Manufacturing method of active material dispersion liquid

By using a sensor to adjust the supply speed and power of the dispersion machine based on measured quality values, the method addresses the challenges of dispersing fine particles in high-viscosity liquids, ensuring consistent quality and safety in the production of active material dispersions.

JP2024139161AInactive Publication Date: 2024-10-09MITSUBISHI PENCIL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023049979
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods face challenges in dispersing fine particles in liquids with high viscosity, leading to difficulties in achieving homogeneous dispersions, controlling quality, and risking equipment failure due to high pressure and power loads, especially when the concentration is high.

Method used

A method involving continuous dispersion using a sensor to measure quality values in the exit line of the dispersion machine, adjusting the supply speed and power of the dispersion machine based on measured trends to achieve controlled quality, particularly through particle size distribution management.

Benefits of technology

Enables the production of active material dispersions with consistent quality by controlling particle size distribution and physical properties, reducing the risk of equipment failure and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139161000001
    Figure 2024139161000001
  • Figure 2024139161000002
    Figure 2024139161000002
Patent Text Reader

Abstract

To provide a method for acquiring an active material dispersion liquid, of which the quality value is controlled, when manufacturing the active material dispersion liquid by dispersing an active material in a solvent.SOLUTION: In a manufacturing method of an active material dispersion liquid, an active material mixture containing at least an active material and a solvent is continuously supplied to a disperser and dispersed, and the obtained active material dispersion liquid is continuously discharged from the disperser. In the manufacturing method of the active material dispersion liquid, a quality value of the active material dispersion liquid discharged from the disperser is measured at predetermined time intervals using a sensor, which is installed in an outlet line of the disperser, and an increase / decrease tendency of the quality value is calculated from quality value measurements at a plurality of latest points. A supply speed of the active material dispersion liquid to the disperser and / or a motive force of the disperser is adjusted in accordance with the calculated increase / decrease tendency.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an active material dispersion containing at least an active material and a solvent. The active material dispersion produced by the present invention can be used as a slurry for electrode plates of lithium ion secondary batteries. [Background technology]

[0002] Various methods are known for producing slurries for lithium ion secondary battery plates and for producing carbon black dispersions for lithium ion secondary batteries.

[0003] For example, Patent Document 1 discloses a method for producing a positive electrode slurry for a lithium ion secondary battery, which contains a positive electrode active material for a lithium ion secondary battery, a binder, a conductive material, and an organic solvent, and includes the following step (1): mixing at least the positive electrode active material for a lithium ion secondary battery, the binder, and the organic solvent at a predetermined temperature at which the storage elastic stress of a binder solution for measuring storage elastic stress, which contains the binder and the organic solvent, satisfies a predetermined reduction range, from when at least a part of the positive electrode active material for a lithium ion secondary battery, at least a part of the binder, and at least a part of the organic solvent are initially mixed until when at least all of the positive electrode active material for a lithium ion secondary battery and all of the binder are mixed. The present invention discloses a method for producing a positive electrode slurry for a lithium ion secondary battery, comprising the steps of:

[0004] Patent Document 2 describes a method for producing a carbon black dispersion for batteries, which contains carbon black, N-methyl-2-pyrrolidone, a polyvinylidene fluoride polymer, and a dispersant, in which the carbon black content is 10 to 30 parts by mass relative to 100 parts by mass of the dispersion, the dispersant content is 1 to 6 parts by mass relative to 100 parts by mass of the carbon black, and the polyvinylidene fluoride polymer content x is 20 parts by mass or less relative to 100 parts by mass of the carbon black, and x=a / Mw (where a is 11×10 5 ≦a≦22×10 6where Mw is the weight average molecular weight of the polyvinylidene fluoride polymer), and the carbon black dispersion for batteries is dispersed using a shear type disperser so that the viscosity of the dispersion has a minimum viscosity value of 0.1 to 3 Pa s within a shear rate range of 1 / s or more and less than 100 / s. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-174535 A (claims, etc.) [Patent Document 2] JP 2017-135062 A (claims, etc.) Summary of the Invention [Problem to be solved by the invention]

[0006] In order to disperse fine particles in water, a dispersant is generally used and the mixture is stirred with a stirrer, but the mixture containing the active material is viscous and difficult to disperse. In particular, when the mixture becomes highly concentrated, it is not easy to continuously produce a homogeneous dispersion even with a high-performance stirrer.

