Electrode, secondary battery, battery pack, and vehicle

By using a titanium-containing composite oxide and carbon fibers in the electrode's active material layer with specific pore diameters, the battery achieves improved high-temperature cycle performance, addressing the challenge of maintaining electrolyte retention and conductive integrity.

JP2024139017AActive Publication Date: 2024-10-09KK TOSHIBA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023049783
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face challenges in maintaining high-temperature cycle performance, which is crucial for applications in vehicles and stationary systems.

Method used

Incorporating an active material-containing layer in electrodes with a titanium-containing composite oxide and carbon fibers, where the peak pore diameter ranges from 0.1 to 0.3 micrometers, ensuring uniform electrolyte retention and conductive paths that withstand volume changes.

Benefits of technology

The solution enhances the battery's cycle performance even in high-temperature environments, maintaining electrolyte retention and preventing conductive path destruction, thus improving energy density and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139017000001_ABST
    Figure 2024139017000001_ABST
Patent Text Reader

Abstract

To provide an electrode, a secondary battery, a battery pack, and a vehicle, having excellent high-temperature cyclic performance.SOLUTION: According to an embodiment, an electrode is provided. The electrode includes an active material-containing layer. The active material-containing layer includes an active material and carbon fiber. The active material includes a titanium-containing composite oxide. The active material-containing layer has a peak indicating a maximum logarithmic differential pore volume, in a logarithmic differential pore volume distribution curve by a mercury intrusion method. A pore diameter PD at the peak is greater than 0.1 μm and 0.3 μm or less. According to another embodiment, a secondary battery includes a positive electrode, a negative electrode, and an electrolyte. At least one of the positive electrode and the negative electrode is the electrode according to the one embodiment. According to still another embodiment, a battery pack is provided. This battery pack includes the secondary battery according to the other embodiment. According to yet another embodiment, a vehicle is provided. This vehicle includes the battery pack according to the still other embodiment.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]

[0002] Lithium ion secondary batteries, such as non-aqueous electrolyte secondary batteries, are rechargeable batteries that are charged and discharged by the movement of lithium ions between a positive electrode and a negative electrode. The positive electrode and the negative electrode hold a non-aqueous electrolyte containing lithium ions. Non-aqueous electrolyte secondary batteries are expected to be used not only as power sources for small electronic devices, but also as medium- to large-sized power sources for in-vehicle and stationary applications, and therefore require improved high-temperature cycle performance. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2021-44221 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide an electrode, a secondary battery, a battery pack, and a vehicle that are excellent in high-temperature cycle performance. [Means for solving the problem]

[0005] According to an embodiment, an electrode is provided. The electrode includes an active material-containing layer. The active material-containing layer includes an active material and carbon fiber. The active material includes a titanium-containing composite oxide. The active material-containing layer shows a peak indicating a maximum logarithmic differential pore volume in a logarithmic differential pore volume distribution curve obtained by mercury intrusion porosimetry. The pore diameter PD of the peak is greater than 0.1 μm and less than or equal to 0.3 μm.

[0006] According to another embodiment, the secondary battery includes a positive electrode, a negative electrode, and an electrolyte, wherein at least one of the positive electrode and the negative electrode is an electrode according to the embodiment.

[0007] According to another embodiment, a battery pack is provided, the battery pack including a secondary battery according to the embodiment.

[0008] According to another embodiment, a vehicle is provided, the vehicle including a battery pack according to an embodiment. [Brief description of the drawings]

[0009] [Figure 1] 1 is an example of an active material-containing layer of an electrode. [Diagram 2] 3 is an example of a logarithmic differential pore volume distribution curve of an active material-containing layer measured by mercury intrusion porosimetry. [Diagram 3] An example of a secondary battery. [Figure 4] 4 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 3. [Diagram 5] FIG. 13 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery. [Figure 6] 6 is an enlarged cross-sectional view of a portion B of the secondary battery shown in FIG. 5. [Figure 7] FIG. 1 is a perspective view illustrating an example of a battery pack. [Figure 8] FIG. 2 is an exploded perspective view illustrating an example of a battery pack. [Figure 9] FIG. 2 is a block diagram showing an example of an electrical circuit of a battery pack. [Figure 10] FIG. 1 is a partially see-through view illustrating an example of a vehicle. [Figure 11] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle. [Figure 12] Relationship between peak pore diameter PD and total pore volume TA. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (First embodiment) According to the present embodiment, an electrode is provided. The electrode includes an active material-containing layer. The active material-containing layer includes an active material and carbon fibers. The active material includes a titanium-containing composite oxide.

[0011] In the active material-containing layer of the electrode according to the embodiment, the active material and the carbon fiber are mixed. The carbon fiber can form a conductive path over a long distance compared to granular carbon. Therefore, in the active material-containing layer of the electrode according to the embodiment, the conductive path between the active materials is not easily broken even when the volume of the active material changes.

[0012] In addition, the electrode according to the embodiment has an active material-containing layer in which the pore diameter PD of the peak showing the maximum height, i.e., the mode diameter, is large enough to hold the electrolyte, and the full width at half maximum of the peak is relatively small. Therefore, it can be said that this active material-containing layer has a pore distribution in which pores large enough to hold the electrolyte are distributed relatively uniformly. Therefore, it can be said that the electrolyte is held uniformly in this active material-containing layer.

[0013] From the above, the electrode according to the embodiment can achieve excellent cycle performance even in a high-temperature environment. Hereinafter, in this specification, the cycle performance in a high-temperature environment may be referred to as "high-temperature cycle performance."

