Bonding method of wood, bonded article and bondable wood
A bonding method for wood using an alkaline oxidizing agent to form a delignified layer for adhesive strength comparable to synthetic adhesives, addressing the challenges of maintaining wood properties and avoiding chemical emissions.
Patent Information
- Application Number
- JP2023049988
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for bonding wood without adhesives often result in altered physical properties and texture, insufficient strength, or require high temperatures and specialized equipment.
A bonding method involving a surface treatment with an alkaline aqueous solution containing an oxidizing agent to remove lignin, forming a delignified layer with exposed cellulose, followed by wet pressing and drying to create a strong adhesive bond without altering the wood's original properties.
The method achieves adhesive strength comparable to synthetic adhesives while maintaining the wood's original physical properties and texture, without using fossil fuel-derived adhesives or emitting volatile chemicals.
Smart Images

Figure 2024139168000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a bonding method for bonding pieces of wood together without using an adhesive, to a bonded product formed by bonding pieces of wood together, and to wood that can be bonded using water without an adhesive. [Background technology]
[0002] Until now, wood has mainly been joined using adhesives. There are natural and synthetic adhesives used in the wood industry, but in recent years, synthetic adhesives have become mainstream. The main synthetic adhesives are phenolic resin adhesives, resorcinol adhesives, and water-based polymeric isocyanate adhesives. Most of these synthetic adhesives for wood are synthetic chemical products derived from petrochemicals, but in recent years, there has been a growing trend to move away from fossil resources. In addition, many synthetic adhesives may release volatile chemicals such as formaldehyde into the surrounding environment, and some consumers do not want such chemicals to volatilize.
[0003] In response to this, self-adhesive technologies that do not use synthetic adhesives have also been researched for a long time. For example, a method has been reported in which lignin is softened by heat generated by friction between wood surfaces to bond them together (e.g., Non-Patent Document 1).
[0004] Non-Patent Document 2 and Patent Document 1 describe that compressed wood, which is much stronger than natural wood, can be obtained by immersing wood in a boiling aqueous solution containing sodium hydroxide and sodium sulfite to remove part of the lignin and hemicellulose in the wood, followed by hot pressing. The density of the compressed wood is 1 g / cm 3 Its tensile strength is said to be more than 10 times that of untreated wood, and its specific strength exceeds that of lightweight titanium alloys. It is also described that by stacking multiple pieces of wood during hot pressing, the pieces of wood are bonded together.
[0005] Non-Patent Document 3 describes that one side of two cedar boards was immersed in a 1N NaOH aqueous solution for one day, and after rinsing, the immersed surface was gently rubbed with the corner of a melamine sponge. The two cedar boards were then placed together under a load and dried, and the two boards were bonded together. It also describes that the aqueous solution was changed to a 1N hypochlorous acid aqueous solution, and the two woods were bonded together in the same manner. Non-Patent Document 3 also describes that these aqueous solutions were used for delignification. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2020-516497 [Non-patent literature]
[0007] [Non-Patent Document 1] Ajith KA Gedara et al., “Adhesiveless Bonding of Wood - A Review with a Focus on Wood Welding”, BioResources 16(3), 6448-6470 (2021) [Non-Patent Document 2] Jianwei Song et al., “Processing bulk natural wood into a high-performance structural material”, Nature, vol 554, 224-228 (2018) [Non-Patent Document 3] Nakamura, Noboru, "Possibility of joining method using hydrogen bonds by fibrillation of solid wood," Abstracts of the 70th Annual Meeting of the Japan Wood Research Society (Tottori), H16-06-1500 (2020) Summary of the Invention [Problem to be solved by the invention]
[0008] In the method of joining wood by softening lignin as described in Non-Patent Document 1, the joining surface becomes hot and special equipment is required. In addition, although compressed wood produced by the methods described in Non-Patent Document 2 and Patent Document 1 can join wood pieces together, the physical properties and texture of the wood pieces are significantly different from those of wood. Furthermore, when wood pieces are bonded together using the method described in Non-Patent Document 3, the strength is insufficient.
[0009] The present invention has been made to solve the above problems, and aims to provide a method for strongly bonding wood pieces together without adhesive while maintaining the original physical properties and texture of the wood. It also aims to provide a bonded product bonded in this way. Furthermore, it aims to provide wood to be used in such a bonding method. [Means for solving the problem]
[0010] The above problem is a method for bonding wood pieces together without using an adhesive, a surface treatment step of removing lignin from the surfaces of both wood materials using an alkaline aqueous solution containing an oxidizing agent to form a delignified layer in which cellulose is exposed on the surface of the remaining lignin portions; a wet pressing step in which the delignified layers are placed opposite each other and pressed against each other to bring the cellulose layers into contact with each other in a wet state; and A drying step is performed to dry the material while it is pressed. The problem is solved by providing an adhesion method, in which the ratio (d2 / d1) of the density (d2) of the remaining lignin part after the drying step to the density (d1) of the remaining lignin part before the surface treatment step is 1.5 or less.
[0011] In this case, the average thickness of the delignified layer formed in the surface treatment step is preferably 0.1 to 3 mm. It is also preferable that the aqueous solution contains hypochlorite. In the surface treatment step, the lignin is removed and the wood surface can be rubbed to expose fibrillated cellulose. After the surface treatment step, the wood can be dried once, and then the cellulose in the delignified layer can be moistened with water, and then the wood can be subjected to a wet pressing step.
[0012] The above-mentioned problem is a joint product formed by bonding pieces of wood together, which has a delignified layer at the joint and has a density (d2) of the remaining lignin of 0.8 g / cm 3 The problem can also be solved by providing a joined product in which the average thickness of the delignified layer at the joint is 0.05 to 1.5 mm, and the proportion of arabinose among the neutral sugars contained in the delignified layer is 0.5 mass % or less.