[0007] In the process of obtaining a dispersion of fine particles, in order to achieve the desired physical properties, it is common to adjust the operating conditions of the process equipment based on the dispersion composition, experiments, experience, etc., and then measure and confirm the physical properties of the final dispersion. However, the physical properties of the final dispersion may not match those of the target, and it is therefore necessary to control the physical properties of the dispersion in parallel with the production.

[0008] In addition, if the dispersion liquid has a high viscosity, it is difficult to deliver the liquid, and production (dispersion) must be performed at a low speed, making quality control extremely difficult. If one tries to complete the dispersion in a short time, excessive pressure and power load will be applied to the entire process equipment, increasing the risk of breakdowns, which is not desirable.

[0009] If the dispersion liquid is highly viscous and highly concentrated and tends to solidify, accurate measurement using this confirmation method is difficult, so there is a need to find a method that allows measurement and confirmation without releasing the dispersion liquid from the sealed process.

[0010] An object of the present invention is to provide a method for obtaining an active material dispersion having a controlled quality value when an active material dispersion is produced by dispersing an active material in a solvent. [Means for solving the problem]

[0011] The inventors discovered that by providing a sensor for measuring quality values ​​within the process, particularly in the outlet line of the disperser, and measuring the quality value of the dispersion within the outlet line, it is possible to accurately predict the time at which the dispersion will approach the target quality from the measured quality value, and thus completed the present invention.

[0012] That is, the present invention provides a method for producing an active material dispersion, which comprises continuously supplying an active material mixture containing at least an active material and a solvent to a disperser to disperse the active material, and continuously discharging the obtained active material dispersion from the disperser, measuring the quality value of the active material dispersion discharged from the disperser at predetermined time intervals using a sensor installed on the outlet line of the disperser; Calculate the increase or decrease trend of the quality value from the quality value measurements of the most recent multiple points, The supply rate of the active material mixture to the disperser and / or the power of the disperser are adjusted according to the calculated increase / decrease tendency. The present invention relates to a method for producing an active material dispersion comprising the steps of: Effect of the Invention

[0013] When an active material dispersion is produced by dispersing an active material in a solvent using a dispersing machine, by employing the method of the present invention, an active material dispersion with controlled quality values ​​can be continuously obtained. In particular, when the particle size distribution of the active material dispersion is used as the quality value, the dispersion state of the active material dispersion can be well controlled, and the physical properties of the battery material obtained from the active material dispersion can be suitably controlled. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In the present invention, an active material mixture containing at least an active material and a solvent is continuously supplied to a disperser and dispersed to obtain an active material dispersion. The active material mixture is a mixture in which at least an active material and a solvent are simply mixed by a mixer such as a disperser or a planetary mixer. The active material mixture is continuously supplied to the disperser using a pump or the like, and is finely dispersed by the action of the disperser. Dispersion by the disperser is preferably performed in a closed system.

[0015] As the dispersing machine, a powerful device having a beating ability such as a homomixer under high speed rotation, a high pressure homogenizer, an ultra-high pressure homogenizer, an ultrasonic dispersion processor, a planetary mixer, a combimix, a kneader, a rotation-revolution mixer, a Henschel mixer, a ball mill, a bead mill, a thin film rotating type high speed agitator, a screw type mixer, a paddle mixer, a dispersing type mixer, a turbine type mixer, a propeller mixer, a blender, an ultrasonic homogenizer, a colloid mill, a pebble mill, a beater, a disk type refiner, a conical type refiner, a double disk type refiner, a grinder, etc. can be used. Such a dispersing machine is preferable because it crushes the active material in parallel with the affinity between the active material and the solvent. Two or more types of dispersing machines may be used in combination.

[0016] In the present invention, the active material dispersion obtained through dispersion by the disperser is continuously discharged from the disperser, and the discharged active material dispersion is led to a storage tank or a next process device through an outlet line. The operation of discharging the active material dispersion is preferably carried out using a pump or the like capable of controlling the dispersion flow rate. In addition, the discharge operation is preferably carried out in a state where the active material dispersion is sealed without being exposed to the outside.

[0017] During the discharge operation, the quality value of the active material dispersion discharged from the disperser is measured at predetermined time intervals using a sensor installed in the outlet line of the active material dispersion. The quality value of the active material dispersion may be continuously measured, and the measured values ​​may be collected at a predetermined time interval. The measurement interval is approximately 1 / 100 of the residence time T of the active material dispersion in the disperser. Then, the increase / decrease tendency of the quality value of the active material dispersion is calculated from the most recent measured values. The most recent 5 or more measured values ​​may be used for the calculation.

