Inkjet ink composition and recording method
A water-based ink composition with composite acrylic resin particles and specific solubility parameters addresses nozzle clogging and abrasion resistance issues in inkjet printing on non- or low-ink absorbing media, enhancing both clogging recovery and image durability.
Patent Information
- Application Number
- JP2023050497
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Inkjet inks used on non- or low-ink absorbing recording media face issues with abrasion resistance due to resin particles forming a film on the surface, which can lead to nozzle clogging in the inkjet head, as the resin particles dissolve and stick to the head's walls, hindering normal ejection and recovery from clogging.
A water-based ink composition containing resin particles composed of composite acrylic resins, with specific Hansen solubility parameters for the resins, and a water-soluble low-molecular organic compound, designed to prevent resin dissolution in the inkjet head while ensuring good abrasion resistance on the recording medium.
The solution effectively improves both nozzle clogging recovery and abrasion resistance of images on non- or low-ink absorbing media by using composite resin particles with tailored solubility parameters, ensuring efficient ink ejection and high-quality image durability.
Smart Images

Figure 2024139522000008 
Figure 2024139522000009 
Figure 2024139522000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink-jet ink composition and a recording method. [Background technology]
[0002] Inkjet recording methods are capable of recording high-definition images with a relatively simple device, and have been rapidly developed in various fields. Due to the revolutionary progress in inkjet recording technology in recent years, printing methods using inkjet recording methods are now being used in the field of high-definition image recording, where photography and offset printing have been used up until now. In particular, various proposals have been made regarding inks that can record high-quality images on non-ink-absorbing or low-ink-absorbing recording media.
[0003] However, images recorded on non-ink-absorbent or low-ink-absorbent recording media may not have sufficient abrasion resistance because the coloring material does not easily penetrate into the recording media. Therefore, studies have been conducted to improve abrasion resistance by adding resin particles to the ink to form a coating on the surface of the image (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-203077 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the resin particles contained in the ink composition are intended to form a coating on the surface of an image, and therefore generally have a tendency to stick. If the resin particles in the ink composition contained in the inkjet head are dissolved and stuck to the wall of the inkjet head, the ink cannot be ejected normally even if the nozzle is cleaned, and the clogging recovery property is reduced. In other words, there is a trade-off between the clogging recovery property of the nozzle and the abrasion resistance of the image.
[0006] Therefore, there is a demand for an inkjet ink composition (hereinafter also simply referred to as "ink composition") that provides good abrasion resistance of an image recorded on a recording medium and good recovery from clogging of nozzles of an inkjet head, and a recording method using the ink composition. [Means for solving the problem]
[0007] One embodiment of the ink-jet ink composition according to the present invention comprises: A water-based ink containing a color material, resin particles, and a water-soluble low-molecular-weight organic compound, the water-soluble low-molecular-weight organic compound contains an amide having a normal boiling point of 215 to 290° C. in an amount of 0.5 to 9.0% by mass relative to the total mass of the ink composition; the resin particles are composite resin particles composed of a first resin and a second resin, each of which is an acrylic resin; The first resin and the second resin are the square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter δph=√(δp 2 +δh 2 ) wherein Δph1 of the first resin is 4.0 to 4.8 MPa 1 / 2 and Δph2 of the second resin is more than 2.6 and less than 3.7 MPa. 1 / 2 It is.
[0008] One aspect of the recording method according to the present invention is to The method includes an ink deposition step of ejecting the ink-jet ink composition of the above embodiment from an ink-jet head and depositing the ink on a recording medium. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an ink jet recording apparatus. [Diagram 2] FIG. 2 is an enlarged cross-sectional view illustrating an ink-jet head. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment of the present invention will be described below. The embodiment described below is an example of the present invention. The present invention is not limited to the following embodiment, and includes various modified forms implemented within the scope of the present invention. Note that not all of the configurations described below are essential configurations of the present invention. Note that in this specification, "(meth)acrylic acid" means "acrylic acid" or "methacrylic acid". Furthermore, "(meth)acrylate" means "acrylate" or "methacrylate".
[0011] 1. Inkjet ink composition The ink-jet ink composition according to one embodiment of the present invention is a water-based ink containing a colorant, resin particles, and a water-soluble low-molecular-weight organic compound, the water-soluble low-molecular-weight organic compound containing 0.5 to 9.0% by mass of an amide having a standard boiling point of 215 to 290° C. relative to the total mass of the ink composition, the resin particles being composite resin particles made of a first resin and a second resin which are acrylic resins, and the first resin and the second resin are each a square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter δph=√(δp 2 +δh 2 ) but the δph1 of the first resin is 4.0 to 4.8 MPa 1 / 2 and δph2 of the second resin is more than 2.6 and less than 3.7 MPa. 1 / 2 It is.
[0012] In a nozzle where non-ejection occurs due to air bubbles or the like in the inkjet head, the ink composition remains in the pressure chamber and dries due to heat from the platen or the like. This causes the resin constituting the resin particles contained in the ink composition to melt and adhere to the inkjet head, resulting in clogging. For example, resin adhesion to the nozzle plate can be removed by wiping, but clogging caused by resin adhesion in the inkjet head may not be eliminated by wiping. Furthermore, clogging caused by resin adhesion in the inkjet head may not be eliminated by flushing, even if it can be eliminated to some extent by suction cleaning. In such a case, performing suction cleaning to eliminate clogging caused by resin adhesion in the inkjet head may interrupt printing due to suction cleaning, which is disadvantageous in terms of recording productivity.
[0013] It has now been found that by using composite resin particles as a resin for forming a coating on a recording medium, both the clogging recovery properties of the nozzle and the abrasion resistance of the image can be improved. The composite resin particles are, for example, composed of one resin and another resin, and have a structure in which the one resin is encapsulated in the other resin. The one resin present inside the composite resin particles is unlikely to come into contact with a component that dissolves the resin, such as an organic solvent contained in the ink, in the ink, whereas the other resin present outside the composite resin particles is likely to come into contact with the organic solvent in the ink. In this case, if the other resin present on the outside is unlikely to dissolve in the organic solvent, it is possible to prevent the resin particles from dissolving in the inkjet head and causing clogging. In addition, if the one resin present on the inside is likely to dissolve in the organic solvent, after attachment to the recording medium, the resin particles are deformed by heating or the like, and the one resin comes out from the inside to the outside and comes into contact with the organic solvent or the like, so that the resin particles are sufficiently dissolved, the ink coating film is smoothed, and the abrasion resistance of the recorded matter is improved. As the organic solvent or the like used together with the composite resin particles, amides having high resin solubility are preferable.
[0014] However, since the amides are difficult to dry after the ink is applied to the recording medium, there is a problem that the ink does not dry sufficiently in the post-heating process, and the abrasion resistance of the recorded matter is deteriorated. Or, in order to dry sufficiently, it is necessary to perform the post-heating process for a long time or at a high temperature. On the other hand, the drying property of the ink can be improved by reducing the content of the amides in the organic solvent etc. contained in the ink, but the conventional composite resin particles are difficult to dissolve in such organic solvents, and are still insufficient in terms of making the resin particles easy to dissolve after being applied to the recording medium. Therefore, even if the content of the amides in the organic solvent etc. is small, it is desired that the other resin present on the outside of the composite resin particles is difficult to dissolve in the organic solvent, and the one resin present on the inside of the composite resin particles is easily dissolved in the organic solvent.
[0015] Here, it is possible to change the design of the resin particles using the Hansen solubility parameter, which is an index of the solubility of the material components, but the solubility of the composite resin particles in organic solvents could not be sufficiently controlled with the conventional design based on the HSP value. More specifically, the conventional Hansen solubility parameter (HSP value) uses the polar component δp, the hydrogen bond component δh, and the dispersion component δd, but when designing composite resin particles by taking these three components into account, it was not possible to achieve desirable performance.
[0016] As a result of intensive research by the present inventors, it was found that the dispersion component δd has a low correlation with the solubility in organic solvents, and therefore a design that takes this into account did not result in favorable performance. Focusing on the polar component δp and the hydrogen bond component δh of the Hansen solubility parameters, the square root of these δph (i.e., δph = √(δp 2 +δh 2 It has been newly discovered that desirable composite resin particles can be obtained by designing the particles based on the above-mentioned formula (1).
[0017] That is, according to the inkjet ink composition of this embodiment, Δph1 of one of the resins in the composite resin particles is 4.0 to 4.8 MPa. 1 / 2 The other resin has a δph2 of more than 2.6 and less than 3.7 MPa.1 / 2 By doing so, even if the content of amides having a normal boiling point of 215 to 290°C is small, one resin can be easily dissolved while the other resin is difficult to dissolve, resulting in good abrasion resistance of the image recorded on the recording medium and good recovery from clogging of the nozzles of the inkjet head. Amides with normal boiling points of 215 to 290°C are also called specific amides. It is speculated that the δph1 of one resin is closer to the δph of certain amides than the δph2 of the other resin, making the other resin less soluble and the one resin more soluble. In addition, certain amides, such as 2-pyrrolidone, have a δph of 15.1 MPa. 1 / 2 and ε-caprolactam has a δph of 14.4MPa. 1 / 2 Certain amides have a δph of 10.0 to 18.0 MPa. 1 / 2 is preferred. Each component of the inkjet ink composition according to this embodiment will be described in detail below.