[0013] The above-mentioned problems can also be solved by providing a dried wood having a delignified layer in which lignin on the surface has been removed and cellulose is exposed on the surface of the remaining lignin, the delignified layer having a ratio of arabinose of 0.5 mass% or less among neutral sugars, and capable of being bonded using water without an adhesive, and the average thickness of the delignified layer is preferably 0.1 to 3 mm. Effect of the Invention
[0014] According to the bonding method of the present invention, it is possible to strongly bond pieces of wood together without adhesives while maintaining the original physical properties and texture of the wood. The bonded product thus bonded is firmly bonded without adhesives. It is also possible to provide wood that can be bonded using water without adhesives. [Brief description of the drawings]
[0015] [Figure 1] 1 is a graph showing the shear strength of bonded articles obtained in Examples 2-1 to 2-8 (with fibrillation) in Example 2. [Diagram 2] 1 is a graph showing the shear strength of bonded articles obtained in Examples 2-9 to 2-16 (without fibrillation) in Example 2. [Diagram 3] 1 is a graph showing the shear strength of bonded articles obtained in Examples 2-17 to 2-22 (evaluation of concentration dependency) in Example 2. [Figure 4] 1 is a cross-sectional photograph of a pre-bonding test piece in Example 3 after dyeing. [Diagram 5] 1 is a cross-sectional photograph of a bonded article in Example 3 after dyeing. [Figure 6] 1 is a graph showing the residue yield versus immersion time in an analytical test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention relates to a bonding method for bonding wood pieces together without using an adhesive. The wood used in the present invention is not particularly limited, and may be a coniferous or broad-leaved tree. Examples of coniferous trees include cedar, cypress, larch, Abies sachalinensis, Douglas fir, red pine, red spruce, Yezo spruce, Scots pine, Japanese cypress, and spruce. Examples of broad-leaved trees include birch, oak, ash, zelkova, and silver maple. Different kinds of wood pieces may be bonded together, not just the same kind of wood pieces. The shape of the wood pieces to be joined is also not particularly limited. Flat surfaces of boards or square timber may be bonded together, or curved surfaces may be bonded together. The shape is not particularly limited as long as the surface-treated surfaces can come into contact with each other.
[0017] The bonding method of the present invention includes a surface treatment step, a wet pressing step, and a drying step. As shown in the examples below, by bonding through these steps, a bonding strength equivalent to that of a synthetic adhesive was obtained even though the bonding was performed without an adhesive, and a surprisingly high strength was achieved. Each of these steps will be described in detail below.
[0018] [Surface treatment process] First, in the surface treatment step, lignin is removed from the surfaces of both pieces of wood using an alkaline aqueous solution containing an oxidizing agent, thereby forming a delignified layer in which cellulose is exposed on the surface of the remaining lignin parts.
[0019] The aqueous solution used here is an alkaline aqueous solution containing an oxidizing agent. By contacting the surface of the wood with this aqueous solution, the lignin and hemicellulose on the surface are removed to expose the cellulose. At this time, it is not necessary to remove all of the lignin and hemicellulose present on the surface of the wood, and it is acceptable for some of them to remain. By using an alkaline aqueous solution containing an oxidizing agent, lignin and hemicellulose are removed, but cellulose remains. As shown in the [Analysis Test] below, it was found that when an alkaline aqueous solution containing an oxidizing agent was used, the removal rate of hemicellulose was high and the remaining rate of cellulose was high. It is believed that this reduces damage to the cellulose and makes it easier for the cellulose to hydrogen bond with each other, resulting in a high adhesive strength.
[0020] The oxidizing agent contained in the aqueous solution used in the present invention is not particularly limited, but oxoacid salts of chlorine, such as hypochlorite, chlorite, and chlorate, are preferred. Considering the oxidizing power, hypochlorite or chlorite are more preferred, and hypochlorite is even more preferred. As the counter cation of the oxoacid of chlorine, cations such as sodium, potassium, calcium, and magnesium are preferred, and among these, alkali metal cations are preferred. Therefore, as the oxidizing agent used in the present invention, alkali metal salts of oxoacid of chlorine are preferred. Among them, alkali metal salts of hypochlorous acid are preferably used, and sodium hypochlorite is particularly preferred. Note that these salts are dissociated into cations and anions in the aqueous solution. For example, an aqueous solution prepared by adding sodium hydroxide to an aqueous solution of hypochlorous acid contains sodium hypochlorite.
[0021] The content of the oxidizing agent in the aqueous solution is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and even more preferably 4% by mass or more, while the content of the oxidizing agent is preferably 15% by mass or less, more preferably 12% by mass or less, and even more preferably 10% by mass or less.
[0022] In order to keep the aqueous solution alkaline and improve the stability of the oxidizing agent such as hypochlorite, the aqueous solution may further contain an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide. The pH of the aqueous solution is preferably 11 or more, more preferably 12 or more, and even more preferably 13 or more.
[0023] The aqueous solution may contain a surfactant. As shown in the examples below, when the surface is not fibrillated, the adhesive strength is often increased by adding a surfactant to the aqueous solution. On the other hand, when fibrillation is performed after long-term contact with the aqueous solution, a higher adhesive strength is often obtained without the use of a surfactant. Therefore, it is preferable to determine the suitability of using a surfactant by taking into consideration the operation and conditions during adhesion. As the surfactant, any of anionic surfactants, cationic surfactants, and nonionic surfactants may be used and is selected appropriately.
[0024] The method of bringing the aqueous solution into contact with the wood is not particularly limited. The board may be immersed in the aqueous solution, or the aqueous solution may be applied or sprayed. When immersing the board in the aqueous solution, the board may be floated with the adhesive side facing down to form a delignified layer on the adhesive side, or the board may be submerged in the aqueous solution to form a delignified layer on the entire surface, or the board may be positioned and immersed to the desired depth. Application or spraying may also be performed in a continuous process. The delignified layer may also be formed only in the required areas by masking.
