322 A Summary of the Invention [Problem to be solved by the invention]

[0004] For example, if cement-based solidification materials are stored for a long period of time under high humidity conditions, such as when the relative humidity exceeds 60%, they may harden (form clumps) due to moisture absorption. In this case, the cement-based solidification materials may become unusable as materials for ground improvement work. In addition, it may be very time-consuming to recover and dispose of the cement-based solidification materials from storage facilities, etc. The object of the present invention is to provide a powdered ground improvement material containing a powdered cement-based solidification material, which is less likely to harden (clump) due to moisture absorption even under high humidity conditions, such as a relative humidity of more than 60%, and which can suppress the leaching of hexavalent chromium. [Means for solving the problem]

[0005] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned object can be achieved by a powdery ground improvement material comprising a powdery cement-based solidification material and a powdery thiosulfate-containing additive, wherein the powdery thiosulfate-containing additive has a water content of 3.0% or less and the amount of the powdery thiosulfate-containing additive is 0.5 to 10 parts by mass per 100 parts by mass of the powdery cement-based solidification material, and have completed the present invention.

[0006] The present invention provides the following [1] to [5]. [1] A powdered ground improvement material comprising a powdered cement-based solidification material and a powdered thiosulfate-containing additive, wherein the powdered thiosulfate-containing additive has a water content of 3.0% or less, and the amount of the powdered thiosulfate-containing additive is 0.5 to 10 parts by mass per 100 parts by mass of the powdered cement-based solidification material. [2] The powdered ground improvement material according to [1] above, wherein the powdered thiosulfate-containing additive contains sodium thiosulfate or potassium thiosulfate at a content of 80 mass% or more. [3] The powdered ground improvement material according to [1] or [2] above, wherein the powdered cement-based solidification material contains cement, gypsum, and ground granulated blast furnace slag. [4] A method for producing a powdered ground improvement material, comprising: a water content measuring step for measuring the water content of a powdered thiosulfate-containing additive; a selection step for selecting the powdered thiosulfate-containing additive as a material for a powdered ground improvement material when the water content obtained in the water content measuring step is 3.0% or less, and not selecting the powdered thiosulfate-containing additive as a material for a powdered ground improvement material when the water content obtained in the water content measuring step is more than 3.0%; and a mixing step for mixing the powdered thiosulfate-containing additive selected as the material for the powdered ground improvement material in the selection step with a powdered cement-based solidification material to obtain a powdered ground improvement material, wherein the amount of the powdered thiosulfate-containing additive in the mixing step is 0.5 to 10 parts by mass relative to 100 parts by mass of the powdered cement-based solidification material. [5] A ground improvement method using a powdery ground improvement material described in any one of [1] to [3] above, characterized in that the powdery ground improvement material is supplied to the ground to be improved, either as powder or mixed with water to form a slurry. Effect of the Invention

[0007] The powdered ground improvement material of the present invention contains a powdered thiosulfate-containing additive having a moisture content of 3.0% or less, and is therefore less likely to harden (form clumps) due to moisture absorption, even under high humidity conditions, such as a relative humidity of more than 60%. In addition, since the powdery soil improvement material of the present invention contains a thiosulfate, it is possible to suppress the elution of hexavalent chromium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The powdery soil improvement material of the present invention contains a powdery cement-based solidification material and a powdery thiosulfate-containing additive. [A. Powdered cement-based solidification material] In this specification, the term "cement-based solidification material" refers to a combination of cement and a cement admixture that is mixed as necessary. Examples of cement include various types of Portland cement such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, and low-heat Portland cement, mixed cements such as blast-furnace cement and fly ash cement, and ecocement. In addition, when blended cement is used as the cement, ground granulated blast furnace slag, fly ash, etc. contained in the blended cement are treated as cement admixtures described below, and are not included in the amount of cement described below.

[0009] The Blaine specific surface area of ​​the cement is preferably 2,500 to 6,000 cm 2 / g. The value is 2,500 cm 2 / g or more, the strength development of the ground improvement material is further improved. 2 When the molecular weight is 1 / g or less, the labor required for grinding during cement production does not become excessive. The amount of cement is preferably 45-70% by mass, more preferably 50-65% by mass, and particularly preferably 55-60% by mass, based on the proportion of the cement-based solidification material (100% by mass). When the proportion is 45% by mass or more, the strength development of the ground improvement material (for example, the uniaxial compressive strength of the improved ground) is further improved. When the proportion is 70% by mass or less, the proportion of ground granulated blast furnace slag can be increased, and the effect of suppressing the elution of hexavalent chromium can be further improved.