[0014] FIG. 1 is a schematic diagram showing an example of an active material-containing layer of an electrode according to an embodiment. The active material-containing layer shown in FIG. 1 includes active material particles 50, carbon fibers 51, and granular carbon 52. The active material particles 50 and the granular carbon 52 are in contact with the long and thin string-like carbon fibers 51. The carbon fibers 51 and the granular carbon 52 form a conductive path. The granular carbon 52 is present between the active material particles 50. The carbon fibers 51 can be present between the active material particles 50 that are spaced apart from each other. An electrolyte (not shown) can be impregnated into the gaps between the active material particles 50 and the granular carbon 52. The granular carbon 52 may be omitted. In the active material-containing layer shown in FIG. 1, even if the granular carbon 52 is omitted, the conductive path by the carbon fibers 51 is maintained.

[0015] FIG. 2 is a graph showing an example of a logarithmic differential pore volume distribution curve obtained by mercury intrusion of the active material-containing layer of the electrode according to the embodiment. In the graph of FIG. 2, the vertical axis is the logarithmic differential pore volume, and the horizontal axis is the pore diameter. The active material-containing layer of the electrode according to the present embodiment shows a peak indicating the maximum logarithmic differential pore volume in the logarithmic differential pore volume distribution curve obtained by mercury intrusion. The pore diameter PD of the peak is greater than 0.1 μm and less than 0.3 μm. The pore diameter PD of the peak, i.e., the mode diameter, is the size of the pore diameter with the highest abundance ratio among the multiple pores provided in the active material-containing layer. When the PD is within this range, a sufficient amount of electrolyte can be retained in the active material-containing layer. When the PD is sufficiently large, the electrolyte can easily impregnate the electrode even under high temperature conditions, and it is possible to suppress the liquid drying up during high temperature cycles. On the other hand, if the PD is too large, the strength of the electrode is weakened and the cycle performance is reduced. Therefore, it is preferable that the PD is greater than 0.1 μm and less than 0.3 μm. The logarithmic differential pore volume distribution curve of the active material containing layer was obtained by the method described below. The graph shown in Fig. 2 relates to Example 1 described below. In the graph in Fig. 2, PD is 0.12 µm.

[0016] The full width at half maximum of the peak is 0.1 μm or less. A small full width at half maximum of the peak indicates that the pores provided in the active material-containing layer are uniform in size. If the pores provided in the active material-containing layer are uniform in size, the electrolyte is uniformly held in the active material-containing layer, and the reaction between the active material and the electrolyte is likely to occur uniformly. There is no particular lower limit for the full width at half maximum of the peak, but in one example, it is 0.01 μm or more. The full width at half maximum of the peak is preferably 0.06 μm or less, and more preferably 0.05 μm or less. In the graph of FIG. 2, the full width at half maximum is 0.04 μm.

[0017] The logarithmic differential pore volume distribution curve and the cumulative pore volume distribution curve of the active material-containing layer by mercury intrusion porosimetry can be obtained, for example, by the following method. First, when the electrode is included in a secondary battery, the secondary battery is put into a discharged state, and then disassembled to remove the electrode. This disassembly is performed in a glove box under an inert gas atmosphere such as argon. The discharged state refers to a state in which the battery is discharged until the charge rate becomes 0%. The removed electrode is washed with a solvent and then dried. For example, ethyl methyl carbonate is used as the solvent. The dried electrode is cut to obtain a plurality of test pieces. The size of the test piece is, for example, a strip shape with a short side of 1.25 cm and a long side of 2.5 cm.

[0018] Next, a plurality of test pieces are placed in a measurement cell of a measuring device, and mercury is allowed to penetrate into the pores of the test pieces. The number of test pieces is, for example, 16 to 32. As the measurement cell, for example, a 5 cc cell for large pieces with a stem volume of 0.4 cc is used. As the measuring device, for example, an Autopore 9520 (Autopore 9520 model manufactured by Shimadzu Corporation) is used. In the measurement, for example, the initial pressure is set to 7 kPa, and the final pressure is set to 414 MPa. 7 kPa corresponds to 1.0 psia (pound per square inch absolute pressure), which corresponds to a pore with a diameter of approximately 180 μm. Also, 414 MPa corresponds to approximately 6 psia, which corresponds to a pore with a diameter of approximately 0.003 μm. The mercury contact angle is set to 130 degrees, and the mercury surface tension is set to 485 dynes / cm. By processing the obtained data, the logarithmic differential pore volume distribution curve, the cumulative pore volume distribution curve, the total pore surface area, and the total pore volume of the active material-containing layer can be obtained.

[0019] The total pore surface area TA of the active material-containing layer measured by mercury porosimetry is 4 m 2 It is preferable that the TA is 8 m / g or more. When the TA is large, it can be said that a plurality of fine pores are provided in the active material-containing layer. There is no particular upper limit to the size of the TA, but according to one example, it is 8 m 2 / g or less. TA is 5m 2 / g or more, and 2 It is more preferable that the molecular weight is 1 / g or more.

[0020] The total pore volume TV of the active material-containing layer measured by mercury porosimetry is preferably 0.15 mL / g or less. A smaller TV means fewer voids in the active material-containing layer. The use of an electrode having such an active material-containing layer can increase the energy density of a secondary battery. On the other hand, in terms of increasing the amount of electrolyte held by the active material-containing layer, TV is preferably 0.04 mL / g or more. In terms of high energy density and the ability to hold a sufficient amount of electrolyte, TV is more preferably 0.05 mL / g or more and 0.15 mL / g or less.

[0021] The value MD-PD obtained by subtracting the peak pore diameter PD from the median diameter MD of the active material-containing layer measured by mercury porosimetry is preferably -0.02 μm or more and 0.02 μm or less. The MD of the active material-containing layer is the pore diameter when the cumulative volume is 50% in the cumulative pore volume distribution curve of the active material-containing layer measured by mercury porosimetry. When the value MD-PD is within this range, it can be said that PD and MD are almost equal. It can be said that such an active material-containing layer has a more uniform pore diameter. The value MD-PD is more preferably -0.01 μm or more and 0.01 μm or less.