[0025] The temperature of the aqueous solution when contacting the wood is not particularly limited, and may be room temperature or may be heated appropriately. The time of contacting the aqueous solution is also not particularly limited. Considering the adhesiveness, the longer the contact time between the wood and the aqueous solution, the better, preferably 1 hour or more, more preferably 2 hours or more, even more preferably 5 hours or more, and particularly preferably 10 hours or more. On the other hand, if the contact time between the wood and the aqueous solution is too long, the cellulose may be damaged and the adhesive strength may decrease. In addition, the amount of water absorbed by the wood may be too large, which may require extra drying energy or cause the wood to deform. The contact time between the wood and the aqueous solution is preferably 200 hours or less, more preferably 100 hours or less, and even more preferably 60 hours or less.
[0026] It is preferable to bring the aqueous solution into contact with the wood as described above to remove lignin and hemicellulose from the surface of the wood, wash the wood, and then subject the wood to the wet pressing process. The washing method is not particularly limited, but washing with water is preferable. At this time, the wood may be immersed in washing water, washed with running water, or sprayed with washing water. In addition, the surface may be lightly rubbed or ultrasonic vibration may be applied while washing to improve the washing efficiency.
[0027] In the surface treatment step, it is preferable to remove lignin and expose fibrillated cellulose by rubbing the wood surface. This fibrillates the cellulose fibers on the wood surface, increasing the surface area, and increasing the number of hydrogen bonds formed during adhesion, improving the adhesive strength. This is particularly effective when the time for contacting the wood with the aqueous solution is short or when the aqueous solution does not contain a surfactant. The timing for rubbing the wood surface for fibrillation may be before or after the washing, or may be performed simultaneously, but it is preferable to rub the wood surface while it is still wet. There is no particular limitation on the method for rubbing the wood surface, and it can be rubbed with the loop surface of a hook-and-loop fastener or a scrubbing brush.
[0028] A delignified layer is formed by passing through the surface treatment process. The formed delignified layer becomes white as the brown color derived from lignin disappears. FIG. 4 shows a cross-sectional photograph of a pre-bonded test piece in Example 3-6 of Example 3 after dyeing. The test piece is dried before being subjected to the wet pressing process after passing through the surface treatment process, and an aqueous solution containing 1 g of phloroglucin, 50 mL of ethanol, and 25 mL of concentrated hydrochloric acid is uniformly dripped onto the test piece to color the lignin reddish purple. This color reaction is known as the phloroglucin hydrochloric acid reaction and is widely used for coloring lignin. In this color reaction, coloring occurs by reacting with the aldehyde group of coniferyl aldehyde constituting the terminal in lignin, so if the aldehyde group has disappeared, coloring does not occur. Therefore, the lack of coloring does not mean that the entire amount of lignin has been removed. In Fig. 4, the portion of the remaining lignin 1 is dyed deep reddish purple, and the boundary with the undyed white delignified layer 2 is clear, showing that a delignified layer having a thickness of about 1 mm has been formed. The thickness of the delignified layer in the present invention refers to the thickness obtained by measuring the portion that remains undyed when dyed by the above-mentioned method, and in the case where fibrillation is performed before the wet pressing step, it refers to the thickness before fibrillation.
[0029] The average thickness of the delignified layer is adjusted as appropriate depending on the form of the wood to be bonded and the required adhesive strength, but is preferably 0.1 to 3 mm. If the average thickness is too thin, the contact between the cellulose particles may be insufficient, resulting in a decrease in adhesive strength. The average thickness is more preferably 0.2 mm or more, and even more preferably 0.5 mm or more. On the other hand, if the average thickness is too thick, the cellulose fibers in the delignified layer may be damaged, which may also result in a decrease in adhesive strength and a decrease in productivity. The average thickness is more preferably 2.5 mm or less, and even more preferably 2 mm or less.
[0030] In the surface treatment process of the present invention, the hemicellulose contained in the delignified layer is easily decomposed, and in particular, the arabinose and xylose contained therein are easily decomposed and removed, while the residual rate of glucose is high. As a result, it is believed that cellulose is easily hydrogen-bonded with itself, resulting in high adhesive strength. This point is supported by the analysis results of neutral sugars contained in a sample in the [Analysis Test] (Analysis of Neutral Sugars) of the Example, in which wood flour with a particle size of 355 to 212 μm was immersed in "Kitchen Haiter" for 24 hours at room temperature. As mentioned above, a delignified layer with a thickness of about 1 mm is formed by immersing wood in "Kitchen Haiter" for 16 hours at room temperature, so the wood flour with a particle size of 355 to 212 μm can be considered to have the same composition as the delignified layer as a whole, and can be said to be a model of the delignified layer.
[0031] Among the neutral sugars contained in the delignified layer formed in the surface treatment step of the present invention, the content of arabinose is preferably 0.5% by mass or less. A low content of arabinose provides high adhesive strength. The content of arabinose is more preferably 0.3% by mass or less, even more preferably 0.2% by mass or less, and particularly preferably 0.1% by mass or less. For the same reason, it is also preferable that the content of xylose among the neutral sugars contained in the delignified layer is 6.5% by mass or less, more preferably 6% by mass or less, and even more preferably 5.5% by mass or less. The content of xylose is usually 2% by mass or more. For the same reason, the content of glucose among the neutral sugars contained in the delignified layer is preferably 77% by mass or more, more preferably 78% by mass or more, and even more preferably 79% by mass or more. The neutral sugars analyzed here were five types, namely arabinose, xylose, mannose, glucose, and galactose, which are the main components of cellulose and hemicellulose. The content of each neutral sugar was expressed as mass %, with the total content of these sugars being 100 mass %.
