Method for producing modified metal oxide particles, modified metal oxide particles, photocurable composition, and cured product

By modifying metal oxide particles through heating in a nitrogen-containing polar solvent, the method addresses optical property impairment in optical members, enhancing transparency and reducing heat damage in translucent compositions.

JP2024138960AInactive Publication Date: 2024-10-09TOKYO OHKA KOGYO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023049698
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Optical members containing metal oxide particles produced by the solvothermal method often suffer from impaired optical properties when exposed to light, particularly in translucent compositions, and photosensitive compositions used for these members can cause heat damage.

Method used

The method involves heating crude metal oxide particles, potentially surface-treated with a capping agent, in a nitrogen-containing polar organic solvent containing water to modify their surfaces, resulting in modified metal oxide particles that can be incorporated into a photocurable composition to enhance optical properties.

Benefits of technology

The modified metal oxide particles improve the optical properties of translucent compositions, allowing for the production of cured products with better transparency and reduced heat damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138960000001
    Figure 2024138960000001
  • Figure 2024138960000002
    Figure 2024138960000002
  • Figure 2024138960000003
    Figure 2024138960000003
Patent Text Reader

Abstract

To provide: a method for producing modified metal oxide particles that, when added to a translucent composition, provide a translucent composition that exhibits good optical properties; modified metal oxide particles produced by the method; a photocurable composition that comprises the modified metal oxide particles and a transparent base material component; and a cured product of the photocurable composition.SOLUTION: Crude metal oxide particles prepared by a solvothermal method, which may be optionally surface-treated with a capping agent, are heated in a nitrogen-containing polar organic solvent containing water so as to produce modified metal oxide particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing modified metal oxide particles by subjecting crude metal oxide particles to a specified treatment, modified metal oxide particles that can be produced by the method, a photocurable composition containing the modified metal oxide particles, and a cured product made of the photocurable composition. [Background technology]

[0002] Conventionally, various inorganic particles have been blended into compositions used to form materials with various functions in order to impart functionality to the materials. For example, high refractive index materials are used to form optical components. As high refractive index materials, for example, compositions in which metal oxide particles such as titanium oxide and zirconium oxide are dispersed in an organic component are used (Patent Documents 1 and 2). Metal oxide particles such as titanium oxide and zirconium oxide are generally produced by a solvothermal method, which is a method for producing metal oxide particles by reacting raw material compounds, which are precursors of metal oxide particles, in a solvent at a predetermined temperature and a predetermined pressure. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] WO 2020 / 106860 [Patent Document 2] International Publication No. 2019 / 017305 Summary of the Invention [Problem to be solved by the invention]

[0004] Optical elements made of a composition in which metal oxide particles are dispersed in an organic component are often exposed to light. Furthermore, when forming a light-transmitting optical member or the like, a photosensitive composition that is cured by exposure to light is often used because there is no heat damage to the materials constituting the device equipped with the optical member. However, when the composition constituting the optical component contains metal oxide particles produced by a solvothermal method, the optical properties of the optical component are often impaired due to exposure during production of the optical component or exposure of the optical component itself.

[0005] The present invention has been made in consideration of the above problems, and has an object to provide a method for producing modified metal oxide particles which, when added to a light-transmitting composition, give a light-transmitting composition exhibiting good optical properties, modified metal oxide particles produced by the method, a photocurable composition containing the modified metal oxide particles and a transparent base component, and a cured product of the photocurable composition. [Means for solving the problem]

[0006] The present inventors have found that the above-mentioned problems can be solved by heating crude metal oxide particles prepared by a solvothermal method, which may be optionally surface-treated with a capping agent, in a nitrogen-containing polar organic solvent containing water to produce modified metal oxide particles, and have thus completed the present invention. Specifically, the present invention provides the following.

[0007] A first aspect of the present invention is a method for producing a crude metal oxide particle (A) selected from crude metal oxide particles (A1) prepared by a solvothermal method and crude metal oxide particles (A2) obtained by capping the surfaces of the crude metal oxide particles (A1) with a capping agent, the method comprising dispersing the crude metal oxide particles (A) in a nitrogen-containing polar organic solvent (S) containing water; and heating crude metal oxide particles (A) in a nitrogen-containing polar organic solvent (S) to obtain modified metal oxide particles having a modified surface.

[0008] A second aspect of the present invention is modified metal oxide particles produced by the method according to the first aspect.

[0009] A third aspect of the present invention is a photocurable composition comprising the modified metal oxide particles according to the second aspect and a transparent substrate component.

[0010] A fourth aspect of the present invention is a cured product of the photocurable composition according to the third aspect. Effect of the Invention

[0011] According to the present invention, there can be provided a method for producing modified metal oxide particles which, when added to a light-transmitting composition, provide the light-transmitting composition with good optical properties, modified metal oxide particles produced by the method, a photocurable composition containing the modified metal oxide particles and a transparent base component, and a cured product of the photocurable composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Method for producing surface-modified metal oxide particles> The method for producing surface-modified metal oxide particles includes dispersing crude metal oxide particles (A) in a nitrogen-containing polar organic solvent (S) containing water, and heating the crude metal oxide particles (A) in the nitrogen-containing polar organic solvent (S).

[0013] <Coarse metal oxide particles (A)> The crude metal oxide particles (A) are selected from crude metal oxide particles (A1) prepared by a solvothermal method and crude metal oxide particles (A2) obtained by capping the surfaces of the crude metal oxide particles (A1) with a capping agent. The "solvothermal method" is a method for producing metal oxide particles by reacting a raw material compound, which is a precursor of the metal oxide particle, in a solvent at a predetermined temperature and a predetermined pressure. The raw material compound used in the solvothermal method is typically an organometallic compound such as a metal alkoxide.

[0014] Impurities originating from the raw material compounds and the solvent used in the solvothermal process are attached or bonded to the particle surfaces of the crude metal oxide particles (A1) prepared by the solvothermal process. Furthermore, on the surface of the crude metal oxide particles (A2) obtained by capping with a capping agent, there is present capping agent that is not bonded to the surface of the crude metal oxide particles (A2) or that is bonded incompletely to the surface of the crude metal oxide particles (A2). For this reason, the crude metal oxide particles (A) often contain organic substances or organic groups. The amount of organic substances contained in the crude metal oxide particles (A) is measured by thermogravimetric analysis (TGA). The amount of organic substances contained in the crude metal oxide particles (A) is preferably 5% by mass or more and 20% by mass or less, more preferably 10% by mass or more and 15% by mass or less, based on the mass of the crude metal oxide particles (A).

[0015] As the metal oxide particles constituting the crude metal oxide particles (A), various metal oxide particles that have been conventionally used for various purposes can be used without any particular limitation.

[0016] The type of metal oxide constituting the crude metal oxide particles (A) is not particularly limited as long as the desired effect is not impaired. The crude metal oxide particles (A) may be particles made of a single metal oxide or particles made of two or more metal oxides. The metal oxide constituting the crude metal oxide particles (A) may contain two or more kinds of metal elements. The metal element contained in the metal oxide constituting the crude metal oxide particles (A) is preferably at least one selected from the group consisting of Ag, Cu, In, Sn, Ti, Hf, Al, Zr, Zn, Sn, Ce, Ga, Y, V, Ta, W, Mo, Nb, Mn, Fe, Co, Ni, Ru, Rh, Re, Pd, Os, Ir, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu. From the viewpoint of being able to provide modified metal oxide particles with a high refractive index, among the above metal elements, at least one selected from the group consisting of Ti, Al, Zr, Zn, Sn, Y, Nb, Ta and Ce is preferred, and Ti is particularly preferred. Suitable examples of metal oxides constituting the coarse metal oxide particles (A) include aluminum oxide (Al 2 O 3 ), titanium dioxide (TiO 2 ), hafnium oxide (HfO2 ), zirconium oxide (ZrO 2 ), indium oxide (In 2 O 3 ), zinc oxide (ZnO), tin oxide (SnO 2 ), lanthanum oxide (La 2 O 3 ), yttrium oxide (Y 2 O 3 ), niobium oxide (Nb 2 O 5 ), tantalum oxide (Ta 2 O 5 ), cerium oxide (CeO 2 ), and ruthenium oxide (RuO 2 As the metal oxide constituting the crude metal oxide particles (A), titanium oxide is preferred.

[0017] The shape of the crude metal oxide particles (A) is not particularly limited. Examples of the shape of the crude metal oxide particles (A) include a sphere, an elliptical sphere, a cube, a rectangular parallelepiped, a pyramid, a needle, a column, a rod, a plate, and a thin plate, and the like, and the sphere and the column are preferred.

[0018] The average diameter of the primary particles constituting the crude metal oxide particles (A) is not particularly limited as long as the desired effect is not impaired. The average diameter of the primary particles constituting the crude metal oxide particles (A) is, for example, preferably 50 nm or less, more preferably 20 nm or less, even more preferably 15 nm or less, and particularly preferably 10 nm or less. The lower limit of the average diameter of the primary particles constituting the crude metal oxide particles (A) may be, for example, 1 nm or more. The average diameter of the primary particles constituting the coarse metal oxide particles (A) is measured by X-ray diffraction method.

[0019] [Coarse metal oxide particles (A1)] The crude metal oxide particles (A1) are prepared by a solvothermal method, which is a method for producing metal oxide particles by reacting a metal oxide precursor in the presence of a specific solvent (Z) in a closed vessel at a specific high temperature and pressure. The solvent (Z) may contain additives such as amines, if necessary.

[0020] (Metal oxide precursor) As the metal oxide precursor, any metal compound can be used as long as it can produce the desired crude metal oxide particles (A1). Examples of metal oxide precursors include metal chlorides, organometallic complexes, metal alkoxides, and metal hydroxides. Among these, metal alkoxides, organometallic complexes, and metal hydroxides are preferred. An organometallic complex is a compound in which a ligand such as ethyl acetoacetate, 2,4-pentanedione (acetylacetone) or the like is coordinated to a metal element such as titanium, aluminum, zirconium, etc. In the organometallic complex, an alkoxy group having 1 to 4 carbon atoms may be bonded to the metal element.

