Lightweight foamed concrete raw material and method for producing lightweight foamed concrete
By using quicklime from seashells in the production of lightweight cellular concrete, the method addresses environmental conservation and equipment requirements, achieving stable compressive strength and crack prevention in ALC production.
Patent Information
- Application Number
- JP2023049418
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing lightweight aerated concrete (ALC) do not effectively utilize industrial waste for environmental conservation and require special equipment, leading to challenges in crack prevention and maintaining compressive strength.
Utilizing quicklime derived from seashells, processed by controlled heating and crushing, as a raw material for ALC, which is mixed with conventional materials to form a slurry, followed by autoclave curing, to produce lightweight cellular concrete with reduced shrinkage and improved crack resistance.
The method allows for stable maintenance of compressive strength comparable to conventional products, reduces greenhouse gas emissions, and effectively prevents cracking without requiring special equipment, while utilizing industrial waste for environmental benefit.
Smart Images

Figure 2024138752000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a raw material for lightweight cellular concrete and a method for producing lightweight cellular concrete. [Background technology]
[0002] Generally, lightweight aerated concrete (hereinafter referred to as ALC) is made by adding water to a mixture of silicate raw materials such as natural silica stone and silica sand, and calcareous raw materials such as quicklime made from limestone, cement, and gypsum, and then adding metallic aluminum to the mixture to foam it. The green cake obtained in the first curing step is then cut to the required size with a piano wire, and then the second curing step is performed using steam curing at high temperature and pressure in an autoclave.
[0003] The resulting ALC can be cut to the required dimensions to produce a variety of molded products, and used as building materials such as ALC panels for a wide range of applications including various exterior walls, partitions, roofs, and floors.
[0004] ALC panels can develop cracks for various reasons. For example, in Patent Document 1, attention is focused on reducing the drying shrinkage rate, and crack generation is controlled by adjusting the mixture ratio of inexpensive small grain siliceous raw material and the grain size of quartz crystals of another siliceous raw material.
[0005] Patent Document 2 describes a method for controlling cracks in large-scale ALC undergoing carbonation curing by using powdered steelmaking slag. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2001-19571 A [Patent Document 2] JP 2005-281087 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the method of Prior Patent Document 1 does not contribute to environmental conservation by using industrial waste. In addition, Prior Patent Document 2 is a shrinkage reduction measure related to a manufacturing method having a carbonation process for imparting moisture absorption and desorption properties to ALC, and cannot be immediately applied to the original manufacturing method of ALC.
[0008] Therefore, the present invention provides a raw material for ALC that can be produced using conventional production equipment without requiring any special equipment, is easy to control the quality of, has a small drying shrinkage rate, has excellent crack prevention performance, and can stably maintain the same level of compressive strength as conventional products, and a method for producing ALC using the raw material. [Means for solving the problem]
[0009] As a result of extensive research, the inventors have come up with the following invention. [1] Provided is a quicklime mixed raw material for lightweight cellular concrete, in which the weight ratio of the CaO component of the shell-derived quicklime to the weight of the CaO component in the limestone-derived quicklime is 20% to 100%. [2] The method for producing quicklime mixed raw material for ALC described in [1] is provided, in which coarsely crushed scallop shells are subjected to a heat treatment at 800°C to 1150°C and a refinement treatment until the 63 μm sieve residue is 50 mass% or less, thereby obtaining shell-derived quicklime. [3] Provided is a method for producing lightweight cellular concrete using the quicklime mixed raw material for ALC described in [1] and [2].
[0010] About shells Here, the shells include scallops, surf clams, clams, oysters, pearl oysters, etc., and large shells are preferred, with scallops being particularly preferred.
[0011] Method for baking and refining shells The coarsely crushed shells are stirred and fired at a temperature controlled at 800°C to 1150°C to produce calcined fired shell powder. A coarsely crushed shells is fed from the coarsely crushed shells fed from the coarsely crushed shells into a rotary kiln or electric furnace, which are preferably used for continuous firing at a temperature controlled at about 800°C to 1150°C while stirring the coarsely crushed shells.
