Method for manufacturing burned product

By combining calcium phosphate and phosphorus-containing waste in a controlled ratio, the method addresses dusting issues in fired products, ensuring stable α-type belite formation and cost reduction.

JP2024139141APending Publication Date: 2024-10-09TAIHEIYO CEMENT CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023049952
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

The production of fired products containing calcium silicate (belite) with a small amount of Al2O3 and Y2O3 results in dusting due to rapid volumetric expansion during phase transitions, leading to handling difficulties and equipment clogging, and the use of calcium phosphate as a phosphorus source increases manufacturing costs.

Method used

A method involving the use of calcium phosphate and phosphorus-containing waste as phosphorus sources in a specific mass ratio, controlling the phosphorus content to improve reactivity and maintain stable α-type belite, thereby suppressing dusting while reducing costs.

Benefits of technology

The method effectively suppresses dusting by maintaining stable α-type belite and reduces manufacturing costs by optimizing the phosphorus content in the fired product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139141000003
    Figure 2024139141000003
  • Figure 2024139141000004
    Figure 2024139141000004
  • Figure 2024139141000005
    Figure 2024139141000005
Patent Text Reader

Abstract

To provide a method for manufacturing a burned product with reduced dusting.SOLUTION: A method for manufacturing a burned product includes a step of burning a mixed material including soil, a calcium source, and a phosphorus source. The mixed material includes, as the phosphorus source, (A) calcium phosphate and (B) phosphorus-containing waste, and the mass ratio of (B) phosphorus-containing waste to (A) calcium phosphate [(B) / (A)] is 5 / 95 to 50 / 50 in terms of P2O5. The content of the phosphorus source in the mixed material is an amount in which the content of phosphorus in the burned product is 0.7 mass% or more in terms of P2O5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a fired product. [Background technology]

[0002] Due to a major accident at a nuclear power plant, radioactive cesium was released and deposited over a wide area in the external environment. It is believed that this radioactive cesium was released in a 1:1 ratio of cesium-134 and cesium-137, and cesium-137 in particular has a half-life of 30 years and can have adverse effects on the human body for a long period of time. Therefore, in order to reduce the impact on human health and the living environment, there is a demand to remove radioactive cesium from radioactive cesium-contaminated waste such as soil to which the deposited radioactive cesium has adhered.

[0003] Conventionally, as a method for removing radioactive cesium from radioactive cesium-contaminated soil, for example, a method has been proposed in which the radioactive cesium-contaminated soil is mixed with a calcium source having a specific particle size distribution to obtain a mixed material, and then the mixed material is fired to volatilize the radioactive cesium in the soil (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-128174 A Summary of the Invention [Problem to be solved by the invention]

[0005] The fired material produced by firing the above-mentioned mixed materials is a mineral called belite, whose main component is calcium silicate (2CaO·SiO2) with small amounts of Al2O3 and Fe2O3 dissolved therein. The crystal layer of this belite has polymorphs such as α-type, α'-type, β-type, and γ-type. This polymorph is α-type at high temperatures during firing, but is prone to undergo a phase transition from α'-type to β-type to γ-type upon cooling. In particular, when the phase transition occurs from α'-type or β-type to γ-type, it is known to cause a powdering phenomenon (hereinafter referred to as "dusting") due to the sudden volume expansion. When such dusting occurs, the handling becomes poor, and the dust is carried by the air current and flows back, causing adverse effects such as clogging the equipment, making stable operation difficult. The present inventors have conducted research to solve such problems and have found that dusting can be suppressed by adding calcium phosphate as a phosphorus source to the mixed material in an amount such that the phosphorus content in the fired product obtained after firing is at least 2 mass% when converted to P2O5 (Reference Example). However, the use of calcium phosphate reagent leads to a problem of unavoidable increase in production costs. An object of the present invention is to provide a method for producing a fired product in which dusting is suppressed, and a method for suppressing dusting of a fired product. [Means for solving the problem]

[0006] As a result of intensive research to solve the above problems, the present inventors have found that, when preparing the mixed material, by combining (A) calcium phosphate and (B) phosphorus-containing waste as phosphorus sources, and controlling the content of the phosphorus source in the mixed material using the ratio of the two amounts converted into P2O5 and the P2O5 converted value of the phosphorus content in the fired product obtained after firing as indicators, the reactivity with SiO2 in the mixed material is improved, and even if the fired product is cooled after firing, a phase transition to γ-type is unlikely to occur, and stable α-type belite is maintained, so that dusting of the fired product can be suppressed. Moreover, it has been found that even if the content of the phosphorus source is significantly reduced, dusting of the fired product can be sufficiently suppressed, and therefore costs can be significantly reduced.