[0018] Next, the supply speed of the active material and the solvent to the disperser is adjusted according to the calculated increase / decrease tendency. In particular, the quality value after 2 to 4 times the residence time T from the measurement is adjusted to approach the target value. This controls the residence time in the disperser until the active material dispersion passes through the disperser. Alternatively, in addition to or instead of this, the power of the disperser, for example, the rotation speed of the stirring blade of the disperser, is adjusted. When the power of the disperser is increased, the rotation speed of the stirring blade increases, and the dispersion of the active material dispersion liquid is increased. This controls the dispersibility of the active material dispersion liquid by the action of the disperser.

[0019] It is preferable to continuously perform a series of operations, consisting of measuring the quality value of the active material dispersion discharged from the disperser, calculating the increase / decrease tendency from the measured quality value, and adjusting the supply rate of the active material dispersion to the disperser in accordance with the calculated increase / decrease tendency, using an automated device. Alternatively, in addition to or instead of this, it is preferable to continuously perform a series of operations consisting of measuring the quality value of the active material dispersion discharged from the disperser, calculating the increase / decrease tendency from the measured quality value, and adjusting the power of the disperser in accordance with the calculated increase / decrease tendency using an automated device.

[0020] The automatic control device includes at least the steps of measuring a quality value of the active material dispersion liquid discharged from the disperser, calculating an increase / decrease trend of the quality value from the measured quality value, and adjusting the supply speed of the active material mixture liquid to the disperser in accordance with the calculated increase / decrease trend.

[0021] Alternatively, the automatic control device may additionally or instead include at least the steps of measuring a quality value of the active material dispersion liquid discharged from the disperser, calculating an increase / decrease trend of the quality value from the measured quality value, and adjusting the power of the disperser in accordance with the calculated increase / decrease trend. This makes it possible to appropriately control the quality of the active material dispersion.

[0022] The quality value of the active material dispersion liquid includes various physical properties, and in particular, the particle size distribution of the active material dispersion liquid can be used. Hereinafter, the case where the particle size distribution is used as the quality value will be described. As the particle size distribution, the median diameter is preferably used. The median diameter of particles is the value, i.e., the median value (D50), for which half of all particles in the active material dispersion are larger than this particle size and the remaining half are smaller than this particle size.

[0023] The particle size distribution is evaluated for all solid particles dispersed in the dispersion liquid, including at least the active material and the conductive material.

[0024] The particle size distribution can be measured by a laser diffraction method. The laser diffraction method is a method for measuring the particle size distribution of particles contained in a dispersion by irradiating the dispersion with laser light and measuring the angle dependency of the intensity of the light scattered by the particles, and is a commonly known evaluation method. As a laser diffraction method measuring device, a commercially available product such as SALD-2300 (manufactured by Shimadzu Corporation) can be used.

[0025] The particle size distribution is measured at a predetermined time interval. The particle size distribution may be measured continuously, and the measured values ​​may be collected at predetermined time intervals. The interval for measuring the particle size distribution is approximately 1 / 100 of the residence time of the active material dispersion in the disperser. The increase / decrease tendency of the median diameter of the active material dispersion is then calculated from the most recent particle size distribution measurement values ​​at multiple points. The most recent 5 or more particle size distribution measurement values ​​may be used for the calculation.

[0026] Next, the supply rate of the active material mixture to the disperser and / or the power of the disperser are adjusted according to the calculated increase / decrease tendency of the median diameter, thereby controlling the residence time of the active material dispersion in the disperser until it passes through the disperser.

[0027] Specifically, if the median diameter of the active material dispersion tends to increase, the supply speed of the active material mixture is decreased and / or the power of the disperser is increased to lengthen the residence time of the active material dispersion in the disperser and / or to increase the energy of the active material dispersion, which results in an increase in the dispersing action of the disperser of the active material dispersion and a decrease in the median diameter of the active material dispersion.

[0028] Conversely, if the median diameter of the active material dispersion tends to decrease, the supply speed of the active material mixture is increased and / or the power of the disperser is reduced to shorten the residence time of the active material dispersion in the disperser and / or to reduce the energy to the active material dispersion, which results in a decrease in the dispersing action of the disperser on the active material dispersion and an increase in the median diameter of the active material dispersion. In this way, the particle size distribution of the active material dispersion can be controlled.

[0029] The dispersion liquid can be collected by providing a ball valve at the top of the piping of the outlet line, opening the valve when collecting the dispersion liquid, inserting a rod into the inside of the piping through the opening of the ball, and attaching the dispersion liquid to the rod. Alternatively, the dispersion liquid can be collected by inserting the tip of a pipette or syringe into the inside of the piping through the opening of the ball and sucking up the dispersion liquid. The collected dispersion liquid is fed into a particle size measuring device to analyze the particle size distribution.

