Water-based coating composition and corrosion prevention coating method
The aqueous coating composition, with a specific formulation of water-dispersible epoxy resin, amine curing agent, and scaly pigments, addresses cracking issues in water-based paints by minimizing drying property differences, ensuring a crack-resistant film at bolt joints and complex shapes.
Patent Information
- Application Number
- JP2023050378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Water-based paint compositions containing scaly pigments with high aspect ratios are prone to cracking when applied in high temperature and high humidity environments, particularly at bolt joints in steel structures, due to differences in drying properties between the surface layer and interior of the coating film.
An aqueous coating composition is developed using a water-dispersible epoxy resin, an amine curing agent with water-soluble amines, and scaly pigments with an aspect ratio of 30 to 120, adjusted to a volume concentration of 10.0 to 24.0% by volume, to suppress cracking by minimizing differences in drying properties.
The composition forms a coating film that is resistant to peeling and cracking, even under thermal stress, maintaining integrity at bolt joints and other complex shapes.
Smart Images

Figure 2024139438000001 
Figure 2024139438000002 
Figure 2024139438000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous coating composition and an anticorrosive coating method using said coating composition, and in particular to an aqueous coating composition capable of forming a coating film that is resistant to peeling and cracking. [Background technology]
[0002] In the repair of a coated object due to deterioration of the coating film, a coating composition has been developed that can prevent peeling of the coating film by adjusting the linear expansion coefficient of the coating film to a small value.
[0003] JP 2018-080332 A (Patent Document 1) describes a coating composition containing a resin component and a pigment, in which the linear expansion coefficient at a temperature equal to or lower than the glass transition temperature of the non-volatile content is 3.2 × 10 -5 / K or less, and it is described that such a coating composition can significantly prevent peeling of the coating film, and therefore a coating composition capable of forming a coating film having excellent durability and suitable for repair can be provided.
[0004] JP 2019-196417 A (Patent Document 2) describes a coating composition containing a resin component and a pigment, in which the linear expansion coefficient at a temperature equal to or lower than the glass transition temperature of the non-volatile content contained in the coating composition is 2.5 × 10 -5 / K~5.4×10 -5 / K, and when a coating film having a thickness of 200 μm is formed from the coating composition, the water vapor permeability of the coating film is 0.1 to 1.4 g / m 2 It is described that a coating composition capable of forming a coating film having excellent corrosion resistance and peeling resistance can be provided by using such a coating composition.
[0005] Patent Documents 1 and 2 describe that the linear expansion coefficient of a coating film can be reduced by increasing the proportion of pigment in the non-volatile content, and that among pigments, scaly pigments are particularly effective in reducing the linear expansion coefficient.
[0006] In Japanese Patent No. 6945030 (Patent Document 3), focusing on the effect of scaly pigments in suppressing the intrusion of corrosive factors, it is described that, for a coating composition containing a high amount of scaly pigments, by lowering the average inclination angle of the scaly pigments in a coating film formed from the coating composition to a specific range and increasing the packing rate of the scaly pigments to a specific range, a coating film excellent in environmental barrier properties can be formed without impairing the appearance of the topcoat coating film. Here, it is also described that the aspect ratio of the scaly pigment is preferably 30 to 100 from the viewpoint of improving the environmental barrier properties, and that the average particle size of the scaly pigments is preferably 10 to 100 μm from the viewpoint of orientation in the coating film.
[0007] In recent years, there has also been a shift from solvent-based paints to water-based paints at repair sites in order to reduce health hazards for painters and residents.
[0008] JP 2016-186021 A (Patent Document 4) describes a two-liquid water-based epoxy resin coating composition that contains at least (A) an epoxy resin, (B) a curing agent, (C) a viscosity modifier, (D) a pigment, and (E) water. Patent Document 4 also describes that the scaly pigment, due to its shape, exhibits the effect of inhibiting the intrusion of corrosive factors such as water, oxygen, and chlorides, and the effect of reducing the internal stress of the coating film, and that by reducing the internal stress of the coating film, the adhesion of the coating film to the substrate can be further improved, and that the (D) pigment preferably contains at least one scaly pigment selected from the group consisting of talc, mica, kaolin clay, glass flake, and micaceous iron oxide, and has an aspect ratio of 1.2 to 100.
[0009] JP 2018-053028 A (Patent Document 5) describes a two-component reactive curing type aqueous coating composition for undercoat coating, which contains an epoxy resin and an amine resin. Patent Document 5 also describes that such a coating composition may contain a scale-shaped inorganic powder having an aspect ratio of 2 to 1000, and that the inclusion of the inorganic powder tends to improve the chemical resistance of the resulting undercoat coating film.
[0010] In addition, Patent Documents 4 and 5 also state that if the aspect ratio of the scale-like pigment is too small, it is difficult to obtain a shielding effect, and that if the aspect ratio of the scale-like pigment is too large, painting workability may be impaired or the scale-like pigments may not be properly arranged during film formation.
[0011] Japanese Patent No. 5273752 (Patent Document 6) describes an aqueous epoxy resin coating composition that contains a base agent containing an epoxy resin emulsion and a curing agent containing an amine resin emulsion and has an adjusted viscosity at a specific shear rate, and describes that such a coating composition can provide an aqueous epoxy resin coating composition that is excellent in workability and corrosion resistance. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2018-080332 A [Patent Document 2] JP 2019-196417 A [Patent Document 3] Patent No. 6945030 [Patent Document 4] JP 2016-186021 A [Patent Document 5] JP 2018-053028 A [Patent Document 6] Patent No. 5273752 Summary of the Invention [Problem to be solved by the invention]
[0013] Under these circumstances, the present inventors have investigated water-based paint compositions containing scaly pigments and have found that when water-based paint compositions containing scaly pigments that have a specific aspect ratio and are expected to have peeling-inhibiting effects are applied in high-temperature and high-humidity environments, cracks in the paint film sometimes occur. When repairing steel structures, it is also necessary to paint the joints (bolted joints) between steel plates, and cracks in the paint film have been frequently observed, especially when painting bolted joints.
