Resin composition for emulsion, emulsion composition and coating agent

The combination of aliphatic polyester resin and controlled cellulose nanofiber content in emulsion compositions addresses sedimentation stability and film-forming issues, resulting in stable and strong film formation with enhanced properties.

JP2024139361AInactive Publication Date: 2024-10-09MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023050257
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional emulsion compositions containing aliphatic polyester resins suffer from insufficient sedimentation stability and inadequate film-forming properties, with limited progress in improving these critical characteristics.

Method used

A resin composition for emulsion comprising an aliphatic polyester resin with specific aliphatic polyhydric alcohol and aliphatic polycarboxylic acid units, combined with cellulose nanofibers, where the cellulose nanofiber content is controlled within a specific range to enhance sedimentation stability and film-forming properties.

Benefits of technology

The composition achieves excellent sedimentation stability and film-forming properties, with improved tensile strength and heat seal strength after film formation, while maintaining biodegradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139361000001
    Figure 2024139361000001
Patent Text Reader

Abstract

To provide an emulsion composition which is excellent in sedimentation stability, and is also excellent in film formation property.SOLUTION: A resin composition for emulsion contains an aliphatic polyester-based resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polyvalent carboxylic acid unit as main constitutional units, and a cellulose nanofiber (B), wherein a content of the cellulose nanofiber (B) is less than 2 pts.mass with respect to 100 pts.mass of the aliphatic polyester-based resin (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for emulsions containing a biodegradable resin, and more particularly to a resin composition for emulsions, an emulsion composition, a coating agent, and the like, which contain an aliphatic polyester resin. [Background technology]

[0002] In recent years, research and development of various biodegradable resins has been progressing against the background of demands for reducing the environmental burden. In particular, from the viewpoint of promoting the elimination of organic solvents, a resin composition for emulsion containing a biodegradable resin has attracted attention.

[0003] For example, as a resin composition for emulsion having excellent biodegradability, an emulsion composition has been proposed in which an aliphatic polyester resin such as polylactic acid or polybutylene succinate is emulsified using a dispersant such as polyvinyl alcohol, and it is expected that this composition will be used in various applications such as adhesives, paints, and coating agents (e.g., Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-204038 A [Patent Document 2] JP 2004-238579 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, emulsion compositions containing conventional aliphatic polyester resins sometimes have insufficient sedimentation stability, and further improvement is required. Furthermore, research and development into emulsion compositions that have improved sedimentation stability and also have excellent film-forming properties, which are one of the important required properties, has not yet progressed sufficiently. [Means for solving the problem]

[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an emulsion composition and the like which has excellent sedimentation stability and also excellent film-forming properties.

[0007] Means for Solving the Problems The present inventors have conducted extensive research in light of the above circumstances and have discovered that, by using a specific aliphatic polyester resin and controlling the content of a specific cellulose material relative to the aliphatic polyester resin within a specific range, it is possible to provide an emulsion composition having excellent sedimentation stability and excellent film-forming properties, thereby completing the present invention.

[0008] The present invention provides the following [1] to

[17] . [1] The resin composition for emulsions comprises an aliphatic polyester resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polycarboxylic acid unit as main structural units, and a cellulose nanofiber (B), wherein the content of the cellulose nanofiber (B) is less than 2 parts by mass per 100 parts by mass of the aliphatic polyester resin (A). [2] The resin composition for emulsions according to [1], wherein the cellulose nanofibers (B) have an average fiber diameter of 1 to 1000 nm. [3] The resin composition for emulsion according to [1] or [2], wherein the cellulose nanofiber (B) is a hydrophilic cellulose nanofiber (b1). [4] The resin composition for emulsion according to any one of [1] to [3], wherein the aliphatic polyester resin (A) has a melt flow rate of less than 80 g / 10 min at 190° C. and 2.16 kg. [5] The resin composition for emulsion according to any one of [1] to [4], further comprising a polyvinyl alcohol-based resin. [6] An emulsion composition comprising the resin composition for emulsion according to any one of [1] to [5]. [7] The emulsion composition according to [6], wherein the dispersed particle size is 10 μm or less. [8] A coating agent comprising the resin composition for emulsion according to any one of [1] to [5]. [9] The coating agent according to [8], wherein the substrate to be coated is a paper substrate.

[10] The coating agent according to [8], wherein the object to be coated is a plastic substrate.

[11] A molded article obtained by using the resin composition for emulsion according to any one of [1] to [5].

[12] A film obtained by using the resin composition for emulsion according to any one of [1] to [5].

[13] A cosmetic preparation comprising the resin composition for emulsion according to any one of [1] to [5].

[14] An agricultural composition comprising the resin composition for emulsions according to any one of [1] to [5].

[15] A coating material comprising the resin composition for emulsion according to any one of [1] to [5].

[16] An ink containing the resin composition for an emulsion according to any one of [1] to [5].

[17] A pressure-sensitive adhesive comprising the resin composition for emulsion according to any one of [1] to [5]. Effect of the Invention

[0009] According to the present invention, it is possible to provide an emulsion composition and the like which has excellent sedimentation stability and also excellent film-forming properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in more detail below based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0011] In this specification, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "it is preferably greater than X" or "it is preferably less than Y". Furthermore, "X and / or Y (X and Y are optional)" means at least one of X and Y, and means the following three cases: X only, Y only, and X and Y.

[0012] An emulsion resin composition according to an embodiment of the present invention (hereinafter, sometimes referred to as "the present emulsion resin composition") is a resin composition for emulsions that contains an aliphatic polyester resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polycarboxylic acid unit as main constituent units, and a cellulose nanofiber (B), characterized in that the content of the cellulose nanofiber (B) is less than 2 parts by mass per 100 parts by mass of the aliphatic polyester resin (A). The present emulsion resin composition can provide an emulsion composition that is excellent in sedimentation stability and film-forming properties.