[0021] Examples of metal oxide precursors include metal alkoxides such as titanium methoxide, titanium ethoxide, titanium propoxide, titanium isopropoxide, titanium butoxide, titanium amyloxide, titanium hexyloxide, titanium cyclopentoxide, titanium cyclohexyloxide, titanium allyloxide, titanium phenoxide, titanium methoxyethoxide, titanium ethoxyethoxide, aluminum methoxide, aluminum ethoxide, aluminum propoxide, aluminum isopropoxide, aluminum butoxide, aluminum amyloxide, aluminum hexyloxide, aluminum cyclopentoxide, aluminum cyclohexyloxide, aluminum allyloxide, aluminum phenoxide, aluminum methoxyethoxide, aluminum ethoxyethoxide, methoxyzirconium, ethoxyzirconium, propoxyzirconium, isopropoxyzirconium, and butoxyzirconium; Propoxy bisethyl acetoacetate, titanium dibutoxy bisethyl acetoacetate, titanium dipropoxy bis 2,4-pentanedionate, bis(2,4-pentanedionato) titanium oxide, titanium dibutoxy bis 2,4-pentanedionate, aluminum dipropoxy ethyl acetoacetate, aluminum dibutoxy ethyl acetoacetate, aluminum propoxy bis ethyl acetoacetate, aluminum butoxy bis ethyl acetoacetate Examples of the organic metal complexes include aluminum 2,4-pentanedionate, aluminum 2,2,6,6-tetramethyl-3,5-heptanedionate, zirconium dibutoxide bis(2,4-pentanedionate), bis(2,4-pentanedionato)zirconium oxide, and zirconium dipropoxide bis(2,2,6,6-tetramethyl-3,5-heptanedionate); and metal hydroxides such as titanium hydroxide, zirconium hydroxide, and aluminum hydroxide.

[0022] The metal oxide precursors may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0023] (Solvent (Z)) The solvent (Z) consists of water and / or an organic solvent. The organic solvent is preferably an organic solvent having an oxygen atom in the molecule.Specific examples of the organic solvent include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 4-methyl-2-pentanol, 2,2-dimethyl-1-propanol, tetrahydrofurfuryl alcohol, benzyl alcohol, phenethyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene ... monohydric alcohols such as propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, and tripropylene glycol monoethyl ether; (poly)alkylene glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol; (poly)alkylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate;Other ethers such as ethylene glycol dimethyl ether, ethylene glycol methyl ethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol methyl ethyl ether, propylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol methyl ethyl ether, dipropylene glycol diethyl ether, tetrahydrofuran, and dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-heptanone, 3-heptanone, cyclopentanone, and cyclohexanone; methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, 3-methoxypropionate, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl 3-methoxypropionate, ethyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, ethyl 3-methoxy ... methyl phosphate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutylpropionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutanoate, and other esters other than (poly)alkylene glycol monoalkyl ether acetate; and amide compounds such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. As the organic solvent, preferred are alcohol compounds such as monohydric alcohols, (poly)alkylene glycols, and (poly)alkylene glycol monoalkyl ether acetates, as well as carbonyl compounds such as ketones and esters other than (poly)alkylene glycol monoalkyl ether acetates. In the specification of the present application, a compound having an alcoholic hydroxyl group and a carbonyl group is referred to as an alcohol compound for the sake of convenience.

[0024] In the solvothermal method, the temperature and pressure at which the metal oxide precursor is reacted are not particularly limited, and are appropriately selected depending on the type of the metal oxide precursor and the type of the solvent (Z). The amount of the solvent (Z) used is not particularly limited as long as the crude metal oxide particles (A1) are satisfactorily produced.

[0025] <Coarse metal oxide particles (A2)> The crude metal oxide particles (A2) are prepared by capping the surfaces of the crude metal oxide particles (A1) with a capping agent.

[0026] (Capping agent) As the capping agent, any capping agent that has been conventionally used for surface treatment of metal oxide particles can be used without any particular limitation. Suitable examples of the capping agent include at least one selected from the group consisting of silane coupling agents, carboxylic acid compounds, alcohol compounds, thiol compounds, sulfonate compounds, phosphonate compounds, and phosphate compounds. Examples of the carboxylic acid compounds include carboxylic acids and their acid halides.

[0027] Specific examples of capping agents include n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, n-dodecyltrimethoxysilane, n-dodecyltriethoxysilane, n-hexadecyltrimethoxysilane, n-hexadecyltriethoxysilane, n-octadecyltrimethoxysilane, n-octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenethylphenyltrimethoxysilane, and phenethylethyl Triethoxysilane, 3-{2-methoxy[poly(ethyleneoxy)]}propyltrimethoxysilane, 3-{2-methoxy[poly(ethyleneoxy)]}propyltriethoxysilane, 3-{2-methoxy[tri(ethyleneoxy)]}propyltrimethoxysilane, 3-{2-methoxy[tri(ethyleneoxy)]}propyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, 1-hexenyltrimethoxysilane, 1-hexenyltriethoxysilane silane, 1-octenyltrimethoxysilane, 1-octenyltriethoxysilane, 3-aminopropyltrimethoxysilane (KBM-903 (Shin-Etsu Silicones)), 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 3-acryloylpropyltriethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane silane coupling agents such as silane, 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropyltriethoxysilane; phenolic compounds such as phenol; carboxylic acids such as octanoic acid, acetic acid, propionic acid, 2-[2-(methoxyethoxy)ethoxy]acetic acid, oleic acid, lauric acid, benzoic acid, 2-acryloyloxyethyl succinic acid, and 2-acryloyloxyethyl phthalic acid; acid halides of these carboxylic acids;Alcohol compounds such as ethanol, n-propanol, isopropanol, n-butanol, n-heptanol, n-hexanol, n-octanol, n-dodecyl alcohol, n-octadecanol, benzyl alcohol, triethylene glycol monomethyl ether, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, allyl alcohol, oleyl alcohol, ethylene glycol monoallyl ether, propylene glycol monoallyl ether, and 3-allyloxypropanol; 1-hexanethiol, 1-heptanethiol, 1-octanethiol, 2-ethyl-1-hexanethiol, 1-nonanethiol, 1-decanethiol, 1-undecanethiol, 1-dodecanethiol, 1-tridecanethiol, 1-tetradecanethiol, thiol compounds such as 1-pentadecanethiol, 1-hexadecanethiol, 1-heptadecanethiol, 1-octadecanethiol, 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, and 2-mercaptobenzothiazole; sulfonate compounds such as sodium 2,3-dimercaptopropanesulfonate monohydrate and sodium dodecyl sulfate; phosphonate compounds such as dodecylphosphonic acid, octylphosphonic acid, (11-mercaptoundecyl)phosphonic acid, (11-(acryloyloxy)undecyl)phosphonic acid, 11-methacryloyloxyundecylphosphonic acid, and [2-[2-(2-methoxyethoxy)ethoxy]ethyl]phosphonic acid ethyl ester; and phosphate compounds such as tris(2,4-di-tert-butylphenyl)phosphate.

[0028] The method for capping the surfaces of the crude metal oxide particles (A1) with a capping agent is not particularly limited as long as it is a method that can bring the crude metal oxide particles (A1) into contact with the capping agent. For example, a liquid capping agent or a solution of the capping agent may be dropped or sprayed onto the powdered crude metal oxide particles (A1), and then the two may be mixed uniformly. Alternatively, the crude metal oxide particles (A1) may be dispersed in an organic solvent that does not fall under the category of the capping agent, and then the crude metal oxide particles (A1) may be mixed with a capping agent.

[0029] The amount of the capping agent used when capping the surface of the crude metal oxide particles (A1) with the capping agent is not particularly limited as long as the desired crude metal oxide particles (A) can be obtained. The amount of the capping agent is preferably 1% by mass or more and 300% by mass or less, more preferably 5% by mass or more and 200% by mass or less, based on the mass of the crude metal oxide particles (A1).

[0030] (Organic solvent) Suitable examples of organic solvents that can be used when capping the surfaces of the crude metal oxide particles (A1) with a capping agent include (poly)alkylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; ethylene glycol dimethyl ether, ethylene glycol methyl ethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol methyl ethyl ether, propylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol methyl ethyl ether, dipropylene glycol diethyl ether, tetrahydrofuran, and dioxane. Ethers other than (poly)alkylene glycol monoalkyl ether acetates; ketones such as acetone, methyl ethyl ketone, 2-heptanone, 3-heptanone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, Examples of the carbonyl compounds include methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, and ethyl 2-oxobutanoate; and amide compounds such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.These organic solvents can be used alone or in combination of two or more kinds.

[0031] <Nitrogen-containing polar organic solvent (S)> In preparing the modified metal oxide particles, the crude metal oxide particles (A) are dispersed in a nitrogen-containing polar organic solvent (S), which contains water.

[0032] The nitrogen-containing organic solvent (S) is not particularly limited as long as it is an organic solvent having a nitrogen atom. Suitable examples of the nitrogen-containing organic solvent (S) include amine compounds such as triethylamine, triisopropylamine, piperidine, piperazine, morpholine, and aniline; nitrogen-containing aromatic heterocyclic compounds such as pyridine and pyrimidine; and compounds having an amide structure (>N-CO-). Among these, compounds having an amide structure are preferred because of the high dispersibility of the crude metal oxide particles (A) in the solvent.

[0033] A preferred example of the compound having an amide structure is a compound represented by the following formula (S1). [ka] (In formula (S1), R S1 and R S2 are each independently an alkyl group having 1 to 3 carbon atoms; R S3 is expressed by the following formula (S1-1) or (S1-2): [ka] It is a group represented by the following formula: In formula (S1-1), R S4 is a hydrogen atom or a hydroxyl group, and R S5 and R S6 Each of R is independently an alkyl group having 1 to 3 carbon atoms. S7 and R S8 are each independently a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.

[0034] Among the compounds represented by formula (S1), R S3 Specific examples when is a group represented by formula (S1-1) include N,N,2-trimethylpropionamide, N-ethyl,N,2-dimethylpropionamide, N,N-diethyl-2-methylpropionamide, N,N,2-trimethyl-2-hydroxypropionamide, N-ethyl-N,2-dimethyl-2-hydroxypropionamide, and N,N-diethyl-2-hydroxy-2-methylpropionamide.

[0035] Among the compounds represented by formula (S1), R S3 Specific examples when is a group represented by formula (S1-2) include urea compounds such as N,N,N',N'-tetramethylurea and N,N,N',N'-tetraethylurea.