[0014] Therefore, an object of the present invention is to provide an aqueous coating composition capable of forming a coating film that is less susceptible to peeling and cracking. Another object of the present invention is to provide a corrosion-resistant coating method using such an aqueous coating composition. [Means for solving the problem]
[0015] The present inventors have found that the use of a scaly pigment having an aspect ratio of 30 or more in an aqueous coating composition containing a water-dispersible epoxy resin and an amine curing agent can provide an effect of imparting peeling suppression to the coating film. However, on the other hand, when a thermal cycle test is performed on a bolt joint coated with such a coating composition, cracks are found to occur in the coating film. One of the reasons for this is thought to be that the inclusion of a large amount of scaly pigment having a high aspect ratio makes it easy for differences in drying properties to occur between the surface layer and the inside of the coating film. In particular, since the coating of a bolt joint is prone to have thickness differences between the thick and thin film parts due to its complex shape, it is thought that the difference in drying properties between the surface layer and the inside of the coating film is significant. In addition, the difference in drying properties between the surface layer and the inside of the coating film also affects the curing of the water-dispersible epoxy resin. The curing of the water-dispersible epoxy resin progresses as the evaporation of water progresses, so the curing of the water-dispersible epoxy resin in the inside of the coating film progresses more slowly than the curing of the water-dispersible epoxy resin in the surface layer of the coating film. For this reason, the surface layer of the coating film, which has hardened first, is unable to keep up with the shrinkage inside the coating film that occurs as a result of hardening, and this is also thought to be a cause of cracks.
[0016] As a result of further investigations, the inventors discovered that by adjusting the volume concentration of the scaly pigment in the coating film-forming components, using a water-soluble amine as the amine hardener, and adjusting the logarithmic decrement measured under specific conditions, it is possible to suppress the occurrence of cracks in the coating film even when painting bolted joints, and thus completed the present invention.
[0017] Accordingly, the aqueous coating composition of the present invention is an aqueous coating composition comprising (A) a water-dispersible epoxy resin, (B) an amine curing agent, (C) a scaly pigment, and (D) water, wherein the (B) amine curing agent comprises at least one (B1) water-soluble amine, the (C) scaly pigment comprises at least one (C1) scaly pigment having an average aspect ratio of 30 to 120, and the volume concentration of the (C) scaly pigment in the coating film-forming components is 10.0 to 24.0 volume %, and the aqueous coating composition is characterized in that a coating film is formed by applying an amount of the coating composition to a steel plate with an applicator such that the dry film thickness is 60 to 80 μm, and the coating film is left for one hour under conditions of 23°C and 50% relative humidity immediately after application, and the logarithmic decrement is measured under conditions of 23°C and 50% relative humidity using a rigid pendulum physical property tester equipped with a knife-edge type pendulum weighing 300 g, and the logarithmic decrement is within 0.60.
[0018] In a preferred embodiment of the aqueous coating composition of the present invention, the volume concentration of all pigments in the coating film-forming components is 20 to 36% by volume.
[0019] In another preferred embodiment of the aqueous coating composition of the present invention, the average particle size of the (C1) scaly pigment having an average aspect ratio of 30 to 120 is 10 to 80 μm, and the content of the (C1) scaly pigment having an average aspect ratio of 30 to 120 in the (C) scaly pigment is 50 mass% or more.
[0020] In another preferred embodiment of the aqueous coating composition of the present invention, (C1) the scaly pigment having an average aspect ratio of 30 to 120 is mica.
[0021] In another preferred embodiment of the aqueous coating composition of the present invention, at least one of the water-soluble amines (B1) is a polyether amine resin.
[0022] In another preferred embodiment of the aqueous coating composition of the present invention, the coating composition is a coating composition for natural drying at ambient temperature.
[0023] The corrosion-resistant coating method of the present invention is characterized in that the aqueous paint composition of the present invention described above is applied to a surface to be coated to form a coating film on the surface to be coated, and then a paint other than the paint composition is applied onto the coating film. Effect of the Invention
[0024] According to the aqueous coating composition of the present invention, it is possible to provide an aqueous coating composition capable of forming a coating film which is resistant to peeling and cracking. Also, according to the anticorrosive coating method of the present invention, it is possible to provide an anticorrosive coating method using such an aqueous coating composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention relates to a water-based coating composition and a corrosion-resistant coating method.
[0026] The aqueous coating composition of the present invention is an aqueous coating composition containing a water-dispersible epoxy resin, an amine curing agent, a scaly pigment, and water. In this specification, this coating composition is also referred to as the "aqueous coating composition of the present invention" or the "coating composition of the present invention". The water-dispersible epoxy resin is the (A) component, and is also referred to as the "(A) water-dispersible epoxy resin". The amine curing agent is the (B) component, and is also referred to as the "(B) amine curing agent". The scaly pigment is the (C) component, and is also referred to as the "(C) scaly pigment". Water is the (D) component, and is also referred to as the "(D) water".
[0027] In this specification, the aqueous coating composition is a coating composition containing water as a main solvent. The water used in the coating composition of the present invention is not particularly limited, but preferred examples include tap water, ion-exchanged water, distilled water, and other pure water. When the coating composition is to be stored for a long period of time, water sterilized by ultraviolet irradiation or the like may be used to prevent the growth of mold and bacteria. In the coating composition of the present invention, the amount of water is preferably 20 to 60% by mass, more preferably 30 to 50% by mass.