[0030] The particle size distribution is measured at a predetermined interval. The interval for measuring the particle size distribution is approximately 1 / 100 of the residence time T of the active material dispersion in the disperser. The median diameter measurement values ​​used for calculation can be the most recent 5 or more points. Specifically, the slope a (e.g., mPa s / sec) and intercept b (the latest median diameter value) of the change in the median diameter of the dispersion are calculated from the most recent median diameter measurements, and the supply speed of the mixture is adjusted so that the predicted median diameter value Y after a specified time approaches the target median diameter value.

[0031] When the predicted value Y is greater than the target value, the pump is adjusted to further disperse the active material dispersion liquid and reduce the median diameter by decreasing the supply speed of the mixed liquid or increasing the peripheral speed of the dispersing machine. Conversely, when the predicted value Y is smaller than the target value, the pump is adjusted to suppress the dispersion of the active material dispersion liquid and increase the median diameter by increasing the supply speed of the mixed liquid or decreasing the peripheral speed of the dispersing machine. The greater the deviation between the target value and the predicted value Y, the greater the change in the supply speed of the mixed liquid.

[0032] By programming the operation of calculating the predicted median diameter Y after a certain time from the particle size distribution measurement value and feeding it back to the pump that supplies the dispersion liquid, the adjustment of the particle diameter of the dispersion liquid can be automated. The correlation coefficient used to calculate the slope of the most recent median diameter transition of the dispersion liquid can also be used as a criterion for determining the amount of change in the supply rate of the mixed liquid. This makes it possible to improve the accuracy of particle diameter control of the dispersion liquid when the measurement values ​​vary greatly due to noise, etc.

[0033] This makes it possible to control the dispersion state of the active material dispersion, and even if the mixed state of the mixed liquid supplied to the disperser fluctuates, the particle size and other physical properties of the active material dispersion can be controlled. The method of the present invention controls the residence time of the active material mixture in the disperser and / or the dispersion action of the disperser due to the mechanical force applied to the active material mixture, using the particle size distribution of the active material dispersion as an index.

[0034] As the active material, a positive electrode active material usable for the positive electrode of a lithium ion battery having the property of reversibly absorbing and eluding lithium ions, or a negative electrode active material usable for the negative electrode of a lithium ion battery can be used.

[0035] Examples of the positive electrode active material include composite oxides of lithium and transition metals such as lithium-nickel composite oxide, lithium-cobalt composite oxide, lithium-manganese composite oxide, lithium-nickel-manganese composite oxide, lithium-nickel-cobalt composite oxide, lithium-nickel-aluminum composite oxide, lithium-nickel-manganese-cobalt composite oxide, lithium-nickel-manganese-aluminum composite oxide, lithium-nickel-manganese-aluminum composite oxide, and lithium-nickel-cobalt-manganese-aluminum composite oxide; transition metal sulfides such as TiS2, FeS, and MoS2; MnO, V---2O5, and V6O 13 , transition metal oxides such as TiO2, and olivine-type lithium phosphate.

[0036] The olivine-type lithium phosphate contains, for example, at least one element selected from the group consisting of Mn, Cr, Co, Cu, Ni, V, Mo, Ti, Zn, Al, Ga, Mg, B, Nb, and Fe, as well as lithium, phosphorus, and oxygen. These compounds may have some elements partially substituted with other elements in order to improve their properties.

[0037] A preferred positive electrode active material is a lithium-nickel composite oxide, and more preferably, the lithium-nickel composite oxide is represented by the formula: LiNi X M1 Y M2 Z and a lithium-nickel composite oxide represented by the formula (I and M2): O2 (M1 and M2 each represent at least one metal element selected from the group consisting of Al, B, an alkali metal, an alkaline earth metal, and a transition metal; 0.8≦X≦1.0, 0≦Y≦0.2, and 0≦Z≦0.2). These positive electrode active materials may be used alone or in combination of two or more.

[0038] In the positive electrode dispersion liquid of the present invention, the content of the positive electrode active material is preferably 50 to 70 mass %, and more preferably 50 to 63 mass %, based on the total amount of the positive electrode dispersion liquid, from the viewpoints of ensuring battery capacity and ensuring the fluidity of the dispersion liquid.

[0039] The positive electrode dispersion liquid of the present invention contains carbon nanotubes and a positive electrode active material, and may contain a solid electrolyte such as a sulfide solid electrolyte, an oxide solid electrolyte, a dry polymer electrolyte, a gel polymer electrolyte, or a quasi-solid electrolyte, as necessary.