[0010] In the present invention, examples of cement admixtures include finely divided blast furnace slag, gypsum, silica fume, fly ash, dried finely divided fresh concrete sludge (fine powder obtained by drying and pulverizing the residue remaining after recovering aggregate from sludge water, returned concrete, or remaining concrete), and finely divided limestone. The Blaine specific surface area of ​​the ground granulated blast furnace slag is preferably 3,000 to 10,000 cm 2 / g. The value is 3,000 cm 2 / g or more, the strength development of the ground improvement material is further improved. 2 When the molecular weight is 1 / g or less, the material is easily available and the cost is not excessively high. The amount of ground granulated blast furnace slag is preferably 15-45% by mass, more preferably 20-40% by mass, and particularly preferably 25-35% by mass, based on the cement-based solidification material (100% by mass). When the ratio is 15% by mass or more, the effect of suppressing the elution of hexavalent chromium can be further enhanced. When the ratio is 45% by mass or less, the ratio of cement can be increased, and the strength development of the ground improvement material is further improved.

[0011] Examples of gypsum include anhydrite, hemihydrate, and dihydrate. The Blaine specific surface area of ​​the gypsum is preferably 2,000 to 5,000 cm 2 / g. The value is 2,000 cm 2 When the value is 5,000 cm / g or more, the reactivity of gypsum is improved. 2 When the viscosity is 100 / g or less, the strength development of the ground improvement material is further improved. The amount of gypsum (anhydride equivalent) is preferably 3 to 17 mass%, more preferably 5 to 15 mass%, and particularly preferably 7 to 13 mass%, in terms of the proportion in the cement-based solidification material (100 mass%). When the proportion is 3 to 17 mass%, the strength development of the ground improvement material is further improved. In addition, when gypsum hemihydrate or gypsum dihydrate is used as the gypsum, the mass of water in the gypsum is not included in the mass of the cement-based solidification material.

[0012] The amount of other cement admixtures (specifically, the total amount of silica fume, fly ash, and limestone fine powder) is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less, in terms of the ratio in the cement-based solidification material (100% by mass). When the ratio is 30% by mass or less, the ratios of cement, ground granulated blast furnace slag, and gypsum can be increased, improving the strength development of the ground improvement material and further enhancing the effect of suppressing the elution of hexavalent chromium.

[0013] [B. Powdered thiosulfate-containing additives] Examples of thiosulfates that are components of the powdered thiosulfate-containing additive include sodium thiosulfate and potassium thiosulfate. As the thiosulfate, a hydrate may be used, but from the viewpoint of the effect of the present invention (suppression of caking due to moisture absorption), an anhydrate is preferred. The content of thiosulfate in the powdery thiosulfate-containing additive is preferably 80% by mass or more, more preferably 84% by mass or more, even more preferably 88% by mass or more, and particularly preferably 92% by mass or more. Examples of components other than thiosulfate include various impurities contained in the raw materials used in the production of the powdered thiosulfate-containing additive.

[0014] The water content of the powdered thiosulfate-containing additive is 3.0% or less, more preferably 2.5% or less, even more preferably 2.0% or less, even more preferably 1.5% or less, even more preferably 1.0% or less, and particularly preferably 0.5% by mass or less. If the water content exceeds 3.0%, it becomes difficult to obtain the effect of the present invention (suppression of caking due to moisture absorption). In this specification, the term "water content" (unit: %) refers to the mass ratio of water to a solid in a dry state (one that does not contain water) multiplied by 100 ([mass of water] × 100 ÷ [mass of solid in a dry state]).

[0015] The particle size distribution of the powdered thiosulfate-containing additive is such that the proportion of particles having a particle size of 0.6 mm or less is 50% by mass or more (preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more). The amount of the powdered thiosulfate-containing additive is 0.5 to 10 parts by mass, preferably 1 to 8 parts by mass, more preferably 2 to 7.5 parts by mass, even more preferably 3 to 7 parts by mass, and particularly preferably 4 to 6 parts by mass, relative to 100 parts by mass of the powdered cement-based solidification material. If the amount is less than 0.5 parts by mass, it becomes difficult to obtain the effects of the present invention (particularly, the inhibition of caking due to moisture absorption), whereas if the amount exceeds 10 parts by mass, there are drawbacks such as an increase in costs due to the large amount of thiosulfate-containing additive.

[0016] [C. Other Materials] The powdery ground improvement material of the present invention can contain any material that can be blended (e.g., a powdery expansive material, a powdery cement admixture, etc.) other than the powdery cement-based solidification material and the powdery thiosulfate-containing additive. The amount of such optionally blendable materials (the total amount if two or more types are used) is preferably 10 mass% or less, more preferably 5 mass% or less, and particularly preferably 2 mass% or less, in terms of the proportion in the powdered ground improvement material (100 mass%).