[0013] As an example of an embodiment of the present resin composition for emulsion, for example, an aqueous resin composition for emulsion containing component (A), component (B), a dispersant (C) such as a polyvinyl alcohol-based resin, and a dispersion medium (D) such as water is suitable. As an example of an embodiment of the present invention, an emulsion composition containing the present resin composition for emulsion (hereinafter, sometimes referred to as the present emulsion composition) is preferable. The present emulsion composition is obtained by using the present emulsion resin composition, specifically, by a known production method such as a phase inversion emulsification method using the present emulsion resin composition. The present resin composition for emulsion and the present emulsion composition will be described in detail below.

[0014] [Component (A)] The component (A) is, for example, an aliphatic polyester resin having, as main constituent units, an aliphatic polyhydric alcohol unit represented by the following formula (1) and an aliphatic polycarboxylic acid unit represented by the following formula (2).

[0015] -OR 11 -O- (1) [In formula (1), R 11 represents a divalent chain aliphatic hydrocarbon group, and when copolymerized, the number of types is not limited to one.

[0016] -OC-R 21 -CO- (2) [In formula (2), R 21 represents a divalent chain aliphatic hydrocarbon group, and when copolymerized, the number of types is not limited to one.

[0017] The term "unit" means a structural unit contained in the aliphatic polyester resin derived from a monomer component used in the production of the aliphatic polyester resin, and the term "main structural unit" means that the structural unit derived from the target monomer component is contained in the total structural units of the component (A) at 50 mol% or more. The content of the structural unit derived from the target monomer is preferably 60 mol% or more, more preferably 70 mol% or more, and even more preferably 80 to 100 mol%. For example, it is preferable that the aliphatic polyester resin is produced by polymerizing a raw material containing an aliphatic polyhydric alcohol and an aliphatic polycarboxylic acid component at 50 mol% or more, preferably 60 mol% or more, more preferably 70 mol% or more, and even more preferably 80 to 100 mol% of the total monomer components used in the polymerization reaction of the aliphatic polyester resin.

[0018] The aliphatic polyhydric alcohol that gives the polyhydric alcohol unit of formula (1) is not particularly limited, but for example, an aliphatic polyhydric alcohol having 2 to 10 carbon atoms is preferable, and an aliphatic polyhydric alcohol having 4 to 6 carbon atoms is more preferable. Specific examples include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, diethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc. Among them, 1,4-butanediol is preferable. The aliphatic polyhydric alcohol may be used alone or in combination of two or more kinds.

[0019] The aliphatic polycarboxylic acid component that gives the aliphatic polycarboxylic acid unit of formula (2) is an aliphatic polycarboxylic acid or an aliphatic polycarboxylic acid derivative such as an alkyl ester thereof, and the aliphatic polycarboxylic acid is not particularly limited, but is preferably an aliphatic polycarboxylic acid having 2 to 40 carbon atoms, more preferably an aliphatic polycarboxylic acid having 4 to 10 carbon atoms. Specific examples include succinic acid, adipic acid, suberic acid, sebacic acid, and dodecanedioic acid. Among them, succinic acid, adipic acid, and sebacic acid are preferred, and succinic acid and adipic acid are more preferred. The aliphatic polycarboxylic acid components may be used alone or in combination of two or more.

[0020] Specific examples of the (A) component include, for example, an aliphatic polyester resin containing 1,4-butanediol and succinic acid, and an aliphatic polyester resin containing 1,4-butanediol, adipic acid, and succinic acid. More specifically, from the viewpoint of significantly achieving the effects of the present invention, suitable examples include polybutylene succinate and polybutylene succinate adipate. Among these, polybutylene succinate adipate is preferred.

[0021] When the aliphatic polycarboxylic acid is succinic acid, the proportion of constituent units derived from succinic acid in all polycarboxylic acid units of the aliphatic polyester resin is usually 50 to 100 mol %, preferably 80 to 100 mol %, and more preferably 90 to 100 mol %.

[0022] Furthermore, when the aliphatic polycarboxylic acid is succinic acid and adipic acid, the proportion of the succinic acid-derived constituent units in all polycarboxylic acid units of the aliphatic polyester resin is usually 50 to 95 mol%, preferably 60 to 93 mol%, and more preferably 70 to 90 mol%, and the proportion of the adipic acid-derived constituent units in all polycarboxylic acid units is usually 5 to 50 mol%, preferably 7 to 40 mol%, and more preferably 10 to 30 mol%.

[0023] The component (A) preferably has the following physical properties:

[0024] The weight average molecular weight (Mw) of the component (A) is preferably 10,000 or more, more preferably 20,000 or more, and even more preferably 50,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less, and even more preferably 400,000 or less. The weight average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0025] The melt flow rate (MFR) of component (A), when measured at 190°C and 2.16 kg, is usually 0.1 g / 10 min or more, preferably 0.5 g / 10 min or more, more preferably 1 g / 10 min or more, and is less than 80 g / 10 min, preferably 60 g / 10 min or less, more preferably 40 g / 10 min or less, even more preferably 20 g / 10 min or less, and particularly preferably 10 g / 10 min or less.

[0026] The melting point of component (A) is preferably 70° C. or higher, more preferably 75° C. or higher, and is preferably 250° C. or lower, more preferably 200° C. or lower, even more preferably 150° C. or lower, and particularly preferably 100° C. or lower. When there are multiple melting points, it is preferable that at least one of the melting points is within the above range.

[0027] In the present resin composition for emulsion, the component (A) may be used alone or in combination of two or more kinds. For example, two or more kinds of aliphatic polyester resins having different polyhydric alcohol units or polyvalent carboxylic acid units may be mixed and used.

[0028] The content of the component (A) is not particularly limited, but is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the total amount of the emulsion composition, and is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 60% by mass or less.

[0029] [(B) component] The resin composition for emulsion contains cellulose nanofibers (B). The cellulose nanofibers (B) are obtained by defibrating and / or pulverizing various cellulose raw materials such as bamboo, rice straw, wheat straw, rice husks, herbaceous plants, seaweed, etc., according to a conventional method, and although various known cellulose nanofibers can be used, the content ratio thereof is important in the resin composition for emulsion. That is, in a resin composition for emulsion containing the specific aliphatic polyester resin (A) and cellulose nanofiber (B), it is important that the content of the cellulose nanofiber (B) is less than 2 parts by mass per 100 parts by mass of the aliphatic polyester resin (A). If the content of the cellulose nanofibers (B) exceeds the above range, the film-forming properties of the emulsion composition tend to decrease. On the other hand, if the cellulose nanofibers (B) are not contained, the sedimentation stability of the emulsion composition tends to decrease, making it difficult to achieve both sedimentation stability and film-forming properties.