[0018] 1.1 Colorants The inkjet ink composition according to this embodiment contains a coloring material. The coloring material is not particularly limited, but examples thereof include pigments and dyes. <Pigments> Among the above color materials, pigments are not only insoluble or poorly soluble in water, but also have the property of being resistant to fading due to light, gas, etc. Therefore, records recorded with inks using pigments have good water resistance, gas resistance, light resistance, and storage stability. Both inorganic and organic pigments can be used as pigments. Among these, at least one of carbon black and organic pigments, which belong to inorganic pigments, is preferred because they have good color development and are less likely to settle when dispersed due to their small specific gravity.
[0019] Examples of inorganic pigments include, but are not limited to, carbon black, iron oxide, and titanium oxide.
[0020] The carbon black is not particularly limited, but examples thereof include furnace black, lamp black, acetylene black, and channel black (CI Pigment Black 7). In addition, examples of commercially available carbon black products include No. 2300, 900, MCF88, No. 20B, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA100, and No. 2200B (all trade names, manufactured by Mitsubishi Chemical Corporation), Color Black FW1, FW2, FW2V, FW18, FW200, S150, S160, S170, Pretex 35, U, V, and 140U, Special Black 6, 5, 4A, 4, and 250 (all trade names, manufactured by Degussa AG), Conductex SC, Raven 1255, 5750, 5250, 5000, 3500, 1255, and 700 (all trade names, manufactured by Columbia Carbon Japan Ltd.), and Columbian Chemicals. Examples of such oil-based solvents include those manufactured by Cabot Chemicals, Regal 400R, 330R, 660R, Mogul L, Monarch 700, 800, 880, 900, 1000, 1100, 1300, 1400, and Elftex 12 (all trade names, manufactured by Cabot Corporation).
[0021] The organic pigment is not particularly limited, but examples thereof include quinacridone pigments, quinacridonequinone pigments, dioxazine pigments, phthalocyanine pigments, anthrapyrimidine pigments, anthanthrone pigments, indanthrone pigments, flavanthrone pigments, perylene pigments, diketopyrrolopyrrole pigments, perinone pigments, quinophthalone pigments, anthraquinone pigments, thioindigo pigments, benzimidazolone pigments, isoindolinone pigments, azomethine pigments, and azo pigments. Specific examples of organic pigments include the following:
[0022] Pigments used in cyan inks include CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 15:34, 16, 18, 22, 60, 65, 66, CI Vat Blue 4, and 60.
[0023] Pigments used in magenta inks include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48(Ca), 48(Mn), 57(Ca), 57:1, 88, 112, 114 , 122, 123, 144, 146, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 179, 184, 185, 187, 202, 209, 219, 224, 245, 254, 264, and CI Pigment Violet 19, 23, 32, 33, 36, 38, 43, and 50.
[0024] Pigments used in the yellow inks include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 16, 17, 24, 34, 35, 37, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, 99, 108, 109, 110, 113, 114, 117, 120, 124, 128, 129, 133, 138, 139, 147, 151, 153, 154, 155, 167, 172, 180, 185, 213.
[0025] In addition, pigments used in color inks other than cyan, magenta, and yellow are not particularly limited, but examples thereof include CI Pigment Green 7, 10, CI Pigment Brown 3, 5, 25, 26, CI Pigment Orange 1, 2, 5, 7, 13, 1 4, 15, 16, 24, 34, 36, 38, 40, 43, and 63.
[0026] Examples of pigments used in the white ink include white inorganic pigments such as CI Pigment White 6, 18, and 21, titanium oxide, zinc oxide, zinc sulfide, antimony oxide, magnesium oxide, and zirconium oxide. In addition to the white inorganic pigments, white organic pigments such as white hollow resin particles and polymer particles can also be used.
[0027] In addition to the above pigments, pearl pigments and metallic pigments can also be used. Examples of pearl pigments include pigments having pearlescent or interference luster, such as titanium dioxide-coated mica, fish scale foil, and bismuth oxychloride. Examples of metallic pigments include particles of simple elements or alloys of aluminum, silver, gold, platinum, nickel, chromium, tin, zinc, indium, titanium, copper, and the like.
[0028] The pigments may be used alone or in combination of two or more kinds.
[0029] <dye> Among the above coloring materials, examples of the dye include, but are not limited to, acid dyes, direct dyes, reactive dyes, and basic dyes. Specific examples of the dye include CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 144, 173, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Directed Black 19, 38, 51, 71, 154, 168, 171, 195, CI Reactive Red 14, 32, 55, 79, 249, CI Reactive Black 3, 4, 35. The dyes may be used alone or in combination of two or more.
[0030] The content of the coloring material is preferably 0.5 to 15 mass %, more preferably 1 to 10 mass %, and particularly preferably 1 to 5 mass %, relative to the total mass (100 mass %) of the ink composition.
[0031] 1.2 Resin particles The inkjet ink composition according to this embodiment contains resin particles. The resin particles are composite resin particles made of a first resin and a second resin, which are acrylic resins. In the resin particles, the first resin and the second resin have a square root δph=√(δp 2 +δh 2 ) wherein Δph1 of the first resin is 4.0 to 4.8 MPa 1 / 2 and Δph2 of the second resin is more than 2.6 and less than 3.7 MPa. 1 / 2 It is.
[0032] The content of the resin particles (converted into solid content) is preferably 1 to 20 mass % relative to the total mass of the ink composition, more preferably 2 to 15 mass %, further preferably 3 to 12 mass %, particularly preferably 3 to 10 mass %, and even more preferably 4 to 8 mass %. When the content of the resin particles is within the above range, both the abrasion resistance and the clogging recovery property tend to be well balanced.
[0033] 1.2.1 Form The composite resin particles preferably have a phase-separated structure in which a phase (portion) made of the first resin and a phase (portion) made of the second resin are separated from each other.
[0034] The composite resin particles may have a form in which the first resin and the second resin respectively constitute a part and the other part of the resin particle. For example, the first resin and the second resin may constitute the peripheral part and the central part of the resin particle, or may have other forms. For example, the positions of the first resin and the second resin in the composite resin particle may not be a simple configuration but may be complex and intertwined, or the part made of the first resin and / or the part made of the second resin may be separated into a plurality of parts and not continuous, constituting the composite resin particle. In addition, the boundary between the first resin and the second resin in the composite resin particle is not limited to a clear boundary, and the composition of the resin may change continuously from the first resin to the second resin.
[0035] It is preferable that the composite resin particles have a phase-separated structure in which a phase made of the first resin and a phase made of the second resin are separated, and the phase made of the first resin is encapsulated in the phase made of the second resin. When the composite resin particles have such a form, it is possible to more effectively prevent the resin particles from dissolving in the inkjet head and causing clogging, and after attachment to the recording medium, the resin particles dissolve more thoroughly, making the ink coating smooth and improving the abrasion resistance of the recorded matter.
[0036] The term "encapsulation" refers to one phase being present inside the other phase, and one phase may be partially exposed. In this case, the location of one phase in the other phase is not particularly limited, and one phase may be present in a single or multiple separated portions near the center or at any position shifted from the center. Examples of such a form include a core-shell structure and a sea-island structure.
[0037] As one form of composite resin particles, those in which the other of the first resin and the second resin mainly constitutes the vicinity of the periphery (shell portion) of the composite resin particle and one mainly constitutes the vicinity of the center (core portion) of the resin particle are called composite resin particles with a core-shell structure, or core-shell resin particles. Here, the resin portion constituting the periphery of the core-shell resin particle is called the shell resin, and the resin portion constituting the center is called the core resin. The core portion may be located in a place other than the center of the resin particle. Also, a part of the core resin may be exposed on the outermost surface of the resin particle. The core portion may be spherical or non-spherical. Among them, core-shell resin particles having the first resin as the core portion and the second resin as the shell portion are preferred in terms of better clogging recovery and abrasion resistance.
[0038] Another form of the composite resin particles may be a composite resin particle having an island-in-sea structure in which one of the first and second resins is present as an island in a sea of the other of the first and second resins. In the composite resin particles having an island-in-sea structure, the one of the resins may be partially exposed on the outermost surface of the resin particles, and the islands may be present not only uniformly but also unevenly inside the composite resin particles. The shape of the islands may be spherical or non-spherical, and the size of the islands may vary. Among these, composite resin particles having an island-in-sea structure consisting of islands made of the first resin and a sea made of the second resin are preferred in terms of better clogging recovery and abrasion resistance.