[0028] In the coating composition of the present invention, the amount of the coating film-forming component is preferably 40 to 80 mass %, more preferably 50 to 70 mass %. In this specification, the coating film-forming component refers to the components excluding volatile components such as solvents, and is the component that will ultimately form a coating film, but in the present invention, the components remaining when the coating composition is dried in an oven at 110°C for 3 hours are treated as the coating film-forming component.
[0029] The coating composition of the present invention contains a water-dispersible epoxy resin. Here, the water-dispersible epoxy resin is an epoxy resin that can be dispersed in water and is present in the aqueous coating composition of the present invention in a dispersed state. The water-dispersible epoxy resin is preferably present in the form of an epoxy resin emulsion or an epoxy resin dispersion. In this specification, the resin emulsion means an emulsion in which a resin is dispersed in an aqueous medium mainly composed of water, and the resin dispersion means a dispersion in which a resin is dispersed in an aqueous medium mainly composed of water. The epoxy resin emulsion is not particularly limited, but is prepared by emulsifying an epoxy resin in an aqueous medium mainly composed of water by a normal forced emulsification method (a method using an emulsifier and a high-speed stirrer, etc.). Here, examples of the emulsifier include polyethers such as polyoxyethylene alkylphenol ether-based nonionic surfactants and polyoxyethylene-polyoxypropylene block copolymers; and adducts of at least one of the nonionic surfactants and the polyethers with a diisocyanate compound. The emulsifier may be used alone or as a blend of two or more types. Commercially available epoxy resin emulsions include, for example, Epolsion EA-1, 2, 3, 7, 12, 20, 55, and HD2 (manufactured by Henkel Japan Co., Ltd.); Yuka Resin KE-002, KE-116, E-1022, and KE-301C (manufactured by Yoshimura Oil Chemicals Co., Ltd.); Adeka Resin EM-101-50 (manufactured by Adeka Corporation); jER W1155R55, jER W3435R67, and jER W2821R70 (manufactured by Mitsubishi Chemical Corporation). Commercially available epoxy resin dispersions include, for example, Beckpox EP2381 (manufactured by Allnex Co., Ltd.); and EPI-REZ6530-WH-53 (manufactured by Momentive Co., Ltd.).
[0030] Aqueous dispersion type epoxy resins are resins that have epoxy groups in their molecules and can be cured by the reaction of the epoxy groups. Epoxy resins are generally known as resins with excellent anticorrosive properties because they have high adhesion to substrates, particularly metal substrates, and also have the effect of shielding the substrate from environmental factors (e.g., water, oxygen, etc.) that affect the corrosion of substrates, particularly metal substrates (shielding effect).
[0031] The water-dispersible epoxy resin is preferably a resin having at least two epoxy groups in one molecule, and is, for example, obtained by reacting a polyhydric alcohol or a polyhydric phenol with a halohydrin. Specific examples include bisphenol A type epoxy resins, halogenated bisphenol A type epoxy resins, novolac type epoxy resins, polyglycol type epoxy resins, bisphenol F type epoxy resins, epoxidized oil, 1,6-hexanediol diglycidyl ether, and neopentyl glycol diglycidyl ether.
[0032] The water-dispersible epoxy resin may be a modified epoxy resin, such as a urethane-modified epoxy resin, an amine-modified epoxy resin, an isocyanate-modified epoxy resin, an acrylic-modified epoxy resin, a polyester-modified epoxy resin, or a dimer acid-modified epoxy resin.
[0033] The epoxy equivalent of the water-dispersible epoxy resin is preferably 100 to 1,000 g / eq, more preferably 200 to 700 g / eq, and even more preferably 400 to 600 g / eq. When the epoxy equivalent is 100 g / eq or more, sufficient coating film properties are easily obtained. On the other hand, when the epoxy equivalent is 1,000 g / eq or less, the leveling property is not easily deteriorated and a uniform coating film is easily obtained. The epoxy equivalent of the epoxy resin can be determined according to JIS K 7236:2001 "Determination of the epoxy equivalent of epoxy resins".
[0034] In the coating composition of the present invention, the amount of the water-dispersible epoxy resin in the coating film-forming components is preferably 20 to 60 mass %. The water-dispersible epoxy resin may be used alone or in combination of two or more kinds.
[0035] The coating composition of the present invention includes an amine curing agent. In this specification, the amine curing agent is an amine that reacts with water-dispersible epoxy resins, particularly with the epoxy groups, and is used to promote or control the curing reaction. As the amine curing agent, a resin having active hydrogen that reacts with epoxy groups is preferred, and a polyamine resin is more preferred. A polyamine resin is a resin having at least two amino groups in one molecule. Examples of polyamine resins include resins made by condensation polymerization of amines and aldehydes, etherification of amines with alcohols, ring-opening polymerization of amines having a heterocyclic structure (such as ethyleneimine), condensation of amines and carboxylic acids, or Mannich reaction of amines, formaldehyde, and ketones or phenols. Here, a polyamine resin that also has an amide bond in the molecule, such as a resin made by condensation of amines and carboxylic acids, is also called a "polyamidoamine resin" or "polyamidoamine". In addition, ring-opening polymerization of alkylene oxides such as ethylene oxide and propylene oxide can be used for etherification of amines with alcohols.
[0036] Examples of amines that can be used in producing the polyamine resin include aliphatic polyamines such as ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, triaminopropane, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, isophoronediamine, and 1,3-bisaminomethylcyclohexane; aromatic polyamines such as phenylenediamine, metaxylylenediamine, paraxylylenediamine, and diaminodiphenylmethane; and amines having a heterocyclic structure such as ethyleneimine.