[0017] [D. Method for producing the powdered ground improvement material of the present invention] The method for producing a powdery ground improvement material of the present invention includes: (a) a water content measuring step of measuring the water content of a powdery thiosulfate-containing additive (one type or two or more types); (b) a selection step of selecting the powdery thiosulfate-containing additive as a material for a powdery ground improvement material when the water content obtained in the water content measuring step is 3.0% or less, and conversely, not selecting the powdery thiosulfate-containing additive as a material for a powdery ground improvement material when the water content obtained in the water content measuring step is more than 3.0%; and (c) a mixing step of mixing the powdery thiosulfate-containing additive selected as the material for the powdery ground improvement material in the step (b) with a powdery cement-based solidification material to obtain a powdery ground improvement material. In step (c) (mixing step), the amount of the powdered thiosulfate-containing additive is 0.5 to 10 parts by mass (the preferred amount is as described above) relative to 100 parts by mass of the powdered cement-based solidification material.

[0018] [E. Ground improvement method] The ground improvement method using the powdered ground improvement material of the present invention (hereinafter referred to as the ground improvement method of the present invention) includes a ground improvement material supplying step of supplying the powdered ground improvement material of the present invention, either as powder or as a slurry (cement milk) by adding water, to the ground to be improved. The ground improvement may be carried out by injecting a slurry into the ground and mixing and stirring it, or by injecting a slurry into voids in the ground (using the ground improvement material as a grout material). The ground improvement method of the present invention can include a slurry preparation step of mixing the powdery ground improvement material of the present invention with water to prepare a slurry, prior to the ground improvement material supply step. In this case, the amount of water is preferably 40 to 80 parts by mass, more preferably 45 to 75 parts by mass, even more preferably 50 to 70 parts by mass, and particularly preferably 55 to 65 parts by mass, based on 100 parts by mass of the powdery ground improvement material. When the amount is 40 parts by mass or more, the pumpability is further improved. When the amount is 80 parts by mass or less, the strength (e.g., uniaxial compressive strength) of the improved ground (ground after solidification) can be further increased.

[0019] Unit volume of ground (soil) (1m 3 The amount of the powdery ground improvement material per unit area is preferably 50 to 500 kg, more preferably 100 to 400 kg. When the amount is 50 kg or more, the strength of the improved ground (e.g., uniaxial compressive strength) can be increased. When the amount is 500 kg or less, excessive costs can be avoided. EXAMPLES

[0020] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Example 1] (1) Materials used (a) Cement Ordinary Portland cement (Blaine specific surface area: 3,300 cm 2 / g) was used. (b) Ground granulated blast furnace slag Blaine specific surface area is 4,000cm 2 A commercially available product (a cement admixture manufactured by DC Corporation; product name: Cerament) with a molecular weight of 1000 g was used. (c) Plaster Blaine specific surface area is 3,500cm 2 / g was used. (d) Thiosulfate-containing additive A (Example): Sodium thiosulfate (water content: 0.1%; powder; proportion of particles having a particle size of 0.6 mm or less: 95% by mass; anhydrate; purity: 95% by mass or more; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (e) Thiosulfate-containing additive B (Example) Sodium thiosulfate (water content: 1.5%; powder; proportion of particles having a particle size of 0.6 mm or less: 77% by mass; anhydrous; purity: 89% by mass or more; made in China) (f) Thiosulfate-containing additive C (comparison example): Sodium thiosulfate (water content: 3.8%; powder; proportion of particles having a particle size of 0.6 mm or less: 57% by mass; anhydrous; purity: 92% by mass or more; made in China) (g) Thiosulfate-containing additive D (comparative example): sodium thiosulfate (water content: 52.2%; granular; proportion of particles having a particle size of 0.6 mm or less: 0% by mass; pentahydrate; purity: 99% by mass or more; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0021] (2) Preparation of soil improvement material A ground improvement material was obtained by mixing 60 parts by mass of cement, 30 parts by mass of ground granulated blast furnace slag, 10 parts by mass of gypsum (total of 100 parts by mass), and 5.0 parts by mass of "thiosulfate-containing additive A." (3) Measurement of the moisture content of the soil improvement material after long-term storage under high humidity 100 g of the soil improvement material obtained in (2) above was stored at a temperature of 15 to 25°C and a relative humidity of 80% for 720 hours (30 days), after which the moisture content was measured by the loss on drying method. The moisture content was 4.4%.

