Catalyst for treating exhaust gases from biomass fuel combustion

A catalyst with manganese or iron supported on titanium oxide effectively addresses potassium poisoning in biomass fuel exhaust treatment, enhancing denitrification performance and maintaining catalyst activity.

JP2024138911APending Publication Date: 2024-10-09JGC CATALYSTS & CHEMICALS LTD

Patent Information

Application Number
JP2023049633
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing catalysts used in coal and thermal power plants to treat exhaust gases from biomass fuel combustion are ineffective in suppressing potassium (K) poisoning, leading to a decrease in catalyst activity.

Method used

A catalyst structure is developed with a specific amount of manganese (Mn) or iron (Fe) supported on a titanium oxide support, which adsorbs potassium and other poisonous substances, maintaining denitrification performance.

Benefits of technology

The catalyst effectively suppresses potassium poisoning, enhances initial denitrification performance, and maintains catalyst activity by adsorbing harmful elements, thereby improving the treatment of exhaust gases from biomass fuel combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138911000001
    Figure 2024138911000001
Patent Text Reader

Abstract

To provide a catalyst that is capable of inhibiting potassium poisoning.SOLUTION: A catalyst according to the present invention has a structure with an active metal component supported on a titanium oxide carrier. This catalyst includes at least one of manganese and iron. The total of manganese content in terms of MnO2 and iron content in terms of Fe2O3 is 0.03 wt.% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for treating exhaust gas generated after burning biomass fuel.

[0002] Coal and thermal power plants are equipped with catalysts to treat exhaust gases such as nitrogen oxides generated after fuel combustion. In recent years, biomass fuels have been used as fuels to reduce CO2 emissions. Unlike fossil fuels, biomass fuels contain potassium (K) and calcium (Ca). These elements are the cause (poisoning substances) of reducing the activity (poisoning) of the catalyst. In order to suppress Ca poisoning, a method of treating exhaust gas using a catalyst having deposit holes with a width of 4 to 20 μm and a depth of 20 to 300 μm is known (for example, Patent Document 1). The deposit holes are formed by mixing an oxide containing Ti, Si, and W with an oxide containing Ti and W and then firing the mixture. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2016-123954 Summary of the Invention [Problem to be solved by the invention]

[0004] In Patent Document 1, a catalyst having deposit holes is used, so that Ca poisoning can be suppressed. However, since no measures are taken to suppress K poisoning, when this catalyst is used to treat biomass fuel exhaust gas containing K, the activity of this catalyst decreases. In other words, the catalyst in Patent Document 1 has a problem in that it cannot suppress K poisoning. [Means for solving the problem]

[0005] The present inventors have found that a catalyst capable of suppressing K poisoning can be realized by including a specific amount of Mn or Fe in the catalyst. That is, the catalyst according to the present invention has a structure in which an active metal component is supported on a titanium oxide support, includes at least one of manganese and iron, and the sum of the manganese content calculated as MnO2 and the iron content calculated as Fe2O3 is 0.03% by weight or more. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0006] The present invention relates to a catalyst (hereinafter, simply referred to as catalyst) having a structure in which an active metal component is supported on a titanium oxide support. The active metal component is NO x The catalyst has the ability to react with NH3 and decompose it into N2 (denitrification performance). This catalyst contains manganese (Mn) or iron (Fe). Mn and Fe adsorb potassium (K), which is a poison of the active metal component, and therefore prevent K from being adsorbed to the active metal component. In other words, catalyst poisoning can be suppressed, and the decrease in the denitrification performance of the catalyst can be suppressed. The total of the Mn content and Fe content in the catalyst is 0.03% by weight or more. This makes it easier to suppress K poisoning of the catalyst. This total is preferably 0.1% by weight or more. On the other hand, in a catalyst, the lower the Mn and Fe content, the higher the content of the active metal component and titanium oxide support can be, and the lower the NO x This can increase the initial activity of the reaction that decomposes MnO2 to N2. Therefore, the total content of Mn and Fe in the catalyst is preferably 4% by weight or less, more preferably 3% by weight or less, and even more preferably 1% by weight or less. Here, the Mn content is expressed as a percentage converted into MnO2, and the Fe content is expressed as a percentage converted into Fe2O3.