[0030] From the viewpoint of achieving a high level of both the sedimentation stability and the film-forming properties, the content of the cellulose nanofibers (B) is preferably 0.05 to 1.5 parts by mass, more preferably 0.1 to 1.2 parts by mass, even more preferably 0.2 to 1.0 part by mass, and particularly preferably 0.3 to 0.8 parts by mass, relative to 100 parts by mass of the aliphatic polyester resin (A).

[0031] The principle by which it is possible to provide an emulsion composition having excellent sedimentation stability and excellent film-forming properties by setting the content of cellulose nanofibers (B) in this emulsion resin composition to less than 2 parts by mass per 100 parts by mass of aliphatic polyester resin (A) is not entirely clear, but the inventors speculate that by using a small amount of cellulose nanofibers that have a network structure and are thixotropic relative to the aliphatic polyester resin (A), the emulsion particles are well dispersible in water and have good coatability.

[0032] The average fiber diameter of the cellulose nanofibers (B) is, for example, preferably 1 to 1000 nm, more preferably 1.5 to 700 nm, even more preferably 2 to 500 nm, particularly preferably 2 to 250 nm, and particularly preferably 2 to 100 nm. If the average fiber diameter of the cellulose nanofibers (B) exceeds the upper limit, the sedimentation stability tends to decrease and the film-forming properties also tend to decrease. Furthermore, if the average fiber diameter of the cellulose nanofibers (B) exceeds the upper limit, the tensile properties and heat seal strength after film formation also tend to decrease. The average fiber diameter of the cellulose nanofibers (B) may be 2 to 50 nm or 2 to 25 nm.

[0033] The average fiber diameter of the cellulose nanofibers (B) can be measured in accordance with conventional methods by randomly selecting at least 10 fibers from a fiber image obtained using an electron beam microscope or the like, and calculating the average length of each fiber in the short axis direction. More specifically, for example, after a process such as drying and removing water, organic solvents, etc. from the cellulose nanofiber dispersion liquid as necessary, observation is performed using an electron microscope image at a magnification of about 5000x, 10000x, or 50000x depending on the size of the fibers constituting the cellulose nanofibers, and an arbitrary axis of image width is assumed in the obtained image, and the sample and observation conditions (magnification, etc.) are adjusted so that, for example, 20 or more fibers cross the axis. After obtaining an observation image that satisfies this condition, two random axes are drawn vertically and horizontally per image on this image, and the fiber diameter of the fibers crossing the axis is read visually. At least three images of the surface portion that do not overlap are taken with an electron microscope, and the value of the fiber diameter of the shorter width (short width) of the fibers crossing the two axes is read (thus, information on the fiber diameter of at least 20 fibers x 2 x 3 = 120 fibers is obtained), and the average value (number average width) of the obtained values ​​is calculated. The number average width data of the short width obtained in this way is calculated as the average fiber diameter.

[0034] The average fiber length of the cellulose nanofibers (B) is not limited to the following, but is preferably 50 to 10,000 nm, more preferably 80 to 5,000 nm, and even more preferably 100 to 2,500 nm. The average fiber length can be determined, for example, by analyzing the electron microscope image used to measure the average fiber diameter.

[0035] The aspect ratio (average fiber length / average fiber diameter) of the cellulose nanofibers (B) is not particularly limited, and is, for example, 5 to 10,000, 10 to 6,000, 15 to 2,000, 20 to 1,500, 30 to 1,000, or the like.

[0036] The cellulose nanofiber (B) used in the resin composition for emulsion includes hydrophilic cellulose nanofiber (b1) and hydrophobic cellulose nanofiber (b2). The cellulose nanofiber (B) may be used alone or in combination of two or more kinds.

[0037] Hydrophilic cellulose nanofibers (b1) refer to cellulose nanofibers that have a high affinity for water, that is, that are easily soluble in water or easily miscible with water, while hydrophobic cellulose nanofibers (b2) refer to cellulose nanofibers that have a low affinity for water, that is, that are poorly soluble in water or poorly miscible with water. The hydrophilic cellulose nanofibers (b1) and the hydrophobic cellulose nanofibers (b2) can be obtained by appropriately selecting a known production method. The hydrophilic cellulose nanofibers (b1) can be obtained, for example, by a grinder method in which a cellulose-based material is prepared into microfibrillated nanofibers using a grinder, a pulverization treatment using a ball mill, or a TEMPO (2,2,6,6-tetramethylpiperidine-1-oxy radical) oxidation method in which a carboxyl group or the like is introduced onto the surface. The hydrophobic cellulose nanofibers (b2) can be obtained, for example, by a method in which a part or all of the hydroxyl groups on the surface of the cellulose nanofiber are replaced with hydrophobic groups, or a method in which a hydrophobic surface treatment is performed using a surface treatment agent such as a silane coupling agent.

[0038] Among various cellulose nanofibers (B), hydrophilic cellulose nanofibers (b1) are preferred in the resin composition for emulsions. The use of hydrophilic cellulose nanofibers (b1) can improve sedimentation stability, and further tends to improve tensile properties and heat seal strength after film formation. From this viewpoint, among the hydrophilic cellulose nanofibers (b1), anion-modified hydrophilic cellulose nanofibers in which anionic groups have been introduced are preferred. The amount of anionic groups in the anion-modified hydrophilic cellulose nanofibers is not limited to the following, but is, for example, about 0.05 to 3.0 mmol / g, and about 0.5 to 2.5 mmol / g.

