Magnetic material, magnet, and magnetic powder
A hexagonal crystal structured magnetic material with balanced A and B elements in specific phases enhances coercive force and saturation magnetization, addressing existing magnetic material limitations and offering cost-effective production.
Patent Information
- Application Number
- JP2023050356
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing magnetic materials face challenges in achieving high saturation magnetization and coercive force, with compositions that are either too low in A elements leading to reduced saturation or too high, causing soft magnetism precipitation and decreased coercive force.
A magnetic material with a hexagonal crystal structure comprising elements A (Fe, Co, Ni, Cu, Zn, Ti, Al) and B (P, Si, S, B, N) is developed, with a first phase containing Fe and P, and a second phase having a lower M element content than the first phase, ensuring a specific atomic ratio balance to enhance coercive force.
The solution results in improved magnetic properties, particularly increased coercive force, while maintaining high saturation magnetization, and allows for cost-effective production with lower raw material costs compared to rare earth magnets.
Smart Images

Figure 2024139422000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a magnetic body, a magnet, and a magnetic powder. [Background technology]
[0002] Patent Document 1 describes an invention relating to a fine powder magnet of Fe-PB system.
[0003] Patent Document 2 describes an invention relating to ferromagnetic ultrafine particles containing Fe, Co and P.
[0004] Non-Patent Document 1 describes the use of (Fe,Co)2(P,Si) single crystals as a permanent magnet material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 58-84955 [Patent Document 2] Japanese Patent Application Publication No. 2-180003 [Non-patent literature]
[0006] [Non-Patent Document 1] H.Yibole, B.Lingling-Bao, JYXu, H.Alata, O.Tegus, W.Hanggai, NHvan Dijk, E.Brueck, F. Guillou, Acta Materialia, 221,(2021)117388 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a magnetic material having high saturation magnetization and coercive force. [Means for solving the problem]
[0008] In order to achieve the above object, the magnetic material of the present invention is a magnetic material having a hexagonal crystal structure containing an element A and an element B, The A element is one or more selected from Fe, Co, Ni, Cu, Zn, Ti, and Al, and the B element is one or more selected from P, Si, S, B, C, and N, The magnetic body has a first phase and a second phase, the first phase has the crystal structure; the first phase contains at least Fe and P; The total content ratio of the A element in the first phase based on the number of atoms is C A1 The total content of the B element in the first phase is C B1 As, 1.50≦C A1 / C B1 < 4.00, Fe, Co and Ni are defined as M elements, and the total content of M elements in the first phase is C M1 The total content of the M element in the second phase is C M2 As, {C M2 / (1-C M2 )}<{C M1 / (1-C M1 )}.
[0009] The area ratio of the second phase in a cross section of the magnetic body may be 5% or more and 30% or less.
[0010] The second phase may contain one or more elements selected from Y, La, Ce, Pr, Nd and Sm.
[0011] At least a portion of the second phase may have a total content of Al, Mg and Sn exceeding 50 atomic %.
[0012] The second phase may contain an A element.
[0013] The magnet of the present invention includes the above magnetic material.
[0014] The magnetic powder of the present invention contains the above-mentioned magnetic material. [Brief description of the drawings]
[0015] [Figure 1] 1 is a SEM image of Example 1. [Diagram 2] 1 is an SEM image of Comparative Example 5. [Diagram 3] 1 is an element mapping image of Example 1. [Figure 4] 13 is an element mapping image of Comparative Example 5. [Diagram 5] 1 is a SEM image of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the present invention will be described based on the embodiments shown in the drawings.
[0017] The magnetic body according to this embodiment has a hexagonal crystal structure containing an element A and an element B. The element A is one or more selected from Fe, Co, Ni, Cu, Zn, Ti, and Al, and the element B is one or more selected from P, Si, S, B, C, and N.
[0018] The hexagonal crystal structure is in the space group P62m.
[0019] The hexagonal crystal structure may contain at least Fe as the A element, and may contain at least P as the B element.
[0020] The hexagonal crystal structure may contain at least Fe and Co as the element A. The hexagonal crystal structure of the first phase 11 may contain at least P and Si as the element B.