[0022] The relationship between the total pore surface area TA of the active material-containing layer and the peak pore diameter PD measured by mercury porosimetry is preferably represented by the following formula (1). TA = a × PD + b (1) Here, in the formula, a is a=-17, and in the formula, b is 7≦b≦10.6. An active material-containing layer in which the relationship between TA and PD falls within this range is less likely to deteriorate due to side reactions. The larger the TA, the higher the electrolyte retention of the electrode, so that the electrolyte is less likely to dry up during high-temperature cycles. However, if the TA exceeds a threshold value, side reactions accompanied by gas generation and the like may occur, resulting in a decrease in cycle performance. The smaller the PD, the greater the number of pores, so the larger the threshold value of TA. Thus, since there is a negative correlation between PD and TA, a is a negative value. It is more preferable that b used in formula (1) is 8≦b≦10.6.

[0023] The electrode according to the embodiment can be used as either a positive electrode or a negative electrode, but is preferably used as a negative electrode.

[0024] The electrodes according to the embodiment will be described in detail below.

[0025] The electrode may include an active material-containing layer and a current collector. The active material-containing layer is supported on at least one surface of the current collector. The active material-containing layer may be supported on one surface or both surfaces of the current collector. The active material-containing layer may further include granular carbon and a binder in addition to the active material and fibrous carbon.

[0026] The active material includes a titanium-containing composite oxide. The titanium-containing composite oxide is x TiM y Nb 2-y O 7±z (0≦x≦5, 0≦y≦0.5, -0.3≦z≦0.3, M is at least one metal element other than Ti and Nb, A is at least one of Li and Na), Li 2+a Na2Ti6O 14 (0≦a≦6), and Li x It is preferable that the material contains at least one compound represented by a general formula selected from the group consisting of TiO2 (0≦x≦1).

[0027] The titanium-containing composite oxide is preferably lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), monoclinic titanium dioxide (TiO2), anatase titanium dioxide, rutile titanium dioxide, hollandite titanium composite oxide, orthorhombic titanium composite oxide, and monoclinic niobium titanium composite oxide.

[0028] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+a M(I) 2-b Ti 6-c M(II)dO 14+σ Here, M(I) is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb, and K. M(II) is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).

[0029] As an example of the monoclinic niobium titanium composite oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium composite oxides include Li xNb2TiO7 (0≦x≦5) is an example of a monoclinic niobium titanium composite oxide. x Ti 1-y M3 y+z Nb 2-zO7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x<5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.

[0030] The carbon fibers and granular carbon are blended as a conductive agent to improve current collecting performance and reduce the contact resistance between the active material and the current collector.

[0031] Carbon fiber is a fibrous carbon having a ratio L1 / S1 of 50 or more between the length L1 in the longitudinal direction and the diameter of a cross section perpendicular to the longitudinal direction, i.e., the thickness S1. The ratio L1 / S1 is preferably 150 or more and 10,000 or less. The diameter of a cross section perpendicular to the longitudinal direction of the carbon fiber, i.e., the thickness, is preferably 1 nm or more and 200 nm or less (0.001 μm or more and 0.2 μm or less). The length of the carbon fiber is preferably 5 μm or more and 50 μm or less. An example of the carbon fiber is vapor grown carbon fiber (VGCF). An example of the vapor grown carbon fiber is carbon nanotube (CNT) and carbon nanofiber (CNF). One of these may be used as the carbon fiber, or two or more may be combined and used as the carbon fiber.

[0032] In the active material-containing layer, the amount of carbon fiber per 100 parts by mass of active material is preferably 0.01 parts by mass or more and 10 parts by mass or less, more preferably 0.1 parts by mass or more and 5 parts by mass or less. If the amount of carbon fiber is large, the electronic conductivity of the active material-containing layer can be increased. On the other hand, if the amount of carbon fiber is excessively large, the energy density may decrease.

[0033] Granular carbon is granular carbon having a ratio L2 / S2 of the length of the major axis L2 to the length of the minor axis S2 of less than 50. Granular carbon also includes flake carbon. Examples of granular carbon include carbon black such as acetylene black and carbonaceous materials such as graphite. One of these may be used as the granular carbon, or two or more of them may be used in combination as the granular carbon.

[0034] In the active material-containing layer, the amount of granular carbon per 100 parts by mass of active material is preferably 0 to 10 parts by mass, more preferably 1 to 5 parts by mass. If the amount of granular carbon is large, the electronic conductivity of the active material-containing layer can be increased. On the other hand, if the amount of granular fiber is excessively large, the energy density may decrease.

[0035] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the negative electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0036] In the active material-containing layer, the amount of binder per 100 parts by mass of active material is preferably 0 parts by mass or more and 10 parts by mass or less, more preferably 1 part by mass or more and 5 parts by mass or less. If the amount of binder is large, the binding between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, if the amount of binder is excessively large, the energy density may decrease.

[0037] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted into and extracted from the active material. For example, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.

[0038] The current collector may also include a portion on the surface of which no active material-containing layer is formed, and this portion can function as a current collecting tab.

[0039] The density of the active material-containing layer is 2.3 g / cm 3 More than 3g / cm 3 It is preferable that the density is 2.5 g / cm or less. 3 More than 2.8g / cm 3 It is more preferable that:

[0040] Next, a method for manufacturing an electrode according to an embodiment will be described.

[0041] First, the carbon fiber, the binder, and the pure water were mixed and stirred using a planetary mixer. The binder used here was the first binder. As the solvent, for example, N-methyl-2-pyrrolidone, etc., may be used in addition to the pure water. The stirring speed was, for example, 10 rpm to 60 rpm, and the stirring time was 5 minutes to 2 hours. Then, the active material and granular carbon were added to this mixture and further stirred using a planetary mixer. During stirring, the stirring speed was 40 rpm, and the stirring time was 30 minutes. Further stirring was performed using a bead mill. By further stirring using a bead mill, the dispersibility of the mixture is improved. As the bead mill, for example, a continuous horizontal ready mill RMH-03 manufactured by Imex Co., Ltd. was used. The flow rate of the bead mill was, for example, 10 mL / min to 50 mL / min. The rotation speed of the bead mill was 500 rpm to 2500 rpm. Then, the second binder was added and stirred using a planetary mixer to prepare a dispersion slurry.