[0032] [Wet pressing process] In the wet pressing step following the surface treatment step, the delignified layers are placed opposite each other and pressed against each other to bring the cellulose of the delignified layers into contact with each other in a wet state.
[0033] At this time, it is important to bring the cellulose molecules in the delignified layers into contact with each other in a wet state. This allows the cellulose molecules in the delignified layer of one wood to approach the cellulose molecules in the delignified layer of the other wood via water molecules. The pressing method is not particularly limited as long as it can bring the delignified layers into close contact with each other. For example, pressing can be performed using a press. Considering that the layers will be subjected to the next drying step while still pressed, it is preferable to use an apparatus that can perform pressing and heating simultaneously.
[0034] The pressure in the wet pressing step is not particularly limited as long as it is a pressure that allows the delignified layers to adhere to each other. Pressure may be applied mechanically using a press or the like, or pressing may be performed by binding with a rubber belt or the like. The adhesion should be maintained while taking into consideration the type, dimensions, shape, etc. of the wood. In order to obtain adhesive strength with good reproducibility, a high pressure is preferable. The pressure is preferably 0.1 MPa or more, more preferably 0.3 MPa or more, even more preferably 0.5 MPa or more, and particularly preferably 0.7 MPa or more. On the other hand, if the pressure is too high, the entire wood will be compressed, and the physical properties and texture of the wood will change. Therefore, the pressure is preferably 3 MPa or less, more preferably 2 MPa or less, and even more preferably 1.5 MPa or less.
[0035] [Drying process] In the drying process following the wet pressing process, both pieces of wood are dried while still pressed. At this time, water molecules present between cellulose molecules that are close to each other are removed, and the hydroxyl groups of cellulose are bonded to each other by hydrogen bonds, which is thought to develop adhesive strength between the pieces of wood. Therefore, it is important to continue applying pressure during the drying process, and it is preferable to maintain the pressure in the wet pressing process. If a press is used, an automatic pressure-controlled hot press machine that can prevent a pressure drop due to the contraction of the wood during pressing and continue to apply a constant pressure is preferably used. Also, if a device such as a clamp is used, it is preferable to tighten it appropriately in accordance with the contraction of the wood. By drying while still pressing in this way, a bonded product in which the pieces of wood are bonded to each other is obtained.
[0036] The drying temperature is not particularly limited as long as it is a temperature at which water can be removed. Drying at room temperature is acceptable, but if it is desired to shorten the drying time, heating may be used. The heating temperature in the case of heating is preferably 30°C or higher, more preferably 40°C or higher, and even more preferably 50°C or higher. On the other hand, if the heating temperature is too high, there is a risk of the wood being deformed or denatured. The heating temperature is preferably 90°C or lower, more preferably 80°C or lower, and even more preferably 70°C or lower.
[0037] The time for drying under pressure is set appropriately taking into consideration the drying time, type of wood, dimensions, shape, etc. If drying is to be done naturally under pressure at room temperature, it is better to dry for a long time, but if drying is to be done at high temperatures in a heat press, it is better to dry for a relatively short time. The time for drying under pressure is usually about one hour to one month. It is also preferable to cure the wood under appropriate temperature and humidity after removing the pressure and then use it for various purposes.
[0038] The bonded product obtained by the drying process is a product in which wood pieces are bonded together without the use of adhesives. Here, the ratio (d2 / d1) of the density (d2) of the lignin remaining part after the drying process to the density (d1) of the lignin remaining part before the surface treatment process is 1.5 or less. By making the ratio (d2 / d1) 1.5 or less, it is possible to bond wood pieces together without adhesives while maintaining the original physical properties and texture of the raw wood material. The ratio (d2 / d1) is preferably 1.4 or less, more preferably 1.3 or less, even more preferably 1.25 or less, and particularly preferably 1.2 or less. On the other hand, the lower limit of the ratio (d2 / d1) is 1 if there is no change in the density of the lignin remaining part, but in reality, it may be slightly below 1 because the moisture content may increase or there may be variation depending on the measurement location.
[0039] [Joined products] The bonded product of the present invention is a bonded product formed by bonding pieces of wood together, has a delignified layer at the bonded part, and has a density (d2) of the remaining lignin of 0.8 g / cm 3 The bonded product has a bonding strength of 0.5% by mass or less, and the proportion of arabinose among the neutral sugars contained in the delignified layer is 0.5% by mass or less. Preferably, the bonded product is bonded through the surface treatment step, the wet pressing step, and the drying step. As shown in the examples below, a bonded product having an adhesive strength equivalent to that obtained with a general-purpose synthetic adhesive has also been obtained, and the bonded product is surprisingly strong even when bonded without an adhesive.
[0040] The density of the remaining lignin (d2) is 0.8 g / cm 3 The bonded product of the present invention is made by bonding wood pieces together without using adhesives while maintaining the original physical properties and texture of the raw wood material, so the density (d2) of the remaining lignin does not increase significantly from that of the raw wood material, and the light weight of wood can be maintained. The density (d2) is preferably 0.7 g / cm 3 It is preferably 0.65 or less, and more preferably 0.6 g / cm or less. 3 Below 0.55g / cm 3 or less than 0.5g / cm 3The lower limit of density (d2) is usually 0.3 g / cm, depending on the type of wood. 3 That's all.
[0041] The delignified layer at the joint is formed by compressing and bonding two delignified layers formed on the surfaces of two pieces of wood material. As described above, the average thickness of the delignified layer formed in the surface treatment step is preferably 0.1 to 3 mm, but the delignified layer in the jointed product is compressed to about 1 / 4 of the thickness. Therefore, the average thickness of the delignified layer at the joint formed by compressing two delignified layers is preferably 0.05 to 1.5 mm. If the average thickness is too thin, the adhesive strength may be insufficient. The average thickness is more preferably 0.1 mm or more, and even more preferably 0.25 mm or more. On the other hand, if the average thickness is too thick, the adhesive strength may also be insufficient and may be undesirable from the viewpoint of productivity. The average thickness is more preferably 1.25 mm or less, and even more preferably 1 mm or less. The thickness of the delignified layer at the joint can also be measured by utilizing color development due to the phloroglucinic acid reaction as described above.