[0037] The polyamine resin may be a modified polyamine resin. The modified polyamine resin is a polyamine resin in which a portion of the amino group is modified. The amino group can be modified by a known method, such as amidation of the amino group, Mannich reaction of the amino group with a carbonyl compound, or addition reaction of the amino group with an epoxy group.
[0038] In the coating composition of the present invention, the amine curing agent contains at least one water-soluble amine. Here, the water-soluble amine is an amine that is soluble in water and is present in the aqueous coating composition of the present invention in a dissolved state. In this specification, the water-soluble amine as the amine curing agent is the (B1) component, and is also referred to as "(B1) water-soluble amine".
[0039] Since the water-soluble amine (B1) is dissolved in the coating composition of the present invention, the curing of the water-soluble amine and the water-dispersible epoxy resin is not easily affected by the difference in drying between the surface layer and the inside of the coating film, which may occur when a large amount of scaly pigment with a high aspect ratio is contained. Therefore, by using the water-soluble amine (B1), the effect of suppressing the occurrence of cracks in the coating film can be obtained.
[0040] As the (B1) water-soluble amine, a resin having active hydrogen that reacts with an epoxy group is preferred, and a polyamine resin is more preferred. In the coating composition of the present invention, it is preferred that at least one of the (B1) water-soluble amines is a polyether-based amine resin. The polyether-based amine resin is a polyamine resin having a polyether structure in the molecule, and examples thereof include polyoxyethylene diamine and polyoxypropylene diamine. Examples of the (B1) water-soluble amine other than the polyether-based amine resin include modified polyamines and modified polyamidoamines.
[0041] The proportion of the water-soluble amine (B1) in the amine curing agent (B) is preferably 5 to 100 mass %. Also, the proportion of the polyether amine resin as the water-soluble amine (B1) in the amine curing agent (B) is preferably 5 to 30 mass %, more preferably 5 to 20 mass %.
[0042] The (B) amine curing agent may contain a water-dispersible polyamine resin together with the (B1) water-soluble amine. Here, the water-dispersible polyamine resin is a polyamine resin that can be dispersed in water. The water-dispersible polyamine resin is preferably present in the form of an emulsion or dispersion.
[0043] The active hydrogen equivalent of the (B) amine curing agent is preferably 80 to 350 g / eq. When the coating composition of the present invention contains a plurality of (B) amine curing agents, the above "active hydrogen equivalent of the (B) amine curing agent" is the average value of the active hydrogen equivalents of the (B) amine curing agents used.
[0044] In the coating composition of the present invention, the amount of the amine curing agent (B) in the coating film-forming components is preferably 5 to 25 mass %.
[0045] In the aqueous coating composition of the present coating, from the viewpoints of the hardening and drying properties and corrosion resistance of the coating film, the blending ratio of the amine curing agent (B) is preferably such that the active hydrogen equivalent of the amine curing agent (B) is 0.5 to 2.0 equivalents, and more preferably 0.7 to 1.4 equivalents, per equivalent of the epoxy group of the epoxy resin.
[0046] The coating composition of the present invention contains a scaly pigment. The scaly pigment is a pigment having a thin and flat shape like a foil, and specific examples thereof include metal pigments such as zinc, nickel, chromium, tin, copper, silver, platinum, gold, and aluminum, as well as glass flakes, talc, mica, kaolin clay, and micaceous iron oxide. Metal pigments also include alloy pigments such as stainless steel. In addition, scaly pigments such as talc and mica may be surface-treated with metal oxides such as titanium oxide. In particular, aluminum (aluminum flakes), glass flakes, and mica are characterized by a relatively high aspect ratio, and are therefore suitable as scaly pigments intended to suppress peeling of the coating film, and mica is particularly suitable among them. In addition to suppressing peeling of the coating film, the scaly pigments also have the effect of improving corrosion resistance by suppressing the intrusion of corrosive factors from the outside, and the effect of reducing the internal stress of the coating film.
[0047] In the coating composition of the present invention, the scaly pigment includes at least one type of scaly pigment having an average aspect ratio of 30 to 120. In this specification, the scaly pigment having an average aspect ratio of 30 to 120 is referred to as component (C1), and is also referred to as "(C1) scaly pigment having an average aspect ratio of 30 to 120."
[0048] The scaly pigment of component (C1) has an average aspect ratio of 30 or more, and thus has the effect of suppressing peeling of the coating film. On the other hand, if the average aspect ratio is too large, the orientation of the scaly pigment in the coating film decreases, so the average aspect ratio of the scaly pigment of component (C1) is 120 or less. The average aspect ratio of the scaly pigment of component (C1) is preferably 50 to 80.
[0049] In this specification, the average aspect ratio of a scaly pigment refers to the ratio (D / T) of the average particle diameter (D) to the average thickness (T) of the scaly pigment. Here, the average particle diameter refers to the 50% particle diameter (D 50 ) and is determined from the particle size distribution measured using a laser diffraction / scattering particle size distribution analyzer. The particle size of a scaly pigment is expressed as the sphere equivalent diameter measured by the laser diffraction / scattering method. The average thickness is the average value of the thicknesses measured using a SEM (scanning electron microscope) for 100 or more scaly pigment particles.
[0050] The average particle size of the scaly pigment of component (C1) is preferably 10 to 80 μm, and more preferably 15 to 60 μm. If the average particle size is smaller than 10 μm, it is difficult to obtain the peeling suppression effect, and if it is larger than 80 μm, the appearance of the coating film applied over the coating film will be deteriorated.
[0051] The content of (C1) the scaly pigment having an average aspect ratio of 30 to 120 in the scaly pigment (C) is preferably 50% by mass or more, and more preferably 60 to 90% by mass.
[0052] The scaly pigment of component (C1) is preferably mica.