[0039] The composite resin particles are preferably composite resin particles having a core-shell structure or a sea-island structure, since they have better clogging recovery properties and abrasion resistance. In an image of a composite resin particle observed under a transmission electron microscope (TEM), a core part observed as a single continuous part is considered to have a core-shell structure. A structure similar to the core-shell structure, but in which the core part is observed as two or more discontinuous parts or in which a greater number of parts are observed, is considered to have a sea-island structure. With regard to the core part and island part, when there is one core part, it is called a core part, and when the core part is divided into two or more parts or even more parts, it is called an island part.
[0040] Composite resin particles are preferred from the viewpoint of facilitating adjustment of the solubility of the resin particles, since the resin properties of the first resin and the second resin can be controlled independently. An example of the resin property is the δph in the present invention. In addition, other resin properties such as the glass transition point of the resin and the degree of crosslinking may be controlled. For example, the shell and sea are composed of the second resin, and the second By using a resin that is difficult to dissolve in ink, the resin particles are difficult to dissolve in ink during recording. In addition, by forming the core and islands from a first resin and using a resin that is easy to dissolve on a recording medium, the resin particles are easy to dissolve on the recording medium. In other words, it is preferable that the composite resin particles have at least one of a core-shell structure in which the first resin is the core and the second resin is the shell, and a sea-island structure in which the first resin exists in the second resin in the form of islands, and in this case, clogging recovery and abrasion resistance tend to be more excellent.
[0041] 1.2.2 Resin components <First resin> The first resin constituting a part of the composite resin particles may be a homopolymer or a copolymer.
[0042] The square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter δph = √(δp 2 +δh 2 ) In the first resin, Δph1 is 4.0 to 4.8 MPa. 1 / 2 However, 4.2 to 4.8 MPa 1 / 2 Preferably, the pressure is 4.4 to 4.8 MPa. 1 / 2 More preferably, the pressure is 4.5 to 4.7 MPa. 1 / 2 When Δph1 of the first resin is within the above range, the composite resin particles become more easily dissolved and quickly dissolve on the recording medium to form a coating, and the abrasion resistance of the image tends to be improved.
[0043] Here, in this specification, the "Hansen solubility parameter (HSP value)" is a value that consists of three components, namely, a dispersion component (δd), a polar component (δp), and a hydrogen bond component (δh), and indicates the solubility behavior of a material that contributes to the cohesive energy density. In addition, the HSP value in this specification is the solubility parameter (unit: MPa) calculated from the software HSPiP (Hansen Solubility Parameters in Practice), version 5.3.06. 1 / 2 )
[0044] The δph1 of the first resin is determined by multiplying the δph of the homopolymer of each monomer used in the synthesis of the first resin by the volume ratio of the homopolymer of each monomer to the total volume number of all homopolymers of each monomer, and averaging the δph. In order to set the δph1 of the first resin within the above range, for example, a monomer component constituting the resin may be used that has a δph within the above range, or when multiple types of monomers are used, multiple types of monomers may be selected and their mass ratios may be determined so that the δph of the resin falls within the above range.
[0045] The lower limit of the glass transition temperature (hereinafter also referred to as "Tg") of the first resin is preferably 10°C or more, more preferably 60°C or more, even more preferably 63°C or more, even more preferably 65°C or more, and particularly preferably 67°C or more. The upper limit is preferably 95°C or less, more preferably 80°C or less, and more preferably 75°C or less. When the Tg of the first resin is 80°C or less, the first resin is easily dissolved on the recording medium by a heat treatment or the like to form a coating, so that the abrasion resistance of the image tends to be better. In addition, when the Tg of the first resin is 10°C or more, even when the head scans on a heated platen, the first resin can be suppressed from melting in the ink, so that clogging recovery tends to be good.
[0046] When the first resin is a homopolymer, the glass transition temperature (Tg) of the first resin may be that described in various documents (for example, the Polymer Handbook, etc.). In the present invention, "Tg" is calculated based on the estimation method of DW Van Krevelen, which is calculated based on the contribution of each atomic group to the glass transition temperature and the molecular weight thereof (DW Van Krevelen, Klaas te Nijenhuis, "Properties of Polymers, Fourth Edition", Elsevier Science, 2009). In this specification, values from the Synthia module of the known software BIOVIA Materials Studio 2020 (manufactured by Dassault Systems) are used. On the other hand, when the first resin is a copolymer, the Tg of the first resin is calculated by the Tgn (unit: K) of various homopolymers and the mass fraction (Wn) of the monomer. It can be calculated using the following FOX formula.
[0047]
number
[0048] Where, Wn: mass fraction of each monomer, Tgn: Tg of homopolymer of each monomer (unit: K), Tg: Tg of copolymer (unit: K)
[0049] In order to set the Tg of the first resin within the above range, a monomer having a Tg within the above range may be used for preparing the resin, or the monomers used for preparing the resin may be selected or the mass fraction may be adjusted so that the Tg of the first resin falls within the above range.
[0050] An acrylic resin is used as the first resin. The acrylic resin is a resin having at least a (meth)acrylic monomer unit, and is preferable in that various physical properties can be easily controlled and are easily available. The content of the (meth)acrylic monomer unit is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. The content of the (meth)acrylic monomer unit may be 100% by mass, and is preferably 90% by mass or less in that various physical properties are easily obtained. The acrylic resin may be a resin having a (meth)acrylic monomer unit and a monomer unit other than the (meth)acrylic monomer unit, and in this case, it is preferable in that various physical properties of the resin can be easily adjusted. Examples of the other monomer units include vinyl monomer units. In addition, the acrylic resin preferably has an aromatic monomer unit. Examples of the aromatic monomer unit include an aromatic vinyl monomer unit and an aromatic (meth)acrylic monomer unit, and a resin having an aromatic vinyl monomer unit is preferable. Here, when the total constituent units of the first resin are taken as 100% by mass, the lower limit of the aromatic monomer unit constituent ratio is preferably 5% by mass or more, more preferably 10% by mass or more, and particularly preferably 15% by mass or more. On the other hand, the upper limit of the content of the aromatic monomer unit is preferably 100% by mass or less, more preferably 95% by mass or less, and particularly preferably 90% by mass or less. When the content ratio of the aromatic monomer unit in the first resin is within the above range, adhesion is generated when the first resin is dissolved, so that the adhesion between the recording medium and the resin coating is good, and as a result, the abrasion resistance of the image also tends to be good.
[0051] The (meth)acrylic monomer unit is not particularly limited, but in order to increase the glass transition point or to form a crosslinked resin as described below, at least a portion of the (meth)acrylic monomer unit may contain a bifunctional or higher functional (meth)acrylic monomer unit, which is a crosslinkable component.
[0052] Examples of the difunctional or higher functional (meth)acrylic monomer unit include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and 1,2-dimethylphenyl di(meth)acrylate. glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, ethoxylated bisphenol A di(meth)acrylate, propoxylated bisphenol A di(meth)acrylate, propoxylated ethoxylated bisphenol A di(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, Examples of the ethoxylated isocyanuric acid tri(meth)acrylate include pentaerythritol (meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, and ethoxylated pentaerythritol tetra(meth)acrylate.
[0053] The first resin may contain a monofunctional (meth)acrylic monomer unit as the (meth)acrylic monomer unit. Examples of the monofunctional (meth)acrylic monomer unit include a hydrophilic (meth)acrylate monomer unit, a hydrophobic (meth)acrylate monomer unit having an alkyl group having 3 or more carbon atoms, a hydrophobic (meth)acrylate monomer unit having a cyclic structure, a (meth)acrylamide monomer unit, or an N-substituted derivative thereof.
[0054] The hydrophilic (meth)acrylate monomer unit is not particularly limited, but examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, α-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, (poly)ethylene glycol (meth)acrylate, methoxy (poly)ethylene glycol (meth)acrylate, ethoxy (poly)ethylene glycol (meth)acrylate, and (poly)propylene glycol (meth)acrylate. Among these, methyl (meth)acrylate and ethyl (meth)acrylate are preferred. Here, "hydrophilic" refers to a solubility of 0.3 g or more in 100 mL of water (20°C).
[0055] The hydrophobic (meth)acrylate monomer unit having an alkyl group having 3 or more carbon atoms is not particularly limited, but examples thereof include (meth)acrylates having an alkyl group having 3 or more carbon atoms, such as n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cetyl (meth)acrylate, neopentyl (meth)acrylate, and behenyl (meth)acrylate. Among these, lauryl (meth)acrylate is preferred. Here, "hydrophobic" means that the solubility in 100 mL of water (20°C) is less than 0.3 g.
[0056] The hydrophobic (meth)acrylate monomer unit having a cyclic structure is not particularly limited, but examples thereof include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, adamantyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.