[0036] The compound represented by formula (S1) is preferably a urea compound, and the urea compound is preferably N,N,N',N'-tetramethylurea.

[0037] Preferred examples of the compound having an amide structure other than the compound represented by formula (S1) include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N,N,2-trimethylpropionamide, and 1,3-dimethyl-2-imidazolidinone.

[0038] The compound having an amide structure may be used alone or in combination of two or more kinds.

[0039] The amount of the nitrogen-containing organic solvent (S) used is not particularly limited as long as the desired effect is obtained. The amount of the nitrogen-containing organic solvent (S) used is not particularly limited, and is preferably from 50 to 5,000 parts by mass, more preferably from 70 to 1,000 parts by mass, and even more preferably from 100 to 500 parts by mass, per 100 parts by mass of the crude metal oxide particles (A).

[0040] The amount of water contained in the nitrogen-containing polar organic solvent (S) is not particularly limited as long as the desired effect is obtained. The amount of water is typically preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 7 parts by mass or less, relative to 100 parts by mass of the nitrogen-containing organic solvent (S). There is no particular lower limit to the amount of water, but an example of the amount is 0.1 parts by mass or more relative to 100 parts by mass of the nitrogen-containing organic solvent (S).

[0041] When preparing the modified metal oxide particles, the dispersion medium in which the crude metal oxide particles (A) are dispersed may contain an organic solvent other than the nitrogen-containing organic solvent (S) as long as the desired effect is not impaired. Examples of organic solvents other than the nitrogen-containing organic solvent (S) include (poly)alkylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; ethers other than (poly)alkylene glycol monoalkyl ether acetates such as diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, and tetrahydrofuran; acetone, methyl ethyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone, etc. ketones; esters other than (poly)alkylene glycol monoalkyl ether acetate, such as methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, and ethyl 2-oxobutanoate; and aromatic hydrocarbons such as toluene and xylene.

[0042] The content of other organic solvents in the dispersion medium is preferably 20% by mass or less, more preferably 10% by mass or less, further preferably 5% by mass or less, and particularly preferably 0% by mass, based on the mass of the dispersion medium.

[0043] The temperature at which the crude metal oxide particles (A) are heated in the nitrogen-containing polar organic solvent (S) is not particularly limited as long as the modified metal oxide particles can be obtained. The temperature at which the crude metal oxide particles (A) are heated is, for example, 50°C to 200°C, preferably 60°C to 180°C, more preferably 70°C to 160°C, and particularly preferably 70°C to 90°C and 140°C to 160°C. The crude metal oxide particles (A) may be heated in the nitrogen-containing polar organic solvent (S) multiple times at different temperatures, for example, at 70° C. to 90° C., followed by heating at 140° C. to 160° C. Such multiple heating operations may be carried out as a series of operations in the same vessel without recovering the crude metal oxide particles (A) from the dispersion. Alternatively, after the desired number of heating operations, the crude metal oxide particles (A) may be recovered from the dispersion, and the recovered crude metal oxide particles may be dispersed again in the nitrogen-containing polar organic solvent (S) and further heated a desired number of times. The temperature to which the crude metal oxide particles (A) are heated in the nitrogen-containing polar organic solvent (S) may be changed continuously in one heat treatment. The temperature change may be a temperature increase, a temperature decrease, or a combination of a temperature increase and a temperature decrease. By this heating, the crude metal oxide particles (A) are modified to obtain modified metal oxide particles.

[0044] The pressure conditions when the crude metal oxide particles (A) are heated in the nitrogen-containing polar organic solvent (S) are not particularly limited. The pressure conditions may be atmospheric pressure conditions, pressurized conditions, or reduced pressure conditions below atmospheric pressure. Preferably, the heating of the crude metal oxide particles (A) in the nitrogen-containing polar organic solvent (S) is carried out in a nitrogen purged environment at atmospheric pressure. The nitrogen flow rate in the nitrogen purged environment is preferably 50 mL / min or less, more preferably 50 mL / min or less. The lower limit of the nitrogen flow rate is not particularly limited, but may be, for example, 1 mL / min or more.

[0045] The time for heating the crude metal oxide particles (A) in the nitrogen-containing polar organic solvent (S) is not particularly limited. The time for heating the crude metal oxide particles (A) is, for example, 5 minutes or more and 360 minutes or less, preferably 10 minutes or more and 180 minutes or less, and more preferably 30 minutes or more and 90 minutes or less.

[0046] The heat treatment of the crude metal oxide particles (A) in a nitrogen-containing polar organic solvent (S) is as follows: Heat at 70℃ to 90℃ for 30 to 90 minutes, or Heat at 140℃ to 160℃ for 30 to 90 minutes, or A combination of heating at 70° C. to 90° C. for 30 to 90 minutes and then heating at 140° C. to 160° C. for 30 to 90 minutes is preferred.

[0047] <Additive (B)> The nitrogen-containing organic solvent (S) may contain an additive (B). By preparing the modified metal oxide particles using a nitrogen-containing organic solvent containing the additive (B), the total light transmittance of the cured product of the photocurable composition containing the modified metal oxide particles tends to be improved. The additive (B) is preferably at least one selected from the group consisting of a basic compound, an acidic compound, and a capping agent.

[0048] The amount of additive (B) is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 7 parts by mass or less, relative to 100 parts by mass of the nitrogen-containing organic solvent (S). There is no particular lower limit to the amount of additive (B), but an example of the amount is 0.05 parts by mass or more relative to 100 parts by mass of the nitrogen-containing organic solvent (S).

[0049] The basic compound includes an amine compound represented by the following formula (b1). NRR'R'' ... (b1) In formula (b1), R, R', and R'' each independently represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Examples of basic compounds include ammonia, methylamine, ethylamine, n-propylamine, isopropylamine, dimethylamine, diethylamine, di-n-propylamine, diisopropylamine, trimethylamine, triethylamine, methyldiethylamine, N-ethyldiisopropylamine, tri-n-propylamine, and triisopropylamine.

[0050] As the acidic compound, both organic acidic compounds and inorganic acidic compounds can be used. As the acidic compound, it is preferable to use an organic acidic compound. Among the organic acidic compounds, aliphatic carboxylic acids are preferable, and aliphatic carboxylic acids having 1 to 4 carbon atoms are more preferable. Examples of organic acidic compounds include carboxylic acids such as formic acid, acetic acid, propionic acid, butanoic acid, isobutanoic acid, pentanoic acid, hexanoic acid, citric acid, oxalic acid, 2-nitrophenylacetic acid, 2-ethylhexanoic acid, dodecanoic acid, and 2-hydroxy-1,2,3-propanetricarboxylic acid; sugar acids such as ascorbic acid, tartaric acid, and glucuronic acid; and sulfonic acids such as benzenesulfonic acid and p-toluenesulfonic acid. Examples of inorganic acidic compounds include phosphonic acid (HP(=O)(OH) 2 ), phosphoric acid (H 3 PO 4 ), hydrochloric acid, nitric acid, boric acid, etc.

[0051] As the capping agent, the capping agents described for the crude metal oxide particles (A2) can be used. As the capping agent, silane coupling agent is preferred.Suitable examples of silane coupling agent include ω-aminoalkyltrialkoxysilane such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-mercaptopropyltrimethoxysilane; ω-mercaptoalkyltrialkoxysilane such as 3-mercaptopropyltriethoxysilane; ω-(meth)acryloyloxyalkyltrialkoxysilane such as 3-acryloyloxypropyltrimethoxysilane, 3-acryloylpropyltriethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, and 3-methacryloyloxypropyltriethoxysilane; ω-isocyanatoalkyltrialkoxysilane such as 3-isocyanatopropyltrimethoxysilane and 3-isocyanatopropyltriethoxysilane; ω-glycidoxyalkyltrialkoxysilane such as 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane. Among these silane coupling agents, ω-aminoalkyltrialkoxysilane is preferred because of its good modifying effect. As the ω-aminoalkyltrialkoxysilane, 2-aminoethyltrialkoxysilane, 3-aminopropyltrialkoxysilane, and 4-aminobutyltrialkoxysilane are preferred. As the ω-aminoalkyltrialkoxysilane, ω-aminoalkyltrimethoxysilane and ω-aminoalkyltriethoxysilane are preferred.

[0052] From the viewpoint of capping the crude metal oxide particles (A), the amount of the capping agent used is preferably 0.05 parts by mass or more and 15 parts by mass or less, and more preferably 0.1 parts by mass or more and 10 parts by mass or less, per 100 parts by mass of the crude metal oxide particles (A).

[0053] By carrying out the method for producing surface-modified metal oxide particles by adding a capping agent to the modified metal oxide particles, the surfaces of the modified metal oxide particles can be further modified with the capping agent. The modified metal oxide particles have a metal oxide particle surface that is more easily modified with a capping agent than the crude metal oxide particles (A1) or the crude metal oxide particles (A2).

[0054] <<Photocurable composition>> The photocurable composition includes modified metal oxide particles and a transparent substrate component. Essential and optional components contained in the photocurable composition will be described below.

[0055] <Modified metal oxide particles> The modified metal oxide particles are modified metal oxide particles produced by the above-mentioned method for producing modified metal oxide particles.

[0056] <Transparent base component> The transparent base component contains a photopolymerizable compound (M) as a curable component. The photopolymerizable compound (M) is a compound having a radical polymerizable group-containing group or a cationically polymerizable group-containing group.

[0057] The radical polymerizable group-containing group typically includes a group containing an ethylenically unsaturated double bond. As the ethylenically unsaturated double bond-containing group, an alkenyl group-containing group including an alkenyl group such as a vinyl group or an allyl group is preferable, and a (meth)acryloyl group-containing group is more preferable. The cationic polymerizable group-containing group typically includes an epoxy group-containing group, an oxetanyl group-containing group, a vinyloxy group-containing group, etc. Among these, the epoxy group-containing group and the vinyloxy group-containing group are preferred. The epoxy group-containing group is preferably an alicyclic epoxy group-containing group or a glycidyl group. The alicyclic epoxy group is an aliphatic cyclic group in which two carbon atoms as adjacent ring constituent atoms in the aliphatic cyclic group are bonded via an oxygen atom. In other words, the alicyclic epoxy group has an epoxy group containing a three-membered ring consisting of two carbon atoms and one oxygen atom on the aliphatic ring.