[0053] The (C) scaly pigment preferably contains, together with the (C1) component scaly pigment, a scaly pigment having an average aspect ratio of less than 30. In this specification, the scaly pigment having an average aspect ratio of less than 30 is referred to as the (C2) component, and is also referred to as "(C2) scaly pigment having an average aspect ratio of less than 30."
[0054] The orientation of the scale-like pigment in the coating film can be improved by using (C2) a scale-like pigment having an average aspect ratio of less than 30 in combination with (C1) a scale-like pigment having an average aspect ratio of 30 to 120. The scale-like pigment of component (C2) preferably has an average aspect ratio of 1.2 to 30.
[0055] The average particle size of the scaly pigment of component (C2) is preferably 3 to 30 μm.
[0056] The content of (C2) the scaly pigment having an average aspect ratio of less than 30 in (C) the scaly pigment is preferably from 0 to 50 mass %, and more preferably from 10 to 35 mass %.
[0057] The scaly pigment of component (C2) is preferably talc.
[0058] In the coating composition of the present invention, the volume concentration of the scaly pigment in the coating film-forming components is 10.0 to 24.0% by volume, and preferably 12 to 24% by volume. By making the volume concentration of the scaly pigment in the coating film-forming components 24% by volume or less, it is possible to prevent a difference in drying property between the surface layer and the interior of the coating film.
[0059] In this specification, the volume concentration of the scaly pigment in the coating film-forming components is the proportion of the total volume of the scaly pigment to the total volume of the coating film-forming components, and can be determined by calculation from the composition and specific gravity of the components that make up the coating film-forming components.
[0060] The coating composition of the present invention may contain an additional pigment in addition to the scaly pigment. The additional pigment is not particularly limited, and may be any pigment commonly used in the coating industry, such as an anti-rust pigment, an extender pigment, or a coloring pigment. The additional pigment may be used alone or in combination of two or more.
[0061] Examples of the rust-preventive pigment include zinc powder, zinc oxide, barium metaborate, calcium silicate, aluminum phosphate, condensed aluminum phosphate, aluminum tripolyphosphate, zinc phosphate, zinc phosphite, potassium phosphite, calcium phosphite, aluminum phosphite, calcium zinc phosphate, zinc aluminum phosphate, zinc phosphomolybdate, aluminum phosphomolybdate, magnesium phosphate, vanadate / phosphoric acid mixed pigment, etc. Among these, from the viewpoint of corrosion prevention, phosphoric acid-based rust-preventive pigments are preferred. Examples of the phosphoric acid-based rust-preventive pigments include salts of phosphoric acid compounds such as phosphoric acid, phosphorous acid, and polyphosphoric acid (magnesium salts, calcium salts, zinc salts, aluminum salts, phosphomolybdate salts, etc.). In the coating composition of the present invention, the amount of the rust-preventive pigment in the coating film-forming components is, for example, 0 to 16% by mass.
[0062] Examples of the extender pigment include silica, talc, mica, calcium carbonate, barium sulfate, etc. In the coating composition of the present invention, the amount of the extender pigment in the coating film-forming components is, for example, 10 to 40% by mass.
[0063] Examples of color pigments include titanium oxide, iron oxide, carbon black, yellow lead, molybdate orange, ultramarine, Prussian blue, phthalocyanine blue, phthalocyanine green, quinacridone red, naphthol red, benzimidazolone yellow, Hansa yellow, benzimidazolone orange, dioxazine violet, etc. In the coating composition of the present invention, the amount of color pigment in the coating film-forming components is, for example, 0 to 30 mass %.
[0064] In the coating composition of the present invention, the volume concentration of the total pigment in the coating film forming components is preferably 20 to 36 volume %, more preferably 25 to 33 volume %. The volume concentration of the total pigment also affects the corrosion resistance of the coating film and cracking during painting of the bolt part. If the volume concentration of the total pigment is too low, cracking is less likely to occur during painting of the bolt part, but peeling suppression and corrosion resistance are reduced, and if it is too high, cracking and corrosion resistance may occur during painting of the bolt part.
[0065] In this specification, the volume concentration of the total pigment in the film-forming components is the ratio of the total volume of the pigment to the total volume of the film-forming components, and can be calculated from the composition and specific gravity of the components that make up the film-forming components. The volume concentration of the total pigment in the film-forming components is generally also called pigment volume concentration (PVC).
[0066] The coating composition of the present invention is applied to a steel plate with an applicator in an amount such that the dry film thickness is 60 to 80 μm to form a coating film, and the coating film is left for 1 hour under conditions of 23°C and 50% relative humidity immediately after application, and the logarithmic decay rate of the coating film is measured under conditions of 23°C and 50% relative humidity using a rigid pendulum physical property tester equipped with a knife-edge type pendulum weighing 300 g. The logarithmic decay rate is within 0.60, preferably 0.1 to 0.60, and more preferably 0.2 to 0.56. Here, as the rigid pendulum physical property tester, for example, a rigid pendulum physical property tester RPT-3000W manufactured by A&D Co., Ltd. can be used.
[0067] The logarithmic decrement measured under the above specified conditions can be used to estimate the change in viscosity during the coating film formation process. The water-dispersed epoxy resin and amine curing agent, which are components of the water-based paint composition, form a coating film when the solvent evaporates and the dispersed particles fuse and react. During the fusion and reaction, a change in viscosity occurs, which increases the logarithmic decrement.