[0057] The (meth)acrylamide monomer unit or its N-substituted derivative is not particularly limited, but examples thereof include (meth)acrylamide, N-hydroxymethyl(meth)acrylamide, diacetone acrylamide, N,N-dimethyl(meth)acrylamide, and other (meth)acrylamides or their N-substituted derivatives.
[0058] Examples of the aromatic monomer unit include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, chlorostyrene, and divinylbenzene.
[0059] Furthermore, the first resin may have a monomer unit other than the above monomer units, for example, a carboxylic acid monomer unit, etc. When the first resin has a carboxylic acid monomer unit, the relative acid value of the composite resin particles can be controlled.
[0060] The carboxylic acid monomer unit is not particularly limited, but examples thereof include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, etc. Among these, (meth)acrylic acid is preferred. Here, the "carboxylic acid monomer unit" refers to a polymerizable monomer unit having a carboxyl group and a polymerizable unsaturated group.
[0061] The above monomers may be used alone or in combination of two or more kinds.
[0062] The first resin may be crosslinked. In the case of being crosslinked, for example, the first resin may contain a difunctional or higher (meth)acrylic monomer unit which is the above-mentioned crosslinkable component, may contain a difunctional or higher monomer unit having a polymerizable functional group other than a (meth)acrylic group, or may be crosslinked using a crosslinking agent that imparts a crosslinked structure to the resin.
[0063] The first resin is preferably, but not limited to, a resin with a low content of a crosslinkable component, more preferably not a crosslinked resin containing a crosslinkable component, and is preferably a resin having a monofunctional (meth)acrylic monomer unit. When the first resin is a resin other than a crosslinked resin, it dissolves quickly on the recording medium to form a coating, which may improve adhesion to the recording medium and abrasion resistance of the image.
[0064] The monofunctional (meth)acrylic monomer unit is not particularly limited, but may be a hydrophilic (meth)acrylate monomer unit, a hydrophobic (meth)acrylate monomer unit having an alkyl group having 3 or more carbon atoms, a hydrophobic (meth)acrylate monomer unit having a cyclic structure, a (meth)acrylamide monomer unit or an N-substituted derivative thereof, etc. Specific examples of these monofunctional (meth)acrylic monomers include the same ones as those exemplified above.
[0065] <Second resin> The second resin constituting a part of the composite resin particle can be composed of the same as the first resin described above, and independent of the first resin, except that the Δph2 is within the following range. An acrylic resin is used as the second resin.
[0066] The square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter δph = √(δp 2 +δh 2 ) In the second resin, δph2 is greater than 2.6 and less than 3.7 MPa 1 / 2 However, 2.7 to 3.5 MPa 1 / 2 is preferably 2.7 to 3.3 MPa. 1 / 2More preferably, the pressure is 2.7 to 3.2 MPa. 1 / 2 More preferably, the pressure is 2.8 to 3.1 MPa. 1 / 2 It is more preferable that the second resin has a Δph2 within the above range. When the Δph2 of the second resin is within the above range, the composite resin particles are less likely to dissolve in the ink, and clogging recovery tends to be good. In addition, it is easy to achieve excellent foreign matter suppression, abrasion resistance, and OD value. Note that when simply written as ○ to △ (○ and △ are numerical values), it means that the numerical values at the ends of the range are included.
[0067] The second resin may be a homopolymer or a copolymer. In addition, it is preferable that the content of the crosslinkable component in the second resin is higher than that in the first resin, since the composite resin particles tend to be less soluble in the ink and the clogging recovery tends to be good.
[0068] The lower limit of the Tg of the second resin is preferably 60°C or higher, more preferably 65°C or higher, even more preferably 70°C or higher, even more preferably 75°C or higher, and particularly preferably 80°C or higher. The upper limit is preferably 110°C or lower, more preferably 100°C or lower, even more preferably 95°C or lower, and particularly preferably 90°C or lower. When the Tg of the second resin is 110°C or lower, the second resin dissolves on the recording medium by heat treatment or the like to form a coating, and the image tends to have good abrasion resistance. In addition, when the Tg of the second resin is 60°C or higher, Even when the head scans over a heated platen, the second resin can be prevented from melting in the ink, which tends to improve clogging recovery. The difference between the Tg of the first resin and the Tg of the second resin (Tg of the second resin - Tg of the first resin) is preferably 3 to 25°C, more preferably 5 to 20°C, further preferably 10 to 19°C, and particularly preferably 15 to 18°C.
[0069] The Tg of the second resin can be determined in the same manner as that of the first resin.
[0070] As the second resin, an acrylic resin having a (meth)acrylic monomer unit is used, as in the first resin. Also, as in the first resin, the second resin may have a monomer unit other than the above-mentioned monomer units, such as a carboxylic acid monomer unit. By having the second resin have a carboxylic acid monomer unit, it is possible to control the relative acid value of the composite resin particles. Specific examples of the carboxylic acid monomer unit include the same as those exemplified above.
[0071] 1.2.3 Physical properties In composite resin particles, the weighted average δph = (v1δph1 + v2δph2) / (v1 + v2) based on the volume ratio (v1 / v2) of the first resin and the second resin is 3.4 to 4.1 MPa. 1 / 2 It is preferable that the pressure is 3.5 to 4.0 MPa. 1 / 2 More preferably, the pressure is 3.6 to 3.9 MPa. 1 / 2 More preferably, the pressure is 3.6 to 3.8 MPa. 1 / 2 When the weighted average Δph of the composite resin particles is within the above range, the image tends to have better rub-off resistance and better clogging recovery properties.
[0072] The δph1 of the first resin is higher than the δph2 of the second resin, 1.0Mpa 1 / 2 It is preferable that the temperature is higher than 1.0 to 2.0 MPa. 1 / 2 More preferably, it is 1.2 to 2.0 MPa. 1 / 2 More preferably, it is 1.4 to 2.0 MPa. 1 / 2 It is particularly preferable that the temperature is higher than 1.5 to 1.8 MPa. 1 / 2 When the difference between Δph1 of the first resin and Δph2 of the second resin is within the above range, the abrasion resistance of the image tends to be better and the recovery from clogging tends to be better.
[0073] The composite resin particles preferably have a volume average particle diameter of 90 nm to 250 nm, more preferably 190 nm to 220 nm, even more preferably 90 nm to 190 nm, particularly preferably 100 nm to 160 nm, and even more particularly preferably 120 nm to 160 nm. When the volume average particle diameter of the composite resin particles is within the above range, the resin tends to have a good balance of solubility. That is, the composite resin particles are less likely to dissolve in the ink, and the clogging recovery is more favorable. In addition, after being ejected onto a recording medium, the composite resin particles are easily dissolved and a coating is quickly formed, so that the abrasion resistance of the image is good. When the volume average particle diameter of the composite resin particles does not exceed the above range, the composite resin particles increase the scattering of light, so that the OD value of the image decreases and the glossiness is less likely to be poor. The term "volume average particle diameter" refers to the volume-based average particle diameter measured using a particle size distribution measuring device that uses dynamic light scattering as the measurement principle. In the examples described below, the Nanotrac WAVE II The average particle size (nm) of the composite resin particles measured by a Microtrack Bell Instrument is used.
[0074] In the composite resin particles, the mass ratio of the first resin to the second resin (first resin / second resin) is preferably 0.3 to 3.5, more preferably 0.4 to 3.0, and even more preferably 0.5 to 2.0. Furthermore, the lower limit of the mass ratio (first resin / second resin) is more preferably 1 / 1.8 or more, even more preferably 1 / 1.5 or more, and particularly preferably 1 / 1.3 or more. Further, it is preferably 0.8 or more, and more preferably 1.0 or more. The upper limit of the mass ratio (first resin / second resin) is preferably 1 / 0.6 or less, and more preferably 1 / 0.7 or less. More preferably, the mass ratio is less than 1 / 0.8, and particularly preferably less than 1 / 0.8. When the mass ratio (first resin / second resin) is greater than or equal to the above range, the resin particles tend to dissolve easily in the post-heating step, and the abrasion resistance tends to be superior. When the mass ratio (first resin / second resin) is less than or equal to the above range, the resin particles tend to dissolve less easily in the ink, and the clogging recovery tends to be excellent.
[0075] The acid value of the second resin is preferably 5 to 35 mgKOH / g, more preferably 7 to 20 mgKOH / g, and even more preferably 10 to 15 mgKOH / g. When the acid value of the composite resin particles is within the above range, both the clogging recovery property and the abrasion resistance of the image tend to be improved.