[0042] Next, the dispersion slurry is applied to one or both sides of a current collector, and the coating is dried to obtain a laminate of the active material-containing layer and the current collector. The laminate is then pressed to obtain an electrode.

[0043] The electrode according to the first embodiment described above includes an active material-containing layer containing an active material and carbon fibers, and in a logarithmic differential pore volume distribution curve of the active material-containing layer measured by mercury intrusion porosimetry, the pore diameter PD of the peak showing the maximum logarithmic differential pore volume is greater than 0.1 μm and less than 0.3 μm. The full width at half maximum of the peak is less than 0.1 μm. By using this electrode, a secondary battery having excellent cycle performance can be realized even in a high-temperature environment of 60° C. or more. This secondary battery has excellent cycle performance, particularly in a high-temperature environment of 70° C. or more.

[0044] Second embodiment According to the second embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. At least one of the negative electrode and the positive electrode is the electrode according to the first embodiment. When either the negative electrode or the positive electrode is the electrode according to the first embodiment, the counter electrode may have a different configuration from that of the first embodiment.

[0045] The secondary battery according to the second embodiment may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.

[0046] Moreover, the secondary battery according to the second embodiment can further include an exterior member that houses the electrode group and the electrolyte.

[0047] Furthermore, the secondary battery according to the second embodiment may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.

[0048] The secondary battery according to the second embodiment may be, for example, a lithium ion secondary battery. The secondary battery includes a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.

[0049] Fig. 3 is a cross-sectional view that illustrates an example of a secondary battery according to embodiment 2. Fig. 4 is an enlarged cross-sectional view of part A of the secondary battery illustrated in Fig. 3.

[0050] The secondary battery 100 shown in Figures 3 and 4 includes a bag-shaped exterior member 2 shown in Figures 3 and 4, an electrode group 1 shown in Figure 3, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.

[0051] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0052] As shown in Fig. 3, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 4, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.

[0053] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 4. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.

[0054] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.

[0055] As shown in FIG. 3, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.

[0056] The secondary battery according to the second embodiment is not limited to the secondary battery having the configuration shown in FIGS. 3 and 4, but may be a battery having the configuration shown in FIGS.

[0057] Fig. 5 is a partially cutaway perspective view showing typically another example of the secondary battery according to embodiment 2. Fig. 6 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 5.

[0058] The secondary battery 100 shown in Figures 5 and 6 includes an electrode group 1 shown in Figures 5 and 6, an exterior member 2 shown in Figure 5, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.

[0059] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0060] The electrode group 1 is a laminated type electrode group, as shown in Fig. 6. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.

[0061] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.

[0062] The negative electrode current collector 3a of each negative electrode 3 includes a portion 3c on one side of which the negative electrode active material-containing layer 3b is not supported on any surface. This portion 3c serves as a negative electrode current collector tab. As shown in FIG. 6, the portion 3c serving as the negative electrode current collector tab does not overlap with the positive electrode 5. In addition, the multiple negative electrode current collector tabs (portions 3c) are electrically connected to a strip-shaped negative electrode terminal 6. The tip of the strip-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.

[0063] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6, and is drawn out to the outside of the exterior member 2.

[0064] The counter electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.

[0065] 1) Counter electrode The counter electrode may include an active material-containing layer and a current collector. The active material-containing layer may be supported on one surface of the current collector or on both surfaces. The active material-containing layer may contain an active material, a conductive agent, and a binder. The active material-containing layer may or may not contain fibrous carbon. The counter electrode is the negative electrode when the electrode according to the embodiment is the positive electrode, and is the positive electrode when the electrode according to the embodiment is the negative electrode. The counter electrode is preferably the positive electrode. Here, the description will be made assuming that the counter electrode is the positive electrode.

[0066] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain, as the positive electrode active material, one type of compound alone or a combination of two or more types of compounds. Examples of the oxide and the sulfide include compounds into which Li or Li ions can be inserted and desorbed.

[0067] Examples of such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≦ 1, Li x Fe 1-y Mn yPO4; 0 < x ≤ 1, 0 < y < 1, Li x CoPO4; 0 < x ≤ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) is included.

[0068] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≤ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≤ 1), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) is included. Using these compounds as the positive electrode active material can increase the positive electrode potential.

[0069] When using a room temperature molten salt as the electrolyte of the battery, lithium iron phosphate, Li xIt is preferable to use a positive electrode active material containing VPO4F (0≦x≦1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide, or a mixture thereof. These compounds have low reactivity with room temperature molten salts, so that the cycle life can be improved. Details of the room temperature molten salt will be described later.

[0070] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less can smoothly diffuse lithium ions in the solid.

[0071] The specific surface area of ​​the positive electrode active material is 0.1 m 2 / g or more 10m 2 / g or less. 2 A positive electrode active material having a specific surface area of ​​10m / g or more can secure sufficient sites for absorbing and releasing Li ions. 2 A positive electrode active material having a specific surface area of ​​100 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.

[0072] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxy methyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0073] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.

[0074] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in an amount of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.

[0075] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.

[0076] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.

[0077] By making the amount of the conductive agent 3% by mass or more, the above-mentioned effects can be achieved. Also, by making the amount of the conductive agent 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.

[0078] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.

[0079] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.

[0080] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.

[0081] The electrode can be produced, for example, by the following method. First, an active material, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, an electrode is produced. The mixture is mixed to obtain a mixture, which is then formed into pellets, which can then be placed on a current collector to obtain an electrode.