[0022] (4) Measurement of particle size distribution of soil improvement materials after long-term storage under high humidity At the same time point as in (3) above (after 30 days of storage), a sieving test was conducted on the soil improvement material. The results were as follows: (a) Percentage of particles with a particle size exceeding 4.75 mm: 0.2% by mass (b) The proportion of particles with a particle size of more than 2.80 mm and less than 4.75 mm: 0.6% by mass (c) The proportion of particles having a particle size of more than 2.00 mm and less than 2.80 mm: 6.8% by mass (d) Percentage of particles having a particle size of more than 1.00 mm and less than 2.00 mm: 30.6% by mass (E) Percentage of particles having a particle size of 1.00 mm or less: 61.8% by mass

[0023] [Examples 2 to 4, Comparative Examples 1 to 4] The experiment was carried out in the same manner as in Example 1, except that the constituent materials of the soil improvement material were changed as shown in Table 1. In Comparative Example 4, the soil improvement material was prepared without using a thiosulfate-containing additive. The above results are shown in Table 1. In Table 1, "blast furnace slag" refers to "ground granulated blast furnace slag." "Parts" refers to parts by mass.

[0024] [Table 1]

[0025] From Table 1, it can be seen that in Comparative Examples 1 to 4, for example, the proportion of granules having a particle size exceeding 4.75 mm was 1.2 to 8.6 mass%, and the degree of solidification (clumping) of the granules constituting the ground improvement material was large, whereas in Examples 1 to 4, the proportion was 0.2 to 0.8 mass%, and the progress of solidification (clumping) of the granules was suppressed. In particular, in Examples 1 and 2 in which thiosulfate-containing additives A and B were used in an amount of 5.0 parts by mass, the proportion of particles having a particle size of more than 2.80 mm and not more than 4.75 mm was 0.6% by mass for both, which shows that the progress of caking (lumping) of the particles was significantly suppressed. The moisture content of the ground improvement materials at this time was 2.3-4.7% in Examples 1-4 and 4.6-5.1% in Comparative Examples 1-3, and it was found that the difference in moisture content due to the different types of thiosulfate-containing additives was small. From this, it can be inferred that the difference in particle size distribution between the Examples and Comparative Examples is not due to the difference in moisture content of the ground improvement materials, but is due to the difference in moisture content of the thiosulfate-containing additives before long-term storage under high humidity (before moisture absorption).

Claims

1. A powdery ground improvement material comprising a powdery cement-based solidification material and a powdery thiosulfate-containing additive, The powdered thiosulfate-containing additive has a water content of 3.0% or less, and the amount of the powdered thiosulfate-containing additive is 0.5 to 10 parts by mass relative to 100 parts by mass of the powdered cement-based solidification material. A powdered ground improvement material.

2. The powdery ground improvement material according to claim 1, wherein the powdery thiosulfate-containing additive contains sodium thiosulfate or potassium thiosulfate at a content of 80 mass% or more.

3. 2. The powdered ground improvement material according to claim 1, wherein the powdered cement-based solidification material contains cement, gypsum, and ground granulated blast furnace slag.

4. A moisture content measuring step of measuring the moisture content of a powdery thiosulfate-containing additive; A selection process in which, when the moisture content obtained in the moisture content measurement process is 3.0% or less, the powdered thiosulfate-containing additive is selected as a material for the powdered ground improvement material, and, when the moisture content obtained in the moisture content measurement process is more than 3.0%, the powdered thiosulfate-containing additive is not selected as a material for the powdered ground improvement material; A mixing step of mixing the powdered thiosulfate-containing additive selected as a material for the powdered ground improvement material in the selection step with a powdered cement-based solidification material to obtain a powdered ground improvement material; and A method for producing a powdery ground improvement material, characterized in that in the mixing step, the amount of the powdery thiosulfate-containing additive is 0.5 to 10 parts by mass relative to 100 parts by mass of the powdery cement-based solidification material.

5. A ground improvement method using the powdery ground improvement material according to any one of claims 1 to 3, A ground improvement method comprising the steps of: supplying the above powdery ground improvement material either as powder or mixed with water to form a slurry, to the ground to be improved.

Citation Information

Patent Citations

  • Hexavalent chromium leach reducing agent for hydraulic material, and method for reducing hexavalent chromium leach

    JP2000086322A

  • Powder shape composition with hexavalent chromium elution preventing function and solidification agent added with the composition

    JP2009165812A

  • Foundation improver, improved soil and production method of improved soil

    JP2019178274A

  • Thermal storage material particle-containing resin pellet, and manufacturing method of thermal storage material particle-containing resin pellet

    JP2019218518A

  • Additive for ground improvement, and material for ground improvement, cement milk and ground improvement method based on that additive

    JP2021080408A

Cited By

  • Ground improvement body

    JP7850855B1