[0007] That is, the present invention provides the following [1] to [5]. [1] A method for producing a fired product, comprising the step of firing a mixed material containing soil, a calcium source, and a phosphorus source, The mixed material contains, as phosphorus sources, (A) calcium phosphate and (B) phosphorus-containing waste, and the mass ratio of (A) calcium phosphate to (B) phosphorus-containing waste [(B) / (A)] is 5 / 95 to 50 / 50 when converted into P2O5; The content of the phosphorus source in the mixed material is an amount such that the phosphorus content of the fired product is 0.7 mass% or more when converted into P2O5. A method for producing a fired product. [2] The method for producing a fired product according to [1] above, wherein the phosphorus source in the mixed material has an average particle diameter of 600 μm or less. [3] The method for producing a fired product according to [1] or [2] above, wherein the firing temperature is 1200 to 1550°C. [4] The method for producing a fired product according to any one of [1] to [3] above, wherein the phosphorus-containing waste comprises at least one selected from sewage sludge waste, agricultural and fishery phosphorus-containing waste, industrial phosphorus-containing waste, and food-related phosphorus-containing waste. [5] A method for suppressing dusting of a fired product, comprising a step of firing a mixed material containing soil, a calcium source, and a phosphorus source, The mixed material contains, as phosphorus sources, (A) calcium phosphate and (B) phosphorus-containing waste, and the mass ratio of (A) calcium phosphate to (B) phosphorus-containing waste [(B) / (A)] is 5 / 95 to 50 / 50 when converted into P2O5; The content of the phosphorus source in the mixed material is an amount such that the phosphorus content of the fired product is 0.7 mass% or more when converted into P2O5. A method for suppressing dusting of baked goods. Effect of the Invention

[0008] According to the present invention, the phase transition to γ-type belite is unlikely to occur and stable α-type belite is maintained, so that a fired product with suppressed dusting can be produced. Moreover, even if the content of the phosphorus source is significantly reduced, dusting can be sufficiently suppressed, so that a fired product can be produced at low cost. [Brief description of the drawings]

[0009] [Figure 1] 1 is a photograph showing the appearance of a molded product (mixed material) used in Example 3 before firing. [Diagram 2] 1 is a photograph showing the appearance of the fired product obtained in Example 3. [Diagram 3] 1 is a photograph showing the appearance of the fired product obtained in Comparative Example 1. [Figure 4] 1 is a photograph showing the appearance of the fired product obtained in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The method for producing a fired product of the present invention includes a step of firing a mixed material containing soil, a calcium source, and a phosphorus source, and is characterized in that (A) calcium phosphate and (B) phosphorus-containing waste are combined as the phosphorus source in the mixed material, and the content of the phosphorus source in the mixed material is controlled using the ratio of the two amounts converted into P2O5 and the P2O5 converted value of the phosphorus content in the fired product obtained after firing as indicators. By controlling in this way, the reactivity with SiO2 in the mixed material is improved, substitution solid solution is promoted, and stable α-type belite is generated, thereby suppressing dusting. In addition, since α-type belite does not undergo a phase transition to γ-type, dusting due to sudden volume expansion is suppressed.

[0011] (soil) The soil is not particularly limited, but examples include construction waste soil and contaminated soil. Examples of construction waste soil include soil and waste soil generated by excavation at construction sites and dredging in civil engineering works, and soil generated by cutting in mountains and hills. Contaminated soil can be, for example, soil contaminated with heavy metals (arsenic, chromium, etc.), organic matter (organochlorine compounds, volatile organic compounds, etc.), or radioactive materials (cesium, iodine, etc.). Other examples include soil excavated from former factory sites related to the chemical industry or metallurgy. Note that soil contaminated with radioactive cesium may also contain disaster waste such as rubble. Here, in this specification, "radioactive cesium" refers to cesium-134 and cesium-137, which are radioactive isotopes of cesium. The soil may be used alone or in combination of two or more kinds.