[0082] 2) Electrolyte The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.

[0083] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.

[0084] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.

[0085] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.

[0086] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.

[0087] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.

[0088] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.

[0089] 3) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.

[0090] 4) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.

[0091] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.

[0092] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.

[0093] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.

[0094] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.

[0095] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.

[0096] 5) Negative terminal The negative electrode terminal can be made of a material that is electrochemically stable at the Li absorption / release potential of the negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.

[0097] 6) Positive terminal The positive electrode terminal can be formed from a material that is electrically stable in a potential range of 3 V to 4.5 V (vs. Li / Li+) relative to the redox potential of lithium and has electrical conductivity. Examples of the material for the positive electrode terminal include aluminum and aluminum alloys containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. In order to reduce the contact resistance with the positive electrode collector, the positive electrode terminal is preferably formed from the same material as the positive electrode collector.

[0098] Next, the secondary battery according to the second embodiment will be described in more detail with reference to the drawings.

[0099] The secondary battery according to the second embodiment includes the electrode according to the first embodiment, and therefore the secondary battery according to the second embodiment has excellent high-temperature cycle performance.

[0100] (Third embodiment) According to a third embodiment, a battery pack is provided. The battery pack according to the third embodiment includes a plurality of secondary batteries according to the second embodiment. In the battery pack according to the third embodiment, the individual cells may be electrically connected in series or in parallel, or may be connected in a combination of series and parallel.

[0101] Fig. 7 is a perspective view showing an example of a battery pack according to the third embodiment. The battery pack 200 shown in Fig. 7 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the second embodiment.

[0102] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 7 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.

[0103] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.

[0104] The battery pack according to the third embodiment includes the secondary battery according to the second embodiment, and therefore has excellent high-temperature cycle performance.

[0105] (Fourth embodiment) According to a fourth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the third embodiment. The battery pack may include a single secondary battery according to the second embodiment, instead of the battery assembly according to the third embodiment.

[0106] Fig. 8 is an exploded perspective view showing an example of a battery pack according to a fourth embodiment. Fig. 9 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 8. The battery pack 300 shown in Figs. 8 and 9 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).

[0107] 8 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be capable of housing a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to house the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.

[0108] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.

[0109] At least one of the plurality of unit cells 100 is a secondary battery according to the second embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 9. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.

[0110] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.

[0111] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.

[0112] The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.

[0113] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.

[0114] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100 and transmits the detection signal to the protection circuit 346. The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353. The external terminal 350 for current supply is for outputting a current from the secondary battery to the outside and / or for inputting a current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, a current is supplied to the outside through the external terminal for current supply. Also, when the battery pack is charged, a charging current (including regenerative energy of the power of an automobile or the like) is supplied to the battery pack through the external terminal for current supply.

[0115] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via wiring 35. The protection sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction facing the printed wiring board 34 via the assembled battery 200. The protection sheet 33 is made of, for example, resin or rubber.

[0116] The protection circuit 346 controls charging and discharging of the multiple cells 100. The protection circuit 346 also cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345 or a detection signal transmitted from each cell 100 or the battery pack 200. The protection circuit 346 may be a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source, and may be used as a protection circuit for the battery pack.

[0117] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.

[0118] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.

[0119] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.

[0120] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the plurality of assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal and a negative terminal, respectively, of the external terminals for current supply.

[0121] Such a battery pack is used in applications requiring excellent cycle performance when a large current is drawn, for example, in a high-temperature environment. Specifically, the battery pack is used, for example, as a stationary battery or an on-board battery for various vehicles. The battery pack is particularly suitable for use as an on-board battery.

[0122] The battery pack according to the fourth embodiment includes the secondary battery according to the second embodiment or the battery pack according to the third embodiment, and therefore has excellent high-temperature cycle performance.

[0123] Fifth embodiment According to a fifth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fourth embodiment. Examples of the vehicle according to the fifth embodiment include a two-wheeled to four-wheeled hybrid electric vehicle, a two-wheeled to four-wheeled electric vehicle, an electric-assisted bicycle, and a railroad car.

[0124] Fig. 10 is a partial see-through view that illustrates an example of a vehicle according to an embodiment. The vehicle 400 illustrated in Fig. 10 includes a vehicle body 40 and a battery pack 300 according to a fourth embodiment. In the example illustrated in Fig. 10, the vehicle 400 is a four-wheeled automobile. The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.

[0125] 10 illustrates an example in which the battery pack 300 is mounted in an engine compartment located in front of the vehicle body 40, but the mounting position of the battery pack 300 is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment of the vehicle body 40, at the rear of the vehicle body, or under the seat.

[0126] This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.

[0127] The vehicle according to the fifth embodiment may be equipped with a plurality of battery packs 300. In this case, the batteries included in each battery pack 300 may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. For example, when each battery pack 300 includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. Alternatively, when each battery pack 300 includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections.

[0128] FIG. 11 is a diagram that shows an example of a control system for an electrical system in a vehicle according to an embodiment. The vehicle 400 shown in FIG. 11 is an electric vehicle. The vehicle 400 includes a vehicle body 40, a vehicle power supply 41, a vehicle ECU (Electric Control Unit) 42 that is a higher-level control device of the vehicle power supply 41, an external terminal (a terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45. The vehicle 400 has the vehicle power supply 41 mounted, for example, in an engine room, at the rear of the vehicle body, or under a seat. Note that, in the vehicle 400 shown in FIG. 11, the mounting location of the vehicle power supply 41 is shown only in outline.

[0129] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.

[0130] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.

[0131] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the second embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.

[0132] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.

[0133] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.

[0134] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.

[0135] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 11) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a to 200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a to 200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed near the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.

[0136] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.

[0137] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.

[0138] In the vehicle according to the fifth embodiment, the battery pack recovers, for example, regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy. The regenerative braking mechanism rotates the drive motor 45 when braking the vehicle 400, and converts the kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.