[0042] The content of neutral sugars contained in the delignified layer forming the joint of the present invention is the same as the content of neutral sugars contained in the delignified layer formed in the surface treatment step described above. That is, the content of arabinose among the neutral sugars contained in the delignified layer forming the joint of the present invention is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, even more preferably 0.2% by mass or less, and particularly preferably 0.1% by mass or less. The content of xylose and glucose among the neutral sugars contained in the delignified layer is also the same as the content of neutral sugars contained in the delignified layer formed in the surface treatment step described above.
[0043] [Gluable wood] One embodiment of the present invention is dried wood having a delignified layer in which the lignin on the surface has been removed and cellulose is exposed on the surface of the remaining lignin, the delignified layer containing neutral sugars in which the proportion of arabinose is 0.5 mass% or less, and the wood is capable of being glued using water without an adhesive.
[0044] Wood can also be bonded to wood by drying once after the surface treatment step, wetting the cellulose in the delignified layer with water, and then subjecting it to a wet pressing step. Therefore, it is possible to distribute the wood in a dried state after the surface treatment step without consecutively performing the surface treatment step, the wet pressing step, and the drying step. By separating the surface treatment step using chemicals, anyone can easily bond wood using only water. Therefore, it is applicable not only to industrial applications but also to DIY applications. In this case, the wood obtained by drying once is wood that does not contain the free water that was contained immediately after the surface treatment step.
[0045] The content of neutral sugars contained in the delignified layer at this time is also the same as the content of neutral sugars contained in the delignified layer formed in the surface treatment step described above. That is, the content of arabinose among the neutral sugars contained in the delignified layer forming the joint of the present invention is preferably 0.5 mass% or less, more preferably 0.3 mass% or less, even more preferably 0.2 mass% or less, and particularly preferably 0.1 mass% or less. Furthermore, the content of xylose and glucose among the neutral sugars contained in the delignified layer is also the same as the content of neutral sugars contained in the delignified layer formed in the surface treatment step described above. Furthermore, the thickness of the delignified layer is the same as that explained in the surface treatment step.
[0046] [Application] The wood bonding method of the present invention can be applied to various applications. Since it does not use adhesives derived from fossil fuels such as petroleum, it is expected to be accepted by users who are concerned about reducing the burden on the environment. In addition, since it does not emit volatile organic compounds such as formaldehyde, it can be used for building materials, interior materials, furniture, etc. that can improve the living environment. EXAMPLES
[0047] [Example 1] (wood) The tree species used in this example were larch, cedar, Douglas fir, cypress and spruce, and the raw material boards used in the tests had a width of 60 mm (65 mm for Examples 1-6 only), a thickness of 10 mm and a length of 320 mm.
[0048] (Removal of lignin) A wooden board was immersed in a commercially available kitchen bleach ("Kitchen Haiter" manufactured by Kao Corporation) at room temperature. The immersion time is as shown in Table 1. The bleach is an aqueous solution containing sodium hypochlorite (oxidizing agent, 6 mass%), sodium hydroxide (alkali agent), and sodium alkyl ether sulfate (surfactant) with a pH of 13 to 13.5. At this time, since the wood floats on the water, only the underside is immersed in the bleach, and the lignin on the surface is removed and whitened, forming a delignified layer. The sample was removed from the bleach and then washed with water, and fibrillated as described below.
[0049] (Fibrillation) Using a handheld sanding machine, the surface of the delignified layer was rubbed with the nylon hook surface of the hook-and-loop fastener on the base surface without attaching sandpaper. The treatment time was adjusted appropriately.
[0050] (press) After fibrillation, and in a moist state, the test pieces were stacked with the delignified layers facing each other and pressed in a hot press. The pressing pressure is shown in Table 1. The temperature of the upper side of the press was set to 50°C, 60°C or 80°C, but the lower side was not heated. Moisture in wood moves from the higher temperature to the lower temperature. The test pieces were pressed in the press for 24 hours and dried. The dimensions (thickness and width) of the jointed products thus obtained were measured.
[0051] (Bending test) The bonded products were left to stand for several months after pressing and then thoroughly dried before being subjected to a bending test. The bending test was performed with a three-point, four-point load (span 300 mm, crosshead speed 2 mm / min). The obtained bending strength and bending modulus are shown in Table 1 together with the dimensions (thickness and width) and fracture mode of the bonded products subjected to the test.
[0052] (glue) In Examples 1-24 and 1-25, a bleach solution was not used, but a water-based adhesive that is widely used for bonding wood as a structural material was used instead, which is made by mixing and reacting an aqueous solution of polyvinyl alcohol with an isocyanate.
[0053] [Table 1]
[0054] As shown in Table 1, by immersing wood in a bleaching agent containing sodium hypochlorite, sodium hydroxide, and a surfactant, a delignified layer was formed and cellulose was exposed. The delignified layers were then placed facing each other, the cellulose was brought into contact with each other in a wet state, and the wood was dried while being pressed, allowing the wood to be firmly bonded together. It was found that the longer the immersion time in the bleaching agent and the higher the pressing pressure, the greater the adhesive strength. However, if the pressing pressure is too high, the thickness becomes smaller and the density increases, changing the original physical properties of the wood.
[0055] In the joints using larch that failed in bending without adhesive (Examples 1-2, 3, 5, and 6), the failure occurred in bending rather than shear, as in the joints using adhesive (Examples 1-24 and 25), and bending strength and bending modulus were comparable to those obtained when adhesive was used.