[0039] Among the above, one or more selected from the group consisting of carboxy group-modified hydrophilic cellulose nanofibers, carboxymethyl group-modified hydrophilic cellulose nanofibers, sulfone group-modified hydrophilic cellulose nanofibers, and phosphate ester group-modified hydrophilic cellulose nanofibers are preferred, and carboxy group-modified hydrophilic cellulose nanofibers are particularly preferred.

[0040] The carboxyl group-modified hydrophilic cellulose nanofiber is preferably, for example, one in which the hydroxyl group at the C6 position of the glucose unit in the cellulose molecule is selectively oxidized to a carboxyl group. Such cellulose nanofibers are obtained by oxidizing natural cellulose such as wood pulp using a co-oxidant in the presence of an N-oxyl compound (e.g., 2,2,6,6-tetramethylpiperidine-1-oxyradical (TEMPO) or 4-acetamide-TEMPO) and subjecting the cellulose to defibration (refining) treatment.

[0041] Examples of commercially available cellulose nanofibers (B) that can be used include, but are not limited to, LeoCrysta (registered trademark, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Cellenpia (registered trademark, manufactured by Nippon Paper Industries Co., Ltd.), AuroVisco (registered trademark, manufactured by Oji Holdings Co., Ltd.), and Stellafine (registered trademark, manufactured by Marusumi Paper Co., Ltd.).

[0042] [(C) Dispersant] The dispersant (C) that can be used in the present emulsion resin composition can be any commonly used known dispersant. For example, water-soluble polymers, various surfactants, etc. can be mentioned. These can be used alone or in combination of two or more kinds.

[0043] Examples of water-soluble polymers include, but are not limited to, polyvinyl alcohol resins (hereinafter referred to as "PVA resins"), cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxybutyl methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, aminomethyl hydroxypropyl cellulose, and aminoethyl hydroxypropyl cellulose (excluding the cellulose nanofibers of (B)), starch, tragacanth, pectin, glue, alginic acid or a salt thereof, gelatin, polyvinylpyrrolidone, polyacrylic acid or a salt thereof, polymethacrylic acid or a salt thereof, polyacrylamide, polymethacrylamide, copolymers of vinyl acetate and unsaturated acids such as maleic acid, maleic anhydride, acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and crotonic acid, copolymers of styrene and the above unsaturated acids, copolymers of vinyl ethers and the above unsaturated acids, and salts of the above copolymers. Examples of the surfactant include nonionic surfactants, cationic surfactants, anionic surfactants, etc. Specific examples include, but are not limited to, polyoxyethylene nonylphenyl ether, polyoxyethylene octylnonyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene alkyl allyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyalkylene alkyl ether phosphate monoethanolamine salt, polyoxyethylene lauryl amino ether, polyoxyethylene stearyl amino ether, and other polyoxyethylene alkyl amino ethers. Among these, the PVA-based resin (C1) is preferably used from the viewpoint of achieving the remarkable effects of the present invention.

[0044] [PVA resin (C1)] The PVA resin (C1) that can be used in the present resin composition for emulsion includes unmodified PVA resins and modified PVA resins.

[0045] The unmodified PVA resin can be produced by saponifying a vinyl ester polymer obtained by polymerizing a vinyl ester compound.

[0046] Examples of such vinyl ester compounds include vinyl formate, vinyl acetate, vinyl trifluoroacetate, vinyl propionate, vinyl butyrate, vinyl caprate, vinyl laurate, vinyl versatate, vinyl palmitate, vinyl stearate, etc., with vinyl acetate being preferred. The vinyl ester compounds may be used alone or in combination of two or more.

[0047] The modified PVA resin can be produced by copolymerizing the vinyl ester compound with an unsaturated monomer copolymerizable with the vinyl ester compound, followed by saponification.

[0048] Examples of the unsaturated monomer copolymerizable with the vinyl ester compound include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, α-octadecene, etc., hydroxyl group-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, etc., and derivatives such as acylated products thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, undecylenic acid, etc., salts thereof, monoesters, or dialkyl esters thereof; amides such as diacetone acrylamide, acrylamide, methacrylamide, etc.; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, etc., or salts thereof. These can be used alone or in combination of two or more kinds.

[0049] The modified PVA resin may have a primary hydroxyl group in the side chain, for example, a number of primary hydroxyl groups in the side chain is usually 1 to 5, preferably 1 to 2, and particularly preferably 1. Furthermore, the modified PVA resin may preferably have a secondary hydroxyl group in addition to the primary hydroxyl group. Examples of such modified PVA resins include PVA resins having a hydroxyalkyl group in the side chain, PVA resins having a 1,2-diol structural unit in the side chain, and the like.

[0050] The average saponification degree of the PVA resin (C1) is preferably 70 mol% or more, more preferably 75 to 99 mol%, even more preferably 78 to 95 mol%, and particularly preferably 82 to 90 mol%. If the average saponification degree is too low, the water resistance of the film obtained by using the resin composition for emulsion tends to decrease.

[0051] In particular, when an unmodified PVA resin is used as the PVA resin (C1), the average saponification degree is preferably 75 mol% or more, more preferably 78 to 95 mol%, and even more preferably 82 to 90 mol%. If the average saponification degree is too low, the water resistance of the film obtained by using the resin composition for emulsion tends to decrease.

[0052] When a modified PVA resin is used as the PVA resin (C1), the average saponification degree is preferably 72 mol% or more, more preferably 75 to 99 mol%, and even more preferably 80 to 95 mol%. If the average saponification degree is too low, the water resistance of the film obtained by using the resin composition for emulsion tends to decrease.

[0053] The average degree of saponification is measured in accordance with JIS K 6726 3.5.

[0054] The viscosity of a 4 mass% aqueous solution of the PVA resin (C1) at 20° C. is preferably 10 to 70 mPa s, more preferably 13 to 45 mPa s, and even more preferably 17 to 40 mPa s. If the viscosity is too low, the stability of the emulsion composition tends to decrease.

[0055] When an unmodified PVA resin is used as the PVA resin (C1), the viscosity of a 4 mass% aqueous solution of the unmodified PVA resin at 20° C. is preferably 5 to 50 mPa s, more preferably 13 to 45 mPa s, and even more preferably 17 to 40 mPa s. If the viscosity is too low, the stability of the emulsion composition tends to decrease.