[0058] In the specification of this application, (meth)acrylic means both acrylic and methacrylic, (meth)acryloyl means both acryloyl and methacryloyl, and (meth)acrylate means both acrylate and methacrylate.

[0059] When the photopolymerizable compound (M) has a radically polymerizable group-containing group, the photopolymerizable compound (M) may be a monofunctional compound having one radically polymerizable group or a polyfunctional compound having two or more radically polymerizable groups, and is preferably a polyfunctional compound. As the photopolymerizable compound (M) having a radical polymerizable group-containing group, a compound having one or more (meth)acryloyl groups, such as a (meth)acrylate compound or a (meth)acrylamide compound, is preferred, and a (meth)acrylate compound having one or more (meth)acryloyl groups is more preferred.

[0060] Examples of monofunctional compounds having a radical polymerizable group-containing group include (meth)acrylamide, methylol (meth)acrylamide, methoxymethyl (meth)acrylamide, ethoxymethyl (meth)acrylamide, propoxymethyl (meth)acrylamide, butoxymethoxymethyl (meth)acrylamide, N-methylol (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, (meth)acrylic acid, fumaric acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, citraconic acid, citraconic anhydride, crotonic acid, 2-acrylamido-2-methylpropanesulfonic acid, tert-butylacrylamidosulfonic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylamide ... acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-phenoxy-2-hydroxypropyl (meth)acrylate, 2-(meth)acryloyloxy-2-hydroxypropyl phthalate, glycerin mono(meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dimethylamino (meth)acrylate, glycidyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, half (meth)acrylate of phthalic acid derivative, etc. These monofunctional compounds can be used alone or in combination of two or more.

[0061] Examples of polyfunctional compounds having a radical polymerizable group-containing group include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexane glycol di(meth)acrylate, dimethylol tricyclodecane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 2,2-bis(4-(meth)acryloxydi Examples of suitable polyfunctional compounds include polyfunctional compounds such as 2,2-bis(4-(meth)acryloxypolyethoxyphenyl)propane, 2-hydroxy-3-(meth)acryloyloxypropyl(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, phthalic acid diglycidyl ester di(meth)acrylate, glycerin triacrylate, glycerin polyglycidyl ether poly(meth)acrylate, urethane (meth)acrylate (i.e., tolylene diisocyanate), a reaction product of trimethylhexamethylene diisocyanate, hexamethylene diisocyanate, and 2-hydroxyethyl (meth)acrylate, methylene bis(meth)acrylamide, (meth)acrylamide methylene ether, and a condensation product of a polyhydric alcohol and N-methylol (meth)acrylamide, as well as triacrylformal. These polyfunctional compounds can be used alone or in combination of two or more kinds.

[0062] Among these photopolymerizable compounds (M) having a radical polymerizable group-containing group, polyfunctional compounds having three or more functional groups are preferred, polyfunctional compounds having four or more functional groups are more preferred, and polyfunctional compounds having five or more functional groups are even more preferred, since they tend to increase the strength of the cured product.

[0063] When the photocurable composition contains modified metal oxide particles, depending on the composition of the photocurable composition, localization of the modified metal oxide particles may occur in the cured film formed using the photocurable composition, such that a layer rich in the modified metal oxide particles and a layer poor in the modified metal oxide particles are formed. From the viewpoint of suppressing such localization, the photocurable composition preferably contains a compound represented by the following formula (M1) or the following formula (M2) as the photopolymerizable compound (M) having a radical polymerizable group-containing group. [ka] (MA-(OR m1 ) nm1 -X-CH 2 ) 2 -CH-X-(R m1 -O) nm1 -MA···(M2)

[0064] In the formula (M1) and the formula (M2), each MA is independently a (meth)acryloyl group. Each X is independently an oxygen atom, -NH-, or -N(CH 3 )-. R m1 are each independently an ethane-1,2-diyl group, a propane-1,2-diyl group, or a propane-1,3-diyl group. m2 is a hydroxyl group, an alkyl group having 1 to 4 carbon atoms, or -X-(R m1 -O) nm1 It is a group represented by -MA (X is the same as above). nm1 and nm2 each independently represent 0 or 1.

[0065] In formula (M1), R m2Examples of the alkyl group having 1 to 4 carbon atoms as the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. Among these alkyl groups, a methyl group and an ethyl group are preferred.

[0066] Preferred examples of the compound represented by formula (M1) and the compound represented by formula (M2) include pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, and the following compounds 1) to 32), in which MA is a (meth)acryloyl group. 1)(MA-NH-CH 2 ) 4 -C 2)(MA-N(CH 3 )-CH 2 ) 4 -C 3) (MA-O-CH 2 CH 2 CH 2 -O-CH 2 ) 4 -C 4) (MA-O-CH 2 CH 2 -O-CH 2 ) 4 -C 5) (MA-O-CH 2 CH 2 CH 2 -NH-CH 2 ) 4 -C 6) (MA-O-CH 2 CH 2 -NH-CH 2 ) 4 -C 7) (MA-O-CH 2 CH 2 CH 2 -N(CH 3 )-CH 2 ) 4 -C 8) (MA-O-CH 2 CH2 -N(CH 3 )-CH 2 ) 4 -C 9)(MA-NH-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -NH-MA) 3 10)(MA-N(CH 3 )-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -N(CH 3 )-GHOST) 3 11)(MA-O-CH 2 CH 2 CH 2 -O-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -O-CH 2 CH 2 CH 2 -O-MA) 3 12)(MA-O-CH 2 CH 2 -O-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -O-CH 2 CH 2 -O-MA) 3 13)(MA-O-CH 2 CH 2 CH 2 -NH-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -NH-CH 2 CH 2 CH 2 -O-MA) 3 14)(MA-O-CH 2 CH 2 -NH-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -NH-CH 2 CH 2 -O-MA) 3 15)(MA-O-CH 2 CH 2 CH 2 -N(CH 3 )-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -N(CH 3 )-CH 2 CH 2 CH 2 -O-MA) 3 16)(MA-O-CH 2 CH 2 -N(CH 3 )-CH 2 ) 3 -C-CH 2 -O-CH 2 -C-(CH 2 -N(CH 3 )-CH 2 CH 2 -O-MA) 3 17)(MA-NH-CH 2 ) 2 -CH-NH-MA 18)(MA-N(CH 3 )-CH 2 ) 2 -CH-N(CH 3 )-GHOST 19)(MA-O-CH 2 CH 2 CH 2 -O-CH 2 ) 2 -CH-O-CH 2 CH 2 CH 2 -O-MA 20)(MA-O-CH2 CH 2 -O-CH 2 ) 2 -CH-CO-CH 2 CH 2 -O-MA 21)(MA-O-CH 2 CH 2 CH 2 -NH-CH 2 ) 2 -CH-NH-CH 2 CH 2 CH 2 -O-MA 22)(MA-O-CH 2 CH 2 -NH-CH 2 ) 2 -CH 2 -NH-CH 2 CH 2 -O-MA 23)(MA-O-CH 2 CH 2 CH 2 -N(CH 3 )-CH 2 ) 2 -CH 2 -N(CH 3 )-CH 2 CH 2 CH 2 -O-MA 24)(MA-O-CH 2 CH 2 -N(CH 3 )-CH 2 ) 2 -CH 2 -N(CH 3 )-CH 2 CH 2 -O-MA 25)(MA-NH-CH 2 ) 3 -C-CH 2 CH 3 26)(MA-N(CH 3 )-CH 2 ) 3 -C-CH 2 CH 3 27)(MA-O-CH 2 CH2 CH 2 -O-CH 2 ) 3 -C-CH 2 CH 3 28)(MA-O-CH 2 CH 2 -O-CH 2 ) 3 -C-CH 2 CH 3 29)(MA-O-CH 2 CH 2 CH 2 -NH-CH 2 ) 3 -C-CH 2 CH 3 30)(MA-O-CH 2 CH 2 -NH-CH 2 ) 3 -C-CH 2 CH 3 31)(MA-O-CH 2 CH 2 CH 2 -N(CH 3 )-CH 2 ) 3 -C-CH 2 CH 3 32)(MA-O-CH 2 CH 2 -N(CH 3 )-CH 2 ) 3 -C-CH 2 CH 3

[0067] In terms of suppressing localization of the modified metal oxide particles in the cured product, the ratio of the total mass of the compound represented by formula (M1) and the compound represented by formula (M2) to the mass of the photopolymerizable compound (M) is preferably 20 mass% or more and 70 mass% or less, more preferably 30 mass% or more and 70 mass% or less, and even more preferably 40 mass% or more and 70 mass% or less.

[0068] In terms of ease of forming a cured product with a high refractive index, the photocurable composition preferably contains, as the photopolymerizable compound (M) having a radical polymerizable group-containing group, a compound having an S atom at the center and radical polymerizable group-containing groups at both ends, and having an aromatic ring, which may have a substituent, and an S atom at a divalent linking portion connecting the center and each end, more preferably a compound having (meth)acryloyl groups at both ends, and having a diphenyl sulfide skeleton as a combination of the central S atom and the aromatic ring constituting the divalent linking portion, and even more preferably a compound represented by the following formula (m-1). [ka]

[0069] In formula (m-1), R 1 , and R 2 R is independently a hydrogen atom or a methyl group. 3 , and R 4 each independently represents an alkyl group having 1 to 5 carbon atoms; p and q each independently represents 0 or 1.

[0070] Examples of the aromatic ring in the linking portion include aromatic hydrocarbon rings such as a benzene ring, a naphthalene ring, an anthracene ring, and a phenanthroline ring; and aromatic heterocycles such as a furan ring, a pyrrole ring, a thiophene ring, a pyridine ring, a thiazole ring, and a benzothiazole ring. Of these, a benzene ring (e.g., a 1,4-phenyl group, etc.) is preferred. Examples of the substituent in the linking portion include an alkyl group, an alkoxy group, an alkylcarbonyl group, an alkoxycarbonyl group, an alkylcarbonyloxy group, an alkylamino group, a dialkylamino group, an alkylamide group, an alkenyl group, an alkynyl group, a halogen atom, a cyano group, a nitro group, an alkylthiol group, and an N-alkylcarbamate group, etc. Among these, an alkyl group is preferable, and an alkyl group having 1 to 5 carbon atoms is more preferable.