[0012] The crusher is preferably a crusher having a crushing means such as a jaw crusher or a hammer crusher.
[0013] Electric furnace firing method for shells After the roughly crushed shells are finely pulverized, they are preferably fired in a stationary state in an electric furnace at a firing temperature controlled to about 800° C. to 1150° C. This is because there is no sliding caused by a rotor during firing.
[0014] The crusher used after firing is preferably a fine crusher such as a ball mill, a tube mill, or a vibration mill, which can ease the crushing conditions.
[0015] In the rotary kiln, various shells such as oysters, scallops, and pearl oysters are stored in a raw material tank and a specified amount of them is supplied to a coarse crusher, where they are roughly crushed to pieces, for example, about 8 mm in diameter and 10 mm in length. The coarsely crushed shells are then continuously fed into the rotary kiln at a specified speed, where they are fired to crush and pulverize them into fine powder.
[0016] Furthermore, in addition to the tumbling type, the material may be coarsely crushed using a roller type of a vertical mill or a fret mill. In this case, the roller mill type tends to result in over-crushing.
[0017] For example, in a rotary kiln, even coarsely crushed shells are fired at a controlled firing temperature of about 800°C to 1150°C while being stirred at a moderately slow rotation. The coarsely crushed shells are fired while being continuously rotated at a moderately slow rotation, crushed, and fired while being crushed into fine particles, and then converted into quicklime.
[0018] Furthermore, since the material is fired in a stationary state in an electric furnace, it can be pulverized using a fine grinder or the like after being removed from the electric furnace.
[0019] In calcined calcined shell powder, shells are a raw material that does not contain harmful impurities compared to quicklime made from limestone (a hard mineral), and is soft and porous, so when the shells are crushed appropriately and put into a furnace, they become a powder that is easily pulverized at a relatively low temperature compared to quicklime made from limestone (calcination temperature: about 1200°C to 1300°C). This calcined shell powder does not contain any particularly harmful impurities, and for example, in the case of scallops, the pH is high at 11 or higher, and the main component is CaO (about 96 wt%) with MgO and trace amounts of SiO2, Al2O3, FeO, and S.
[0020] The coarse powder is heat-treated in an electric furnace at 800° C. to 1150° C., preferably at a temperature of 850° C. to less than 1100° C. Examples of heat treatment times are 3 hours at 800° C., 1.5 hours at 1000° C., and 1 hour at 1100° C., and the higher the heating temperature, the more preferably the treatment is completed before or after a constant weight is reached in a short time.
[0021] TG-DTA Figure 1 shows the TG-DTA diagram of scallops when the temperature was increased from room temperature to 950°C at a rate of 10°C per minute. Up to 600°C, a weight loss of 2.25% due to the combustion of organic matter was observed, and from 600°C to 799°C, a weight loss due to decarbonation was observed. Above 800°C, the weight loss was limited to 0.07%.
[0022] Crushing The shell-derived quicklime after heating under the above conditions can be lightly crushed with a tumbling type crusher such as a ball mill or a tube mill, and the 63 μm residue (on the sieve) can be 50% by mass or less, and used as a raw material. The 63 μm residue is preferably 20% by mass to 45% by mass. If the 63 μm residue exceeds 50%, the compressive strength decreases. Also, if the 63 μm residue is less than 20% by mass, the material tends to be over-crushed and the shrinkage rate tends to increase, but this is superior to unsubstituted quicklime. Table 1 shows examples of the weight percentage of the residue on the sieve when the shell powder before firing and the shell powder crushed after firing are sieved through a 300 μm sieve, a 150 μm sieve, and a 63 μm sieve.