[0056] [Example 2] The wood used in Example 2 was a board-grained timber of Todomatsu (Japanese larches) with a thickness of 13 mm, a width of 100 mm, and a length of 60 mm, and its density was 0.369 g / cm 3 The composition of the aqueous solution in which the wood was soaked is shown in Table 2. The anionic surfactant used here was "Alscope NS-230" manufactured by Toho Chemical Industry Co., Ltd. This aqueous solution was modeled after a commercially available kitchen bleach ("Kitchen Haiter" manufactured by Kao Corporation). The temperature of the aqueous solution was 20±5°C, and the soaking time was as shown in Table 2. After soaking, the sample was removed from the aqueous solution and washed with water. When fibrillating the delignified layer, it was rubbed with the nylon hook surface of a hook-and-loop fastener under running water to fibrillate while simultaneously washing with water.
[0057] The delignified layers of the samples were stacked facing each other, the moisture on the surfaces was wiped off, and the samples were dried at 60°C for 24 hours at a pressure of 1 MPa using an automatic pressure-controlled hot press. At this time, a rubber sheet and a Teflon sheet were stacked on top and bottom, respectively, so that the Teflon sheet was in contact with the sample. After pressing, the samples were stored and cured for about one week in an environment of 20°C and 65% RH, and the temperature and humidity were adjusted. The plate thickness, density, and moisture content of the resulting bonded products were measured, and a block shear test was performed based on JIS K6852. The results are shown in Table 2. The number of samples for each condition was 9 (n=9), and only Example 2-23 had n=42.
[0058] [Table 2]
[0059] FIG. 1 shows a graph illustrating the shear strength of the bonded products obtained in Examples 2-1 to 2-8, and FIG. 2 shows a graph illustrating the shear strength of the bonded products obtained in Examples 2-9 to 2-16. A tendency was observed in which the shear strength increased with increasing immersion time in the aqueous solution. Furthermore, when the delignified layer was fibrillated, sufficient strength was obtained by immersion for a relatively short period of time even without adding a surfactant. On the other hand, when the delignified layer was not fibrillated, a higher shear strength was obtained by adding a surfactant.
[0060] The graph showing the shear strength of the bonded products obtained in Examples 2-17 to 2-22 is shown in Figure 3. It was shown that the shear strength tends to increase as the concentration of sodium hypochlorite in the aqueous solution increases. It was found that the inclusion of a surfactant can increase the shear strength even when the concentration of sodium hypochlorite is low.
[0061] [Example 3] Using the wood shown in Table 3, tests were carried out in a similar manner to Example 2. The density of Todomatsu is 0.386 g / cm 3 and the density of larch is 0.532 g / cm 3 In this example, as shown in Table 3, wood was immersed in various commercially available aqueous solutions for a given time, and fibrillated as necessary using the nylon hook surface of a hook-and-loop fastener or a scrubbing brush. As the kitchen bleach, "Kitchen Haiter" manufactured by Kao Corporation, which was also used in Example 1, was used. The disinfectant bleach used was "Hospital Haiter" manufactured by Kao Corporation. This is an aqueous solution with a pH of 13 that contains 6% by mass of sodium hypochlorite and sodium hydroxide. The oxygen bleach used was "Wide Haiter ex Power" manufactured by Kao Corporation. This is an aqueous solution with a pH of 2.75, whose main components are hydrogen peroxide and a surfactant (polyoxyethylene alkyl ether). Strongly acidic electrolyzed water is strongly acidic electrolyzed water generated on the anode side by electrolyzing a sodium chloride aqueous solution, and is an aqueous solution whose main component is hypochlorous acid. The acidic cleaning agent used was "Sunpol" manufactured by Kincho Co., Ltd. This is an aqueous solution containing 9.5% by mass of hydrochloric acid, a surfactant (alkyltrimethylammonium salt), a cleaning aid, and the like.
[0062] As the pressing method, there was a case where an automatic pressure control type hot press machine was used as in Example 2, and a case where pressure was applied using a screw type clamp. The pressing conditions were 60°C and 24 hours, except for Example 3-11 (room temperature). After pressing, the joint was stored and cured for about one week under an environment of 20°C and 65% RH, and the temperature and humidity were adjusted, and then the thickness, density, and moisture content of the joint were measured and a block shear test was performed based on JIS K6852. In addition, in Examples 3-8 and 3-12, the joint was not immersed in an aqueous solution, but was bonded using an aqueous adhesive that is widely used when bonding wood as a structural material. The adhesive is a mixture of an aqueous polyvinyl alcohol solution and an isocyanate, which are reacted. The above results are summarized in Table 3. The number of samples for each condition was 6 to 9 (n = 6 to 9).
[0063] In addition, in Examples 3-16 to 3-19, the samples were immersed in an aqueous solution, fibrillated as necessary, washed with water, and then stored for 6 days in an environment of 20°C and 65% RH, and then dried. The dried samples were then immersed in water at 20°C for 3 hours or 24 hours, and pressed. The evaluation results are shown in Table 3. The number of samples for each condition was 9 (n=9).
[0064] [Table 3]
[0065] As shown in Table 3, hydrogen peroxide, hydrochloric acid, and the like could not bond wood (Examples 3-13 to 3-15). It was also found that bonding was possible by forming a delignified layer, drying it, and then immersing it in water again (Examples 3-16 to 3-19).