[0007] Mn and Fe can also adsorb poisoning substances other than K. Examples of poisoning substances include alkali metals, alkaline earth metals, arsenic (As), and lead (Pb). A catalyst containing both Mn and Fe suppresses catalyst poisoning caused by more types of poisoning substances than a catalyst containing only one of them. In order to enhance the effect of suppressing catalyst poisoning, it is preferable that the catalyst contains 0.01 wt% or more of Mn in MnO2 conversion and 0.03 wt% or more of Fe in Fe2O3 conversion. The lower the content of Mn and Fe in the catalyst, the higher the content of the active metal component and titanium oxide carrier of the catalyst can be, and therefore the higher the initial activity of the catalyst can be. Therefore, the content of Mn is preferably 3 wt% or less in MnO2 conversion. The content of Fe is preferably 1 wt% or less.

[0008] The active metal component is easily bonded to the titanium oxide carrier. The active metal component bonded to the titanium oxide carrier has high denitration performance. In addition, a catalyst whose main component is titanium oxide is easy to mold. For these reasons, the titanium oxide content in the catalyst is preferably 60% by weight or more, more preferably 65% ​​by weight or more, and even more preferably 75% by weight or more, calculated as TiO2. The crystal structure of the titanium oxide is preferably anatase type. By using such titanium oxide, the denitration performance is likely to be improved. In addition, the crystallite diameter calculated from the half-width of the diffraction peak of the (101) plane of the anatase type is preferably 5 to 40 nm. When this crystallite diameter is within this range, the titanium oxide is easily bonded to the active metal component. This crystallite diameter is more preferably 5 to 10 nm or less.

[0009] Examples of active metal components include vanadium (V), chromium (Cr), nickel (Ni), copper (Cu), silver (Ag), gold (Au), palladium (Pd), yttrium (Y), cerium (Ce), neodymium (Nd), indium (In), and iridium (Ir) and their oxides. Among these, V and its oxides are inexpensive and have a high decomposition rate of organic halogen compounds contained in exhaust gas. The higher the content of the active metal components in the catalyst, the higher the denitrification performance tends to be. Therefore, the V content is preferably 0.1% by weight or more, and more preferably 3% by weight or more. If this content is too high, the cost increases. Therefore, the V content is preferably 10% by weight or less, more preferably 5% by weight or less, and even more preferably 2% by weight or less. In addition, in a catalyst that does not contain Fe and Mn, the lower the content of the active metal components, the more likely the performance is to deteriorate due to catalyst poison. Therefore, a catalyst having a low content of active metal components (for example, 2.0% by weight or less) is more likely to be effective in suppressing the decrease in denitration performance than a catalyst having a high content of active metal components.

[0010] Tungsten (W) can suppress the transition of the crystal structure of titanium oxide from anatase to rutile. Therefore, it is preferable that the catalyst contains W, and the W content in the catalyst is preferably 3.5% by weight or more in terms of WO3. On the other hand, in order to facilitate the bonding of the active metal component and the titanium oxide support, the W content in the catalyst is preferably 9% by weight or less in terms of WO3.

[0011] Silicon (Si) can suppress the transition of the crystal structure of titanium oxide from anatase to rutile. Therefore, it is preferable that the catalyst contains Si. In order to facilitate the bonding of the active metal component and the titanium oxide support, the catalyst preferably contains 0.1% by weight or more of Si, calculated as SiO2, and more preferably 1.0% by weight or more. On the other hand, in order to improve the moldability of the catalyst, the Si content in the catalyst is preferably 7% by weight or less, calculated as SiO2, and more preferably 3% by weight or less.

[0012] Molybdenum (Mo) can suppress SO2 poisoning of the catalyst. Therefore, it is preferable that the catalyst contains Mo, and the Mo content in the catalyst is preferably 0.05 wt% or more calculated as MoO3. On the other hand, the Mo content in the catalyst is preferably 0.5 wt% or less calculated as MoO3. When the Mo content is within this range, the catalyst can contain a large amount of active metal components and titanium oxide support.