[0076] The acid value is a parameter that indicates hydrophilicity / hydrophobicity, and the larger the value, the more hydrophilic the compound, and the smaller the value, the more hydrophobic the compound. Therefore, if the acid value of the second resin that mainly constitutes the outermost layer of the composite resin particle is less than the above range, the composite resin particle and the organic solvent become more compatible, and the composite resin particle becomes more easily dissolved in the ink, which may cause clogging due to the resin melting in the inkjet head, and may result in poor clogging recovery. On the other hand, if the acid value of the second resin exceeds the above range, the composite resin particle and water become more compatible, and water tends to remain on the recording medium without volatilizing, which may result in a homogeneous coating not being formed, and thus poor abrasion resistance.
[0077] The acid value of the second resin can be calculated from the molecular weight and content of the monomer unit of the second resin constituting the composite resin particles, and the number of anionic groups contained in the monomer unit. Specifically, it is calculated from the composition of the second resin constituting the composite resin particles using the following formula.
[0078] (parts by mass of monomer 2 having an anionic group among monomers constituting the second resin / total parts by mass of all monomers constituting the second resin) / molecular weight of monomer 2)×number of anionic groups in the molecule of monomer 2=A1 (Formula 1) A1 x 56.11 x 1000 = acid value of the second resin (mgKOH / g) (Equation 2)
[0079] The anionic group is a carboxyl group. When there are multiple types of monomers having an anionic group among the monomers constituting the second resin, A2 and A3·· are calculated for each monomer using the same formula as in Formula 1, and the total value of A1+A2+A3+·· is similarly calculated as A1 in Formula 2. The acid value of the second resin is determined from the second resin, assuming that when a phase made of the first resin is encapsulated in a phase made of the second resin, the characteristics attributable to the outermost surface of the composite resin particle are attributable to the resin that constitutes the outermost surface of the composite resin particle.
[0080] The glass transition temperatures of the first resin and the second resin are preferably 60 to 95° C., more preferably 62 to 88° C., and even more preferably 64 to 86° C. When the glass transition temperatures of the first resin and the second resin are within the above range, there is an excellent balance between the inhibition of melting of the resin and the dissolution, and the image tends to have better abrasion resistance and better clogging recovery properties.
[0081] 1.2.4 Synthesis method The method for synthesizing the composite resin particles is not particularly limited, and for example, the composite resin particles can be synthesized by a known emulsion polymerization method or a suitable combination thereof.Specific examples of the method include a batch mixing polymerization method, a monomer dropping method, a pre-emulsion method, a seed emulsion polymerization method, a multi-stage emulsion polymerization method (such as a two-stage emulsion polymerization method), and a phase inversion emulsion polymerization method.
[0082] Here, the composite resin particles are preferably resin particles dispersed with a reactive surfactant. When the surfactant adsorbed to the resin particles is released, it migrates to the interface between the ink and the recording medium, inhibiting the adhesion of the ink coating film and causing a deterioration in abrasion resistance. In contrast, a reactive surfactant is a compound containing a carbon-carbon double bond, and such a double bond is utilized to form a composite resin. Therefore, the resin particles dispersed by the reactive surfactant tend to have better abrasion resistance because the surfactant is less likely to be released from the resin particles and less likely to impair the adhesion of the ink coating.
[0083] The reactive surfactant may be anionic, cationic, nonionic, or amphoteric, but is preferably anionic. When the reactive surfactant is anionic, the dispersion stability of the resin particles becomes better, and the abrasion resistance and clogging recovery property tend to be more excellent.
[0084] The reactive surfactant preferably has an oxyalkylene group. This improves the dispersion stability of the resin particles, and tends to improve the abrasion resistance and clogging recovery. Examples of the oxyalkylene group include an oxyethylene group (-OCH2CH2-), an oxypropylene group (-OCH2CH2CH2- or -OCH2CH(CH3)-), and the carbon number of the oxyalkylene group is preferably 2 to 5, and more preferably 2 to 3. The oxyalkylene group may be a polyoxyalkylene group in which a plurality of oxyalkylene groups are bonded. The repeating unit n of the oxyalkylene group in the polyoxyalkylene group may be 2 to 100, 2 to 50, or 2 to 30.
[0085] Examples of reactive surfactants include polyoxyalkylene alkenyl ether sulfate, polyoxyalkylene alkenyl ether, polyoxyethylene styrenated propenyl phenyl ether sulfate, polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate, polyoxyethylene styrenated propenyl phenyl ether, polyoxyethylene-1-(allyloxymethyl) alkyl ether, α-[2-[(allyloxy)-1-(alkyloxymethyl)]ethyl]-ω-polyoxyethylene sulfate, α-[2-[(allyloxy)-1-(alkyloxymethyl)]ethyl]-ω-polyoxyethylene, alkylaryl sulfosuccinic acid, methacryloyloxypolyoxypropylene sulfate, styrene sulfonic acid, bis(polyoxyethylene polycyclic phenyl ether) methacrylate sulfate, sulfoethyl methacrylate, and salts thereof. Among these, the reactive surfactant is preferably α-[2-[(allyloxy)-1-(alkyloxymethyl)]ethyl]-ω-polyoxyethylene sulfate or polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate.
[0086] The reactive surfactant may be a commercially available product, and examples of such reactive surfactants include ADEKA REASOAP SR-10, SR-1025, SR-20, and SR-3025 (trade names, manufactured by ADEKA CORPORATION, α-[2-[(allyloxy)-1-(alkyloxymethyl)]ethyl]-ω-polyoxyethylene sulfate ester ammonium salt), ADEKA REASOAP ER-10, ER-20, ER-30, and ER-40 (trade names, manufactured by ADEKA CORPORATION, α-[2-[(allyloxy)-1-(alkyloxymethyl)]ethyl]-ω-polyoxyethylene), and AQUALON AR-10, AR-1025, AR-20, and AR-2020 (trade names, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene styrenated propenyl phenyl ether sulfate ester). ammonium salt), Aqualon KH-05, KH-10, KH-1025 (all trade names, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium salt), Aqualon AN-10, AN-30, AN-5065 (all trade names, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene styrenated propenyl phenyl ether), Latemul PD-104, PD-105 (all trade names, manufactured by Kao Corporation, polyoxyalkylene alkenyl ether sulfate ammonium salt), Latemul PD-420, PD-430, PD-450 (all trade names, manufactured by Kao Corporation, polyoxyalkylene alkenyl ether), Eleminol JS-20 (trade name, manufactured by Sanyo Chemical Industries, Ltd., Examples of such an alkylaryl sulfosuccinate include sodium alkylaryl sulfosuccinate, Eleminol RS-3000 (trade name, manufactured by Sanyo Chemical Industries, Ltd., methacryloyloxypolyoxypropylene sulfate sodium salt), Spinomer NaSS (trade name, manufactured by Tosoh Finechem Corporation, styrene sulfonate sodium salt), Antox MS60 (trade name, manufactured by Nippon Nyukazai Co., Ltd., bis(polyoxyethylene polycyclic phenyl ether) methacrylate sulfate amine salt), and Antox MS-2N-D (trade name, manufactured by Nippon Nyukazai Co., Ltd., sulfoethyl methacrylate sodium salt).
[0087] The composite resin particles may be resin particles dispersed by a non-reactive surfactant. Here, the "non-reactive surfactant" is a compound that does not contain a carbon-carbon double bond. The non-reactive surfactant is not particularly limited, but may be, for example, anionic surfactants such as alkyl sulfate salts, alkyl benzene sulfonates, and alkyl carboxylate salts; nonionic surfactants such as alkyl esters of polyethylene glycol, alkyl ethers of polyethylene glycol, and alkyl phenyl ethers of polyethylene glycol.
[0088] The non-reactive surfactant may be a commercially available product, such as Hitenol LA-16, Hitenol NF-13, Hitenol NF-08, Hitenol NF-17, Hitenol 330T, Hitenol LA-10, DKS NL-600, Noigen EA-137, Noigen EA-207D, Plysurf A212C, Plysurf A208B (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Newcol 271A (manufactured by Nippon Nyukazai Co., Ltd.), Latemul WX, Latemul E-150, Emulgen 1108, Emulgen 1150S-60 (all manufactured by Kao Corporation), DOWFAX 2A1 (manufactured by Dow Chemical Co., Ltd.), Eleminol CLS-20, Eleminol HB-29, and Sanmorin OT-70 (all manufactured by Sanyo Chemical Industries, Ltd.).
[0089] On the other hand, the composite resin particles may be soap-free resin particles. Here, "soap-free resin particles" refers to resin particles that can maintain a stable dispersion state without agglomeration without using a dispersant such as a surfactant. With such soap-free resin particles, there is absolutely no detachment of the surfactant from the resin particles, so the adhesion of the ink coating is not impaired and the abrasion resistance tends to be better.
[0090] The composite resin particles are preferably resin particles neutralized with at least an organic amine or ammonia. Such resin particles tend to have better abrasion resistance. Examples of organic amines include (tri)methylamine, (tri)ethanolamine, (tri)ethylamine, dimethylethanolamine, and morpholine. The composite resin particles may be further neutralized with an inorganic alkali such as sodium hydroxide or potassium hydroxide, if necessary.