[0012] (Calcium source) Examples of calcium sources include quicklime (CaO), slaked lime (Ca(OH)2), and calcium carbonate (CaCO3). In this specification, the term "calcium carbonate" includes industrially produced calcium carbonate and natural limestone. The calcium sources may be used alone or in combination of two or more. Among these, from the viewpoint of further suppressing dusting, it is preferable to contain quicklime (CaO).

[0013] (Phosphorus source) The phosphorus source includes calcium phosphate and phosphorus-containing waste materials. The calcium phosphate may be any of monocalcium phosphate (Ca(H2PO4)2), dicalcium phosphate (CaHPO4) and dicalcium phosphate (Ca3(PO4)2), as long as it is a compound formed by chemically combining phosphoric acid (H3PO4) and calcium (Ca), or may be a mixture of two or more of these three types. The calcium phosphate may also be in the form of a hydrate. The phosphorus-containing waste is not particularly limited as long as it is a waste that contains phosphorus, and examples thereof include sewage sludge waste, agricultural and fishery phosphorus-containing waste, industrial phosphorus-containing waste, and food-related phosphorus-containing waste. The phosphorus-containing waste may be incinerated waste. Examples of sewage sludge waste include general sewage sludge and industrial sewage sludge. Examples of agricultural and fishery phosphorus-containing waste include meat and bone meal from livestock and fish, wheat straw, and livestock excrement. Examples of industrial phosphorus-containing waste include sludge discharged from a zinc phosphate conversion treatment process, and cleaning fluids from the processing and degreasing processes of electronic components and printed circuit boards. Examples of food-based phosphorus-containing waste include soybean pulp, soy sauce residue, and leftover food. The phosphorus-containing waste may be used alone or in combination of two or more kinds.

[0014] The phosphorus source is preferably fine from the viewpoint of improving reactivity with SiO2 in the mixed material and promoting substitution solid solution. More specifically, the average particle diameter of the phosphorus source is preferably 600 μm or less, more preferably 300 μm or less, and even more preferably 100 μm or less. The lower limit of the average particle diameter of the phosphorus source is not particularly limited, but from the viewpoint of production efficiency, it is preferably 5 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. Here, in this specification, the "average particle diameter" refers to the particle diameter at 50% of the cumulative volume distribution (median diameter; d 50 The volume cumulative distribution is the distribution obtained by accumulating all particles in order from the smallest to the largest volume, and the particle diameter at 50% of the volume cumulative distribution (median diameter; d 50 ) refers to the particle diameter for the 50% cumulative volume distribution value.

[0015] To adjust the particle size of the phosphorus source, the phosphorus source may be ground. The phosphorus source can be pulverized using a pulverizer. The pulverizer is not particularly limited as long as it is an industrial device, and examples of the pulverizer include a roll mill, an edge runner mill, a centrifugal roller mill, and a disk mill. The phosphorus source may be pulverized by pulverizing calcium phosphate and the phosphorus-containing waste material separately, or by mixing the two and then pulverizing them.

[0016] Before grinding the phosphorus source, the moisture content of each of the calcium phosphate and the phosphorus-containing waste material may be adjusted. The moisture content can be adjusted by, for example, drying on the ground or drying by heating. Of these, it is preferable to extract exhaust gas discharged from the cement manufacturing process and dry by heating. The temperature for drying by heating is preferably 20 to 300°C, and more preferably 75 to 110°C. From the viewpoint of production efficiency, the moisture content of the phosphorus source after moisture adjustment is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less. The lower limit of the moisture content is not particularly limited, and may be 0% by mass. Here, in this specification, the "moisture content" refers to the value calculated from the mass loss when 1 kg of a sample is dried at 105°C until it reaches a constant weight.

[0017] The mass ratio [(B) / (A)] of (A) calcium phosphate in the phosphorus source to (B) phosphorus-containing waste is 5 / 95 to 50 / 50 when converted into P2O5, but from the viewpoint of improving the reactivity with SiO2 in the mixed material and promoting substitution solid solution, it is preferably 6 / 94 to 40 / 60, more preferably 7 / 93 to 30 / 70, even more preferably 8 / 92 to 25 / 75, and even more preferably 13 / 87 to 25 / 75. Among them, when the mass ratio [(B) / (A)] is preferably within the range of 8 / 92 to 25 / 75, and even more preferably 13 / 87 to 25 / 75, the content of the phosphorus source in the mixed material can be sufficiently exhibited even if the phosphorus content of the fired material obtained after firing is significantly reduced to about 1 mass% in terms of P2O5. In addition, when calcium phosphate is in the form of a hydrate, it is calculated based on the mass of calcium phosphate excluding hydration water.