[0139] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.

[0140] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.

[0141] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.

[0142] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.

[0143] The vehicle according to the fifth embodiment is equipped with the battery pack according to the fourth embodiment, and therefore the vehicle according to the fifth embodiment is excellent in driving distance and driving performance. EXAMPLES

[0144] Example 1 First, the carbon fiber, the first binder, and pure water were mixed and stirred using a planetary mixer. As the carbon fiber, a carbon nanotube was used, the diameter of the cross section perpendicular to the length direction, that is, the average thickness S1 in terms of thickness, being 0.1 μm, and the average length L1, being 20 μm. Hereinafter, this carbon fiber is referred to as the first carbon fiber. An active material and granular carbon were added to a mixture of the carbon fiber, the first binder, and pure water, and stirred using a planetary mixer and a bead mill. During stirring, the stirring speed of the planetary mixer was set to 40 rpm, and the stirring time was set to 60 minutes. The flow rate of the bead mill was set to 30 mL / min, and the rotation speed was set to 2000 rpm. As the active material, particles of niobium titanium composite oxide (Nb2TiO7) with an average particle size of 1 μm were used. Hereinafter, this active material is referred to as NTO. As the granular carbon, acetylene black with an average particle size of 0.2 μm was used. Hereinafter, this granular carbon is referred to as AB. Then, the second binder was added and stirred using a planetary mixer to prepare a dispersion slurry. During stirring, the stirring speed was set to 50 rpm and the stirring time was set to 30 minutes. Styrene butadiene rubber was used as the second binder. Hereinafter, this binder is referred to as SBR.

[0145] In the dispersion slurry, the amounts of carbon fiber, granular carbon, first binder, and second binder per 100 parts by mass of active material were 2 parts by mass, 2 parts by mass, 1 part by mass, and 1 part by mass, respectively.

[0146] Next, the dispersion slurry was applied to one or both sides of a current collector, and the coating was dried to obtain a laminate of the active material-containing layer and the current collector.

[0147] An aluminum alloy foil having a thickness of 12 μm was used as the current collector. This laminate was pressed to obtain an electrode. During the pressing process, a roll press was used to adjust the pressure so as to obtain a desired film density. In this example, the density of the active material-containing layer was 2.6 g / cm 3 It was pressed so that it became.

[0148] Example 2 Except for changing the pressing conditions, an electrode was produced in the same manner as in Example 1. The density of the active material-containing layer was 2.7 g / cm 3 It was pressed so that it became.

[0149] Example 3 Except for changing the pressing conditions, an electrode was produced in the same manner as in Example 1. The density of the active material-containing layer was 2.55 g / cm 3 It was pressed so that it became.

[0150] Example 4 An electrode was produced in the same manner as in Example 1, except that the rotation speed of the bead mill and the pressing conditions were changed. The rotation speed of the bead mill was 700 rpm. The density of the active material-containing layer was 2.75 g / cm. 3 It was pressed so that it became.

[0151] Example 5 An electrode was produced in the same manner as in Example 1, except that the rotation speed of the bead mill and the pressing conditions were changed. The rotation speed of the bead mill was 1200 rpm. The density of the active material-containing layer was 2.55 g / cm. 3 It was pressed so that it became.

[0152] Example 6 Except for changing the amount of granular carbon AB and the rotation speed of the bead mill, an electrode was produced in the same manner as in Example 1. The rotation speed of the bead mill was set to 700 rpm. In the dispersion slurry, the amounts of carbon fiber, granular carbon, first binder, and second binder per 100 parts by mass of active material were 2 parts by mass, 4 parts by mass, 1 part by mass, and 1 part by mass, respectively.

[0153] Example 7 An electrode was produced in the same manner as in Example 1, except that the blending amount of granular carbon AB, the rotation speed of the bead mill, and the pressing conditions were changed. The rotation speed of the bead mill was 1200 rpm. The density of the active material-containing layer was 2.75 g / cm. 3 In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 2 parts by mass, 4 parts by mass, 1 part by mass, and 1 part by mass, respectively.

[0154] Example 8 An electrode was produced in the same manner as in Example 1, except that the type of carbon fiber and the pressing conditions were changed. Carbon nanotubes were used as the carbon fibers, and the diameter of the cross section perpendicular to the length direction, i.e., the average thickness S1 was 0.005 μm and the average length L1 was 50 μm. Hereinafter, these carbon fibers are referred to as second carbon fibers. The density of the active material-containing layer was 2.75 g / cm. 3 It was pressed so that it became.

[0155] Example 9 An electrode was produced in the same manner as in Example 8, except that the pressing conditions were changed. The density of the active material-containing layer was 2.8 g / cm 3 It was pressed so that it became.

[0156] Example 10 An electrode was produced in the same manner as in Example 8, except that the rotation speed of the bead mill and the pressing conditions were changed. The rotation speed of the bead mill was 1200 rpm. The density of the active material-containing layer was 2.7 g / cm. 3 It was pressed so that it became.

[0157] Example 11 An electrode was produced in the same manner as in Example 8, except that the blending amount of granular carbon AB was changed and the pressing conditions were changed. The density of the active material-containing layer was 2.6 g / cm 3In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 2 parts by mass, 1 part by mass, 1 part by mass, and 1 part by mass, respectively.

[0158] Example 12 An electrode was produced in the same manner as in Example 1, except that the type of active material was changed, the amount of granular carbon AB was changed, the rotation speed of the bead mill was changed, and the pressing conditions were changed. The active material was a sodium-containing niobium titanium composite compound (Li2Na 1.5 Ti 5.5 Nb 0.5 O 14 The active material was hereinafter referred to as LNT. The rotation speed of the bead mill was 700 rpm. The density of the active material-containing layer was 2.5 g / cm 3 In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 2 parts by mass, 1 part by mass, 1 part by mass, and 1 part by mass, respectively.