[0068] When the logarithmic decrement measured under the above specified conditions is within 0.60, the occurrence of cracks in the coating film can be suppressed. When the logarithmic decrement exceeds 0.60, the reaction proceeds rapidly, and the coating film is subjected to stress due to the remaining reaction portion and the occurrence of hardening distortion, which makes it more likely to crack. Generally, the coating film dries faster at the surface than at the inside, but due to the blocking effect of the (C) scaly pigment contained in the coating composition, the difference in drying properties between the inside and the surface layer becomes even greater, and it is presumed that the difference in reactivity and drying properties between the surface layer and the inside of the coating film becomes large, making it more likely to crack. In addition, when the logarithmic decrement is small, the reaction proceeds slowly, so cracks are less likely to occur, but on the other hand, the drying of the coating film becomes slow. For this reason, from the viewpoint of drying properties, it is preferable to increase the pigment volume concentration or add a hardening accelerator such as a tertiary amine, for example.
[0069] In order to make the logarithmic decrement measured under the above specified conditions within 0.60, it is effective to use (B1) water-soluble amine as the amine curing agent while adjusting the volume concentration of the scaly pigment in the coating film forming components to the range of 10.0 to 24.0 volume %. The logarithmic decrement is also affected by the types and amounts of (A) water-dispersible epoxy resin and (B) amine curing agent, as well as the curing accelerator and curing retarder involved in the reaction. In particular, it is preferable not to add a curing accelerator, since it accelerates the reaction and increases the value of the logarithmic decrement.
[0070] As described in JP 2018-080332 A (Patent Document 1) and JP 2019-196417 A (Patent Document 2), the linear expansion coefficient of the coating film can be reduced by increasing the proportion of the pigment in the coating film-forming components, and among pigments, scaly pigments are highly effective in reducing the linear expansion coefficient. By setting the linear expansion coefficient of the coating film low, it is possible to improve the effect of preventing peeling of the coating film. For this reason, in the coating composition of the present invention, the linear expansion coefficient can be adjusted as described in Patent Document 1 and Patent Document 2, so that the peeling suppression effect can be more reliably imparted. For example, in one embodiment of the coating composition of the present invention, the linear expansion coefficient at a temperature below the glass transition temperature of the coating film-forming components is 3.2 × 10 -5 / K or less, preferably 2.5×10 -5 / K or less, more preferably 2.0×10 -5 / K or less, and the lower limit of the linear expansion coefficient is, for example, 1.5×10 -5 / K or more. Methods for measuring the linear expansion coefficient at temperatures equal to or lower than the glass transition temperature of a coating film-forming component are described in detail in Patent Documents 1 and 2.
[0071] The coating composition of the present invention is preferably a two-liquid coating composition. The two-liquid coating composition is a coating composition consisting of a base agent and a curing agent. The two-liquid coating composition can be prepared by mixing the base agent, the curing agent, and additives selected as necessary at the time of painting. In the present invention, (A) the agent containing a water-dispersible epoxy resin is the base agent, and (B) the agent containing an amine curing agent is the curing agent. (C) The scaly pigment may be contained in either the base agent or the curing agent, but is usually contained in the base agent. (D) Water is usually contained in the base agent and the curing agent, but may be used only in the base agent. Also, a part of (D) water may be used as an additive when mixing the base agent and the curing agent.
[0072] The coating composition of the present invention may contain, as other components, appropriate blends according to the purpose, such as resins not corresponding to component (A), curing agents not corresponding to component (B), dispersants, silane coupling agents, film-forming aids, antifreeze agents, viscosity modifiers, defoamers, rust inhibitors not corresponding to anti-rust pigments, surface conditioners, anti-settling agents, anti-skinning agents, anti-sagging agents, color separation inhibitors, matting agents, adhesion imparting agents, leveling agents, drying agents, catalysts, plasticizers, mildew inhibitors, antibacterial agents, antiviral agents, preservatives, insecticides, antistatic agents, and conductivity imparting agents.
[0073] The coating composition of the present invention can be prepared by mixing various components appropriately selected as required. When the coating composition of the present invention is a two-liquid coating composition, the base agent and the curing agent are prepared in advance, and the base agent, the curing agent, and additives as required can be mixed at the time of painting to prepare the coating composition. The base agent and the curing agent can be prepared by mixing various components appropriately selected as required.
[0074] The coating composition of the present invention has a viscosity of 1 to 1000 (Pa·s, 23°C) at a shear rate of 0.1 (1 / s), and preferably has a viscosity of 0.05 to 10 (Pa·s, 23°C) at a shear rate of 1000 (1 / s).
[0075] In this specification, the viscosity is measured using a rheometer (for example, ARES rheometer manufactured by TA Instruments) after adjusting the liquid temperature to 23°C.
[0076] The means for applying the coating composition of the present invention is not particularly limited, and known coating means such as brush coating, roller coating, trowel coating, spatula coating, flow coater coating, and spray coating (e.g., air spray coating, airless spray coating), can be used.
[0077] The coating composition of the present invention may be dried by either natural drying at ambient temperature or forced drying using a dryer or the like, but the coating composition of the present invention is preferably a coating composition for natural drying at ambient temperature. The ambient temperature is assumed to be about 5 to 35°C.
[0078] The coating composition of the present invention can be applied to painting of structures and the like when they are newly constructed, and can also be applied to painting of structures and the like when they are repainted or repaired.
[0079] The coating composition of the present invention is capable of forming a coating film that is resistant to peeling and cracking, and is therefore suitable as an undercoat coating.
[0080] The substrate to be coated with the coating composition of the present invention has various shapes, for example, a two-dimensional substrate such as a film, sheet, or plate, or a three-dimensional substrate that is a complex three-dimensional object. The surface of the substrate may be smooth or may have irregularities. Specific examples of the substrate include steel materials such as steel plates, steel pipes, and bar steel, and steel structures such as steel towers, bridge facilities, and plants. In particular, the coating composition of the present invention can form a coating film that is unlikely to peel or crack, even when coating a joint (bolt joint) between steel plates.