[0013] Sulfur affects the band structure of V, improving the denitration performance of the catalyst. Therefore, it is preferable that the catalyst contains sulfur (S). Furthermore, the S content in the catalyst is preferably 0.1 wt% or more, and more preferably 0.5 wt% or more, calculated as SO4. On the other hand, the lower this content is, the higher the content of the active metal component and titanium oxide support of the catalyst can be. Therefore, the S content of the catalyst is preferably 5 wt% or less, more preferably 4 wt% or less, and even more preferably 3 wt% or less.

[0014] Examples of catalyst shapes include pellets and honeycombs. A honeycomb structure has many small holes (cells) that run parallel to each other. Examples of honeycomb structure shapes include hexagonal columns, rectangular parallelepipeds, and cylinders. Examples of cell shapes include hexagons, rectangles, and circles. Usually, the size (diameter) of a cell is called the aperture, the space between cells is called the wall, and when focusing on one cell, the distance between the centers of the opposing left and right or top and bottom walls is called the pitch. In a honeycomb structure, the turbulent components of the flow in the exhaust gas are increased, improving the diffusion efficiency of the exhaust gas. As a result, the denitrification efficiency is high.

[0015] NO x As a method for decomposing NO x There is a method in which a reducing agent such as ammonia is added to and brought into contact with a gas containing potassium to cause a reduction reaction. The catalyst of the present invention can be used in this reduction reaction. In particular, since the exhaust gas generated after burning biomass fuel contains a lot of potassium, it is suitable to use a catalyst to treat this exhaust gas. The temperature for reducing this exhaust gas is 200 to 500°C.

[0016] The method for producing the catalyst is described below. A mixture containing a titanium-containing oxide and water is prepared in a <mixture preparation step>. The mixture is kneaded until the water concentration in the mixture is 25-35% by weight in a <kneading step>. The mixture is molded to obtain a molded product in a <molding step>. The molded product is dried at 30-200°C in a <drying step>. The dried molded product is fired at 450-700°C in a <firing step>. Raw materials for the active metal component are added to the mixture during kneading. An Fe or Mn compound is added in any step prior to firing. The production method is described in detail below.

[0017] In the mixture preparation step, a mixture containing a titanium-containing oxide and water is prepared. Examples of the oxide containing titanium include titanium oxide and composite oxides with other metals (Si, W, Mo, etc.). When using solid raw materials, it is preferable to mix them in a powder state. When the raw materials are powders, it is easy to obtain a catalyst in which each component is contained in a uniformly dispersed state. By adding ammonia to the mixture, it is easy to obtain a catalyst in which each component is contained in a more uniformly dispersed state. The moisture content of all the raw materials before kneading the raw materials is 38 to 50% by weight. If the moisture content is lower than 38% by weight, the titanium-containing oxide and water cannot be mixed well. If the moisture content is higher than 50% by weight, the viscosity of the mixture is low, making it difficult to knead.

[0018] Next, the mixture with a water content of 38-50% by weight is kneaded until the water concentration becomes 25-35% by weight. While kneading the mixture, the raw material of the active metal component is added. As this raw material, a V compound is preferable. As the V compound, vanadate, V sulfate, V chloride, etc. are preferably used, and ammonium metavanadate is particularly preferably used. In order to facilitate dispersion of V in the catalyst, it is preferable to add the V compound in the form of an aqueous solution. In particular, it is preferable to dissolve V oxide with an acid. By adding monoethanolamine to the aqueous solution of the V compound, V becomes more easily dispersed in the catalyst.

[0019] The Fe or Mn compound may be added to any mixture prior to the forming step (or to the water prior to preparing the mixture), or may be added by impregnation after forming. Adding these compounds prior to forming eliminates the need for impregnation and subsequent drying, thereby increasing production efficiency. Examples of Fe compounds include Fe salts and oxides. Examples of Mn compounds include Mn salts and oxides. Of the salts, sulfates are preferred because they place less strain on the equipment and the environment. Furthermore, if sulfates are used, S can be added to the catalyst. Adding Fe or Mn in the form of an aqueous solution makes it easier for Fe and Mn to be dispersed in the catalyst, making it easier to suppress catalyst poisoning.

[0020] Also, compounds of Si, W, and Mo can be added to any mixture prior to the molding step (or to water prior to preparation of the mixture). These can be in the form of salts or oxides. These may be contained in titanium-containing oxides.