[0071] R 1 , and R 2 R is independently a hydrogen atom or a methyl group.1 , and R 2 may be different from each other or may be the same. In view of the ease of synthesis and availability of the compound represented by formula (m-1), R 1 , and R 2 are preferably identical.

[0072] R 3 , and R 4 R is independently an alkyl group having 1 to 5 carbon atoms. 3 , and R 4 may be different from each other or may be the same. In view of the ease of synthesis and availability of the compound represented by formula (m-1), R 3 , and R 4 are preferably identical.

[0073] R 3 , and R 4 The alkyl group having 1 to 5 carbon atoms as R may be linear or branched. 3 , and R 4 Examples of the alkyl group having 1 to 5 carbon atoms as the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, and a tert-pentyl group.

[0074] Preferable specific examples of the compound represented by formula (m-1) include the following compounds.

[0075] [ka]

[0076] When the photocurable composition contains a compound represented by formula (m-1) as the photopolymerizable compound (M) having a radical polymerizable group-containing group, the ratio of the mass of the compound represented by formula (m-1) to the mass of the photopolymerizable compound (M) is preferably 10 mass% or more, more preferably 30 mass% or more, even more preferably 50 mass% or more, even more preferably 70 mass% or more, and particularly preferably 100 mass%.

[0077] In order to easily suppress localization of the modified metal oxide particles in the cured product, it is preferable that the photocurable composition contains a sulfur-containing (meth)acrylate represented by the following formula (M3) as the photopolymerizable compound (M) having a radical polymerizable group-containing group. Ar m1 -R m21 -SR m22 -O-CO-CR m23 =CH 2 (M3)

[0078] In formula (M3), Ar m1 R is a phenyl group which may be substituted with a halogen atom. m21 R is a single bond or an alkylene group having 1 to 6 carbon atoms. m22 is an alkylene group having 1 to 6 carbon atoms. m23 is a hydrogen atom or a methyl group.

[0079] Ar m1 is a phenyl group which may be substituted with a halogen atom. When the phenyl group is substituted with a halogen atom, the number of halogen atoms bonded to the phenyl group is not particularly limited. The number of halogen atoms bonded to the phenyl group is preferably 1 or 2, more preferably 1. When two or more halogen atoms are bonded to the phenyl group, the multiple halogen atoms bonded to the phenyl group may be composed of only the same type of halogen atom, or may be composed of two or more types of halogen atoms. Examples of halogen atoms that can be bonded to the phenyl group include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and a fluorine atom, a chlorine atom, and a bromine atom are preferred. Ar m1 As the aryl group, an unsubstituted phenyl group is preferable.

[0080] R m21 is a single bond, or an alkylene group having from 1 to 6 carbon atoms. Examples of the alkylene group having from 1 to 6 carbon atoms include a methylene group, an ethane-1,2-diyl group, a propane-1,2-diyl group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, and a hexane-1,6-diyl group. R m21 As the group, a single bond and a methylene group are preferable, and a single bond is more preferable.

[0081] R m22 is an alkylene group having 1 to 6 carbon atoms. Examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethane-1,2-diyl group, a propane-1,2-diyl group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, and a hexane-1,6-diyl group. R m22 As the alkyl group, a methylene group, an ethane-1,2-diyl group, and a propane-1,3-diyl group are preferable, and an ethane-1,2-diyl group and a propane-1,3-diyl group are more preferable.

[0082] In terms of the ease of obtaining sulfur-containing (meth)acrylates and the suppression of localization of modified metal oxide particles in the cured product, in formula (M3), Ar m1 is a phenyl group, and R m21 It is particularly preferred that is a single bond.

[0083] Suitable specific examples of the sulfur-containing (meth)acrylate represented by formula (M3) include 2-phenylthioethyl (meth)acrylate, 3-phenylthiopropyl (meth)acrylate, 2-benzylthioethyl (meth)acrylate, 3-benzylthiopropyl (meth)acrylate, 2-(2-chlorophenyl)ethyl (meth)acrylate, 2-(3-chlorophenyl)ethyl (meth)acrylate, 2-(4-chlorophenyl)ethyl (meth)acrylate, 3-(2-chlorophenyl)propyl (meth)acrylate, 3-(3-chlorophenyl)propyl (meth)acrylate, 3-(4-chlorophenyl)propyl (meth)acrylate, and 2-(2-fluorophenyl)ethyl (meth)acrylate. , 2-(3-fluorophenyl)ethyl (meth)acrylate, 2-(4-fluorophenyl)ethyl (meth)acrylate, 3-(2-fluorophenyl)propyl (meth)acrylate, 3-(3-fluorophenyl)propyl (meth)acrylate, 3-(4-fluorophenyl)propyl (meth)acrylate, 2-(2-bromophenyl)ethyl (meth)acrylate, 2-(3-bromophenyl)ethyl (meth)acrylate, 2-(4-bromophenyl)ethyl (meth)acrylate, 3-(2-bromophenyl)propyl (meth)acrylate, 3-(3-bromophenyl)propyl (meth)acrylate, and 3-(4-bromophenyl)propyl (meth)acrylate.

[0084] When the photocurable composition contains a sulfur-containing (meth)acrylate represented by formula (M3) as the photopolymerizable compound (M) having a radical polymerizable group-containing group, the ratio of the mass of the sulfur-containing (meth)acrylate represented by formula (M3) to the mass of the photopolymerizable compound (M) is preferably 40 mass% or more and 100 mass% or less, more preferably 60 mass% or more and 100 mass% or less, even more preferably 70 mass% or more and 100 mass% or less, and particularly preferably 80 mass% or more and 100 mass% or less.

[0085] When the photopolymerizable compound (M) has a cationic polymerizable group-containing group, the photopolymerizable compound (M) may be a monofunctional compound having one cationic polymerizable group or a polyfunctional compound having two or more cationic polymerizable groups, and is preferably a polyfunctional compound.

[0086] When the photopolymerizable compound (M) has a vinyloxy group-containing group as a cationic polymerizable group-containing group, the photocurable composition may contain a vinyl ether compound as the photopolymerizable compound (M). Such a vinyl ether compound may be a monofunctional compound or a polyfunctional compound.

[0087] Specific examples of suitable vinyl ether compounds include vinyl phenyl ether, 4-vinyloxytoluene, 3-vinyloxytoluene, 2-vinyloxytoluene, 1-vinyloxy-4-chlorobenzene, 1-vinyloxy-3-chlorobenzene, 1-vinyloxy-2-chlorobenzene, 1-vinyloxy-2,3-dimethylbenzene, 1-vinyloxy-2,4-dimethylbenzene, 1-vinyloxy-2,5-dimethylbenzene, and 1-vinyloxy-2,6-dimethylbenzene. Aromatic monovinyl ethers such as methylbenzene, 1-vinyloxy-3,4-dimethylbenzene, 1-vinyloxy-3,5-dimethylbenzene, 1-vinyloxynaphthalene, 2-vinyloxynaphthalene, 2-vinyloxyfluorene, 3-vinyloxyfluorene, 4-vinyloxy-1,1'-biphenyl, 3-vinyloxy-1,1'-biphenyl, 2-vinyloxy-1,1'-biphenyl, 6-vinyloxytetralin, and 5-vinyloxytetralin. Compounds; 1,4-divinyloxybenzene, 1,3-divinyloxybenzene, 1,2-divinyloxybenzene, 1,4-divinyloxynaphthalene, 1,3-divinyloxynaphthalene, 1,2-divinyloxynaphthalene, 1,5-divinyloxynaphthalene, 1,6-divinyloxynaphthalene, 1,7-divinyloxynaphthalene, 1,8-divinyloxynaphthalene, 2,3-divinyloxynaphthalene, 2,6-divinyloxynaphthalene, 2,7-divinyloxy Examples of the divinyloxybiphenyl include aromatic divinyl ether compounds such as divinyloxynaphthalene, 1,2-divinyloxyfluorene, 3,4-divinyloxyfluorene, 2,7-divinyloxyfluorene, 4,4'-divinyloxybiphenyl, 3,3'-divinyloxybiphenyl, 2,2'-divinyloxybiphenyl, 3,4'-divinyloxybiphenyl, 2,3'-divinyloxybiphenyl, 2,4'-divinyloxybiphenyl, and bisphenol A divinyl ether. These vinyl ether compounds may be used in combination of two or more kinds.

[0088] When the photopolymerizable compound (M) has an epoxy group-containing group as the cationically polymerizable group-containing group, the photocurable composition may contain various epoxy compounds as the photopolymerizable compound (M). Examples of epoxy compounds include bifunctional epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AD ​​type epoxy resins, naphthalene type epoxy resins, and biphenyl type epoxy resins; novolac epoxy resins such as phenol novolac type epoxy resins, brominated phenol novolac type epoxy resins, orthocresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, and bisphenol AD ​​novolac type epoxy resins; cyclic aliphatic epoxy resins such as epoxidized products of dicyclopentadiene type phenolic resins; aromatic epoxy resins such as epoxidized products of naphthalene type phenolic resins; glycidyl ester type epoxy resins such as dimer acid glycidyl ester and triglycidyl ester; glycidyl amine type epoxy resins such as tetraglycidylaminodiphenylmethane, triglycidyl-p-aminophenol, tetraglycidylmeta-xylylenediamine, and tetraglycidylbisaminomethylcyclohexane; triglycidyl heterocyclic epoxy resins such as phenylmethyl isocyanurate; phloroglucinol triglycidyl ether, trihydroxybiphenyl triglycidyl ether, trihydroxyphenylmethane triglycidyl ether, glycerin triglycidyl ether, 2-[4-(2,3-epoxypropoxy)phenyl]-2-[4-[1,1-bis[4-(2,3-epoxypropoxy)phenyl]ethyl]phenyl]propane, and 1,3-bis[4-[1-[4-(2,3-epoxypropoxy)phenyl]-1-[4- trifunctional epoxy resins such as [1-[4-(2,3-epoxypropoxy)phenyl]-1-methylethyl]phenyl]ethyl]phenoxy]-2-propanol; tetrafunctional epoxy resins such as tetrahydroxyphenylethane tetraglycidyl ether, tetraglycidylbenzophenone, bisresorcinol tetraglycidyl ether, and tetraglycidoxybiphenyl; and 1,2-epoxy-4-(2-oxiranyl)cyclohexane adducts of 2,2-bis(hydroxymethyl)-1-butanol.The 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol is commercially available as EHPE-3150 (manufactured by Daicel Corporation).