[0159] (Example 13) An electrode was produced in the same manner as in Example 1, except that the type of active material, the type of carbon fiber, the rotation speed of the bead mill, and the pressing conditions were changed. LNT was used as the active material. Second carbon fiber was used as the carbon fiber. The rotation speed of the bead mill was 1200 rpm. The density of the active material-containing layer was 2.7 g / cm 3 It was pressed so that it became.

[0160] Example 14 An electrode was produced in the same manner as in Example 1, except that the type of active material was changed, the amount of granular carbon AB was changed, the rotation speed of the bead mill was changed, and the pressing conditions were changed. The active material was a titanium composite oxide (Li4Ti5O 12The active material was hereinafter referred to as LTO. The rotation speed of the bead mill was 700 rpm. The density of the active material-containing layer was 2.3 g / cm 3 In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 2 parts by mass, 4 parts by mass, 1 part by mass, and 1 part by mass, respectively.

[0161] Comparative Example 1 An electrode was produced in the same manner as in Example 1, except that the blending amount of granular carbon AB was changed and the pressing conditions were changed. The density of the active material-containing layer was 2.9 g / cm 3 In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 2 parts by mass, 4 parts by mass, 1 part by mass, and 1 part by mass, respectively.

[0162] Comparative Example 2 An electrode was produced in the same manner as in Example 1, except that the number of carbon fibers was 0, the rotation speed of the bead mill was changed, and the pressing conditions were changed. The rotation speed of the bead mill was 2200 rpm. The density of the active material-containing layer was 2.8 g / cm. 3 In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 0 parts by mass, 2 parts by mass, 1 part by mass, and 1 part by mass, respectively.

[0163] Comparative Example 3 An electrode was produced in the same manner as in Example 1, except that the type of carbon fiber, the amount of granular carbon AB, the rotation speed of the bead mill, and the pressing conditions were changed. The second carbon fiber was used as the carbon fiber. The rotation speed of the bead mill was 2200 rpm. The density of the active material-containing layer was 2.8 g / cm. 3In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 2 parts by mass, 4 parts by mass, 1 part by mass, and 1 part by mass, respectively.

[0164] Comparative Example 4 An electrode was produced in the same manner as in Example 1, except that the type of active material and the pressing conditions were changed. LNT was used as the active material. The density of the active material-containing layer was 2.7 g / cm 3 It was pressed so that it became.

[0165] Comparative Example 5 An electrode was produced in the same manner as in Example 1, except that the type of active material was changed, the type of carbon fiber was changed, the blending amount of granular carbon AB was changed, and the pressing conditions were changed. LTO was used as the active material. Second carbon fiber was used as the carbon fiber. The density of the active material-containing layer was 2.8 g / cm 3 In the dispersion slurry, the amounts of the carbon fiber, the granular carbon, the first binder, and the second binder relative to 100 parts by mass of the active material were 2 parts by mass, 1 part by mass, 1 part by mass, and 1 part by mass, respectively.

[0166] (Measurement of logarithmic differential pore volume distribution curve) The logarithmic differential pore volume distribution curves of the electrodes prepared in Examples 1 to 14 and Comparative Examples 1 to 5 were measured by the method described above.

[0167] (Cycle performance evaluation) The cycle performance was evaluated using a three-electrode glass cell. The battery was charged at a current density of 1C in an environment of 70°C until the SOC reached 100%. Then, the battery was discharged at a current density of 1C until the SOC reached 0%, and the discharge capacity was measured. This charge / discharge cycle was counted as one cycle, and the battery was repeatedly charged / discharged until the discharge capacity retention rate relative to the first discharge capacity reached 80%. The results are shown in Table 3.

[0168] The manufacturing methods of the electrodes according to Examples 1 to 14 and Comparative Examples 1 to 5 are summarized in Tables 1 and 2 below.

[0169] [Table 1]

[0170] In Table 1, in the column below the heading "Active Material", the column labeled "Composition" lists the composition of the active material. In addition, in the column below the heading "Carbon Fiber", the columns labeled "Type", "Thickness S1", "Length L1", "L1 / S1", and "Amount (parts by mass)" list the type of carbon fiber, the average thickness S, the average length L, the ratio of the average length L to the average thickness S, and the amount of the active material per 100 parts by mass. In addition, in the column below the heading "Granular Carbon", the columns labeled "Type" and "Amount" list the type of granular carbon and the amount of the granular carbon per 100 parts by mass.

[0171] [Table 2]

[0172] In Table 2, the column labeled "Rotational Speed" lists the rotational speed of the bead mill when the carbon fiber, the first binder, the pure water, the active material, and the granular carbon were stirred, and the column labeled "Density" lists the density of the active material-containing layer when the laminate of the active material-containing layer and the current collector was pressed using a roll press machine.

[0173] The electrodes according to Examples 1 to 14 and Comparative Examples 1 to 5 and the performance of secondary batteries using these electrodes are summarized in the following Table 3 and FIG.

[0174] [Table 3]

[0175] In Table 3, in the column under the heading "Electrode", the columns labeled "Pore Surface Area TA", "Peak Pore Diameter PD", "Median Diameter MD", "MD-PD", and "Full Width at Half Maximum" respectively list the total pore surface area TA, peak pore diameter PD, median diameter MD, the value MD-PD obtained by subtracting the peak pore diameter PD from the median diameter MD, and the full width at half maximum of the peak. In addition, in the column under the heading "Battery", the column labeled "Cycle Number Ratio" lists the ratio of the cycle number of the secondary battery of each Example or Comparative Example to the cycle number of Example 1. Here, the cycle number is the cycle number when the discharge capacity retention rate becomes 80% relative to the discharge capacity of the first cycle under the condition of 70°C.