[0066] (Observation of delignified layer) A delignified layer was formed on a test piece of Todomatsu using "Kitchen Haiter" under the same conditions as in Example 3-6. This test piece was thoroughly aged and dried under the conditions of 20°C and 65% RH to obtain a sample (before bonding test piece). In addition, after forming the delignified layer, it was press-molded and bonded under the same conditions as in Example 3-6 in a wet state, and then thoroughly aged and dried under the conditions of 20°C and 65% RH to obtain a sample (bonded product). An aqueous solution containing 1 g of phloroglucin, 50 mL of ethanol, and 25 mL of concentrated hydrochloric acid was evenly dripped onto the cross sections of the pre-bonded test piece and the bonded product thus obtained, and after a color reaction was caused, the surface was lightly wiped to prepare a dyed sample. This was observed using a microscope (Keyence Corporation, high-speed microscope "VW-9000"), and the thickness of the delignified layer was measured using a function to measure the length between two points on the screen. A cross-sectional photograph of the pre-bonded test piece after dyeing is shown in Figure 4, and a cross-sectional photograph of the bonded product after dyeing is shown in Figure 5. Since lignin has a reddish purple color, the remaining lignin portion 1 was observed to be a deep reddish purple, and the delignified layer 2 was observed to be white. The delignified layer 2 was observed and measured in six places on the test piece before bonding and in four places on the joined product. As a result, the average thickness of the lignin layer 2 on the test piece before bonding was 1.03 mm, with a standard deviation of 0.26 mm. The average thickness of the lignin layer 2 on the joined product was 0.58 mm, with a standard deviation of 0.03 mm. The two lignin layers on the test piece before bonding were bonded at the bonding surface 3 and compressed to become the lignin layer 2 of the joined product, which indicates that the bonding compressed it to about 1 / 4.
[0067] (Density change of remaining lignin) A jointed product of Todomatsu was obtained using "Kitchen Haiter" under the same conditions as in Example 3-6. The raw wood material was Todomatsu board material with a thickness of 13 mm, width of 100 mm, and length of 60 mm. When the raw wood material was sufficiently cured under conditions of 20°C and 65% RH, the density of the board placed on the lower side was 0.311 g / cm 3 The upper plate has a mass of 0.367 g / cm 3 The thickness of the resulting joint was 21 mm, and the average density of the entire joint after sufficient curing under conditions of 20°C and 65% RH was 0.416 g / cm 3The result was as follows. Twelve small test pieces measuring 21 mm in thickness, 10 mm in width, and 10 mm in length were cut out from the bonded product. These small test pieces were divided into 5 pieces in the thickness direction to obtain 5 small test pieces measuring 4 mm in thickness, 10 mm in width, and 10 mm in length, which were numbered 1 to 5 from the top. Small test pieces 1 and 2 originate from the upper plate, and small test pieces 4 and 5 originate from the lower plate. Small test piece 3 includes the bonded delignified layer. The average density of these small test pieces and its deviation value are shown in Table 4. The density ratio of each small test piece before and after bonding was calculated according to the following formula, and the results are also shown in Table 4. Small test pieces 1 and 2: Small test piece average density / Upper raw material density Small test pieces 4 and 5: Small test piece average density / lower raw material density Small test piece 3: Small test piece average density / [(upper raw material density + lower raw material density) / 2]
[0068] [Table 4]
[0069] As shown in Table 4, the density of small test piece 3, which included the compressed and joined delignified layer, increased by about 1.5 times. On the other hand, the density of the other parts only increased by an average of 1.16 times, indicating that the wood could be joined without a significant change in density.
[0070] [Analytical Testing] (Preparation of wood flour) The wood materials used were cedar (heartwood and sapwood), larch, and cypress. These wood materials were crushed in a rotary mill so that the wood would pass through 5 mm holes. The crushed wood was sieved to obtain wood powder with a particle size of 355 to 212 μm. The obtained wood powder was dried at 105°C, and the moisture content was measured.
[0071] (Delignification rate by kitchen bleach) Approximately 0.5 g of wood flour was precisely weighed, and the weight A (g) of the dried wood flour was calculated taking into account the moisture content. The wood flour was soaked in 40 mL of "Kitchen Haiter" at room temperature for 6, 12, 18, and 24 hours. The wood flour was then filtered through a glass filter and dried overnight at 105°C, after which the weight B (g) of the residue was measured. The residue yield (mass%) was calculated as (B / A) x 100. Figure 6 is a graph showing the residue yield versus soaking time.
[0072] (Delignification with kitchen bleach) Approximately 2 g of wood flour from cedar heartwood, cedar sapwood, larch, and cypress was precisely weighed, and the weight A (g) of the dried wood flour was calculated taking into account the moisture content. The wood flour was immersed in 40 mL of "Kitchen Haiter" at room temperature for 24 hours. The wood flour was then filtered through a glass filter and dried overnight at 105°C, after which the weight B (g) of the residue was measured. The decomposition rate (mass%) was calculated as (1-B / A) x 100. The same analysis was performed three times for each tree species, and the average value was calculated. The results are shown in Table 5.
[0073] (Chlorite delignification) Approximately 2 g of wood flour from cedar heartwood, cedar sapwood, larch and cypress was precisely weighed, and the weight C (g) of the dry wood flour was calculated taking into account the moisture content. The wood flour was immersed in 64 mL of 0.2 M acetate buffer (pH 3.5), 0.2 mL of acetic acid and 0.6 g of sodium chlorite were added, and the mixture was heated at 70-75 ° C for 1 hour. The same amount of acetic acid and sodium chlorite were then added, and the mixture was heated again for 1 hour. This treatment was repeated two more times. The treated wood flour was filtered through a glass filter, washed with ion-exchanged water, and dried overnight at 105 ° C, after which the weight D (g) of the residue was measured. During the above operation, the pH of the treatment solution remained acidic at around 3.5. The decomposition rate (mass%) was calculated as (1-D / C) x 100. The same analysis was performed three times for each tree species, and the average value was calculated. The results are shown in Table 5.