[0023] Particle size distribution [Table 1]
[0024] Figures 2 and 3 show SEM images of scallop shell powder before firing and after crushing. In the fine powder with a diameter of under 63 μm, after firing, most of the fine particles smaller than 20 μm, especially the needle-shaped particles, disappear, and most of the particles are crushed into aggregate particles of about 30 μm to 60 μm. The aggregate particles have gaps between each particle, and it can be observed that there is a peak in this area. When comparing particles with a diameter of 63 μm or more, there are relatively many block-shaped uncrushed particles centered around 100 μm. On the other hand, before firing, the particle size distribution range is wide, from needle-shaped fine particles where the shell is split vertically to relatively large fragments. For comparison, an SEM image of the quicklime that is usually used is shown in Figure 4. The fine particles are spherical rather than needle-shaped, and range from small particles to many, with many large particles, and the particle size distribution is wide.
[0025] An example of an X-ray diffraction chart of quicklime derived from calcined and crushed scallop shells is shown in Figure 5. The chart shows the results before and after the shells were heated at 800°C. Before calcination, the material is calcium carbonate, containing a lot of calcite and a small amount of aragonite, but after calcination, the crystalline portion is mostly quicklime, with trace amounts of calcium hydroxide evident, indicating a high level of purity.
[0026] As described above, the suitability of shell-derived quicklime for the present invention is obtained by carrying out specified coarse crushing, heating, and crushing in that order under specified coarse crushing, heating, and crushing conditions, and it is not possible to directly identify shell-derived quicklime having this suitability based solely on its structure or characteristics.
[0027] Raw materials blending ALC was produced using a specified amount of shell quicklime. Excess ALC was also used for production. Excess ALC that met the requirements described in Patent No. 6644184 was used. The raw material mixing ratio was 48 mass% of the excess ALC and silica stone combined, and the raw material mixing ratio was 28-40 mass% silica stone, 6-10 mass% quicklime, 12-22 mass% cement, 2-4 mass% gypsum, and 20-30 mass% (calculated from dry weight) of crust (excess end generated when cutting semi-hardened body before autoclave curing with piano wire and crushed with water), and 0.06 mass% of aluminum powder and water were added to the entire mixture to prepare a slurry.
[0028] Then, the quicklime is replaced with shell-derived quicklime in a predetermined amount of 20% to 100% by mass. At this time, it is preferable to add water later. In particular, it is preferable that the silica stone is dry. Effect of the Invention
[0029] The present invention provides a method for producing ALC with a small shrinkage ratio that does not require special measuring equipment, is easy to manage, does not require special calcination equipment, and is easy to manage quality. It uses shell-derived quicklime raw material at a solid content of 20% to 100% by mass, and can stably maintain the same compressive strength as conventional products. In addition, the amount of carbon dioxide absorbed by the shellfish while alive is equal to the amount of carbon dioxide generated by calcination, and the amount of carbon dioxide in the atmosphere does not increase or decrease during this period. In other words, the amount of carbon dioxide generated is essentially zero in this reaction process. If the thermal energy used for calcination is assumed to be solar power generation or other sources that do not emit carbon dioxide, the amount of carbon dioxide generated is essentially zero in the entire quicklime production process, resulting in reduced greenhouse gas emissions. [Brief description of the drawings]
[0030] [Figure 1] This shows the TG-DTA of scallop shells from room temperature to 950°C. [Diagram 2] FIG. 2 is a SEM image of pre-fired scallop shell powder. [Diagram 3] FIG. 2 shows an SEM image of scallop shell powder after baking. [Figure 4] FIG. 1 is a SEM image of a conventional quicklime powder. [Diagram 5] FIG. 1 shows an X-ray diffraction chart of quicklime raw material derived from crushed scallop shells. [Figure 6] FIG. 2 is a graph showing the pass / fail judgment of the drying shrinkage rate of the present invention. [Figure 7] FIG. 2 is a graph showing pass / fail results of the compressive strength test of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] Ingredients and composition The total amount of the silica stone manufactured by JFE Mineral Co., Ltd. and the shavings obtained in the ALC manufacturing process specified in Patent No. 6644184 were used as excess ALC, making up 48% by mass. The raw material mixing ratio was 8-20% by mass of excess ALC, 28-40% by mass of silica stone, 6-10% by mass of mixed quicklime manufactured by Yoshizawa Co., Ltd., with 20-100% of the quicklime derived from shells, 12-22% by mass of high-early-strength Portland cement manufactured by Taiheiyo Cement Co., Ltd., 2-4% by mass of dihydrate gypsum manufactured by Kokusai Shoji Co., Ltd., and 20-30% by mass of the crust, making up 100% by mass in total. 0.06% by mass of aluminum powder was added and mixed into this mixture.