[0021] The mixture with the moisture content adjusted to 25 to 35% by weight is molded to produce a molded product. The molding method can be extrusion molding. Adding a molding aid makes molding easier. Examples of the molding aid include polyethylene oxide, crystalline cellulose, glycerin, polyvinyl alcohol, etc. The molding aid is preferably added during kneading. Glass fiber may be added to increase strength.

[0022] The molded product is dried at 30 to 200°C for at least 1 hour, and then calcined at 450 to 700°C for at least 1 hour to obtain the catalyst. EXAMPLES

[0023] The production method of the catalyst and the physical properties of the catalyst will be described in detail below with reference to examples. The present invention is not limited to the following examples.

[0024] [Example 1] <Mixture preparation process> A mixture was prepared by mixing 7.57 kg of Ti-W composite oxide raw material (TiO2 / WO3=93 / 7), 15.46 kg of Ti-W-Si composite oxide raw material (TiO2 / WO3 / SiO2=90 / 5 / 5), 229 g of Mn carbonate (manufactured by Nippon Denko Co., Ltd.), and water using the method described in the examples of JP2016-123954A.

[0025] <Mixing process> While kneading this mixture, 415g of 42 wt% ferric sulfate solution (manufactured by Jujo Synthetic Chemical Industry Co., Ltd.) as an Fe compound in terms of Fe2(SO4)3, 1300g of ammonium metavanadate (manufactured by Shinko Chemical Industry Co., Ltd.), 62g of ammonium molybdate (manufactured by Taiyo Koko Co., Ltd.), 2.5kg of 15 wt% ammonia water, water, 188g of polyethylene oxide (Alkox E-160 manufactured by Meisei Chemical Industry Co., Ltd.), and 188g of carboxymethylcellulose (manufactured by Nichirin Co., Ltd.) were added to the mixture. The mixture was then kneaded until the water concentration reached 30 wt%.

[0026] <Forming process, drying process, firing process> The mixture was extruded into a honeycomb shape (80 mm long, 80 mm wide, 450 mm high, cells were rectangular in the height direction (parallel to the long side) with 10 × 10 holes) to obtain a molded product. This molded product was dried at 110°C for more than 1 hour, and then calcined at 540°C for more than 1 hour to obtain a catalyst.

[0027] The preparation conditions of the catalyst are shown in Table 1. The obtained catalyst was analyzed and evaluated as follows. The preparation conditions and analysis and evaluation results of the following examples and comparative examples are also shown in Table 1.

[0028] (1) Catalyst composition (elemental analysis) SO4 Approximately 0.1g of the sample was placed in a crucible, and a combustion improver (Fe·Tin (Sn)·W) was added. The crucible was then set in the device (LECO CS844). It was heated with a high-frequency current to generate SO2, which was then detected and quantified. This value was converted to SO4.

[0029] V, Fe, Mn, W, Si, Mo Approximately 0.2g was taken in a zirconium crucible, 2g of Na2O2 and 1g of NaOH were added, and melted. After melting, 20ml of (1+1) sulfuric acid and water were added to dissolve, and the test solution was diluted to 500ml in a measuring flask. Measurements were performed using an ICP-OES (Agilent 5800 or Shimadzu ICPS-8100). V, Fe, Mn, W, Si, and Mo were measured and converted to V2O5, Fe2O3, MnO2, WO3, SiO2, and MoO3, respectively.

[0030] (2) Denitrification performance (selective catalytic reduction (SCR) activity) and deterioration test The denitration performance was measured as follows. The catalyst was cut into a rectangular parallelepiped (16 mm long, 16 mm wide, 107 mm high, the cell was a square with 2 × 2 holes in the height direction (parallel to the long side)) to prepare an evaluation sample. This was packed into a flow-type reactor. Gas (gas composition: NO x = 180 ppm, NH3 = 180 ppm, SO x = 500 ppm, O2 = 7%, H2O = 10%, N2 = balance) in the reactor SV: 18750 h -1 The gas was passed through the catalyst under the conditions of 100°C and contacted with the evaluation sample at 320°C. x The value (denitrification rate η) calculated from the concentration using the following formula* is denitrification rate η O The denitrification rate η O are also listed in Table 1.