[0018] (mixed material) The mixed material can be prepared by mixing soil, a material containing a calcium source, and a phosphorus source. The method for mixing the materials is not particularly limited, but examples include a method of mixing the materials using a blender, etc. In addition, when firing using a rotary kiln described later, the materials are mixed by rotation in the rotary kiln, so that all or a part of the materials may be directly charged into the bottom of the rotary kiln. Furthermore, the order in which the materials are mixed is not particularly limited, and the soil, calcium source, phosphorus source and other materials may be mixed simultaneously, or the materials may be mixed in any order.

[0019] The mixing ratio of the soil and the calcium source can be determined using the SiO2 in the mixed material as an index. For example, when the calcium source contains CaO, the soil and the calcium source may be mixed so that the mass ratio of SiO2 to CaO in the mixed material (CaO / SiO2) is preferably 1.0 to 3.7, more preferably 1.2 to 3.5, even more preferably 1.4 to 3.3, even more preferably 1.6 to 2.7, and even more preferably 1.8 to 2.55. By setting the mass ratio (CaO / SiO2) in this manner, the reactivity with SiO2 in the mixed material is improved and replacement solid solution is promoted, making it easier to form stable α-type belite.

[0020] In addition, from the viewpoint of improving the reactivity with SiO2 in the mixed material and promoting the substitution solid solution, the mass ratio [SiO2 / (Al2O3+Fe2O3)] of SiO2 to the total amount of Al2O3 and Fe2O3 in the mixed material may be controlled. Such a mass ratio [SiO2 / (Al2O3+Fe2O3)] is preferably 2.0 or more, more preferably 2.2 or more, and even more preferably 2.4 or more. The upper limit of the mass ratio [SiO2 / (Al2O3+Fe2O3)] is usually 5.0 or less, and preferably 4.5 or less.

[0021] The content of the phosphorus source in the mixed material is usually 0.7% by mass or more when the phosphorus content in the fired product is converted into P2O5, but from the viewpoint of improving the reactivity with SiO2 in the mixed material and promoting substitution solid solution, it is preferably 0.9% by mass or more, more preferably 1.2% by mass or more, and even more preferably 1.7% by mass or more. Note that, from the viewpoint of reducing costs, the upper limit of the content of the phosphorus source in the mixed material is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less when the phosphorus content in the fired product is converted into P2O5.

[0022] When using soil contaminated with radioactive cesium as the soil, a chlorine source may be contained from the viewpoint of promoting the volatilization of radioactive cesium and reducing the amount of radioactive waste generated during the removal of radioactive cesium. The chlorine source is not particularly limited as long as it is a compound containing chlorine, and examples thereof include calcium chloride (CaCl2), sodium chloride (NaCl), and potassium chloride (KCl). Among these, calcium chloride is preferred. The chlorine source is used in an amount such that the molar ratio of chlorine to potassium (Cl / K) in the mixed material is preferably 1.4 or less, more preferably 0.01 to 1.3, and even more preferably 0.1 to 1.2. When the molar ratio (Cl / K) is 1.4 or less, potassium and sodium do not volatilize, and more radioactive cesium volatilizes, so that the amount of radioactive waste generated during the removal of radioactive cesium can be reduced.

[0023] (Firing) The mixed material may be fired either continuously or batchwise. When the firing is performed continuously, a rotary kiln, for example, can be used as the firing device. When the firing is performed batchwise, examples of the firing device include an incinerator, an electric furnace, and a microwave heating device. Among them, it is preferable to perform the firing in a continuous manner using a rotary kiln. By using a rotary kiln, the materials roll to increase the contact rate and improve the thermal conductivity, which improves the reactivity with SiO2 in the mixed material, promotes substitution solid solution, and makes it easier to form stable α-type belite.

[0024] The firing temperature of the mixed material is preferably 1200 to 1550° C., more preferably 1240 to 1450° C., further preferably 1260 to 1350° C., and even more preferably 1280 to 1340° C. By firing at such a temperature, the reactivity with SiO2 in the mixed material is improved and substitution solid solution is promoted, so that stable α-type belite is easily formed.

[0025] The firing time is preferably 15 minutes or more, more preferably 30 minutes or more, from the viewpoint of improving the reactivity with SiO2 in the mixed material and promoting substitution solid solution. The upper limit of the firing time is not particularly limited, but is preferably 180 minutes or less, more preferably 120 minutes or less.