[0040] As the negative electrode active material, in addition to graphite, any material can be used without particular limitation, and as long as it is not conductive, for example, metal oxide-based active material particles, silicon-based active material particles, and in particular metal oxide-based negative electrode active material particles can be used.

[0041] For example, titanium oxide can be used as the metal oxide-based negative electrode active material particles. The titanium oxide is not particularly limited as long as it can absorb and release lithium, but for example, spinel-type lithium titanate, ramsdellite-type lithium titanate, titanium-containing metal composite oxide, titanium dioxide (TiO2(B)) having a monoclinic crystal structure, and anatase-type titanium dioxide can be used.

[0042] Spinel-type lithium titanate is Li4+xTi5O 12 (x varies in the range of -1≦x≦3 depending on the charge / discharge reaction). Ramsdellite-type lithium titanate includes Li2+yTi3O7 (y varies in the range of -1≦y≦3 depending on the charge / discharge reaction). TiO2(B) and anatase-type titanium dioxide include Li1+zTiO2 (z varies in the range of -1≦z≦0 depending on the charge / discharge reaction).

[0043] Examples of titanium-containing metal composite oxides include metal composite oxides containing Ti and at least one element selected from the group consisting of P, V, Sn, Cu, Ni, and Fe. Examples of metal composite oxides containing Ti and at least one element selected from the group consisting of P, V, Sn, Cu, Ni, and Fe include TiO2-P2O5, TiO2-V2O5, TiO2-P2O5-SnO2, and TiO2-P2O5-MeO (Me is at least one element selected from the group consisting of Cu, Ni, and Fe).

[0044] Such a metal composite oxide preferably has a microstructure with low crystallinity, in which a crystalline phase and an amorphous phase coexist, or in which an amorphous phase exists alone, which can further improve cycle performance.

[0045] The solvent in the dispersion of the present invention may be water, a water-soluble solvent, or a mixture thereof. As the water, tap water, distilled water, ion-exchanged water, etc. may be used.

[0046] Examples of the water-soluble solvent include ethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,5-pentanediol, 2,5-hexanediol, 3-methyl-1,3-butanediol, 2-methylpentane-2,4-diol, 3-methylpentane-1,3,5-triol, 1,2,3 At least one of alkylene glycols such as 2-hexanetriol, polyalkylene glycols such as polyethylene glycol and polypropylene glycol, glycerols such as glycerol, diglycerol and triglycerol, lower alkyl ethers of glycols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether and diethylene glycol mono-n-butyl ether, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidalidinone can be used.

[0047] Other water-soluble solvents that can be used include amides such as dimethylformamide and dimethylacetamide, and ketones such as acetone. When water and a water-soluble solvent are mixed, the content of the water-soluble solvent is preferably 0.1 to 10% by mass, and more preferably 0.5 to 5% by mass, based on the total amount of the mixed solvent, from the viewpoint of storage stability of the dispersion.

[0048] The content of the active material in the active material dispersion is preferably 30 to 60 mass %, more preferably 35 to 55 mass %, based on the total amount of the active material dispersion, in order to ensure the capacity of the battery and the fluidity of the active material dispersion.

[0049] It is preferable to add a conductive material to the active material dispersion of the present invention. Examples of the conductive material include carbon nanotubes, graphite, and cellulose nanofibers, and it is preferable to use one or more selected from the group consisting of these. It is preferable to supply the conductive material to the disperser as a mixed liquid in which the conductive material is preliminarily mixed with a fluid medium.

[0050] The conductive material is preferably added in an amount of 0.5 to 10 mass % and more preferably 0.5 to 7 mass % in terms of solid content relative to the total amount of the positive electrode dispersion liquid, and more preferably 0.5 to 10 mass % and more preferably 0.5 to 5 mass % in terms of solid content relative to the total amount of the negative electrode dispersion liquid.

[0051] The conductive material used in the present invention is preferably a carbon nanotube (CNT) having a shape substantially formed by rolling a single surface of graphite into a cylindrical shape. Either a single-walled CNT in which a single surface of graphite is rolled into one layer, or a multi-walled CNT in which a single surface of graphite is rolled into two or more layers can be used.

[0052] From the viewpoints of the viscosity, electrical conductivity, and stability of the dispersion, the average outer diameter of the carbon nanotubes is preferably 1 nm or more and 90 nm or less, more preferably 3 nm or more and 30 nm or less, and even more preferably 3 nm or more and 15 nm or less. Here, the average outer diameter of the carbon nanotubes refers to the arithmetic mean value of the outer diameters of a sufficient number n measured using an image of a transmission electron microscope at a magnification of 100,000 times or more.