[0021] The composition of the hexagonal crystal structure is (Fe 1-x Co x ) m (P 1-y S y) may satisfy 0≦x≦0.9, may satisfy 0≦y≦0.6, and may satisfy 1.9≦m≦2.0.
[0022] As shown in Fig. 1, the magnetic body 1 according to this embodiment has a first phase 11 and a second phase 12. Note that Fig. 1 is an SEM image of Example 1, which will be described later.
[0023] As shown in FIG. 1, the second phase 12 may exist between a plurality of first phases 11 .
[0024] The first phase 11 has the above-mentioned hexagonal crystal structure. The first phase 11 contains at least Fe and P. There is no particular limitation on the method for confirming that the first phase 11 has the above-mentioned hexagonal crystal structure. For example, it can be confirmed using a transmission electron microscope (TEM).
[0025] The total content of A elements in the first phase 11 based on the atomic number is C A1 , the total content of B element in the first phase 11 is C B1 As, 1.50≦C A1 / C B1 <4.00.
[0026] C A1 / C B1 If C is too small, that is, if the amount of the element A contained in the first phase 11 is too small, the saturation magnetization of the magnetic body 1 becomes small, and the saturation magnetic flux density of a magnet including the magnetic body 1 becomes small. A1 / C B1 If is too large, that is, if the first phase 11 contains too much element A, a component having soft magnetism, for example, a simple substance of element A such as α-Fe, tends to precipitate. As a result, the coercive force of the magnetic body 1 becomes small, and the coercive force of a magnet including the magnetic body 1 also becomes small.
[0027] If the first phase 11 does not contain Fe, the saturation magnetization and coercivity of the magnetic body will be small, and the saturation magnetic flux density and coercivity of a magnet including the magnetic body will be small. If the first phase 11 does not contain P, the coercivity of the magnetic body will be small, and the coercivity of a magnet including the magnetic body will be small.
[0028] Fe, Co, and Ni are defined as M elements. Fe, Co, and Ni are elements that are relatively likely to have ferromagnetism among A elements. The total content ratio of M elements in the first phase 11 based on the atomic number is defined as C M1 , the total content of M elements in the second phase 12 is C M2 As, {C M2 / (1-C M2 )}<{C M1 / (1-C M1 )}.
[0029] That is, the second phase 12 has a lower content of the M element compared to the first phase 11. Therefore, the second phase 12 is less likely to have ferromagnetism than the first phase 11. This ensures a sufficient magnetic decoupling effect of the second phase 12, and improves the magnetic properties, particularly the coercive force.
[0030] {C M1 / (1-C M1 )} is not particularly limited. For example, it may be 1.50 or more and less than 4.00. M2 / (1-C M2 )} is not particularly limited, and may be, for example, 1.00 or more and less than 2.50.
[0031] {C M1 / (1-C M1 )}-{C M2 / (1-C M2 )}≧0.01.
[0032] As shown in Fig. 2, the coercive force is likely to decrease when the magnetic body 2 does not have the second phase 12. Note that Fig. 2 is an SEM image of Comparative Example 5, which will be described later.
[0033] There is no particular restriction on the content of the second phase 12 in the magnetic body 1. For example, the area ratio of the second phase 12 in the cross section of the magnetic body 1 may be 5% or more and 30% or less.
[0034] If the area ratio of the second phase 12 is too small, the magnetic separation effect is not fully exerted. As a result, the coercive force decreases. If the area ratio of the second phase 12 is too large, it is difficult to effectively utilize the magnetization of the first phase 11. As a result, the saturation magnetization of the magnetic material decreases, and the saturation magnetic flux density of a magnet including the magnetic material decreases.
[0035] There is no particular limitation on the composition of the second phase 12. The second phase 12 may contain either the A element or the B element.
[0036] The second phase 12 may contain one or more elements selected from Y, La, Ce, Pr, Nd, and Sm, and may contain Ce. Hereinafter, Y, La, Ce, Pr, Nd, and Sm may be referred to as R elements. When the second phase 12 contains an R element, the second phase 12 tends to become nonmagnetic. As a result, the magnetic separation effect of the second phase 12 becomes stronger, and the magnetic properties, particularly the coercive force, tend to be improved.