[0026] (cooling) After firing, the fired product is cooled. For example, by cooling the fired product to a temperature of 1000° C. or less within 20 to 40 minutes after firing, stable α-type belite can be easily formed.

[0027] The exhaust gas generated during firing contains volatilized alkali metals and materials scattered during heating (mainly calcium and silica components), so it is usually cooled and solidified, and then collected using a dust collector or scrubber, etc. The collected material may be classified into coarse and fine powders as necessary. In addition, when soil contaminated with radioactive cesium is used as the soil, the radioactive cesium recovered from the exhaust gas is further reduced in volume by washing with water, adsorption, etc. as necessary, and then sealed and stored in a concrete container, etc. This makes it possible to reduce the volume of radioactive waste and store it without it leaking to the outside.

[0028] The fired product can be pulverized as necessary and used as a cement mixture, aggregate (aggregate for concrete, aggregate for asphalt), civil engineering material (backfill material, banking material, roadbed material, etc.), etc. EXAMPLES

[0029] The embodiments of the present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0030] (Materials used) (1) The materials used are as follows: (i) Soil: Decomposed granite soil was used. (ii) Calcium source: Quicklime was used. (iii) Phosphorus source: (A) A monocalcium phosphate reagent was used as calcium phosphate. (B) Sewage sludge incineration ash generated at the Asahikawa Purification Center was used as phosphorus-containing waste. The particle diameter (d 50 ) were all less than 600 μm. (iv) Chlorine source: Calcium chloride reagent was used. (2) Analysis of each material (i) Loss on ignition In accordance with JIS R 5202, the value was used after firing in an electric furnace at 950°C ± 25°C for 1 hour. (ii) Chemical composition The chemical composition of the soil and phosphorus source was analyzed by semi-quantitative analysis using FP method with briquettes made from them and a fluorescent X-ray analyzer (Rigaku ZSX Primus II). Regarding the calcium source, a quantitative analysis was performed using an X-ray fluorescence analyzer and a calibration curve method with a standard sample of quicklime. The salinity of the chlorine source was measured by spectrophotometry. (3)Analysis results The analysis results are shown in Table 1.

[0031] [Table 1]

[0032] Examples 1 to 3 The soil, quicklime and calcium chloride in the following proportions were mixed and stirred in a bag. The mass ratio of SiO2 to CaO in the mixed material (CaO / SiO2) is 2.0 The molar ratio of chlorine to potassium in the mixture (Cl / k) is 1.1 The mass ratio of SiO2 to the total of Al2O3 and Fe2O3 in the mixed material [SiO2 / (Al2O3+Fe2O3)] is 2.42 Next, a phosphorus source was added to this mixture so that the phosphorus content of the fired material was 2.0 mass%, 1.5 mass%, or 1.0 mass% when converted to P2O5, and the mixture was stirred and mixed in a bag to prepare a mixed material. The phosphorus source was contained in such a ratio that the mass ratio of (A) calcium phosphate to (B) phosphorus-containing waste [(B) / (A)] was 10 / 90 when converted to P2O5. Table 2 shows the mixing ratio of each material. Next, the mixed material was finely pulverized using a disk mill. The finely pulverized material was molded into a pellet molder (manufactured by Iwata Kogyo Co., Ltd.) into a size of 30 mm in diameter and 18 mm in height, and then the molded material was placed in a platinum crucible and fired at 1300°C for 1 hour in a box-type electric furnace. After firing, the material was cooled to 1000°C in the electric furnace over a period of 25 to 35 minutes, and then the fired material was taken out and its appearance was observed. In this experiment, all experiments were performed with n=2, and the reproducibility of the appearance was confirmed. A photograph of the appearance of the molded material (mixed material) before firing is shown in FIG. 1, and a photograph of the appearance of the fired material obtained in Example 3 is shown in FIG. 2. Note that FIG. 2 is a photograph of the appearance of the fired material in which no dusting occurred.

[0033] Comparative Example 1 A phosphorus source was added to the mixture so that the phosphorus content of the fired product was 0.5 mass% in terms of P2O5, and the mixture was stirred and mixed in a bag to prepare a mixed material, and a fired product was obtained by the same operation as in Example 1. Then, the appearance of the fired product was observed in the same manner as in Example 1. Note that in this experiment, all experiments were performed with n=2, and the reproducibility of the appearance was confirmed. A photograph of the appearance of the fired product obtained in Comparative Example 1 is shown in FIG. 3. Note that FIG. 3 is a photograph of the appearance of the fired product in which dusting occurred in a part.