[0091] Hereinafter, as an example of composite resin particles, a method for synthesizing core-shell resin particles or sea-island structure resin particles in which the core or island portions are constituted by a first resin and the shell or sea portion is constituted by a second resin will be described in detail.
[0092] (Synthesis method 1) First, particles of the first resin are synthesized by a normal emulsion polymerization method using an aqueous medium. The conditions of the emulsion polymerization may be in accordance with known methods, but for example, when the total amount of monomers used is 100 parts, polymerization can usually be performed using 100 to 500 parts of water (aqueous medium). The polymerization temperature is preferably -10 to 100°C, more preferably -5 to 100°C, and even more preferably 0 to 90°C. The polymerization time is preferably 0.1 to 30 hours, and more preferably 2 to 25 hours. Examples of the emulsion polymerization method include a batch method in which the monomers are charged all at once, a sintering method in which the monomers are charged in a batch, and a sintering method in which the monomers are charged in a batch. A method of feeding the monomers in portions or continuously, a method of adding a monomer pre-emulsion in portions or continuously, or a method of combining these methods stepwise can be adopted. In addition, one or more of polymerization initiators, molecular weight regulators, emulsifiers, etc. used in normal emulsion polymerization can be used as necessary.
[0093] The polymerization initiator is not particularly limited, but may be, for example, a persulfate such as potassium persulfate or ammonium persulfate; an organic peroxide such as diisopropyl peroxydicarbonate, benzoyl peroxide, lauroyl peroxide, or tert-butylperoxy-2-ethylhexanoate; an azo compound such as azobisisobutyronitrile, dimethyl-2,2'-azobisisobutyrate, or 2-carbamoylazaisobutyronitrile; or a redox system combining a radical emulsifier containing a radical emulsifying compound having a peroxide group, sodium hydrogen sulfite, or a reducing agent such as ferrous sulfate. The polymerization initiator may be used alone or in combination of two or more kinds.
[0094] The molecular weight regulator is not particularly limited, but examples thereof include mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, n-hexadecyl mercaptan, n-tetradecyl mercaptan, t-tetradecyl mercaptan, and thioglycolic acid; xanthogen disulfides such as dimethyl xanthogen disulfide, diethyl xanthogen disulfide, and diisopropyl xanthogen disulfide; tetramethyl thiuracil, and the like. Examples of the molecular weight regulator include thiuram disulfides such as thiuram disulfide, tetraethylthiuram disulfide, and tetrabutylthiuram disulfide; halogenated hydrocarbons such as chloroform, carbon tetrachloride, carbon tetrabromide, and ethylene bromide; hydrocarbons such as pentaphenylethane and α-methylstyrene dimer; acrolein, methacrolein, allyl alcohol, 2-ethylhexyl thioglycolate, terpinolene, α-ternepine, γ-ternepine, dipentene, and 1,1-diphenylethylene. The molecular weight regulator may be used alone or in combination of two or more.
[0095] The emulsifier is a surfactant such as the above-mentioned reactive surfactant (reactive emulsifier) or non-reactive surfactant (non-reactive emulsifier). The emulsifier is not particularly limited, but examples thereof include anionic surfactants such as alkyl sulfate salts and alkylbenzene sulfonates; nonionic surfactants such as alkyl esters of polyethylene glycol, alkyl ethers of polyethylene glycol, and alkylphenyl ethers of polyethylene glycol; reactive emulsifiers containing a hydrophilic group, a hydrophobic group, and a radical reactive group; and polymeric emulsifiers in which a hydrophilic group is introduced into a polymer such as a vinyl polymer or a polyester polymer. The emulsifier may be used alone or in combination of two or more. The hydrophilic group is an atomic group having a high affinity for water, and examples thereof include a nitro group, a hydroxyl group, an amino group, a carboxyl group, and a sulfonic acid group. The hydrophobic group is an atomic group having a lower affinity for water than the hydrophilic group, and examples thereof include a linear or branched alkyl group, an alicyclic group, an aromatic ring group, an alkylsilyl group, and a perfluoroalkyl group. If the resin emulsion can be kept in a stable dispersed state without flocculation, it can be produced soap-free without using an emulsifier.
[0096] Next, in the presence of the obtained particles of the first resin, a monomer for the second resin is polymerized. Specifically, core-shell resin particles or sea-island structured resin particles can be formed by seed-polymerizing a monomer for the second resin in a state in which the obtained particles of the first resin are used as seed particles. For example, a monomer for the second resin or a pre-emulsion thereof and, if necessary, a crosslinking agent may be dropped all at once, in portions, or continuously into an aqueous medium in which the particles of the first resin are dispersed. The amount of the particles of the first resin used at this time is preferably 50 to 200 parts by mass per 100 parts by mass of the monomer for the second resin. In the polymerization, a crosslinking agent When used, the second resin can be crosslinked.
[0097] When a crosslinking agent is used, the crosslinking agent is not particularly limited, but examples thereof include phenolic resins and amino resins. Examples of phenolic resins include resol-type phenolic resins obtained by introducing methylol groups by condensing phenols such as phenol and bisphenol A with aldehydes such as formaldehyde in the presence of a reaction catalyst. Examples of aldehydes include formaldehyde, paraformaldehyde, acetaldehyde, and benzaldehyde. In addition, resins in which at least a part of the methylol groups of the above resins is etherified with alcohols having 1 to 8 carbon atoms, such as methyl alcohol, ethyl alcohol, n-butyl alcohol, and isobutyl alcohol, can also be used. Examples of amino resins include methylolated amino resins obtained by reacting an amino component such as melamine, urea, benzoguanamine, spiroguanamine, and dicyandiamide with an aldehyde. Examples of aldehydes include formaldehyde, paraformaldehyde, acetaldehyde, and benzaldehyde. Furthermore, at least a part of the methylol groups of the above resins may be etherified with an alcohol having 1 to 8 carbon atoms, such as methyl alcohol, ethyl alcohol, n-butyl alcohol, or isobutyl alcohol, and the like.
[0098] When a polymerization initiator, a molecular weight regulator, an emulsifier, etc. are used in the polymerization, the same ones as those used in the production of the particles of the first resin can be used. In addition, the conditions such as the polymerization time may be the same as those used in the production of the particles of the first resin.
[0099] (Synthesis method 2) Next, a polymerization method in which the second resin part is synthesized first will be described. First, the second resin part is synthesized. Specifically, a pre-emulsion solution containing the above-mentioned hydrophilic monomer is prepared using a reactive emulsifier or in a soap-free manner, and the pre-emulsion solution is dropped into an aqueous medium together with a polymerization initiator and a crosslinking agent to cause a polymerization reaction, thereby synthesizing the second resin part.
[0100] Next, the obtained second resin part is used as a polymerization site to polymerize the first resin part, and the core-shell resin particles or sea-island structured resin particles according to this embodiment are synthesized. Specifically, a monomer mixture containing the above-mentioned hydrophobic monomer is dropped into an aqueous dispersion medium containing the second resin part, and the first resin part is polymerized to form core-shell resin particles or sea-island structured resin particles. When the second resin part is used as a polymerization site, it is not necessary to include an emulsifier in the monomer mixture, so it can be dropped as monomer oil droplets.
[0101] According to such a multi-stage emulsion polymerization method, the second resin part can be synthesized using a reactive emulsifier or in a soap-free manner, and the first resin part can be synthesized in an emulsifier-free manner, so that the content of the emulsifier in the ink composition can be easily reduced to 0.01% by mass or less. In the ink composition, when the content of the emulsifier contained is 0.01% by mass or less, aggregation of the ink components at the ink interface (air-air-ink gas-liquid interface, ink contact member such as an ink container-ink solid-liquid interface) is suppressed, and the ink composition has excellent storage stability, which is preferable. In addition, when the content of the emulsifier contained in the ink composition is 0.01% by mass or less, the ink composition has excellent foaming and defoaming properties, so that an ink container having an inlet capable of being filled with ink can be preferably used. Here, the term "ink container having an inlet capable of being filled with ink" refers to an ink container having an inlet that can be attached, detached, or opened and closed, which allows the user to easily inject the ink composition, but is prone to foaming during injection. In addition, when the opening area of the inlet is 20 mm 2 This is preferable because it is easy to fill the ink composition. Such an ink container is disclosed in, for example, JP-A-2005-219483 and JP-A-2012-51309.
[0102] In addition, when synthesizing core-shell resin particles or sea-island structure resin particles using a large amount of emulsifier, Even if the emulsifier is an emulsifier having a molecular weight of 0.01%, the content of the emulsifier in the ink composition may be set to 0.01% by mass or less by removing the excess emulsifier after synthesis of the core-shell resin particles.