[0037] There is no particular limitation on the content of the R element in the second phase 12. For example, the total content of the R element in the second phase 12 may be 1 atomic % or more and 30 atomic % or less.
[0038] The second phase 12 may contain one or more selected from Al, Mg, and Sn. In addition, the total content of Al, Mg, and Sn in at least a part of the second phase 12 may be more than 50 atomic % or may be 80 atomic % or more.
[0039] Al, Mg, and Sn are metal elements with relatively low melting points. The second phase 12 containing a large amount of these elements can cover the periphery of the first phase 11 at a low temperature. As a result, the magnetic separation effect of the second phase is more efficiently exerted, and the coercive force is more easily improved.
[0040] There is no particular limitation on the content of the second phase 12 in which the total content of Al, Mg, and Sn exceeds 50 atomic %. For example, the area ratio of the second phase 12 in which the total content of Al, Mg, and Sn exceeds 50 atomic % in the cross section of the magnetic body 1 may be 3% or more and 30% or less.
[0041] The magnetic substance according to the present embodiment may be contained in a magnet or in a magnetic powder. There are no particular limitations on the shape of the magnetic substance, the shape of the magnet, or the shape of the magnetic powder.
[0042] Hereinafter, a method for observing the magnetic body 1 according to this embodiment will be described.
[0043] First, the magnetic body 1 is cut to obtain a cross section. There is no particular limitation on the position of the cross section. Furthermore, the cross section may be surface-treated as necessary. For example, it may be mirror-polished.
[0044] Next, the cross section is observed using SEM-EDS. As shown in Fig. 1, the first phase 11 and the second phase 12 have different brightness, so that the first phase 11 and the second phase 12 can be distinguished from each other. There are no particular limitations on the size and magnification of the observation range, and it is sufficient to select a size and magnification that allows the composition, area ratio, etc. of each phase to be appropriately observed.
[0045] Furthermore, composition analysis by EDS may be used in combination as necessary to distinguish between the first phase 11 and the second phase 12. Fig. 3 is a mapping image in which an Fe mapping image, a P mapping image, a Ce mapping image, and an electron beam image (SEM image) obtained by SEM are superimposed, the Fe mapping image and the Ce mapping image being created by performing composition analysis by EDS in an observation range equivalent to that of Fig. 1. Fig. 4 is a mapping image in which an Fe mapping image and a P mapping image being superimposed, the Fe mapping image and the Ce mapping image being created by performing composition analysis by EDS in an observation range near that of Fig. 2.
[0046] 1 and 3 show that the first phase 11 contains a lot of Fe and P, and the second phase 12 contains a lot of Ce in the magnetic body 1. FIG. 2 and 4 show that the magnetic body 2 contains only the first phase 11 containing a lot of Fe and P.
[0047] In addition, the magnetic body may contain multiple types of second phases that differ from each other in composition, etc. Even in such cases, the multiple types of second phases can be distinguished by appropriately performing the difference in brightness of SEM images, composition analysis by EDS, etc.
[0048] Furthermore, when the magnetic substance is a magnetic powder, a green compact may be produced from the magnetic powder, and a cross section of the green compact may be observed using SEM-EDS.
[0049] The method for measuring the content of each element in each phase will be described below.
[0050] First, an observation image large enough to measure the content ratio of each element is set and observed using SEM-EDS. Then, at least two measurement points, preferably five or more measurement points, are set for each phase. Then, the content ratio of each element at each measurement point is measured by point analysis of EDS. The content ratio of each element in each phase is calculated by averaging the content ratio of each element at each measurement point.
[0051] Figure 5 shows an enlarged SEM image of a part of Figure 1. For example, as shown in Figure 5, measurement points #1 and #2 are set for measuring the composition of the first phase 11, and measurement points #3 and #4 are set for measuring the composition of the second phase 12.
[0052] C in magnetic material 1 A1 / C B1 , {C M2 / (1-C M2 )}, {C M1 / (1-C M1 )} are calculated appropriately using the content ratio of each element in each phase.