[0089] Furthermore, oligomer or polymer type polyfunctional epoxy compounds can also be preferably used. Typical examples of oligomer or polymer type polyfunctional epoxy compounds include phenol novolac type epoxy compounds, brominated phenol novolac type epoxy compounds, orthocresol novolac type epoxy compounds, xylenol novolac type epoxy compounds, naphthol novolac type epoxy compounds, bisphenol A novolac type epoxy compounds, bisphenol AD ​​novolac type epoxy compounds, epoxidized products of dicyclopentadiene type phenol resins, and epoxidized products of naphthalene type phenol resins.

[0090] Other examples of suitable epoxy compounds include polyfunctional alicyclic epoxy compounds having alicyclic epoxy groups.

[0091] Specific examples of the alicyclic epoxy compound include 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-meta-dioxane, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, 3,4-epoxy-6-methylcyclohexyl-3',4'-epoxy-6'-methylcyclohexanecarboxylate, ε-caprolactone-modified 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, and trimethylcaprolactone-modified 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate. Examples of the epoxy resins include dimethyl-3',4'-epoxycyclohexane carboxylate, β-methyl-δ-valerolactone-modified 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexane carboxylate, methylene bis(3,4-epoxycyclohexane), di(3,4-epoxycyclohexylmethyl)ether of ethylene glycol, ethylene bis(3,4-epoxycyclohexane carboxylate), dioctyl epoxycyclohexahydrophthalate, and di-2-ethylhexyl epoxycyclohexahydrophthalate, and epoxy resins having a tricyclodecene oxide group.

[0092] <Solvent (L)> The photocurable composition may contain a solvent (L) for the purpose of adjusting the coating property, etc. The photocurable composition typically contains a solvent (L). The type of the solvent (L) is not particularly limited, but is typically an organic solvent. The solvent (L) is, for example, selected from benzyl alcohol, butyl carbitol acetate (BCA), butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, tetrahydrofuran, diethyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol, dipropylene glycol, acetone, propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), ethyl acetate, butyl acetate, diethylene glycol monoethyl ether acetate, toluene, and combinations thereof.

[0093] <Other ingredients> The photocurable liquid composition may contain various additives in addition to the components described above, as long as the object of the present invention is not impaired. Preferred additives to be incorporated into the photocurable liquid composition include polymerization initiators, curing agents, dispersants, adhesion promoters such as silane coupling agents, antioxidants, aggregation inhibitors, antifoaming agents, surfactants, etc. The surfactant is not particularly limited, and known components such as fluorine-based surfactants and silicon-based surfactants can be used.

[0094] <Polymerization initiator (I)> When the photopolymerizable compound (M) has a radical polymerizable group, a radical polymerization initiator (I1) is used as the polymerization initiator (I). When the photopolymerizable compound (M) has a cationic polymerizable group, a cationic polymerization initiator (I2) is used as the polymerization initiator (I). A photoinitiator is used as the polymerization initiator (I) because it can perform site-selective curing of the photocurable composition and there is no concern about deterioration, volatilization, sublimation, etc. of the components of the photocurable composition due to heat. The polymerization initiator (I) is not particularly limited, and various conventionally known polymerization initiators can be used.

[0095] Specific examples of photoradical polymerization initiators useful as the radical polymerization initiator (I1) include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 2,2-dimethoxy-1,2-diphenyl Ethan-1-one, bis(4-dimethylaminophenyl)ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, O-acetyl-1-[6-(2-methylbenzoyl)-9-ethyl-9H-carbazol-3-yl]ethanone oxime, (9-ethyl-6-nitro-9H-carbazol-3-yl)[4-(2-methoxy-1-methylethoxy)-2-methylphenyl]methanone O-acetyl oxime, 2-(benzoyloxyimino)-1-[4-(phenylthio)phenyl]-1-octanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 4-benzoyl-4'-methyldimethyl sulfide, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, butyl 4-dimethylaminobenzoate, 4-dimethylamino-2-ethylhexylbenzoic acid, 4-dimethylamino-2-isoamylbenzoic acid, benzyl-β-methoxyethyl acetal, benzyl Dimethyl ketal, 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime, o-methylbenzoylbenzoate, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 1-chloro-4-propoxythioxanthone, thioxanthene, 2-chlorothioxanthene, 2,4-diethylthioxanthene, 2-methylthioxanthene, 2-isopropylthioxanthene, 2-ethylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, 2,3-Diphenylanthraquinone, azobisisobutyronitrile, benzoyl peroxide, cumene hydroperoxide, 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, 2-mercaptobenzothiazole, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)-imidazolyl dimer, benzophenone, 2-chlorobenzophenone, p,p'-bisdimethylaminobenzophenone, 4,4'-bisdiethylaminobenzophenone, 4,4'-dichlorobenzophenone, 3,3-dimethyl-4-methoxy Benzophenone, benzil, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, benzoin butyl ether, acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, dichloroacetophenone, trichloroacetophenone, p-tert-butylacetophenone, p-dimethylaminoacetophenone, p-tert-butyltrichloroacetophenone acetophenone, p-tert-butyldichloroacetophenone, α,α-dichloro-4-phenoxyacetophenone, thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, dibenzosuberone, pentyl-4-dimethylaminobenzoate, 9-phenylacridine, 1,7-bis-(9-acridinyl)heptane, 1,5-bis-(9-acridinyl)pentane, 1,3-bis-(9-acridinyl)propane, p-methoxytriazine, 2,4,6-tris(trichloromethyl)-s-triazine, 2-methyl-4,6- Bis(trichloromethyl)-s-triazine, 2-[2-(5-methylfuran-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(furan-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(4-diethylamino-2-methylphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(3,4-dimethoxyphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxyphenyl)-4,Examples of the photoradical polymerization initiator include 6-bis(trichloromethyl)-s-triazine, 2-(4-ethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-n-butoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis-trichloromethyl-6-(3-bromo-4-methoxy)phenyl-s-triazine, 2,4-bis-trichloromethyl-6-(2-bromo-4-methoxy)phenyl-s-triazine, 2,4-bis-trichloromethyl-6-(3-bromo-4-methoxy)styrylphenyl-s-triazine, and 2,4-bis-trichloromethyl-6-(2-bromo-4-methoxy)styrylphenyl-s-triazine. These photoradical polymerization initiators can be used alone or in combination of two or more.

[0096] Among the photoradical polymerization initiators, oxime ester compounds are preferred from the viewpoint of the sensitivity of the photocurable composition, and phosphine oxide compounds are preferred from the viewpoint of good deep curing properties of the photocurable composition.

[0097] Preferable specific examples of the oxime ester compound include the following compounds. [ka]

[0098] Preferred specific examples of the phosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide.

[0099] As the cationic polymerization initiator (I2), a conventionally known cationic polymerization initiator can be used without any particular limitation. Typical examples of the cationic polymerization initiator (I2) include onium salts. As the cationic polymerization initiator (I2), oxonium salts, ammonium salts, phosphonium salts, sulfonium salts, and iodonium salts can be mentioned, with sulfonium salts and iodonium salts being preferred, and sulfonium salts being more preferred.

[0100] The content of the polymerization initiator (I) in the photocurable composition is not particularly limited. The content of the polymerization initiator (I) is appropriately determined depending on the type of the radical polymerizable group or the cationic polymerizable group and the type of the polymerization initiator (I). The content of the initiator (C) in the photocurable composition is preferably 0.01 parts by mass or more and 20 parts by mass or less, more preferably 0.1 parts by mass or more and 15 parts by mass or less, and even more preferably 1 part by mass or more and 10 parts by mass or less, when the mass of the photocurable composition excluding the mass of the above-mentioned solvent (L) is 100 parts by mass.

[0101] <Production method of cured product> The photocurable composition described above is typically made into a cured product by a method including molding the photocurable composition according to the shape of the cured product to be formed, and exposing the molded photocurable composition to light.

[0102] The thickness of the cured film made of the cured product of the photocurable composition is not particularly limited and may be appropriately selected depending on the application. The thickness of the cured film is typically preferably 1 nm or more and 20 μm or less, and more preferably 50 nm or more and 10 μm or less.

[0103] The method of molding the photocurable composition is not particularly limited and is appropriately selected depending on the shape of the cured product. The shape of the cured product is not limited to these, but may be a film shape, a lens shape, a line shape, a prism shape, etc. Among these shapes, a film shape is preferred. The method for molding the photocurable composition is not particularly limited. When the shape of the cured product is a lens shape, a prism shape, or the like, the photocurable composition may be filled into a mold corresponding to the shape of the cured product using a squeegee or the like. When the cured product has a line shape or the like, the photocurable composition may be applied onto a substrate in accordance with the shape of the cured product. Examples of the application method include printing methods such as an inkjet method. Examples of a method for applying the cured product in the form of a film include a method using a contact transfer type application device such as a roll coater, a reverse coater, or a bar coater, or a non-contact type application device such as a spinner (rotary application device), a curtain flow coater, etc. The photocurable composition can also be applied in the form of a film by a printing method such as an inkjet method.

[0104] When the photocurable composition contains a solvent (L), after the photocurable composition is molded into a desired shape, the solvent (L) may be removed from the molded photocurable composition by a method such as heating.

[0105] For example, the photocurable composition molded into a desired shape such as a film may be exposed to light to an extent that the photocurable composition does not completely cure, and then the semi-cured photocurable composition may be shaped by an imprint method or the like. In this case, the shaped semi-cured photocurable composition is further exposed to light to fully cure the photocurable composition to a desired extent. Furthermore, the photocurable composition described above may be applied to a 3D printing method, and a thin-film cured product may be laminated by repeating inkjet printing and curing by exposure to form a cured product of a desired shape.

[0106] As an exposure method for curing the photocurable composition molded by the above method, various methods known as methods for curing photosensitive compositions can be appropriately applied. The molded photocurable liquid composition is exposed to, for example, active energy rays such as ultraviolet rays and excimer laser light.