[0056] When a modified PVA resin is used as the PVA resin (C1), the viscosity of a 4% by mass aqueous solution of the modified PVA resin at 20° C. is preferably 5 to 50 mPa s, more preferably 13 to 40 mPa s, and even more preferably 17 to 30 mPa s. If the viscosity is too low, the stability of the emulsion composition tends to decrease.

[0057] The viscosity of the 4 mass % aqueous solution is measured in accordance with JIS K 6726 3.11.2.

[0058] The average degree of polymerization of the PVA resin (C1) is preferably from 50 to 5,000, more preferably from 150 to 4,000, and even more preferably from 300 to 3,000. The average degree of polymerization can be determined according to the method for calculating the average degree of polymerization described in JIS K 6726.

[0059] In the resin composition for emulsion, the PVA-based resins (C1) may be used alone or in combination with other unmodified PVA-based resins, with other modified PVA-based resins, with an unmodified PVA-based resin and a modified PVA-based resin, or in combination of two or more types of resins differing in average degree of saponification, viscosity, type of modification, amount of modification, etc. may also be used.

[0060] The content of the (C) component is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and particularly preferably 3% by mass or more, based on the total amount of the emulsion composition. Also, it is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 12% by mass or less, and particularly preferably 10% by mass or less. Outside this range, the stability of the emulsion composition tends to decrease.

[0061] [(D) Dispersion medium] The dispersion medium (D) that can be used in the present emulsion resin composition is not particularly limited as long as it is a water-soluble component in the substance and concentration range that does not affect the stability of the emulsion composition, and may be an aqueous solution containing the components, such as water alone or an aqueous polysaccharide solution, and may be used in combination with a small amount of a water-soluble organic solvent. Examples of the organic solvent include methanol, ethanol, and acetone. Of these, water is the most preferable dispersion medium.

[0062] The mass ratio (D / A) of the component (D) to the component (A) is not particularly limited, but from the viewpoint of significantly exhibiting the effects of the present invention, it is, for example, 0.5 to 1.6, preferably 0.7 to 1.4, and more preferably 0.8 to 1.2.

[0063] The content of the (D) component is not particularly limited, but is preferably 25% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more, based on the total amount of the emulsion composition, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less.

[0064] When the dispersion medium is a combination of water and an organic solvent, the content of water in the total amount of the dispersion medium is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. Among these, it is most preferable to use only water as the dispersion medium.

[0065] [Other ingredients] The present emulsion resin composition preferably does not contain any other components in addition to the above-mentioned components, but as long as the other components are within a range that does not impair the effects of the present invention (for example, 10 mass% or less based on the total amount of the emulsion composition), components that have been commonly used in conventional resin compositions may be included. Such components are not particularly limited, but examples thereof include polyester resins other than the polyester resin (A), plasticizers, preservatives, antifungal agents, antibacterial agents, thermoplastic resins, various stabilizers, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, rust inhibitors, curing agents, fillers, etc.

[0066] (Polyester resins other than polyester resin (A)) Examples of polyester resins other than the polyester resin (A) include aliphatic polyester resins having aliphatic oxycarboxylic acid units as the main structural unit. Specific examples of aliphatic oxycarboxylic acid components that provide aliphatic oxycarboxylic acid units include lactic acid, glycolic acid, 2-hydroxy-n-butyric acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxycaproic acid, 6-hydroxycaproic acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-hydroxyisocaproic acid, 3-hydroxyvaleric acid, malic acid, citric acid, and the like, or lower alkyl esters or intramolecular esters thereof. In addition, lactone compounds such as ε-caprolactone are also included in the aliphatic oxycarboxylic acid in the present invention. When optical isomers exist in these, they may be D-form, L-form, or racemic form, and may be in the form of a solid, liquid, or aqueous solution. Among these, lactic acid, glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 6-hydroxycaproic acid, and 3-hydroxyvaleric acid are preferred. These aliphatic oxycarboxylic acids may be used alone or in combination of two or more.

[0067] Specific examples of the aliphatic polyester resin having the aliphatic oxycarboxylic acid unit as the main constituent unit include polylactic acid, polyglycolic acid, poly 3-hydroxybutyrate, poly 4-hydroxybutyrate, poly(3-hydroxybutyrate-co-3-hydroxyvalerate), polycaprolactone, etc.

[0068] The composition of lactic acid contained in polylactic acid is, for example, a molar ratio of D-lactic acid:L-lactic acid=100:0-85:15, or 0:100-15:85. It is also possible to blend other polylactic acids having different composition ratios of D-lactic acid and L-lactic acid.

[0069] Furthermore, the polylactic acid may be a copolymer of the above-mentioned polylactic acid and other oxycarboxylic acids, or may contain a small amount of units derived from a chain extender. Examples of other oxycarboxylic acids include optical isomers of lactic acid (D-lactic acid for L-lactic acid, and L-lactic acid for D-lactic acid), glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxy-n-butyric acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-methyllactic acid, and bifunctional aliphatic oxycarboxylic acids such as 2-hydroxycaproic acid, and lactones such as caprolactone, butyrolactone, and valerolactone. Units derived from such other oxycarboxylic acids can be used in an amount of less than 15 mol% of the total structural units of the polylactic acid.

[0070] In addition, examples of polyester resins other than the polyester resin (A) include aliphatic-aromatic polyester resins having aliphatic polyhydric alcohol units, aliphatic polycarboxylic acid units, and aromatic polycarboxylic acid units as main constituent units. The aliphatic-aromatic polyester resin having an aliphatic polyhydric alcohol unit, an aliphatic polycarboxylic acid unit, and an aromatic polycarboxylic acid unit as main constituent units has, for example, an aliphatic polyhydric alcohol unit represented by the above formula (1), an aliphatic polycarboxylic acid unit represented by the above formula (2), and an aromatic polycarboxylic acid unit represented by the following formula (3) as main constituent units. It may further have the above-mentioned oxycarboxylic acid unit.