[0053] When the magnetic body 1 contains a plurality of types of second phases 12, the total content ratio of the M element in each type of second phase 12 is calculated. Then, the total content ratio of the M element in each type of second phase 12 is weighted and averaged by the area ratio of each type of second phase 12 to obtain CM2 Then, {C M2 / (1-C M2 )}.
[0054] The method for producing the magnetic body according to this embodiment will be described in detail below, but the method for producing the magnetic body is not limited to this, and other known methods may be used.
[0055] (Method 1) First, the composition of the raw material (raw material 1) that mainly constitutes the first phase, and the composition of the raw material (raw material 2) that mainly constitutes the second phase are set. When producing a magnetic body having multiple types of second phases, the composition of each raw material 2 is set according to the composition of each target second phase. Furthermore, the mixing ratio of raw material 1 and raw material 2 is set. The content ratio of the second phase in the finally obtained magnetic body tends to increase as the proportion of raw material 2 is increased.
[0056] Each of the prepared raw materials is weighed so as to obtain a mixture composition obtained by mixing raw materials 1 and 2 having the composition set by the above-mentioned method at the mixing ratio set by the above-mentioned method. Specifically, each raw material is appropriately prepared as a single element of each element, a compound containing each element, and / or an alloy containing each element. There is no particular restriction on the shape of each raw material. For example, it may be in a powder shape.
[0057] Next, the weighed raw materials are mixed. There are no particular limitations on the specific mixing method.
[0058] Next, a ribbon is obtained from the mixed raw materials by the melt spun method. Specifically, first, the mixed raw materials are heated and melted to obtain a molten metal. There is no particular limit to the specific melting method. For example, the mixed raw materials may be placed in a quartz tube nozzle and heated by high-frequency heating. There is also no particular limit to the atmosphere during melting. For example, an inert atmosphere such as an Ar atmosphere may be used, but an active atmosphere such as air may be used from the viewpoint of reducing manufacturing costs.
[0059] Next, the molten metal is injected onto a cooling roll to obtain a ribbon. There is no particular limitation on the material of the cooling roll. For example, the cooling roll may be made of copper or molybdenum. There is no particular limitation on the rotation speed of the cooling roll. For example, it may be 1000 rpm or more and 5000 rpm or less.
[0060] When the cross section of the obtained ribbon was observed by SEM-EDS, it was confirmed that the ribbon was a magnetic material having a first phase and a second phase, and it was confirmed that the obtained ribbon was the magnetic material according to this embodiment.
[0061] There is no particular limitation on the method for obtaining the magnetic powder having the magnetic material according to the present embodiment. For example, the ribbon may be pulverized. There is also no particular limitation on the method for pulverizing the ribbon. For example, the ribbon is pulverized by a rod mill or a stamp mill.
[0062] There is no particular limit to the particle size of the powder particles contained in the magnetic powder. For example, the average particle size may be 0.5 μm or more and 10 μm or less. In addition, the particle size of 99% or more of the powder particles contained in the magnetic powder may be 50 nm or more, or all of the powder particles contained in the magnetic powder may be 50 nm or more. Note that one powder particle usually contains multiple crystals having a hexagonal crystal structure containing elements A and B. Therefore, the particle size of the powder particle is different from the crystal grain size of the crystal.
[0063] There is no particular limit to the method for obtaining a magnet having the magnetic body according to this embodiment. For example, a ribbon is pulverized, the resulting magnetic powder is placed in a mold, pressurized to obtain a compact, and then sintered to obtain a sintered body (sintered magnet). There is no particular limit to the pressure applied when applying pressure. For example, it may be 20 MPa or more and 200 MPa or less. There is no particular limit to the sintering temperature and sintering time. For example, the sintering temperature may be 600°C or more and 1200°C or less, and the sintering time may be 0.2 hours or more and 24 hours or less. There is no particular limit to the atmosphere during sintering. For example, an inert atmosphere such as an Ar atmosphere may be used, but from the viewpoint of reducing manufacturing costs, an active atmosphere such as air may be used.
[0064] Moreover, a bonded magnet can be obtained by mixing magnetic powder and resin and then pressing the mixture.