[0107] The molded photocurable composition may be exposed to light in a position-selective manner, for example, by exposure through a mask. When the exposure is performed in a position-selective manner, the exposed photocurable composition is developed with an organic solvent to remove the unexposed areas, thereby forming a patterned cured product. When development is carried out, it is preferable to thoroughly remove the developer after development by a method such as drying by heating.

[0108] According to the method described above, a cured product having a desired shape can be formed using the above-mentioned photocurable composition containing no solvent (L) or only a small amount of solvent (L).

[0109] As described above, the present inventors provide the following (1) to (20). (1) dispersing crude metal oxide particles (A) selected from crude metal oxide particles (A1) prepared by a solvothermal method and crude metal oxide particles (A2) obtained by capping the surfaces of the crude metal oxide particles (A1) with a capping agent in a nitrogen-containing polar organic solvent (S) containing water; and heating crude metal oxide particles (A) in a nitrogen-containing polar organic solvent (S) to obtain modified metal oxide particles having a modified surface. (2) The method for producing modified metal oxide particles according to (1), wherein the nitrogen-containing polar organic solvent (S) contains at least one additive (B) selected from the group consisting of basic compounds, acidic compounds, and capping agents. (3) The method for producing modified metal oxide particles according to (2), wherein the acidic compound as the additive (B) is an aliphatic carboxylic acid having from 1 to 4 carbon atoms. (4) The method for producing modified metal oxide particles according to (2), wherein the capping agent as the additive (B) is a silane coupling agent. (5) The method for producing modified metal oxide particles according to (4), wherein the silane coupling agent is an ω-aminoalkyltrialkoxysilane. (6) The method for producing modified metal oxide particles according to any one of (1) to (5), wherein the crude metal oxide particles (A) are heated at a temperature of 50°C or higher and 200°C or lower. (7) The method for producing modified metal oxide particles according to (6), wherein the crude metal oxide particles (A) are heated at a temperature of 70°C or higher and 90°C or lower, or 140°C or higher and 160°C or lower. (8) The crude metal oxide particles (A) Heat at 70℃ to 90℃ for 30 to 90 minutes, or Heat at 140℃ to 160℃ for 30 to 90 minutes, or The method for producing modified metal oxide particles according to (7), further comprising heating at 70°C to 90°C for 30 to 90 minutes, followed by heating at 140°C to 160°C for 30 to 90 minutes. (9) The method for producing modified metal oxide particles according to any one of (1) to (8), wherein the nitrogen-containing polar organic solvent (S) is a solvent having a bond represented by -CO-N<. (10) The method for producing modified metal oxide particles according to (9), wherein the nitrogen-containing polar organic solvent (S) is a urea compound. (11) A method for producing modified metal oxide particles according to any one of (1) to (10), wherein the crude metal oxide particles (A) contain at least one metal element selected from the group consisting of Ag, Cu, In, Sn, Ti, Hf, Al, Zr, Zn, Sn, Ce, Ga, Y, V, Ta, W, Mo, Nb, Mn, Fe, Co, Ni, Ru, Rh, Re, Pd, Os, Ir, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu. (12) Crude metal oxide particles (A1) are prepared in a solvent (Z) by a solvothermal method; The method for producing modified metal oxide particles according to any one of (1) to (11), wherein the solvent (Z) consists of water and / or an organic solvent. (13) The method for producing modified metal oxide particles according to (12), wherein the organic solvent is at least one selected from the group consisting of alcohol compounds and carbonyl compounds. (14) The method for producing modified metal oxide particles according to any one of (1) to (13), wherein the crude metal oxide particles (A) are titanium oxide particles. (15) The method for producing modified metal oxide particles according to any one of (1) to (14), wherein the capping agent used to cap the surface of the crude metal oxide particles (A2) is at least one selected from the group consisting of silane coupling agents, carboxylic acid compounds, alcohol compounds, thiol compounds, sulfonate compounds, phosphonate compounds, and phosphate compounds. (16) The method for producing modified metal oxide particles according to (15), wherein the capping agent for capping the surfaces of the crude metal oxide particles (A2) is a silane coupling agent. (17) The method for producing modified metal oxide particles according to any one of (1) to (16), wherein the amount of organic matter contained in the crude metal oxide particles (A) measured by thermogravimetric analysis is 5 mass % or more and 15 mass % or less, based on the mass of the crude metal oxide particles (A). (18) Modified metal oxide particles produced by the method according to any one of (1) to (17). (19) A photocurable composition comprising the modified metal oxide according to (18) above and a transparent substrate component. (20) A cured product of the photocurable composition according to (19). EXAMPLES

[0110] The present invention will be described in more detail below by showing examples, but the scope of the present invention is not limited to these examples.

[0111] <Preparation of Crude Metal Oxide Particles (A) and Modified Metal Oxide Particles> [Preparation Example 1] Titanium oxide particles (a1) were prepared as crude metal oxide particles (A) in benzyl alcohol by the same method as in Example 8 of WO 2020 / 106860. The amount of organic matter contained in the titanium oxide particles (a1) by thermogravimetric analysis was 11.90% by mass. [Preparation Example 2] 100 parts by mass of titanium oxide particles (a1) and 300 parts by mass of N,N,N',N'-tetramethylurea as a nitrogen-containing polar organic solvent (S) were mixed while purging with nitrogen at 30 ml / min. The mixture was heated at 80°C for 60 minutes, and then heated at 150°C for 30 minutes to react the surfaces of the titanium oxide particles (a1) in a nitrogen purged environment. n-Heptane was added to the reaction liquid to precipitate solids, which were then centrifuged to obtain modified titanium oxide particles (P2) in which the surfaces of the titanium oxide particles (a1) were modified. The amount of organic matter contained in the modified titanium oxide particles (P2) by thermogravimetric analysis was 11.01% by mass.

[0112] [Preparation Example 3] 100 parts by mass of titanium oxide particles (a1), 300 parts by mass of N,N,N',N'-tetramethylurea as a nitrogen-containing polar organic solvent (S), and 6 parts by mass of water were mixed while purging with nitrogen at 30 ml / min. The mixture was heated at 80°C for 60 minutes, and then heated at 150°C for 30 minutes to react the surface of titanium oxide particles (a1) in a nitrogen purged environment. n-Heptane was added to the reaction liquid to precipitate solids, and the mixture was centrifuged to obtain modified titanium oxide particles (P3) in which the surface of titanium oxide particles (a1) was modified. The amount of organic matter contained in the modified titanium oxide particles (P3) by thermogravimetric analysis was 10.45% by mass.

[0113] [Preparation Example 4] 100 parts by mass of titanium oxide particles (a1), 300 parts by mass of N,N,N',N'-tetramethylurea as a nitrogen-containing polar organic solvent (S), 3 parts by mass of water, and 3 parts by mass of triethylamine were mixed while purging with nitrogen at 30 ml / min. The mixture was heated at 80°C for 60 minutes, and then heated at 150°C for 30 minutes to react the surface of titanium oxide particles (a1) in a nitrogen purged environment. n-Heptane was added to the reaction liquid to precipitate solids, and the mixture was centrifuged to obtain modified titanium oxide particles (P4) in which the surface of titanium oxide particles (a1) was modified. The amount of organic matter contained in the modified titanium oxide particles (P4) by thermogravimetric analysis was 10.62% by mass.

[0114] [Preparation Example 5] 100 parts by mass of titanium oxide particles (a1), 300 parts by mass of N,N,N',N'-tetramethylurea as a nitrogen-containing polar organic solvent (S), 3 parts by mass of water, and 3 parts by mass of acetic acid were mixed while purging with nitrogen at 30 ml / min. The mixture was heated at 80°C for 60 minutes, and then heated at 150°C for 30 minutes to react the surface of titanium oxide particles (a1) in a nitrogen purged environment. n-Heptane was added to the reaction liquid to precipitate solids, and the mixture was centrifuged to obtain modified titanium oxide particles (P5) in which the surface of titanium oxide particles (a1) was modified. The amount of organic matter contained in the modified titanium oxide particles (P5) by thermogravimetric analysis was 10.83% by mass.

[0115] [Preparation Example 6] 100 parts by mass of titanium oxide particles (a1), 300 parts by mass of N,N,N',N'-tetramethylurea as a nitrogen-containing polar organic solvent (S), 3 parts by mass of water, and 3 parts by mass of acetic acid were mixed while purging with nitrogen at 30 ml / min. The mixture was heated at 80°C for 60 minutes, and the surface of the titanium oxide particles (a1) was reacted in a nitrogen purged environment. n-Heptane was added to the reaction liquid to precipitate solids, and the mixture was centrifuged to obtain modified titanium oxide particles (P6) in which the surface of the titanium oxide particles (a1) was modified. The amount of organic matter contained in the modified titanium oxide particles (P6) by thermogravimetric analysis was 12.22% by mass.

[0116] [Preparation Example 7] 100 parts by mass of the modified titanium oxide particles (P6), 300 parts by mass of N,N,N',N'-tetramethylurea as a nitrogen-containing polar organic solvent (S), and 6 parts by mass of water were mixed while purging with nitrogen at 30 ml / min. The mixture was heated at 80°C for 30 minutes, and then heated at 150°C for 30 minutes, and the surface of the modified titanium oxide particles (P6) was reacted in a nitrogen purged environment. n-Heptane was added to the reaction liquid to precipitate solids, and the mixture was centrifuged to obtain modified titanium oxide particles (P7) in which the surface of the modified titanium oxide particles (P6) was further modified. The amount of organic matter contained in the modified titanium oxide particles (P7) by thermogravimetric analysis was 11.73% by mass.

[0117] [Preparation Example 8] 100 parts by mass of the modified titanium oxide particles (P6), 300 parts by mass of N,N,N',N'-tetramethylurea as a nitrogen-containing polar organic solvent (S), 6 parts by mass of water, and 1 part by mass of 3-aminopropyltrimethoxysilane (KBM-903 (Shin-Etsu Silicone Co., Ltd.)) were mixed while purging with nitrogen at 30 ml / min. The mixture was heated at 80°C for 30 minutes, and then heated at 150°C for 30 minutes to react the surface of the modified titanium oxide particles (P6) in a nitrogen purged environment. n-Heptane was added to the reaction liquid to precipitate solids, and the mixture was centrifuged to obtain modified titanium oxide particles (P8) in which the surface of the modified titanium oxide particles (P6) was further modified. The amount of organic matter contained in the modified titanium oxide particles (P8) by thermogravimetric analysis was 11.28% by mass.