[0071] -OC-R 31 -CO- (3) [In formula (3), R 31 represents a divalent aromatic hydrocarbon group, and when copolymerized, the number of types is not limited to one.

[0072] The aliphatic polyhydric alcohol that provides the polyhydric alcohol unit of formula (1) and the aliphatic polycarboxylic acid component that provides the aliphatic polycarboxylic acid unit of formula (2) are the same as those exemplified in the description of component (A) above.

[0073] The aromatic polycarboxylic acid component that gives the aromatic polycarboxylic acid unit of formula (3) is not particularly limited, but examples thereof include terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, etc. These may be acid anhydrides. In addition, examples of derivatives of aromatic polycarboxylic acids include lower alkyl esters of these aromatic polycarboxylic acids.

[0074] Specific examples of the aliphatic-aromatic polyester resin include polybutylene alkylate terephthalates such as polybutylene adipate terephthalate and polybutylene succinate terephthalate. These can be used alone or in combination of two or more.

[0075] (Plasticizer) Examples of the plasticizer include ester-based plasticizers having an ester bond in the molecule. Examples of the plasticizer include aliphatic dibasic acid ester-based plasticizers such as adipate-based plasticizers, sebacate-based plasticizers, and azelaate-based plasticizers, phthalate-based plasticizers, phosphate-based plasticizers, citrate-based plasticizers, glycolate-based plasticizers, trimellitate-based plasticizers, ricinoleate-based plasticizers, benzoate-based plasticizers, and acetate-based plasticizers. These may be used alone or in combination of two or more.

[0076] [Resin composition for emulsion and method for producing emulsion composition] The present emulsion resin composition and the present emulsion composition can be produced by a known method in the art. For example, the present emulsion composition is produced by a phase inversion emulsification process in which component (A), component (B), dispersant (C), and dispersion medium (D) are mixed together.

[0077] Specifically, the composition is produced by a method in which component (A) is charged into a kneader, and if necessary, a solvent or the like is optionally charged, followed by melt-kneading under heating conditions, and then component (B), a dispersant (C) such as a PVA-based resin (C1), and a dispersion medium (D) such as water are charged, followed by mixing and phase-inversion emulsification of these components. The heating temperature is usually 40 to 250°C, preferably 60 to 200°C, more preferably 60 to 160°C, and even more preferably 80 to 150°C. The heating time is usually 10 to 1,800 seconds, preferably 10 to 600 seconds, and more preferably 20 to 300 seconds.

[0078] Examples of the kneading machine include an extruder, a homogenizer (high pressure), a roll mill, a kneader, an ink roll, a Banbury mixer, etc. Among these, from the viewpoint of productivity, an extruder is preferred, and a multi-screw extruder having two or more screws such as a twin-screw extruder is particularly preferred.

[0079] When producing using an extruder, for example, the component (A) is continuously fed from the hopper of the extruder or a separate supply port and melt-kneaded under heating conditions, and an aqueous dispersion of the component (B), a dispersant (C) such as a PVA-based resin (C1), and a dispersion medium (D) such as water are added from another supply port provided in the extruder, kneaded and dispersed to effect phase inversion emulsification, and then continuously extruded from a die to obtain the present emulsion composition.

[0080] In addition, the present emulsion composition can be obtained by using pellets obtained by melt-kneading the component (A) under heating conditions using an extruder, etc. Specifically, pellets containing the component (A) are continuously supplied from a hopper of an extruder and melt-kneaded under heating conditions, and an aqueous dispersion of the component (B), a dispersant (C) such as a PVA-based resin (C1), and a dispersion medium (D) such as water are added from another supply port provided in the same extruder, kneaded and dispersed to effect phase inversion emulsification, and then continuously extruded from a die to obtain the present emulsion composition.

[0081] [Resin composition for emulsion and emulsion composition] As described above, the present emulsion resin composition obtained from the (A) component, the (B) component, the (C) dispersant such as a PVA-based resin (C1), and the (D) dispersion medium such as water is an aqueous emulsion resin composition. A preferred embodiment of the present invention is an emulsion composition obtained from such an aqueous emulsion resin composition. An aqueous emulsion composition is an emulsion in which particulate matter is dispersed in an aqueous solvent and emulsified, and specifically, an emulsion system in which the dispersion medium (i.e., continuous phase) is an aqueous liquid such as water and / or an organic solvent in which the dispersoid is substantially insoluble or has extremely low solubility.

[0082] The emulsion composition obtained as described above has excellent sedimentation stability. The sedimentation stability of the emulsion composition can be evaluated, for example, by the method described in the Examples below. For example, the sedimentation rate measured by the method described in the Examples below is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, particularly preferably 3% or less, and most preferably 2% or less.

[0083] From the viewpoint of sedimentation stability, the dispersed particle size of the dispersoid in the present emulsion composition is 10 μm or less, preferably 5 μm or less, more preferably 2.5 μm or less, and even more preferably 3.5 μm or less. The lower limit is usually about 0.01 μm. The dispersed particle size is the median size (d50) corresponding to 50% of the cumulative particle size distribution value on a volume basis, and can be measured, for example, by a laser diffraction particle size measuring device (e.g., model number LA-950V2, manufactured by Horiba, Ltd.).

[0084] The emulsion composition of the present invention is excellent in film-forming properties, tensile properties after film formation, and heat seal strength. The film-forming properties and the like can be evaluated by the methods described in the Examples below.

[0085] Films and the like obtained from the present emulsion composition have excellent tensile strength. Specifically, for example, the tensile strength (MPa) measured by the method described in the Examples below is 4 MPa or more, preferably 4.5 to 20 MPa, and even more preferably 5.5 to 15 MPa.

[0086] Molded articles such as films obtained from the emulsion composition have excellent heat seal strength, specifically, for example, a heat seal strength (N / 15 mm) measured by the method described in the Examples below of 2.5 N / 15 mm or more, preferably 2.7 N / 15 mm or more, and more preferably 3.0 to 5 N / 15 mm.