[0065] The above-mentioned compact can be pulverized to obtain a magnetic powder having the magnetic body according to the present embodiment.The above-mentioned sintered body (sintered magnet) can be pulverized to obtain a magnetic powder having the magnetic body according to the present embodiment.
[0066] (Method 2) Hereinafter, a method for producing a magnetic material different from method 1 will be described. In particular, a method for producing a magnetic material having a second phase in which the total content of Al, Mg, and Sn exceeds 50 atomic % will be described. Unless otherwise specified, the method is the same as method 1.
[0067] First, the composition of the raw material (raw material 1) that mainly constitutes the first phase and the composition of the raw material (raw material 2) that mainly constitutes the second phase are set. Furthermore, the mixing ratio of raw material 1 and raw material 2 is set.
[0068] Unlike method 1, at this stage, the raw material 2 constituting the second phase, which mainly contains Al, Mg, and Sn in a total content ratio exceeding 50 atomic %, is not mixed with the raw material 1. If there are other raw materials 2 constituting the second phase, they are mixed with the raw material 1 in the same manner as method 1.
[0069] The subsequent steps up to crushing the ribbon to obtain powder are the same as those in Method 1.
[0070] Next, an alloy powder having a composition of raw material 2 constituting the second phase, in which the total content ratio of mainly Al, Mg and Sn exceeds 50 atomic %, is prepared separately. The alloy powder is an alloy powder that melts at about 1000°C. There is no particular limit to the method for preparing the alloy powder. There is no particular limit to the particle size of the alloy powder, but it may be the same as the particle size of the powder obtained by pulverizing the ribbon.
[0071] Next, the powder obtained by pulverizing the ribbon is mixed with the alloy powder in the above-mentioned mixing ratio. The mixed powder is then placed in a mold and pressed to obtain a compact, which is then sintered. When the cross section of the obtained sintered body (sintered magnet) is observed with SEM-EDS, it can be confirmed that the sintered body (sintered magnet) is a magnetic body having a first phase 11 and a second phase 12, and that it is the magnetic body according to this embodiment. It can also be confirmed that the second phase 12 contains more than 50 atomic % of Al, Mg, and Sn in total.
[0072] There is no particular limit to the pressure during pressing. For example, it may be 20 MPa or more and 200 MPa or less. There is also no particular limit to the sintering temperature and sintering time. For example, the sintering temperature may be 600°C or more and 1200°C or less, and the sintering time may be 0.2 hours or more and 24 hours or less. There is also no particular limit to the atmosphere during sintering. For example, an inert atmosphere such as an Ar atmosphere may be used, but an active atmosphere such as air may be used from the viewpoint of reducing manufacturing costs.
[0073] The above sintered body (sintered magnet) is a magnet having the magnetic body according to this embodiment. Moreover, in order to obtain a magnetic powder having the magnetic body according to this embodiment, the sintered body (sintered magnet) may be pulverized. There is no particular limitation on the pulverization method. Moreover, it is also possible to manufacture a bonded magnet by mixing the magnetic powder obtained by pulverizing the sintered body (sintered magnet) with a resin and applying pressure.
[0074] There are no particular limitations on the applications of the magnetic materials, magnets, etc. according to this embodiment. The magnet according to this embodiment has higher magnetic properties than a ferrite magnet. The magnet according to this embodiment uses cheaper raw materials than a rare earth magnet, so the raw material costs tend to be lower. Furthermore, the magnet according to this embodiment is easier to increase the oxygen concentration in the atmosphere during production compared to a rare earth magnet, so the production costs tend to be lower. Furthermore, the magnet according to this embodiment also has high corrosion resistance.
[0075] The magnetic body, magnet, etc. according to this embodiment have the above-mentioned characteristics and are therefore suitable for use in, for example, motors, generators, and actuators. EXAMPLES
[0076] The present invention will be described below with reference to more detailed examples, but the present invention is not limited to these examples.
[0077] (Experimental Example 1: Examples 1 to 18, Comparative Examples 1 to 7) (Sample preparation) Raw material 1 having the composition shown in Table 1 and raw material 2-1 having the composition shown in Table 2 were mixed in the mixing ratio shown in Table 4 to obtain a ribbon having the same composition as the mixture obtained, and the raw materials in powder form were weighed and mixed to obtain a mixed powder. Specifically, the raw materials in powder form were appropriately prepared as simple substances of each element shown in Tables 1 and 2, compounds containing each element, and / or alloys containing each element.