[0032] Coarse grinding A hammer crusher was used for coarse crushing.
[0033] Heating method An electric furnace was used as the heater for the heat treatment.
[0034] Crushing method A small ball mill with a low rotation speed was used as the crusher.
[0035] The materials used were powdered siliceous raw materials such as silica stone and quartz, powdered calcareous raw materials such as the above-mentioned shell-derived quicklime, conventional quicklime, Portland cement, gypsum, and a foaming agent, which were mixed with water to form a mixed slurry, which was then placed in a formwork.The next step was to foam the mixture, which was created by the gas generated by a foaming agent made of metal powder such as aluminum.
[0036] After that, the piece was cut to a predetermined size and then subjected to a hydrothermal reaction in an autoclave at 180° C. and 10 atm to produce tobermorite.
[0037] By appropriately combining the raw materials, conditions, ranges, and methods described above, it is possible to obtain the lightweight cellular concrete of the present invention having excellent shrinkage characteristics.
[0038] To produce the shell-derived quicklime, scallop shells were selected as the raw material. The scallop shells were roughly crushed to produce a sample with a specific surface area of 6,578 (cm2 / cm3). The sample was fired for two hours in an electric furnace (manufactured by Kyoei Electric Furnace Manufacturing Co., Ltd., model: YK-15B) set at 1,000°C to produce the shell-derived quicklime, the raw material for the desired lightweight cellular concrete. The CaO purity of this quicklime was measured to be 95.0%. The CaO purity of the limestone-derived quicklime was 96.0%.
[0039] A slurry was obtained by mixing quicklime, water, silica stone, early strength cement, gypsum dihydrate, water, aluminum powder, and foam stabilizer in a mixer in the prescribed ratios shown in Table 2. The resulting slurry was poured into a formwork and hardened for about 4 hours by the hydration reaction of the limestone raw material, and then cured under high-temperature, high-pressure steam in an autoclave to create a test specimen.
[0040] [Table 2]
[0041] The central portion of the obtained specimen was cut with a cutter to dimensions of 40mm x 40mm x 160mm and 100mm x 100mm x 100mm, the former being used as the drying shrinkage test specimen and the latter as the compressive strength test specimen. Drying shrinkage and compressive strength tests were carried out on the specimens obtained by the above procedure in accordance with JIS A 5416. The measurement results of the drying shrinkage and compressive strength tests are shown in Table 2. Figure 6 shows a graph of the drying shrinkage judgment, and Figure 7 shows a graph of the compressive strength test judgment.
[0042] Therefore, when the proportion of CaO derived from shells is 20% or more and 100% or less, the drying shrinkage rate in Table 2 is smaller than that of Comparative Example 1, and resistance to cracking is high. Furthermore, since the compressive strength satisfies JIS A 5416, it has sufficient strength for use as an ALC member.
Claims
1. A quicklime mixed raw material for lightweight cellular concrete, in which the weight of the CaO component of the quicklime derived from shells is 20% to 100% of the weight of the CaO component in the quicklime derived from limestone.
2. The method for producing quicklime mixed raw material for ALC according to claim 1, wherein the coarse powder obtained by coarsely crushing scallop shells is heat-treated at 800°C to 1150°C and refined to a degree that the 63 μm sieve residue is 50 mass% or less, to obtain quicklime derived from shells.
3. A method for producing lightweight cellular concrete using the quicklime mixed raw material for ALC according to claim 1 or 2.
Citation Information
Patent Citations
Production of autoclaved lightweight concrete and autoclaved lightweight concrete panel obtained by the same
JP2001019571A
Method for producing building material
JP2005281087A