[0087] In addition, in conventional techniques, there is a tendency for strengths such as tensile strength to be weak after film formation, and for dispersed particles with a large diameter to have low sedimentation stability. However, the emulsion composition of the present invention is useful in that it has excellent sedimentation stability and excellent strengths such as tensile strength after film formation, even when the dispersed particle diameter is relatively large (for example, about 3.0 μm).

[0088] From the viewpoint of further improving the biodegradability of the present emulsion resin composition, it is preferable to use a biodegradable component as the dispersant (C), and among these, it is more preferable to use a PVA-based resin (C1) as the dispersant (C).

[0089] [Application] The present resin composition for emulsion or the present emulsion composition can be used in the form of a molded article (film or the like) obtained by a known molding method, although the form is not limited thereto. Furthermore, the present resin composition for emulsions or the present emulsion composition can be used, for example, as an adhesive, pressure sensitive adhesive, a modifier thereof, a coating agent, a heat sealing agent, a paint, a primer for paint, an ink, a binder, etc., in paper, a film, a sheet, a structural material, a building material, an automobile part, an electric / electronic product, a packaging material, clothing, a medicine, a cosmetic (shampoo, rinse, emulsion, lotion, perfume, etc.), an agricultural composition (pesticide emulsion, etc.), a health food, a food, etc. Among them, a cosmetic, an agricultural composition, a paint, an ink, or an adhesive containing the present resin composition for emulsions or the present emulsion composition is preferable. The present resin composition for emulsion or the present emulsion composition is also suitably used as a coating agent for an object to be coated (an object to be coated).

[0090] The object to be coated with the present resin composition for emulsion is not particularly limited, but is preferably, for example, a paper substrate, and examples of the paper substrate include thermal recording paper, release paper, peeling paper, inkjet paper, carbon paper, non-carbon paper, base paper for paper cups, greaseproof paper, paperboard such as Manila board, white board and liner, printing paper such as general fine paper, medium quality paper and gravure paper, high-grade, medium-grade and low-grade paper, newsprint, etc. For example, a laminate including a layer made of a paper substrate and a layer made of the resin composition for emulsion or the present emulsion composition coated on the paper substrate is also suitable.

[0091] The object to be coated with the resin composition for emulsions is not particularly limited, but is preferably, for example, a paper substrate, and examples of the paper substrate include thermal recording paper, release paper, peeling paper, inkjet paper, carbon paper, non-carbon paper, base paper for paper cups, greaseproof paper, paperboard such as Manila board, white board and liner, printing paper such as general fine paper, medium quality paper and gravure paper, high-grade, medium-grade and low-grade paper, newsprint, etc. For example, a laminate including a layer made of a paper substrate and a layer made of the resin composition for emulsions coated on the paper substrate is also suitable.

[0092] The object to be coated is preferably a plastic substrate, and examples of the plastic substrate include polyethylene terephthalate (PET) resin, polypropylene (PP) resin [biaxially oriented polypropylene (OPP), non-axially oriented polypropylene (CPP)], nylon resin, various biodegradable resins, polyethylene (PE) resin [low density polyethylene (LDPE), high density polyethylene (HDPE)], etc. For example, a laminate including a layer made of a plastic substrate and a layer made of a resin composition for emulsions coated on the plastic substrate is also suitable.

[0093] The coating method using the present resin composition for emulsion or the present emulsion composition is not particularly limited, and examples thereof include roll coating, dip coating, bar coating, nozzle coating, die coating, spray coating, spin coating, curtain coating, and flow coating. EXAMPLES

[0094] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are based on mass.

[0095] First, the following ingredients were prepared: Polybutylene succinate adipate (PBSA) [BiOPBS (FD92PM) manufactured by PTT MCC Biochem, melt flow rate (MFR) 4g / 10min (190℃, 2.16kg), melting point 84℃]

[0096] Cellulose nanofiber 1 [Dai-ichi Kogyo Seiyaku's "LeoCrysta I-2SX", hydrophilic CNF, average fiber diameter 3 nm, aqueous dispersion containing 2% CNF by mass] Cellulose nanofiber 2 [GS Alliance's "PBS / CNF composite," hydrophobic CNF, average fiber diameter 12 nm, CNF content 23% by mass]

[0097] Cellulose microfiber (CMF) [Rettenmaier Japan's "UFC-100", average fiber diameter 6μm]

[0098] ·PVA resin [Unmodified PVA resin, average degree of polymerization 1,700, degree of saponification 87-89%, 4% viscosity at 20°C 20.5-24.5 mPa s]

[0099] [Example 1] Polybutylene succinate adipate was continuously supplied from the hopper of a twin-screw extruder [model number KZW15TW-60MG, Technobel, L / D = 60], and then cellulose nanofiber 1, PVA resin as a dispersant, and water as a dispersion medium were continuously supplied from a supply port provided in the same extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) under conditions of a heating temperature (cylinder temperature) of 90 to 105°C and a heating time of 180 seconds, to obtain an emulsion composition having the mass ratio shown in Table 1.

[0100] [Example 2] Except for changing the amount of cellulose nanofiber 1, the same procedure as in Example 1 was carried out to obtain an emulsion composition having the mass ratio shown in Table 1.

[0101] [Example 3] Polybutylene succinate adipate and cellulose nanofibers 2 were continuously supplied from the hopper of a twin-screw extruder [model number KZW15TW-60MG, Technovel, L / D = 60], and then PVA-based resin as a dispersant and water as a dispersion medium were continuously supplied from a supply port provided in the same extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) under conditions of a heating temperature (cylinder temperature) of 90 to 105°C and a heating time of 180 seconds, to obtain an emulsion composition having the mass ratio shown in Table 1.

[0102] [Comparative Example 1] An emulsion composition having the mass ratio shown in Table 1 was obtained in the same manner as in Example 1, except that cellulose nanofiber 1 was not blended.

[0103] [Comparative Example 2] Except for changing the amount of cellulose nanofiber 1, the same procedure as in Example 1 was carried out to obtain an emulsion composition having the mass ratio shown in Table 1.