[0078] In Experimental Example 1, raw material 2-1 was P2-3 (simple Ce), and the composition of raw material 1 was changed, and the mixing ratio of raw material 1 and raw material 2-1 was changed.
[0079] [Table 1]
[0080] [Table 2]
[0081] [Table 3]
[0082] [Table 4]
[0083] Next, a ribbon was obtained from the mixed powder by melt-spun. Specifically, the mixed powder was first placed in a quartz nozzle for melting and heated to melt. Next, when the mixed powder was entirely melted to form a molten metal, the molten metal was injected onto a cooling roll rotating at 3000 rpm to obtain a ribbon. A copper cooling roll was used.
[0084] Next, the ribbon was pulverized to obtain a powder of magnetic material. A bead mill was used for pulverization. The average particle size of the magnetic material was about 0.6 μm, with a minimum value of 50 nm or more.
[0085] Next, a bulk magnet (sintered magnet) was produced from the powdered magnetic material. Specifically, the powdered magnetic material was first placed in a mold and pressed at 100 MPa to obtain a compact. The compact was then sintered by heating at 1000°C for 1 hour in an Ar atmosphere to produce a bulk magnet.
[0086] Next, the bulk magnet was pulverized in the same manner as the ribbon was pulverized to obtain magnetic powder again. The particle size of the magnetic material was set to be about 0.6 μm on average and 50 nm or more at minimum.
[0087] (Magnetic properties) The magnetic properties of the magnetic material obtained by crushing the bulk magnet were evaluated using a vibrating magnetometer (VSM). Specifically, an external magnetic field of ±1600kA / m was applied to the magnetic material, and the magnetization of the magnetic material was measured. The saturation magnetization σs was defined as the magnetization of the magnetic material when an external magnetic field of +1600kA / m was applied. The coercive force Hc was defined as the absolute value of the negative external magnetic field required to make the magnetization 0. The results are shown in Table 7.
[0088] σs is 70.0 A m 2 / kg or more is good, 60.0A·m 2 / kg or more 70.0A m 2 / kg or less, 60.0A·m 2 / kg was not acceptable.
[0089] Hc was rated as "good" when it was 40.0 kA / m or more, "acceptable" when it was 35.0 kA / m or more and less than 40.0 kA / m, and "unacceptable" when it was less than 35.0 kA / m.
[0090] The saturation magnetic flux density Js of the bulk magnet before pulverization was measured under the same conditions as the saturation magnetization σs of the powdered magnetic material, except that a BH tracer was used. The coercive force HcJ of the bulk magnet before pulverization was measured under the same conditions as the Hc of the powdered magnetic material, except that a BH tracer was used. The results are shown in Table 7.
[0091] Js was rated as good if it was 590mT or higher, acceptable if it was 580mT or higher and less than 590mT, and unacceptable if it was less than 580mT.
[0092] HcJ was rated as good when it was 50.0 kA / m or more, as acceptable when it was 35.0 kA / m or more and less than 50.0 kA / m, and as unacceptable when it was less than 35.0 kA / m.
[0093] (Microstructure, composition of each phase) The identification of each phase was performed by mirror-polishing the cross section of each bulk magnet sample and observing it with SEM-EDS. The first and second phases were identified by element mapping using EDS. The area ratio of the second phase was also calculated by image analysis.
[0094] In addition, point analysis was performed at a sufficient number of measurement points for each of the identified first and second phases. The compositions of the first and second phases in each sample were calculated by averaging the compositions of each measurement point obtained by point analysis. The results are shown in Tables 5 to 7.
[0095] [Table 5]
[0096] [Table 6]
[0097] [Table 7]
[0098] Examples 1 to 18, which have the specified microstructure and composition of each phase, have good magnetic properties. A1 / C B1 In Comparative Example 1, where C was too small, σs decreased. A1 / C B1 In Comparative Example 2, in which the σ was too large, Hc was reduced. In Comparative Example 5, in which the second phase was not included, Hc was reduced. In Comparative Example 6, in which the first phase did not include Fe, σs and Hc were reduced. A1 / C B1 In Comparative Example 7, where Hc was too large, Hc decreased.