[0081] The surface of the substrate may be subjected to pretreatment such as degreasing, chemical conversion treatment, and polishing, or may be coated with a sealer or primer, or an old coating film may be present on at least a part of the surface. The old coating film may cover a part or the whole of the surface of the substrate. In this specification, the old coating film means a coating film that is already present on the substrate when painting, particularly repair, is performed.
[0082] When a substrate has an old coating film on its surface, the substrate surface including the old coating film can be coated with the coating composition of the present invention. If the old coating film is sound, the coating composition of the present invention can be applied onto the old coating film without peeling or removing the old coating film on the substrate surface. Since contaminants such as dust and dirt are attached to the old coating film, the adhesion of a new coating film to the old coating film can be improved by removing the contaminants. Methods for removing contaminants include high-pressure water washing, blasting, scraping, and wiping with a cloth.
[0083] The old coating film preferably contains a resin, and examples thereof include acrylic resin, silicone resin, acrylic silicone resin, styrene acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenolic resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin, amine resin, ketimine resin, and resins obtained by modifying these resins (modified resins), etc. The resins may be used alone or in combination of two or more.
[0084] The old coating film may contain various additives as other components, such as pigments, dispersants, surface conditioners, antioxidants, plasticizers, rust inhibitors, solvents, antibacterial agents, antiviral agents, viscosity adjusters, fillers, defoamers, charge control agents, stress relaxation agents, penetrating agents, light-guiding materials, glittering materials, magnetic materials, phosphors, ultraviolet absorbers, and radical scavengers.
[0085] Next, the anticorrosive coating method of the present invention will be described.
[0086] The corrosion-resistant coating method of the present invention is a method for coating a surface to be coated with the above-mentioned coating composition of the present invention, which is characterized by forming a coating film on the surface to be coated, and further coating a coating material other than the coating composition on the coating film.
[0087] The coating composition of the present invention is capable of forming a coating film that is resistant to peeling and cracking, and is suitable as an undercoat coating. In addition, the coating composition of the present invention contains the scaly pigment (C1) having an average aspect ratio of 30 to 120, so that the coating composition has high environmental barrier properties, and further, by blending an anti-rust pigment, the corrosion resistance can be further improved.
[0088] In the anticorrosive coating method of the present invention, the surface to be coated can be the surface of the above-mentioned substrate.
[0089] In the corrosion-protective coating method of the present invention, the paint applied onto the coating film formed from the coating composition of the present invention is a paint different from the coating composition of the present invention, and a paint suitable for forming an undercoat coating film or a topcoat coating film can be used as appropriate.
[0090] The coating material for forming the intermediate coating film or the top coating film is preferably an aqueous coating material composition, similar to the coating material composition of the present invention.These coating materials can be appropriately mixed with resins, curing agents, solvents, dispersants, silane coupling agents, film-forming aids, antifreezing agents, viscosity regulators, antifoaming agents, rust inhibitors, surface conditioners, antisettling agents, antiskinning agents, antisagging agents, color separation inhibitors, matting agents, adhesion agents, leveling agents, drying agents, catalysts, plasticizers, mildew inhibitors, antibacterial agents, antiviral agents, preservatives, insecticides, antistatic agents, and conductivity agents, etc., according to the purpose. EXAMPLES
[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0092] <Preparation example of coating composition> The base material and the curing agent were prepared by mixing the raw materials according to the formulation shown in Tables 1 to 3. The obtained base material and the curing agent were mixed in the mixing ratio shown in Tables 1 to 3 to prepare a coating composition, and the coating composition was evaluated. The formulations and mixing ratios shown in Tables 1 to 3 are based on mass.
[0093] The raw materials used are as follows: (1)(A) Water-dispersible epoxy resin ADEKA RESIN EM-101-50 (Epoxy resin emulsion manufactured by ADEKA; non-volatile content 47% by mass) (2)(B) Amine hardener Polyamine resin 1: Cardolite NX-8401 (amine resin emulsion manufactured by Cardolite; non-volatile content 57% by mass) Polyamine resin 2: WD11M60 (water-soluble amine resin manufactured by Mitsubishi Chemical Corporation; non-volatile content 60% by mass), (B1) Water-soluble amine Polyamine resin 3: JEFFAMINE T-403 (polyetheramine manufactured by HUNTSUMAN; non-volatile content 100% by mass), (B1) Water-soluble amine (3)(C) Scaly pigment Scaly pigment 1: Mica A (average particle size 23 μm, average aspect ratio 70) Scaly pigment 2: Mica B (average particle size 15 μm, average aspect ratio 70) Scaly pigment 3: Mica D (average particle size 25 μm, average aspect ratio 20) Scaly pigment 4: Mica E (average particle size 25 μm, average aspect ratio 50) Scaly pigment 5: Mica F (average particle size 25 μm, average aspect ratio 120) Scaly pigment 6: Talc (average particle size 14 μm, average aspect ratio less than 20) (4) Additives, etc. Dispersant: DISPERBYK-190 (manufactured by BYK Japan) Silane coupling agent: 3-glycidoxypropyltrimethoxysilane Film forming agent: Dipropylene glycol n-butyl ether Antifreeze: Ethylene glycol Viscosity adjuster: SN Thickener 665T (manufactured by San Nopco) Defoamer: SN Deformer 1312 (San Nopco) Curing accelerator: Ancamine K-34 (Evonic tertiary amine) Rust inhibitor: sodium nitrite
[0094] Coating composition evaluation <Peeling prevention> According to NEXCO Test Method 443 (Test for peeling resistance of paint), a test plate was prepared under the condition of a single film (55-65μm / coat applied three times), and the test was carried out. Epool Smile manufactured by Dai Nippon Toryo Co., Ltd. was used as the epoxy resin paint for protecting the peeling layer. The peel width from the cut part after 30 cycles of heat cycle test (one cycle consists of (i) 50℃×0.5h, (ii) constant rate temperature drop 1.5h, (iii) -30℃×0.5h, (iv) constant rate temperature rise 1.5h) was measured, and the peeling prevention was evaluated according to the following evaluation criteria. The results are shown in Tables 1-3. If the peeling width is 2.0mm or less, the coating has excellent peeling prevention properties. (Evaluation Criteria) 〇: 1.0mm or less △: Over 1.0mm, 2.0mm or less ×: Exceeding 2.0mm
[0095] <Logarithmic decrement rate> The coating composition was applied to a SPCC-SD steel plate with an applicator so that the dry thickness was 60 to 80 μm to form a coating film, and the coating film was left for 1 hour under conditions of 23°C and 50% relative humidity immediately after application, and the logarithmic decrement (unit: no) was measured under conditions of 23°C and 50% relative humidity using a rigid pendulum physical property tester (A&D RPT-3000W) equipped with a knife-edge type pendulum weighing 300 g. The measurement results are shown in Tables 1 to 3. In Comparative Example 5, it is believed that the use of a curing accelerator resulted in a high logarithmic decrement value.