[0176] 12 is a graph showing the relationship between the peak pore diameter PD and the total pore volume TA. The plots for Examples 1 to 15 are shown as black circles, and the plots for Comparative Examples 1 to 5 are shown as white circles. Also shown in the figure are dotted lines corresponding to PD=0.1, TA=-17×PD+10.6 (in formula (1), a=-17, b=10.6), TA=-17×PD+8 (in formula (1), a=-17, b=8), and TA=-17×PD+7 (in formula (1), a=-17, b=7).

[0177] As is clear from the comparison of Examples 1 to 14 and Comparative Examples 1 to 5, electrodes with plots in the range of peak pore diameter PD greater than 0.1 μm and less than 0.3 μm have superior high-temperature cycle performance compared to electrodes outside this range. Furthermore, many of the electrodes with plots in the range surrounded by TA = -17 × PD + 10.6, TA = -17 × PD + 7, PD = 0.1, and PD = 0.3 (light hatched area and dark hatched area in FIG. 12) have higher high-temperature cycle performance compared to electrodes outside this range. Furthermore, many of the electrodes with plots in the range surrounded by TA = -17 × PD + 10.6, TA = -17 × PD + 8, PD = 0.1, and PD = 0.3 (dark hatched area in FIG. 12) have higher high-temperature cycle performance compared to electrodes outside this range.

[0178] The electrode according to at least one embodiment described above includes an active material-containing layer containing an active material and carbon fibers, and in a logarithmic differential pore volume distribution curve of the active material-containing layer measured by mercury intrusion porosimetry, the pore diameter PD of the peak showing the maximum logarithmic differential pore volume is greater than 0.1 μm and not more than 0.3 μm, and the full width at half maximum of the peak is not more than 0.06 μm. By using this electrode, a secondary battery with excellent high-temperature cycle performance can be realized.

[0179] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0180] Reference Signs List 1: electrode group, 2: exterior member, 3: negative electrode, 3a: negative electrode current collector, 3b: negative electrode active material-containing layer, 3c: negative electrode current collector tab, 4: separator, 5: positive electrode, 5a: positive electrode current collector, 5b: positive electrode active material, 6: negative electrode terminal, 7: positive electrode terminal, 21: bus bar, 22: positive electrode side lead, 22a: other end, 23: negative electrode side lead, 23a: other end, 24: adhesive tape, 31: storage container, 3 2... cover, 33... protective sheet, 34... printed wiring board, 35... wiring, 40... vehicle body, 41... vehicle power source, 42... electrical control device, 43... external terminal, 44... inverter, 45... drive motor, 50... active material particles, 51... carbon fiber, 52... granular carbon, 100... secondary battery, 200... battery pack, 200a... battery pack, 200b... battery pack, 200c... battery pack, 3 00...battery pack, 300a...battery pack, 300b...battery pack, 300c...battery pack, 301a...assembled battery monitoring device, 301b...assembled battery monitoring device, 301c...assembled battery monitoring device, 342...positive connector, 343...negative connector, 345...thermistor, 344...protection circuit, 342a...wiring, 343a...wiring, 350...external terminal for energizing, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.

Claims

1. The active material includes a titanium-containing composite oxide and an active material-containing layer includes carbon fibers, the active material-containing layer exhibits a peak indicating a maximum logarithmic differential pore volume in a logarithmic differential pore volume distribution curve measured by mercury intrusion porosimetry; The peak pore diameter PD of the electrode is greater than 0.1 μm and not greater than 0.3 μm.

2. 2. The electrode according to claim 1, wherein a relationship between a total pore surface area TA of the active material-containing layer measured by mercury porosimetry and the peak pore diameter PD is expressed by the following formula (1): TA=a×PD+b (1) Here, in the formula, a=-17, and b is 7≦b≦10.

6.

3. The total pore surface area TA of the active material-containing layer measured by the mercury intrusion method is 4 m 2 3. The electrode of claim 2, wherein the .lambda. / g or greater.

4. 4. The electrode according to claim 1, wherein a total pore volume TV of the active material-containing layer measured by mercury intrusion porosimetry is 0.15 mL / g or less.

5. 4. The electrode according to claim 1, wherein a value MD-PD obtained by subtracting the peak pore diameter PD from the median diameter MD of the active material-containing layer measured by mercury porosimetry is in the range of -0.02 μm to 0.02 μm.

6. The titanium-containing composite oxide is x T.I.M. y Nb 2-y O 7±z (0≦x≦5, 0≦y≦0.5, −0.3≦z≦0.3, M is at least one metal element other than Ti and Nb, and A is at least one of Li and Na), Li 2+a Na 2 Ti 6 O 14 (0≦a≦6), and Li x TiO 2 4. The electrode according to claim 1, comprising at least one compound represented by a general formula selected from the group consisting of (0≦x≦1).

7. 4. The electrode according to claim 1, wherein the diameter of a cross section perpendicular to the longitudinal direction of the carbon fiber is 1 nm or more and 200 nm or less.

8. 4. The electrode according to claim 1, wherein the carbon fibers have a length of 5 μm or more and 50 μm or less.

9. A positive electrode, a negative electrode, and an electrolyte, A secondary battery, wherein at least one of the positive electrode and the negative electrode is the electrode according to claim 1 .

10. A battery pack comprising the secondary battery according to claim 9.

11. An external terminal; A protection circuit; The battery pack of claim 10, comprising:

12. A battery comprising a plurality of the secondary batteries, The battery pack according to claim 10 or 11, wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.

13. A vehicle equipped with the battery pack according to claim 10 or 11.

14. 14. The vehicle of claim 13, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.

Citation Information

Patent Citations

  • Nonaqueous electrolyte battery

    JP2009158396A

  • Nonaqueous electrolyte battery

    JP2014063753A

  • Electrode, rechargeable battery, battery pack, and vehicle

    JP2021044216A

  • Electrode, rechargeable battery, battery pack, and vehicle