[0103] Finally, the mixture is neutralized with an alkali such as sodium hydroxide, potassium hydroxide, an organic amine, or ammonia, preferably with at least an organic amine or ammonia, to adjust the pH, and filtered as necessary to obtain a core-shell resin particle dispersion. In the synthesis method, the monomer concentration, polymerization temperature, stirring speed, polymerization time, etc. can be adjusted to obtain core-shell resin particles or sea-island structure resin particles. In particular, it is preferable to adjust these polymerization conditions when synthesizing the first resin.
[0104] Regarding the method for producing such sea-island structured resin particles and core-shell resin particles, see, for example, Colloids and Surfaces A: Physiochemical and Please refer to Engineering Aspects 153(1999) 255-270.
[0105] 1.3 Water-soluble low molecular weight organic compounds The inkjet ink composition according to this embodiment contains a water-soluble low molecular weight organic compound. The water-soluble low molecular weight organic compound contains 0.5 to 9.0 mass % of amides having a normal boiling point of 215 to 290° C., relative to the total mass of the ink composition.
[0106] In the case of a water-soluble low molecular weight organic compound, "water-soluble" means that the solubility is more than 10% by mass in water at 20°C. For example, after mixing the compound in a given concentration with water at 20°C and stirring, if there is no visible residue or cloudy white mixture, the compound is considered to be dissolved in water. If the compound dissolves in water and the minimum concentration of the compound mixed in water exceeds 10% by mass, the compound is considered to be water-soluble. The mass % used to indicate the solubility is the mass % of the low molecular weight organic compound relative to the total mass of the mixture of water and the low molecular weight organic compound.
[0107] In the water-soluble low-molecular-weight organic compound, the term "low molecular weight" refers to a molecular weight of 300 or less. The molecular weight is preferably 250 or less, more preferably 200 or less, and further preferably 50 to 200.
[0108] The water-soluble low molecular weight organic compound may be an organic solvent that is liquid at room temperature, or may be a solid at room temperature. Examples of a solid at room temperature include those with a melting point higher than room temperature (25°C). The melting point can be measured using differential scanning calorimetry (DSC). The water-soluble low molecular weight organic compound is not particularly limited, but examples thereof include resin-soluble compounds, penetrating compounds, and moisturizing compounds. The water-soluble low molecular weight organic compound may be used alone or in combination of two or more kinds.
[0109] 1.3.1 Amides with normal boiling points of 215-290°C The water-soluble low molecular weight organic compound contains amides having a normal boiling point of 215 to 290° C. in an amount of 0.5 to 9.0% by mass relative to the total mass of the ink composition. The amides are a type of resin-soluble compound. The resin-soluble compound is an organic compound that has the function of dissolving resin and improving abrasion resistance, but is not limited to this function.
[0110] Examples of the amides include cyclic amides and non-cyclic amides. Examples of the amides include cyclic amides (lactams) such as 2-pyrrolidone (2P), 2-piperidone, ε-caprolactam (CPL), N-methyl-ε-caprolactam, N-cyclohexyl-2-pyrrolidone, N-methylpyrrolidone, N-ethylpyrrolidone, N-butylpyrrolidone, 5-methyl-2-pyrrolidone, β-propiolactam, and ω-heptalactam; -Dimethylacetoacetamide, N,N-diethylacetoacetamide, N-methylacetoacetamide, N,N-dimethylisobutyric acid amide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylpropionamide, 3-methoxy-N,N-dimethylpropanamide (DMPA), 3-n-butoxy-N,N-dimethylpropionamide, 3-methoxy-N,N-diethylpropionamide, 3-methoxy-N,N-methylethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-diethylpropionamide, 3-ethoxy-N,N-methylethylpropionamide, 3-n-butoxy chain amides such as 3-n-butoxy-N,N-diethylpropionamide, 3-n-propoxy-N,N-dimethylpropionamide, 3-n-propoxy-N,N-diethylpropionamide, 3-n-propoxy-N,N-methylethylpropionamide, 3-iso-propoxy-N,N-dimethylpropionamide, 3-iso-propoxy-N,N-diethylpropionamide, 3-iso-propoxy-N,N-methylethylpropionamide, 3-tert-butoxy-N,N-dimethylpropionamide, 3-tert-butoxy-N,N-diethylpropionamide, and 3-tert-butoxy-N,N-methylethylpropionamide;
[0111] Examples of amides having a standard boiling point of 215 to 290° C. include 2-pyrrolidone (standard boiling point: 245° C.), ε-caprolactam (standard boiling point: 267° C.), and 3-methoxy-N,N-dimethylpropanamide (standard boiling point: 215° C.), and one or more selected from these are preferred, with ε-caprolactam being more preferred. Such compounds tend to have better resin solubility.
[0112] The amides having a normal boiling point of 215 to 290° C. are preferably compounds that are solid or liquid as a simple substance at room temperature. Examples of such compounds include 2-pyrrolidone, ε-caprolactam, and 3-methoxy-N,N-dimethylpropanamide, and one or more selected from these are preferred, with ε-caprolactam being more preferred. Such compounds tend to have better resin solubility.
[0113] The molecular weight of the amides having a normal boiling point of 215 to 290° C. is preferably 50 to 200, and more preferably 80 to 150. The lower limit of the molecular weight is more preferably 90 or more, and the upper limit is more preferably 130 or less. It is further preferably 100 to 120. If the molecular weight is within the above range, the abrasion resistance tends to be superior.
[0114] The standard boiling point of the amides having a standard boiling point of 215 to 290° C. is more preferably 230 to 290° C., further preferably 250 to 290° C., and particularly preferably 250 to 280° C. When the standard boiling point of the amides is within the above range, the amides are prevented from evaporating before the resin particles are sufficiently dissolved in the post-heating step, the resin particles can be sufficiently dissolved, and after the resin particles are dissolved, the amides evaporate quickly, which tends to result in better abrasion resistance.
[0115] The water-soluble low molecular weight organic compound contains 0.5 to 9.0% by mass of amides having a normal boiling point of 215 to 290°C relative to the total mass of the ink composition, with the lower limit being preferably 1.0% by mass or more, more preferably 1.5% by mass or more, even more preferably 2.0% by mass or more, and particularly preferably 2.5% by mass or more. The upper limit is preferably 8.0% by mass or less, more preferably 7.0% by mass or less, even more preferably 6.0% by mass or less, particularly preferably 5.0% by mass or less, and more particularly preferably 4.0% by mass or less. By setting the specific amides within the above range, there is a tendency for the abrasion resistance and clogging recovery properties to be more excellent.
[0116] 1.3.2 Other water-soluble low molecular weight organic compounds Examples of the resin-soluble compound include aprotic polar solvents such as dimethyl sulfoxide (DMSO) and dioxane, other than the amides having a normal boiling point of 215 to 290° C. The resin-soluble compound may be used alone or in combination of two or more. By using the resin-soluble compound, the adhesion of the composite resin particles to the head and cavity is suppressed, and the adhesion and abrasion resistance to low-absorbency or non-absorbency recording media tend to be improved.
[0117] The penetrating compound is not particularly limited, but examples thereof include alkanediols preferably having 4 or more carbon atoms, such as butanediol, pentanediol, hexanediol, and octanediol; and glycol ethers, such as alkylene glycol monoethers and alkylene glycol diethers. The penetrating compound may be used alone or in combination of two or more. By using such a penetrating compound, the ink filling property (wetting property) and penetrating property into the recording medium tend to be further improved.
[0118] The content of the penetrating compound is preferably 0.1 to 10 mass %, more preferably 0.5 to 8 mass %, and particularly preferably 1.0 to 5 mass %, relative to the total mass (100 mass %) of the ink composition. When the content of the penetrating compound is within the above range, the ink filling (wetting and spreading) and penetrating ability into the recording medium tend to be further improved.
[0119] The moisturizing compound is not particularly limited, but examples thereof include polyol compounds (having 3 or more hydroxyl groups) such as glycerin; alkanediols having preferably 3 or less carbon atoms, such as ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, and propanediol, or alkanediols having a polyether skeleton made of an alkylene glycol having 3 or less carbon atoms. The moisturizing compound may be used alone or in combination of two or more. By using such a moisturizing compound, the ink in the inkjet head is more inhibited from drying, and as a result, clogging recovery tends to be more improved.
[0120] The content of the moisturizing compound is preferably 5 to 30% by mass, more preferably 10 to 25% by mass, and particularly preferably 12 to 23% by mass, relative to the total mass (100% by mass) of the ink composition. By having the content of the moisturizing compound within the above range, drying of the ink in the inkjet head is further suppressed, and as a result, clogging recovery tends to be further improved.