[0096] <Crack resistance> A hexagonal high tension bolt with a screw diameter of M20 and a neck length of 50 mm was attached to a steel plate (3.2 mm thick) with a hole with an inner diameter of 23 mm to prepare a bolted joint. Next, water-based zinc rich paint manufactured by Dai Nippon Toryo Co., Ltd. was applied to the entire surface of the bolted joint so that the dry film thickness was 70 to 80 μm, and the bolted joint was dried for 24 hours in a 23°C, 50% humidity environment. Then, the paint prepared in the above <Preparation Example of Paint Composition> was brush-painted on the obtained coating so that the dry film thickness was 60 to 80 μm, and the paint was dried for 7 days in a 23°C, 50% humidity environment to prepare a test specimen. The test specimen was subjected to a heat cycle test [one cycle consists of (i) 50°C x 0.5 h, (ii) constant rate temperature decrease 1.5 h, (iii) -30°C x 0.5 h, and (iv) constant rate temperature increase 1.5 h], and the test specimen was observed at the 20th cycle after the start and evaluated according to the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation Criteria) 〇: No cracks ×: Cracks occurred
[0097] <Drying> The semi-curing property was evaluated according to JIS K 5551 7.6. The semi-curing property was evaluated according to the following evaluation criteria when the dry film thickness of each paint was set to 60 to 80 μm. The results are shown in Tables 1 to 3. (Evaluation Criteria) ○: Time until semi-hardening is less than 8 hours △: Time until semi-hardening is 8 to 16 hours ×: Time required for semi-curing exceeds 16 hours
[0098] <Corrosion resistance> Test plates were prepared so that the dry film thickness was 55-65μm, and tests were conducted according to JIS K 5551 Type E complex cycle corrosion resistance. The width of rust blisters from the cut part after 120 cycles of complex cycle testing was measured and evaluated according to the following evaluation criteria. (Evaluation Criteria) ○: Rust bulge width from cut part is less than 4mm ×: Rust bulge width from cut part is 4mm or more
[0099] [Table 1]
[0100]
Table 2
[0101]
Table 3
Claims
1. An aqueous coating composition comprising: (A) a water-dispersible epoxy resin; (B) an amine curing agent; (C) a scaly pigment; and (D) water, (B) the amine curing agent comprises at least one (B1) water-soluble amine; (C) The scaly pigment includes at least one type of (C1) scaly pigment having an average aspect ratio of 30 to 120; The volume concentration of the scaly pigment (C) in the coating film forming components is 10.0 to 24.0 volume %; The aqueous coating composition is characterized in that a coating film is formed by applying the coating composition on a steel plate in an amount such that the dry film thickness is 60 to 80 μm using an applicator, and the coating film is left for 1 hour under conditions of 23°C and 50% relative humidity immediately after application, and when the logarithmic decrement of the coating film is measured using a rigid pendulum physical property tester equipped with a knife-edge type pendulum weighing 300 g under conditions of 23°C and 50% relative humidity, the logarithmic decrement of the coating film is within 0.
60.
2. 2. The aqueous coating composition according to claim 1, wherein the volume concentration of the total pigment in the coating film-forming components is 20 to 36 volume %.
3. 3. The coating composition according to claim 1 or 2, characterized in that the average particle size of the scaly pigment (C1) having an average aspect ratio of 30 to 120 is 10 to 80 μm, and the content of the scaly pigment (C1) having an average aspect ratio of 30 to 120 in the scaly pigment (C) is 50 mass% or more.
4. 3. The coating composition according to claim 1, wherein the scaly pigment (C1) having an average aspect ratio of 30 to 120 is mica.
5. 3. The coating composition according to claim 1, wherein at least one of the water-soluble amines (B1) is a polyether amine resin.
6. 3. The coating composition according to claim 1 or 2, characterized in that the coating composition is a coating composition for natural drying at ambient temperature.
7. 3. A corrosion-protective coating method comprising applying the coating composition according to claim 1 or 2 to a surface to be coated to form a coating film on the surface to be coated, and further applying a coating other than the coating composition on the coating film.
Citation Information
Patent Citations
Corrosion-resistant coating composition
JP1982168963A
Corrosion-preventive coating method
JP1999057614A
Anticorrosive coating material composition, anticorrosive coating film, and base material with anticorrosive coating film and method for producing the same
JP2017025158A
Two liquid reaction-curable aqueous coating composition for primer, and multilayer film forming method using the same and coated body
JP2018053028A
File sending method, file receiving method and file transceiving apparatus
WO2020015670A1