[0053] Furthermore, examples of the form of carbon nanotubes include, but are not limited to, graphite whiskers, filamentous carbon, graphite fibers, ultrafine carbon tubes, carbon tubes, carbon fibrils, carbon microtubes, and carbon nanofibers, and these may be used alone or in combination of two or more types (hereinafter simply referred to as "at least one type").

[0054] The purity of the carbon nanotubes used in the present invention is preferably 90 to 100% by mass, particularly preferably 95 to 100% by mass. The purity of the carbon nanotubes is calculated based on the amount of impurities, with ash content measured according to JIS K 1469 or JIS K 6218 being taken as impurities.

[0055] Specific examples of carbon nanotubes that can be used include NC7000 (average outer diameter: 10 nm) manufactured by Nanocyl Corporation, Baytubes C150P (average outer diameter: 11 nm) manufactured by Bayer AG, FloTube 9000 (average outer diameter: 19 nm), FloTube 7320 (average outer diameter: 9 nm), FloTube 7010 (average outer diameter: 9 nm), FloTube 6810 (average outer diameter: 8 nm), FloTube 6120 (average outer diameter: 8 nm), FloTube 6100 (average outer diameter: 8 nm), FloTube 2020 (average outer diameter: 4 nm) manufactured by Cnano Corporation, and MEIJO eDIPS manufactured by Meijo Nano Carbon Co., Ltd. At least one of EC2.0 (average outer diameter 2.0 nm), KORBON-A7 (average outer diameter 1.2 nm) manufactured by KORBON Co., Ltd., NFT-7 (average outer diameter 30 nm) manufactured by Koatsu Gas Kogyo Co., Ltd., and NFT-15 (average outer diameter 30 nm) manufactured by Koatsu Gas Kogyo Co., Ltd. can be used.

[0056] The carbon nanotube content is preferably 0.1 to 15.0% by mass, more preferably 0.1 to 10.0% by mass, even more preferably 0.5 to 8.0% by mass, particularly preferably 1.0 to 6.0% by mass, and most preferably 2.0 to 5.0% by mass, based on the total amount of the dispersion. By setting the carbon nanotube content to 0.1% by mass or more based on the total amount of the dispersion, good conductivity can be ensured when the battery is made, while by setting it to 15.0% by mass or less, the stability of the dispersion can be ensured.

[0057] Carbon nanotubes and flat graphite can also be used in combination. In this case, by making the amount of flat graphite 10% by mass or more relative to the amount of carbon nanotubes, a synergistic effect with the carbon nanotubes can be obtained, and by making the amount 200% by mass or less, the stability of the dispersion can be ensured.

[0058] The dispersion of the present invention may contain graphene. Graphene is a single-atom-thick sp 2 It is a sheet-like material of bonded carbon atoms arranged in a honeycomb-like hexagonal lattice structure made up of carbon atoms and their bonds.

[0059] The dispersion of the present invention may further contain cellulose nanofibers (CeNFs). As the cellulose nanofibers, oxidized cellulose nanofibers obtained by carboxylating cellulose with TEMPO can be preferably used as a dispersant for carbon nanotubes.

[0060] The oxidized cellulose nanofibers used preferably have cellulose type I crystals. The oxidized cellulose nanofibers preferably have a crystallinity of less than 70% as measured by X-ray diffraction. The crystallinity is more preferably 25% or more and less than 70%. If the crystallinity is less than 70%, the carbon nanotubes are oxidized and defibrated to a suitable degree, resulting in good dispersibility.If the crystallinity is more than 70%, the carbon nanotubes are likely to be insufficiently defibrated or crushed, resulting in insufficient dispersibility.

[0061] The fiber length of the oxidized cellulose nanofibers blended in the dispersion is preferably such that 85% or more of the total have a fiber length of 50 nm to 250 nm, and more preferably 30% or more of the total have a fiber length of 100 nm to 150 nm. Furthermore, the oxidized cellulose nanofibers blended in the dispersion preferably have a number average fiber length L of 100 nm to 150 nm, and a ratio of the number average fiber length L to the length-weighted average fiber length Ll (Ll / L) of 1.0 to 1.4.

[0062] When the fiber length of the oxidized cellulose nanofibers is within the above range, the dispersibility of the carbon nanotubes is good. Although the mechanism behind this is unclear, it is presumed to be related to the permeability of the oxidized cellulose nanofibers into the carbon nanotubes.