[0031] Denitrification rate η (%) = [NO in gas before contact x (ppm)-NO in gas after contact x (ppm)] / NO in gas before contact x (ppm) × 100 *

[0032] Furthermore, the reaction rate constant K of the catalyst (initial reaction rate constant K o The higher this value, the higher the denitration performance of the catalyst. K=-V s ×ln(1-([η / 100] / α)) ·······*2 Here, V s is the areal velocity (m3 / (m 2 ×h)) and V s = Volume of catalyst (in this embodiment, 16 mm × 16 mm × 107 mm) ÷ External surface area of ​​honeycomb cell (in this embodiment, cell width 6.7 mm × height 107 mm × 4 (mesh) × 4 (surfaces)) × SV (in this embodiment, 18750 h -1 ) α is the NH3 concentration in the gas before contact C NH3 And NO x Concentration C NOX Ratio of (C NH3 / C NOX ) (in this embodiment, C NH3 / C NOX =180ppm / 180ppm=1).

[0033] The deterioration test was carried out as follows. A catalyst having the same shape as the evaluation sample was immersed in a 3.4% KCl solution, dried at 60°C for 15 hours, and calcined at 320°C for 1.5 hours to prepare a deterioration test sample. The denitrification rate η1 of the deterioration test sample was measured in the same manner as the evaluation sample, and the reaction rate constant K (reaction rate constant K1 after deterioration) was calculated. Furthermore, K1 / K o was calculated. In addition, NO in the gas x The concentration was measured using a chemiluminescence nitrogen oxide analyzer (ECL-88AO, manufactured by Anatech Yanaco Co., Ltd.).

[0034] [Example 2] This example is the same as Example 1, except that Mn carbonate was not mixed in the mixture preparation step.

[0035] [Example 3] This example is the same as Example 1, except that no ferric sulfate liquid was added in the kneading step.

[0036] [Example 4] This example is similar to Example 1, except for the following differences: 681 g of Mn carbonate was added in the mixture preparation step; 1052 g of ferric sulfate liquid was added in the kneading step; and 206 g of ammonium metavanadate was added in the kneading step.

[0037] [Example 5] This example is similar to Example 4, except for the following differences: 37 g of Mn carbonate was added in the mixture preparation step, and 70 g of ferric sulfate liquid was added in the kneading step.

[0038] [Comparative Example 1] This example is similar to Example 1, except for the following differences: Mn carbonate was not mixed in the mixture preparation step, and ferric sulfate liquid and ammonium molybdate were not added in the kneading step.

[0039] [Comparative Example 2] This example is similar to Example 5, except for the following differences: Mn carbonate was not mixed in the mixture preparation step, and ferric sulfate liquid and ammonium molybdate were not added in the kneading step.

[0040] [Table 1]

Claims

1. A catalyst for treating exhaust gas generated after burning biomass fuel, The structure is that active metal components are supported on a titanium oxide carrier. Contains at least one of manganese and iron, MnO 2 The manganese concentration in terms of Fe 2 O 3 The catalyst has a total concentration of 0.03% by weight or more.

2. the active metal component is vanadium; The vanadium is V 2 O 5 The catalyst according to claim 1, characterized in that it contains 0.1 to 2% by weight in terms of converted value.

3. 3. The catalyst according to claim 1, further comprising manganese and iron.

4. the active metal component is vanadium; The vanadium is V 2 O 5 Containing 0.1 to 10% by weight in terms of The titanium is TiO 2 Contains 65% or more by weight, Silicon is converted to SiO 2 Containing 0.1 to 7% by weight in terms of Tungsten WO 3 The catalyst according to claim 1, characterized in that it contains 3.5 to 9% by weight in terms of converted amount.

Citation Information

Patent Citations

  • Low temperature denitration catalytic addictive and preparation method thereof

    CN103537279A

  • NH3-SCR catalyst for resisting multiple poisoning and preparation method thereof

    CN112844366A

  • Honeycomb catalyst for coal and biomass mixed combustion exhaust gas treatment, production method thereof, and coal and biomass mixed combustion exhaust gas treatment method using the same

    JP2016123954A

  • Alkali resistant catalyst

    US20090285741A1

  • Nanoparticular metal oxide / anatase catalysts

    US20120014854A1

Cited By

  • Exhaust gas treatment catalyst, and exhaust gas treatment method

    WO2025238945A1