[0104] [Comparative Example 3] Polybutylene succinate adipate and cellulose microfibers were continuously fed from the hopper of a twin-screw extruder [product number KZW15TW-60MG, Technobel, L / D=60], and then, while continuously feeding PVA resin as a dispersant and water as a dispersion medium from a feed port provided on the same extruder, the mixture was continuously extruded (screw rotation speed: 300 rpm) under conditions of a heating temperature (cylinder temperature) of 90 to 105°C and a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1.

[0105] [Dispersed particle size measurement test] The dispersed particle diameters (median diameters) of the emulsion compositions according to the Examples and Comparative Examples were measured using a laser diffraction particle diameter measuring device (LA-950V2, manufactured by Horiba, Ltd.). The results are shown in Table 1.

[0106] [Settling stability test (settling rate)] The emulsion compositions of the Examples and Comparative Examples were placed in a settling tube (bottom area 9.62 cm 2 The sedimentation rate was calculated based on the reading of the scale on the sedimentation tube (height of the separated layer). The sedimentation rate was calculated based on the following formula. The results are shown in Table 1. [Formula] Sedimentation rate = height of separated layer (cm) / height of total emulsion composition (cm) x 100

[0107] [Film-forming property evaluation] The emulsion compositions of the Examples and Comparative Examples were applied to a PET film substrate using a bar coater to a thickness of 5 μm, and then dried at 105° C., after which the film-forming properties were evaluated according to the following criteria. The results are shown in Table 1. 〇... Films can be formed with uniform thickness. △ Film formation is possible, but the thickness is non-uniform. × High viscosity, film formation not possible.

[0108] [Tensile elongation test, tensile strength test] [Tensile strength measurement test] Tensile elongation tests and tensile strength tests were performed according to JIS K7161. Specifically, the emulsion compositions according to the examples and comparative examples were first applied onto a Teflon (registered trademark) sheet and heated at 105°C for 5 minutes to prepare test films. The tensile elongation (%) and tensile strength (MPa) of the obtained test films were measured using a tensile tester (Shimadzu Corporation, Autograph AG-IS) under the following test conditions. The results are shown in Table 1. [Test conditions] Test speed: 100mm / min Distance between gauge lines 15mm

[0109] [Heat seal strength test] Each emulsion composition adjusted to a solid content of 30% was applied at 5 g / m2 onto a paper substrate. 2 The two test films were then coated with a coating solution of 1.25 kgf / cm and dried at 105°C to prepare test films. 2 The coated surfaces were attached to each other for 2 x 2 seconds at a heat seal temperature of 140°C to obtain a test piece. The test piece was opened 180 degrees so that the heat seal was in the center and the heat seal strength was measured using a tensile tester (Shimadzu Autograph AG-IS) under the following test conditions. The results are shown in Table 1. [Test conditions] Test speed: 300mm / min Distance between gauge lines 15mm

[0110] [Table 1]

[0111] As shown in Table 1, the emulsion compositions of Examples 1 to 3, which have a cellulose nanofiber (B) content within the range specified in the present invention, were excellent in sedimentation stability and film-forming properties. Furthermore, the tensile strength, tensile elongation, and heat seal strength after film formation were also excellent. On the other hand, Comparative Example 1, which did not contain cellulose nanofibers (B), had poor sedimentation stability. Furthermore, Comparative Example 1 was inferior to the Examples in tensile elongation, tensile strength, and heat seal strength after film formation. In Comparative Example 2, in which the content of cellulose nanofibers (B) exceeded the range specified in the present invention, it was not possible to form a film, and in the case of Comparative Example 3, in which cellulose microfibers were used instead of cellulose nanofibers (B), the sedimentation stability and film-forming properties were inferior to those of the Examples. Furthermore, Comparative Example 3 was inferior to the Examples in tensile elongation, tensile strength, and heat seal strength after film formation.

[0112] From the above, it was confirmed that the present invention can provide an emulsion composition and the like which is excellent in sedimentation stability and film-forming properties, as well as in tensile properties and heat seal strength after film formation. [Industrial Applicability]

[0113] The resin composition for emulsions and the emulsion composition of the present invention are particularly useful as various coating agents, for example, as coating agents for paper substrates, coating agents for plastic substrates, and the like.

Claims

1. The resin composition for emulsion contains an aliphatic polyester-based resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polycarboxylic acid unit as main constituent units, and a cellulose nanofiber (B), wherein the content of the cellulose nanofiber (B) is less than 2 parts by mass per 100 parts by mass of the aliphatic polyester-based resin (A).

2. The resin composition for emulsion according to claim 1, wherein the cellulose nanofibers (B) have an average fiber diameter of 1 to 1000 nm.

3. The resin composition for emulsion according to claim 1 or 2, wherein the cellulose nanofiber (B) is a hydrophilic cellulose nanofiber (b1).

4. 3. The resin composition for emulsion according to claim 1, wherein the aliphatic polyester resin (A) has a melt flow rate of less than 80 g / 10 min at 190° C. and 2.16 kg.

5. The resin composition for emulsion according to claim 1 or 2, further comprising a polyvinyl alcohol-based resin.

6. An emulsion composition comprising the resin composition for emulsions according to claim 1 or 2.

7. 7. The emulsion composition according to claim 6, wherein the dispersed particle size is 10 μm or less.

8. A coating agent comprising the resin composition for emulsion according to claim 1 or 2.

9. The coating agent according to claim 8, wherein the substrate to be coated is a paper substrate.

10. 9. The coating agent according to claim 8, wherein the object to be coated is a plastic substrate.

11. A molded article obtained by using the resin composition for emulsion according to claim 1 or 2.

12. A film obtained by using the resin composition for emulsions according to claim 1 or 2.

13. A cosmetic comprising the resin composition for emulsions according to claim 1 or 2.

14. 3. An agricultural composition comprising the resin composition for emulsions according to claim 1 or 2.

15. A paint comprising the resin composition for emulsions according to claim 1 or 2.

16. 3. An ink comprising the resin composition for emulsions according to claim 1 or 2.

17. A pressure-sensitive adhesive comprising the resin composition for emulsions according to claim 1 or 2.

Citation Information

Patent Citations

  • Biodegradable water dispersion