[0063] Furthermore, the oxidized cellulose nanofibers used have a certain amount of remaining alcoholic hydroxyl groups, which allows stronger hydrogen bonding between molecules and structural restoration. When the dispersion is applied, the viscosity decreases during application, making it easier to apply evenly, and the viscosity recovers after application, allowing the material to maintain a uniform state thereafter. In addition, the recovery (increase) of viscosity after application makes the material less likely to aggregate and warp when drying. Alcoholic hydroxyl groups are detected by infrared spectroscopy.

[0064] The negative electrode dispersion liquid may further contain a solid electrolyte such as a sulfide solid electrolyte, an oxide solid electrolyte, a dry polymer electrolyte, a gel polymer electrolyte, or a quasi-solid electrolyte. By using the above-mentioned positive electrode dispersion liquid or negative electrode dispersion liquid, a secondary battery electrode can be obtained.

[0065] In the present invention, a series of operations including measuring the quality value of the active material dispersion discharged from the disperser, calculating the increase / decrease tendency from the measured quality value, and adjusting the supply rate of the active material mixture to the disperser and / or the power of the disperser in accordance with the calculated increase / decrease tendency are carried out. It is preferable to carry out the series of operations using an automated device. In this case as well, the method for producing an active material dispersion is preferably one in which the quality value to be controlled is the particle size distribution. EXAMPLES

[0066] Examples 1 to 9 <Preparation of Conductive Dispersion Liquid> The conductive material, dispersant, and ion-exchanged water were mixed in the compositions and ratios shown in Table 1, Examples 1 to 9, and stirred for 1 hour in a mixer (Combimix; manufactured by Primix Corporation) to obtain a mixed solution. Next, the mixed solution was put into a thin-film rotary high-speed disperser with a capacity of 1.5 L (Beads Mill; zirconia beads φ1.0 mm; manufactured by Willy & Bachofen Co., Ltd.) and dispersed at a peripheral speed of a rotating disk of 10 m / s. Furthermore, the mixed solution was continuously supplied to and discharged from the disperser using a metering pump capable of controlling the flow rate. The initial condition of the bead mill residence time of the mixed solution, i.e., the dispersion treatment time, was set to 15 minutes.

[0067] At that time, an in-line viscosity sensor (FEM-1000V-ST, Sekonic Corporation) installed on the outlet line of the disperser was used to measure the viscosity of the conductive material dispersion discharged from the disperser at 1 second intervals, and when the slope of the viscosity change of the conductive material dispersion from the most recent 20 measurement values ​​was taken as a (mPa s / sec) and the most recent viscosity value was taken as the intercept b, the pump frequency was adjusted to control the supply speed of the conductive material mixture to the disperser so that the predicted viscosity value Y (= 200 × a + b) after 200 seconds became the target viscosity value.

[0068] When the predicted value Y is greater than the target viscosity value, the supply speed of the mixed liquid is decreased or the peripheral speed of the rotation speed of the disperser is increased to further advance the dispersion of the conductive material dispersion and to decrease the viscosity. When the predicted value Y is smaller than the target viscosity value, the supply speed of the mixed liquid is increased or the peripheral speed of the rotation speed of the disperser is decreased to suppress the dispersion of the conductive material dispersion and to increase the viscosity. The above operations were automatically controlled by a program.

[0069] In accordance with the calculated increase / decrease tendency of the viscosity, the supply flow rate of the conductive material mixture liquid was automatically controlled in real time in Examples 1-2 and 5-9, the peripheral speed of the rotation speed of the disperser was automatically controlled in Example 4, and both were automatically controlled in Example 3. By following the above procedure, a homogeneous conductive material dispersion with an almost constant viscosity was continuously obtained from the beginning to the end of production, even though the mixing state of the mixed liquid supplied to the disperser changed from time to time and the viscosity of the mixed liquid fluctuated.

[0070] <Preparation of negative electrode slurry> Conductive material dispersions of Examples 1 to 9 containing at least one conductive material selected from spherical graphite, acetylene black, carbon nanotubes, graphite (flake-like), and graphene as active materials, and carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) as binders were prepared in the proportions shown in Table 2, Examples 1 to 9. After mixing the spherical graphite and CMC using a planetary mixer, the conductive material dispersion was added until the mixture had a suitable hardness for kneading. After kneading for 3 hours, the remaining conductive material dispersion was added little by little, and when the mixture became uniform and fluid, SBR was added to prepare a negative electrode slurry.