[0074] (Quantification of Lignin) The lignin content of wood flour samples treated with "Kitchen Haiter" and chlorite was quantified by the Klason method. Approximately 1 g of wood flour (referred to as E(g)) was precisely weighed and placed in a 50 mL beaker. 10 mL of 72% by mass sulfuric acid was added to the sample, and the mixture was kept at room temperature for 3 hours while being stirred occasionally with a glass rod. Then, 375 mL of ion-exchanged water was added to reduce the sulfuric acid concentration to 3% by mass, and the mixture was heated at approximately 120°C for 30 minutes in an autoclave. After cooling overnight, the mixture was filtered using a glass filter. The lignin residue obtained by filtration was dried in an oven at 120°C, and the weight F(g) was measured. The lignin residual rate (mass%) was calculated by (F / E) x 100. The results are shown in Table 5.
[0075] (Neutral sugar analysis) The alditol-acetate method was used to analyze neutral sugars. Approximately 2 g of wood flour was treated with "Kitchen Haiter" and chlorite, and dried overnight at 105°C. Approximately 0.5 g was precisely weighed and placed in a 30 mL beaker, and 5 mL of 72% sulfuric acid was added and kept at room temperature for 4 hours with occasional stirring. Then, it was transferred to a 300 mL flask using 140 mL of ion-exchanged water and treated at 121°C for 1 hour in an autoclave. After cooling overnight, it was filtered using a glass filter, and the filtrate was diluted to 500 mL. An internal standard substance (inositol solution) was added to 10 mL of the diluted sample, and it was neutralized with barium hydroxide (pH 5.5-6.5). After removing barium sulfate by centrifugation, sodium borohydride (NaBH4) was added to the supernatant. Further, acetic acid was added to decompose the excess sodium borohydride, and the supernatant was removed by an evaporator. The borate was washed off by repeating the addition of methanol several times, and the mostly dried sample was further dried in an oven at 105°C. Then, acetic anhydride (3mL) was added and reacted at 120°C for 3 hours, and the sample after the reaction was analyzed by gas chromatography. The column used was a GL Science, Inc. TC-17, and the device used was a Shimadzu Corporation GC-2014. The same analysis was performed three times for each type, and the average content (mass%) of arabinose, xylose, mannose, glucose, and galactose was calculated. At this time, the total of these five types of neutral sugars was set to 100 mass%. The results are shown in Table 5.
[0076] As shown in Figure 6, the residual rate of cedar wood flour after immersion in "Kitchen Bleach" for 24 hours was approximately 72% by mass, indicating that approximately 28% by mass of the components were decomposed. Table 5 shows the decomposition rates of various wood flours treated with "Kitchen Bleach" and chlorite at room temperature for 24 hours. Table 5 also shows the residual lignin rate and neutral sugar content after each treatment. Table 5 also shows the proportion of each neutral sugar obtained in this way.
[0077] [Table 5]
[0078] As shown in Table 5, the wood flour treated with chlorite showed a higher decomposition rate than that treated with "Kitchen Haiter", and the lignin residual rate was also lower, indicating that chlorite has a higher decomposition ability for lignin than "Kitchen Haiter". In addition, the content of neutral sugars was higher in wood flour treated with chlorite, indicating that chlorite can selectively remove lignin more than "Kitchen Haiter". On the other hand, for neutral sugars other than glucose, "Kitchen Haiter" has a higher decomposition ability than chlorite, and there is a significant difference in the decomposition ability of arabinose and xylose in particular. In addition, the residual rate of cellulose was higher in "Kitchen Haiter" than in chlorite. Therefore, with regard to the decomposition ability of hemicellulose, "Kitchen Haiter" has a higher decomposition ability than chlorite, which may contribute to the strong hydrogen bonds between cellulose. [Explanation of symbols]
[0079] 1. Lignin Remaining Part 2 Delignification layer 3 Adhesive surface
Claims
1. A method for bonding wood pieces together without using adhesive, comprising the steps of: a surface treatment step of removing lignin from the surfaces of both wood materials using an alkaline aqueous solution containing an oxidizing agent to form a delignified layer in which cellulose is exposed on the surface of the remaining lignin portions; a wet pressing step in which the delignified layers are placed opposite each other and pressed against each other to bring the cellulose layers into contact with each other in a wet state; and A drying step is performed to dry the material while it is pressed. A bonding method, in which the ratio (d2 / d1) of the density (d2) of the remaining lignin portion after the drying step to the density (d1) of the remaining lignin portion before the surface treatment step is 1.5 or less.
2. 2. The bonding method according to claim 1, wherein the delignified layer formed in the surface treatment step has an average thickness of 0.1 to 3 mm.
3. 3. The bonding method according to claim 1, wherein the aqueous solution contains a hypochlorite.
4. 3. The bonding method according to claim 1 or 2, wherein in the surface treatment step, lignin is removed and the wood surface is rubbed to expose fibrillated cellulose.
5. 3. The bonding method according to claim 1, further comprising the steps of drying after the surface treatment step, moistening the cellulose in the delignified layer with water, and then subjecting the cellulose to a wet pressing step.
6. A joint product in which wood pieces are bonded together, the joint has a delignified layer, and the density (d2) of the remaining lignin is 0.8 g / cm 3 and the proportion of arabinose among the neutral sugars contained in the delignified layer is 0.5 mass% or less.
7. The jointed article according to claim 6, wherein the average thickness of the delignified layer at the joint is 0.05 to 1.5 mm.
8. A dried wood having a delignified layer in which lignin has been removed from the surface and cellulose is exposed on the surface of the remaining lignin, wherein the proportion of arabinose among the neutral sugars contained in the delignified layer is 0.5 mass% or less, and the wood can be glued using water without an adhesive.
9. The wood material according to claim 8, wherein the delignified layer has an average thickness of 0.1 to 3 mm.
Citation Information
Patent Citations
Composite material and manufacturing method of composite material
JP2015077740A
Strong and durable structural timber and methods for making and using same
JP2020516497A
Delignified wood material, and methods for producing and using same
JP2020534183A
Manufacturing method of cellulose nanofiber and cellulose nanofiber
JP2021095476A
Process for bonding lignocellulosic substrates without an added adhesive and products thereof
US20150258760A1