[0099] The observation results for Example 1 and Comparative Example 5 above are shown below.
[0100] Fig. 1 shows an SEM image of magnetic body 1 (bulk magnet) of Example 1, Fig. 2 shows an SEM image of magnetic body 2 (bulk magnet) of Comparative Example 5, Fig. 3 shows an element mapping image of magnetic body 1 of Example 1, and Fig. 4 shows an element mapping image of magnetic body 2 of Comparative Example 5. Magnetic body 1 shown in Fig. 1 has a first phase 11 and a second phase 12. In contrast, magnetic body 2 shown in Fig. 2 has only the first phase 11.
[0101] The black parts in Figure 1 are the parts outside the range of magnetic body 1. When setting the observation range of magnetic body 1, the observation range was set to the edge part of the magnetic body, so the parts outside the range of the magnetic body are also included in the SEM image.
[0102] The black portions in FIG. 2 are voids present between the first phases 11.
[0103] Figure 5 is an enlarged SEM image of a part of Figure 1. It shows the positions of #1 and #2, which are some of the measurement points for the composition of the first phase, and #3 and #4, which are some of the measurement points for the composition of the second phase. Measurement points for the composition of each phase were set as shown in Figure 5, and the composition at each measurement point was measured.
[0104] (Experimental Example 2: Examples 19 to 28, Examples 33 to 34) A mixed powder was obtained by weighing and mixing the powder-shaped raw materials so as to obtain a ribbon having the same composition as the mixture obtained by mixing raw material 1 having the composition shown in Table 1, raw material 2-1 having the composition shown in Table 2, and raw material 2-2 having the composition shown in Table 2 in the mixing ratio shown in Table 8. The following was carried out under the same conditions as in Experimental Example 1.
[0105] In Experimental Example 2 and Experimental Example 3 described later, Raw Material 1 was P1-1 (Fe 0.60 Co 0.05 P 0.25 S 0.10 (atomic ratio), and the composition and mixing ratio of raw material 2 were changed. As the composition of raw material 1, which has a large effect on the composition of the first phase that mainly produces magnetization, was fixed, the evaluation criteria for the magnetic properties were subdivided from those in Experimental Example 1. The results are shown in Tables 9 to 13.
[0106] σs is 85.0 A m 2 / kg or more is A, 80.0A·m 2 / kg or more 85.0A m 2 / kg is less than B, 75.0A·m 2 / kg or more 80.0A m 2 / kg, C, 70.0A·m 2 / kg or more 75.0A m 2 / kg is less than D, 60.0A·m 2 / kg or more 70.0A m 2 / kg or less, E, 60.0A·m 2 / kg is shown in the table as F. The order of evaluation is A, B, C, D, E, and F, with A to E being rated as good.
[0107] Hc is shown in the table as A if it is 55.0kA / m or more, B if it is 45.0kA / m or more but less than 55.0kA / m, C if it is 40.0kA / m or more but less than 45.0kA / m, D if it is 35.0kA / m or more but less than 40.0kA / m, and E if it is less than 35.0kA / m. The order of evaluation is A, B, C, D, E, with A to D being good.
[0108] Js is shown in the table as A if it is 620mT or more, B if it is 600mT or more and less than 620mT, C if it is 590mT or more and less than 600mT, D if it is 580mT or more and less than 590mT, and E if it is less than 580mT. A is the best rating, followed by B, C, D, and E, with A to D being considered good.
[0109] HcJ is shown in the table as A for 55.0 kA / m or more, B for 50.0 kA / m or more but less than 55.0 kA / m, C for 40.0 kA / m or more but less than 50.0 kA / m, D for 35.0 kA / m or more but less than 40.0 kA / m, and E for less than 35.0 kA / m. The order of evaluation is A, B, C, D, E, with A to D being good.