[0071] <Preparation of negative electrode> The negative electrode slurry obtained by the above method was applied to a copper foil having a thickness of 20 μm by a die coater in a coating amount of 4.0 mg / cm. 2 After coating with the coating solution, the negative electrode was dried with hot air to obtain a sheet-like negative electrode. The following evaluations were carried out using the obtained negative electrode sheet. The results are shown in Table 2.

[0072] <Electrode evaluation> Electrode restoration evaluation The negative electrode sheet was pressed with a press to make the coating density 1.60 g / cm 3 After leaving the film at room temperature under atmospheric pressure for 7 days, the density was measured and evaluated according to the following criteria. The density was calculated from the film thickness. ◎: Density 1.55g / cm 3 less than 〇: Density 1.55g / cm 3 More than 1.60g / cm 3 less than ×: Density 1.60g / cm 3 As it is

[0073] Output characteristics and battery characteristics uniformity evaluation Twenty disks were randomly punched out from the negative electrode sheet to produce 20 coin cells (CR2032). DC resistance was measured using each coin cell, and the output characteristics were evaluated according to the following criteria. In addition, the standard deviation of the measured DC resistance values ​​was calculated, and the uniformity of the battery characteristics was evaluated according to the following criteria. The results are shown in Table 1. Output Characteristics ◎: The average DC resistance of 20 coin cells is less than 30 Ω ○: The average DC resistance of 20 coin cells is 30 Ω or more and less than 40 Ω ×: The average DC resistance of 20 coin cells is 40 Ω or more. Uniformity of battery characteristics 〇: The standard deviation of the DC resistance measurements of 20 coin cells is less than 0.5 Ω ×: The standard deviation of the DC resistance measurements of 20 coin cells is 0.5 Ω or more.

[0074] Comparative Examples 1 to 4 <Preparation of Conductive Dispersion Liquid> A conductive material dispersion was obtained in the same manner as in Example 1, except that the components of the dispersion were combined in the compositions and ratios shown in Comparative Examples 1 to 4 in Table 1, and neither the supply speed of the conductive material mixture to the disperser nor the power of the disperser was adjusted, but manual control was performed based on offline measured values.

[0075] <Preparation of negative electrode slurry> Conductive material dispersions of Comparative Examples 1 to 4 containing at least one conductive material selected from spherical graphite, acetylene black, carbon nanotubes, graphite (flake-like), and graphene as active materials, and carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) as binders were prepared in the proportions shown in Table 2, Comparative Examples 1 to 4. After mixing the spherical graphite and CMC using a planetary mixer, the conductive material dispersion was added until it reached a suitable consistency for kneading, and after kneading for 3 hours, the remaining conductive material dispersion was added little by little, and when it became uniform and fluid, SBR was added to prepare a negative electrode slurry.

[0076] <Preparation of negative electrode> Using the negative electrode slurry obtained by the above method, a negative electrode sheet was obtained in the same manner as in Example 1. The electrode recovery, output characteristics, and battery characteristic uniformity of the obtained negative electrode sheet were evaluated according to the above criteria. The results are shown in Table 2.

[0077] [Table 1]

[0078] [Table 2] [Industrial Applicability]

[0079] According to the method for producing an active material dispersion of the present invention, an active material dispersion that can be used as a slurry for electrode plates of lithium ion secondary batteries can be continuously produced.

Claims

1. A method for producing an active material dispersion, comprising continuously supplying an active material mixture containing at least an active material and a solvent to a disperser, dispersing the active material mixture, and continuously discharging the obtained active material dispersion from the disperser, measuring the quality value of the active material dispersion discharged from the disperser at predetermined time intervals using a sensor installed on the outlet line of the disperser; Calculate the increase or decrease trend of the quality value from the quality value measurements of the most recent multiple points, The supply rate of the active material mixture to the disperser and / or the power of the disperser are adjusted according to the calculated increase / decrease tendency.

2. The method for producing an active material dispersion comprising the steps of:

2. The method for producing an active material dispersion liquid according to claim 1 , wherein the quality value is a median diameter of a particle distribution.

3. The method for producing an active material dispersion liquid according to claim 2 , wherein the median diameter of the particle distribution is measured by a laser diffraction method.

4. 4. The method for producing an active material dispersion liquid according to claim 3, wherein the median diameter of the particle distribution is measured by collecting a part of the active material dispersion liquid discharged from the disperser as a sample at an outlet line from the disperser and introducing the collected sample into a laser diffraction device.

Citation Information

Patent Citations

  • Method for manufacturing carbon black dispersion for lithium ion secondary battery

    JP2017135062A

  • Manufacturing method of cathode slurry for lithium ion secondary battery

    JP2017174535A