[0034] Reference example 1 A sintered product was obtained by the same procedure as in Example 1, except that only calcium phosphate (A) was used as the phosphorus source (mass ratio [(B) / (A)]=0), which was added to the mixture so that the phosphorus content of the sintered product was 2.0 mass% in terms of P2O5, and the mixture was prepared by stirring and mixing in a bag. Then, the appearance of the sintered product was observed in the same manner as in Example 1. Note that in this experiment, all experiments were performed with n=2, and the reproducibility of the appearance was confirmed.

[0035] Comparative Examples 2 to 4 A sintered product was obtained by the same operation as in Example 1, except that only calcium phosphate (A) was used as the phosphorus source (mass ratio [(B) / (A)]=0), and it was added to the mixture so that the phosphorus content of the sintered product in terms of P2O5 was 1.5 mass%, 1.0 mass%, or 0.5 mass%, and the mixture was prepared by stirring and mixing in a bag. Then, the appearance of the sintered product was observed in the same manner as in Example 1. Note that all experiments were performed with n=2, and the reproducibility of the appearance was confirmed. A photograph of the appearance of the sintered product obtained in Comparative Example 2 is shown in FIG. 4. Note that FIG. 4 is a photograph of the appearance of the sintered product in which dusting occurred.

[0036] Examples 4 to 6 A phosphorus source containing (A) calcium phosphate and (B) phosphorus-containing waste in a mass ratio [(B) / (A)] of 20 / 80 in terms of P2O5 was used, and the mixture was added so that the phosphorus content of the fired material was 2.0 mass%, 1.5 mass%, or 1.0 mass% in terms of P2O5, and the mixture was stirred and mixed in a bag to prepare a mixed material. Except for this, a fired material was obtained by the same operation as in Example 1. Then, the appearance of the fired material was observed in the same manner as in Example 1. Note that all experiments were performed with n=2, and the reproducibility of the appearance was confirmed.

[0037] Table 2 shows the blending ratios of the mixed materials used in Examples 1 to 6, Comparative Examples 1 to 4, and Reference Example 1, and the results of the appearance observation.

[0038] [Table 2]

[0039] From Table 2, it can be seen that dusting of the fired product can be suppressed by combining (A) calcium phosphate and (B) phosphorus-containing waste as a phosphorus source, and controlling the content of the phosphorus source in the mixed material using as indicators the quantitative ratio of the two when converted into P2O5, and the P2O5 converted value of the phosphorus content in the fired product obtained after firing.

Claims

1. A method for producing a fired product, comprising a step of firing a mixed material containing soil, a calcium source, and a phosphorus source, The mixed material contains calcium phosphate (A) and phosphorus-containing waste (B) as phosphorus sources, and the mass ratio of calcium phosphate (A) to phosphorus-containing waste (B) [(B) / (A)] is P 2 O 5 When converted, it is 5 / 95 to 50 / 50. The content of the phosphorus source in the mixed material is P 2 O 5 When converted, the amount is 0.7% by mass or more. A method for producing a fired product.

2. The method for producing a fired product according to claim 1 , wherein the phosphorus source in the mixed material has an average particle size of 600 μm or less.

3. The method for producing a fired product according to claim 1, wherein the firing temperature is 1200 to 1550°C.

4. The method for producing a fired product according to any one of claims 1 to 3, wherein the phosphorus-containing waste comprises at least one selected from sewage sludge waste, agricultural and fishery phosphorus-containing waste, industrial phosphorus-containing waste, and food-related phosphorus-containing waste.

5. A method for suppressing dusting of a fired product, the method comprising the steps of firing a mixed material containing soil, a calcium source, and a phosphorus source, The mixed material contains calcium phosphate (A) and phosphorus-containing waste (B) as phosphorus sources, and the mass ratio of calcium phosphate (A) to phosphorus-containing waste (B) [(B) / (A)] is P 2 O 5 When converted, it is 5 / 95 to 50 / 50. The content of the phosphorus source in the mixed material is P 2 O 5 When converted, the amount is 0.7% by mass or more. A method for suppressing dusting of baked goods.

Citation Information

Patent Citations

  • Radioactive cesium removal method

    JP2019128174A