[0110] (Experimental Example 3: Examples 29 to 32, 35 to 42) First, raw material 1 having the composition shown in Table 1, raw material 2-1 having the composition shown in Table 2, and raw material 2-2 having the composition shown in Table 2 were mixed in the mixing ratio shown in Table 8, and the powder-shaped raw materials were weighed and mixed to obtain a mixed powder so as to obtain a ribbon having the same composition as the mixture obtained by mixing the raw material 1 having the composition shown in Table 1, raw material 2-1 having the composition shown in Table 2, and raw material 2-2 having the composition shown in Table 2.
[0111] As in Experimental Example 1, ribbons were obtained from the mixed powder and pulverized to obtain a powder-shaped magnetic material.
[0112] Next, an alloy powder of raw material 2-3 having the composition shown in Table 3 was prepared. The particle size of the alloy powder was set to be equal to the particle size of the powdered magnetic material. Then, the powdered magnetic material and the alloy powder of raw material 2-3 having the composition shown in Table 3 were mixed in the mixing ratio shown in Table 8.
[0113] For example, in Example 39, the powdered magnetic material was composed of raw materials 1-1, 2-1, and 2-2 mixed at a mass ratio of raw material 1-1: raw material 2-1: raw material 2-2 = 92: 3: 2. The powdered magnetic material was mixed with alloy powder of raw material 2-3 at a mass ratio of powdered magnetic material: raw material 2-3 = 97: 3.
[0114] Below, bulk magnets were produced in the same manner as in Experimental Examples 1 and 2. Furthermore, the bulk magnets were pulverized in the same manner as the ribbons were pulverized to obtain magnetic powder. The magnetic properties of the magnetic powder obtained by pulverizing the bulk magnets were then evaluated using the same method and evaluation criteria as in Experimental Example 2. Furthermore, the magnetic properties of the bulk magnets before pulverization were evaluated using the same method as in Experimental Example 2. The results are shown in Tables 9 to 13.
[0115] The observation of the microstructure and the identification of each phase were carried out for each bulk magnet sample by mirror-polishing the cross section and observing it with SEM-EDS. The results are shown in Tables 9 to 13.
[0116] [Table 8]
[0117] [Table 9]
[0118] [Table 10]
[0119] [Table 11]
[0120] [Table 12]
[0121] [Table 13]
[0122] Examples 19 to 42, which had the prescribed microstructure and composition of each phase, had good magnetic properties. [Explanation of symbols]
[0123] 1...Magnetic body (having a first phase and a second phase) 2...Magnetic material (having only the first phase) 11…Phase 1 12...Phase 2
Claims
1. A magnetic material having a hexagonal crystal structure containing elements A and B, The A element is at least one selected from Fe, Co, Ni, Cu, Zn, Ti, and Al, and the B element is at least one selected from P, Si, S, B, C, and N, The magnetic body has a first phase and a second phase, the first phase has the crystal structure; the first phase includes at least Fe and P; The total content ratio of the A element in the first phase based on the number of atoms is C A1 The total content ratio of the B element in the first phase is C B1 As, 1.50≦C A1 / C B1 < 4.00, Fe, Co and Ni are M elements, and the total content ratio of M elements in the first phase based on the atomic number is C M1 The total content ratio of the M element in the second phase is C M2 As, {C M2 / (1-C M2 )}<{C M1 / (1-C M1 )) a magnetic material.
2. 2. The magnetic body according to claim 1, wherein the area ratio of the second phase in a cross section of the magnetic body is 5% or more and 30% or less.
3. 3. The magnetic body according to claim 1, wherein the second phase contains at least one element selected from the group consisting of Y, La, Ce, Pr, Nd and Sm.
4. 3. The magnetic body according to claim 1, wherein the total content of Al, Mg and Sn in at least a portion of the second phase exceeds 50 atomic %.
5. The magnetic body according to claim 1 or 2, wherein the second phase contains an A element.
6. A magnet comprising the magnetic material according to claim 1 or 2.
7. A magnetic powder comprising the magnetic material according to claim 1 or 2.
Citation Information
Patent Citations
Permanent magnet
JP1983084955A
Ferromagnetic ultrafine particle and manufacture thereof, and magnetic recording medium and thermo magnetic recording medium
JP1990180003A