[0118] <Evaluation of metal oxide particle surfaces> The surfaces of the titanium oxide particles (a1) and the modified titanium oxide particles (P4) to (P5) were analyzed using a Fourier transform infrared spectrometer (FT-IR) NICOLET 6700 (manufactured by ThermoScientific Corporation) to obtain FT-IR spectra relating to wavenumber and absorbance. From the obtained FT-IR spectra, the wavenumber of 950 cm originating from Si-O-Si on the surface of the titanium oxide particles (a1) was -1 ~1150cm -1 It was found that the intensity of the peaks derived from the Si-O-Si on the surface of the modified titanium oxide particles (P4) to (P5) was stronger than the intensity of the peaks around the surface of the modified titanium oxide particles (P4) to (P5). This suggests that the organic matter on the titanium oxide particle surface was removed and Si-O-Si bonds were formed. In addition, the surfaces of the titanium oxide particles (a1) and the modified titanium oxide particles (P6) to (P8) were measured using an X-ray photoelectron spectrometer K-Alpha (manufactured by ThermoScientific Corporation).

[0119] [Table 1]

[0120] From Table 1, it can be seen that the carbon ratio on the surface of the modified titanium oxide particles (P6) is lower than that on the surface of the titanium oxide particles (a1). This shows that carbon-containing impurities originating from the titanium oxide particle raw material compound and the solvent used in the solvothermal method present on the titanium oxide particle surface have been removed. Furthermore, the carbon ratio on the surface of the modified titanium oxide particles (P7) is lower than that on the surface of the modified titanium oxide particles (P6). This shows that carbon-containing impurities originating from the titanium oxide particle raw material compound and the solvent used in the solvothermal method on the titanium oxide particle surface are also removed by the second heating. When the silicon ratio and nitrogen ratio of the modified titanium oxide particles (P6) are compared with those of the modified titanium oxide particles (P8) modified by the second heating, it can be seen that the silicon ratio and nitrogen ratio of the modified titanium oxide particles (P8) are higher than those of the modified titanium oxide particles (P6). Furthermore, when the modified titanium oxide particles (P7) obtained by modifying the same modified titanium oxide particles (P6) by a second heating are compared with the modified titanium oxide particles (P8), it is found that the silicon ratio and nitrogen ratio of the modified titanium oxide particles (P8) are higher than those of the modified titanium oxide particles (P7). This shows that the surface of the modified titanium oxide particles was further modified by the 3-aminopropyltrimethoxysilane added in Preparation Example 8.

[0121] <Preparation of Photocurable Composition> In Comparative Examples 1 and 2 and Examples 1 to 6, the following M-1 was used as the photopolymerizable compound (M). M-1: Compound having the following structure [ka]

[0122] In Comparative Examples 1 and 2 and Examples 1 to 6, the titanium oxide particles or modified titanium oxide particles shown in Table 2 were used.

[0123] In Comparative Examples 1 and 2 and Examples 1 to 6, a mixed solvent L-3 obtained by mixing the following L-1 and L-2 in a 1:1 ratio was used as the above-mentioned solvent (L). L-1:HO-(CH 2 CH 2 CH 2 -O) 2 -CH 3 (Dipropylene glycol monomethyl ether) L-2:HO-(C(CH 3 )HCH 2 -O) 3 -CH 3 (Tripropylene glycol monomethyl ether)

[0124] In Comparative Examples 1 and 2 and Examples 1 to 6, the following I-1, which is a radical polymerization initiator (I1), was used as the polymerization initiator (I). I-1: Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide

[0125] In Comparative Examples 1 and 2 and Examples 1 to 6, 8 parts by mass of photopolymerizable compound M-1, 91 parts by mass of titanium oxide particles or modified titanium oxide particles shown in Table 2, and 1 part by mass of polymerization initiator I-1 were dissolved and dispersed in mixed solvent L-3 to a solid content concentration of 10% by mass to obtain a photocurable composition. [Table 2]

[0126] <Heat resistance> The photocurable composition was applied onto a glass substrate using a spin coater, and the film formed from the cured product was prebaked at 110°C for 2 minutes to obtain a coating film having a thickness sufficient to form a cured film with a thickness of 280 nm. The obtained coating film was exposed to an integrated light dose of 5 J / cm using a high-pressure mercury lamp. 2 The exposed coating film was post-exposure baked (PEB) at 185° C. for 2 minutes to obtain a cured film. The refractive index of the resulting cured film was measured using a spectroscopic ellipsometer M-2000UI (manufactured by JA Woollam Co., Ltd.) to determine the refractive index at a wavelength of 520 nm. The total light reflectance was measured at a wavelength of 460 nm using a UV-Vis-NIR spectrophotometer UH4150 (Hitachi High-Tech Science Corporation) and a Spectralon white standard reflector (Labpshere). The total light reflectance of the coating film after exposure before PEB was R1, and the total light reflectance of the cured film after PEB was R2. Based on the improvement rate of the total light reflectance calculated by the following formula, the heat resistance was evaluated according to the following criteria. Improvement rate of total light reflectance (%) = ((R2-R1) of Comparative Example 1-(R2-R1) of Comparative Example 2 or each Example) ×100 / (R2-R1) of Comparative Example 1 (Evaluation Criteria) ◎: Improvement in total light reflectance is 30% or more 〇: Improvement in total light reflectance is 10% or more but less than 30% ×: Improvement in total light reflectance is less than 10%

[0127] <Refractive index> ◯: refractive index higher than that of Comparative Example 1 ×: Refractive index of Comparative Example 1 or lower

[0128] [Table 3]

[0129] Table 2 shows that by using modified metal oxide particles obtained by dispersing crude metal oxide particles (A) in a nitrogen-containing polar organic solvent (S) containing water and heating the resulting mixture, it is possible to prepare a photocurable composition that is less likely to lose transparency when heated and that gives a cured product that exhibits good optical properties.

Claims

1. dispersing crude metal oxide particles (A) selected from crude metal oxide particles (A1) prepared by a solvothermal method and crude metal oxide particles (A2) obtained by capping the surfaces of the crude metal oxide particles (A1) with a capping agent in a nitrogen-containing polar organic solvent (S) containing water; and heating the crude metal oxide particles (A) in the nitrogen-containing polar organic solvent (S) to obtain modified metal oxide particles having a modified surface.

2. 2. The method for producing modified metal oxide particles according to claim 1, wherein the nitrogen-containing polar organic solvent (S) contains at least one additive (B) selected from the group consisting of basic compounds, acidic compounds, and capping agents.

3. The method for producing modified metal oxide particles according to claim 2, wherein the acidic compound as the additive (B) is an aliphatic carboxylic acid having from 1 to 4 carbon atoms.

4. The method for producing modified metal oxide particles according to claim 2 , wherein the capping agent as the additive (B) is a silane coupling agent.

5. The method for producing modified metal oxide particles according to claim 4, wherein the silane coupling agent is an ω-aminoalkyltrialkoxysilane.

6. The method for producing modified metal oxide particles according to claim 1 or 2, wherein the crude metal oxide particles (A) are heated at a temperature of 50°C or more and 200°C or less.

7. The method for producing modified metal oxide particles according to claim 6, wherein the crude metal oxide particles (A) are heated at a temperature of 70°C or higher and 90°C or lower, or 140°C or higher and 160°C or lower.

8. The coarse metal oxide particles (A), Heat at 70°C to 90°C for 30 to 90 minutes, or Heat at 140°C to 160°C for 30 to 90 minutes, or 8. The method for producing modified metal oxide particles according to claim 7, wherein the mixture is heated at 70° C. to 90° C. for 30 to 90 minutes, and then heated at 140° C. to 160° C. for 30 to 90 minutes.

9. 3. The method for producing modified metal oxide particles according to claim 1, wherein the nitrogen-containing polar organic solvent (S) is a solvent having a bond represented by --CO--N<.

10. The method for producing modified metal oxide particles according to claim 9, wherein the nitrogen-containing polar organic solvent (S) is a urea compound.

11. 3. The method for producing modified metal oxide particles according to claim 1 or 2, wherein the crude metal oxide particles (A) contain at least one metal element selected from the group consisting of Ag, Cu, In, Sn, Ti, Hf, Al, Zr, Zn, Sn, Ce, Ga, Y, V, Ta, W, Mo, Nb, Mn, Fe, Co, Ni, Ru, Rh, Re, Pd, Os, Ir, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu.

12. The crude metal oxide particles (A1) are prepared in a solvent (Z) by a solvothermal method, The method for producing modified metal oxide particles according to claim 1 or 2, wherein the solvent (Z) comprises water and / or an organic solvent.

13. The method for producing modified metal oxide particles according to claim 12, wherein the organic solvent is at least one selected from the group consisting of alcohol compounds and carbonyl compounds.

14. The method for producing modified metal oxide particles according to claim 11, wherein the crude metal oxide particles (A) are titanium oxide particles.

15. 3. The method for producing modified metal oxide particles according to claim 1 or 2, wherein the capping agent for capping the surface of the crude metal oxide particles (A2) is at least one selected from the group consisting of silane coupling agents, carboxylic acid compounds, alcohol compounds, thiol compounds, sulfonate compounds, phosphonate compounds, and phosphate compounds.

16. 16. The method for producing modified metal oxide particles according to claim 15, wherein the capping agent for capping the surfaces of the crude metal oxide particles (A2) is a silane coupling agent.

17. 3. The method for producing modified metal oxide particles according to claim 1, wherein the amount of organic matter contained in the crude metal oxide particles (A) measured by thermogravimetric analysis is 5% by mass or more and 15% by mass or less, based on the mass of the crude metal oxide particles (A).

18. 3. Modified metal oxide particles produced by the method of claim 1 or 2.

19. 20. A photocurable composition comprising the modified metal oxide of claim 18 and a transparent substrate component.

20. A cured product of the photocurable composition according to claim 19.

Citation Information

Patent Citations

  • Coated inorganic fine particle and method for producing same

    WO2019017305A1

  • Synthesis, capping, and dispersion of tio 2 nanocrystals

    WO2020106860A1