[0121] The content of the water-soluble low molecular weight organic compound having a standard boiling point of more than 280° C. is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less, based on the total mass (100% by mass) of the ink composition. The lower limit of the content of the water-soluble low molecular weight organic compound having a standard boiling point of more than 280° C. is 0% by mass. By having the content of the water-soluble low molecular weight organic compound having a standard boiling point of more than 280° C. within the above range, the ink composition is suitable for recording on a non-absorbent or low-absorbent recording medium in terms of drying properties. Examples of water-soluble low molecular weight organic compounds having a standard boiling point of more than 280° C. include glycerin.
[0122] It is preferable that the content of the water-soluble low molecular weight organic compound is 30% by mass or less relative to the total mass of the ink, and that the water-soluble low molecular weight organic compound having a normal boiling point of 210° C. or less is 50% by mass or more relative to the total mass of the water-soluble low molecular weight organic compounds. In such a case, there is a tendency for the ink to have an excellent balance between drying and solubility, and to have better abrasion resistance and clogging recovery properties. The content of the water-soluble low molecular weight organic compound is preferably 30% by mass or less, more preferably 28% by mass or less, even more preferably 26% by mass or less, and particularly preferably 25% by mass or less, based on the total mass of the ink. is not particularly limited, but is preferably 10% by mass or more, more preferably 15% by mass or more, and further preferably 20% by mass or more. The content of the water-soluble low molecular weight organic compound having a normal boiling point of 210° C. or less is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, and particularly preferably 70% by mass or more, based on the total mass of the water-soluble low molecular weight organic compound. The upper limit of the content is not particularly limited, but is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less. The standard boiling point of the water-soluble low molecular weight organic compound having a standard boiling point of 210° C. or less is more preferably 150 to 210° C. or less, further preferably 160 to 200° C. or less, and particularly preferably 170 to 200° C. or less. An example of the water-soluble low molecular weight organic compound having a standard boiling point of 210° C. or less is propylene glycol (standard boiling point 188° C.).
[0123] 1.4 Water The inkjet ink composition according to this embodiment is an aqueous ink containing water. The term "aqueous" refers to the inclusion of at least water as a solvent component, and may contain water as a main solvent component. Examples of water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, as well as water with reduced ionic impurities such as ultrapure water. Furthermore, by using water sterilized by ultraviolet irradiation or the addition of hydrogen peroxide, the growth of bacteria and fungi can be suppressed when the inkjet ink composition is stored for a long period of time.
[0124] The content of water in the liquid medium component is preferably 30% by mass or more, and more preferably 30 to 99% by mass. It is further preferably 30 to 95% by mass, more preferably 40 to 90% by mass, and even more preferably 50 to 80% by mass. The liquid medium is a solvent component such as water or a water-soluble low molecular weight organic compound.
[0125] The water content is preferably 40% by mass or more, more preferably 45% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more, relative to the total mass of the ink composition. The upper limit of the water content is not particularly limited, but is, for example, preferably 99% by mass or less, even more preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less, relative to the total mass of the ink composition.
[0126] 1.5 Surfactants The inkjet ink composition according to this embodiment may contain a surfactant that is not a dispersant for the resin particles. Such surfactants are not particularly limited, but include, for example, acetylene glycol surfactants, fluorine-based surfactants, and silicone-based surfactants. Among these, it is preferable to contain at least one of an acetylene glycol surfactant and a silicone-based surfactant. By containing such a surfactant, the dissolution time tends to be easily controlled within a preferred range, the surfactant is easy to obtain, and the filling property of the ink composition tends to be improved.
[0127] The acetylene glycol surfactant is not particularly limited, but for example, one or more selected from 2,4,7,9-tetramethyl-5-decyne-4,7-diol and alkylene oxide adducts of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, and 2,4-dimethyl-5-decyne-4-ol and alkylene oxide adducts of 2,4-dimethyl-5-decyne-4-ol are preferred. Commercially available acetylene glycol surfactants are not particularly limited, but for example, E series such as Olfin 104 series and Olfin E1010 (trade names manufactured by Air Products Japan, Inc.), Surfynol 465 and Surfynol 61 (trade names manufactured by Nissin Chemical Industry CO.,Ltd.) can be mentioned. The acetylene glycol surfactant may be used alone or in combination of two or more kinds.
[0128] The fluorosurfactant is not particularly limited, but examples thereof include perfluoroalkyl sulfonate, perfluoroalkyl carboxylate, perfluoroalkyl phosphate, perfluoroalkyl ethylene oxide adduct, perfluoroalkyl betaine, and perfluoroalkyl amine oxide compound. The commercially available fluorosurfactant is not particularly limited, but examples thereof include S-144, S-145 (manufactured by Asahi Glass Co., Ltd.); FC-170C, FC-430, and Fluorad-FC4430 (manufactured by Sumitomo 3M Co., Ltd.); FSO, FSO-100, FSN, FSN-100, and FS-300 (manufactured by Dupont Co., Ltd.); and FT-250 and 251 (manufactured by Neos Co., Ltd.). The fluorosurfactant may be used alone or in combination of two or more kinds.
[0129] Examples of silicone surfactants include polysiloxane compounds and polyether-modified organosiloxanes. Examples of commercially available silicone surfactants include, but are not limited to, BYK-306, BYK-307, BYK-333, BYK-341, BYK-345, BYK-346, BYK-347, BYK-348, and BYK-349 (all trade names, manufactured by BYK Japan K.K.), KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, KF-643, KF-6020, X-22-4515, KF-6011, KF-6012, KF-6015, and KF-6017 (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0130] The HLB of the surfactant is preferably 6 to 15, more preferably 7 to 14, even more preferably 11 to 14, and particularly preferably 11 to 13. When the HLB of the surfactant is within the above range, the dissolution time tends to be easily controlled within a preferred range, and surfactants having an HLB within the above range are easy to obtain, and the filling property of the ink composition also tends to be improved. Here, "HLB" is an abbreviation for Hydrophile-Lipophile Balance, and is defined by the Griffin method.
[0131] The surface tension of the surfactant is preferably 15 to 45 mN / m, more preferably 17.5 to 40 mN / m, and particularly preferably 20 to 35 mN / m. When the surface tension of the surfactant is within the above range, the ink composition tends to have improved embedding properties. The surface tension (mN / m) can be measured at a liquid temperature of 25°C by the Wilhelmy method using a surface tensiometer (such as the CBVP-Z surface tensiometer manufactured by Kyowa Interface Science Co., Ltd.).
[0132] The inkjet ink composition according to the present embodiment preferably contains 1% by mass or less of a surfactant that is not a dispersant for the resin particles, more preferably 0.8% by mass or less, and even more preferably 0.7% by mass or less. If the content of such a surfactant is within the above range, the abrasion resistance and clogging recovery tend to be more excellent. In addition, the lower limit of the content of such a surfactant is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.3% by mass or more.
[0133] 1.6 Other resins The inkjet ink composition according to this embodiment may contain a resin such as a dispersion resin or a water-soluble resin. By containing a dispersion resin or a water-soluble resin, the gloss of the obtained image tends to be further improved. The dispersion resin is not particularly limited, but examples thereof include polyvinyl alcohols, polyvinylpyrrolidones, polyacrylic acid, acrylic acid-acrylonitrile copolymers, vinyl acetate-acrylic acid ester copolymers, acrylic acid-acrylic acid ester copolymers, styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylic acid ester copolymers, styrene-α-methylstyrene-acrylic acid copolymers, and styrene-α-methylstyrene-acrylic acid-acrylic acid ester copolymers. Examples of the copolymer include copolymers, styrene-maleic acid copolymers, styrene-maleic anhydride copolymers, vinyl naphthalene-acrylic acid copolymers, vinyl naphthalene-maleic acid copolymers, vinyl acetate-maleic acid ester copolymers, vinyl acetate-crotonic acid copolymers, vinyl acetate-acrylic acid copolymers, and salts thereof. Among these, styrene-acrylic acid copolymers are preferred. As the form of the copolymer, any of random copolymers, block copolymers, alternating copolymers, and graft copolymers can be used. In addition, the copolymer may contain wax, but is not limited thereto. Examples of the wax include polyolefin wax such as polyethylene wax, and paraffin wax.
[0134] When wax is contained, the content thereof is preferably 0.01 to 5 mass % relative to the total mass of the ink composition, more preferably 0.1 to 3 mass %, even more preferably 0.1 to 1 mass %, particularly preferably 0.2 to 0.8 mass %, and more particularly preferably 0.3 to 0.7 mass %.
[0135] 1.7 Other Ingredients In order to maintain good storage stability and ejection stability from the head, to improve clogging, or to prevent deterioration of the ink, various additives such as dissolution aids, viscosity adjusters, pH adjusters, antioxidants, preservatives, antifungals, corrosion inhibitors, and chelating agents for capturing metal ions that affect dispersion may also be added as appropriate to the inkjet ink composition according to this embodiment.
[0136] 1.8 Method for producing ink-jet ink composition The inkjet ink composition according to this embodiment can be obtained by mixing the above-mentioned components (materials) in any order and removing impurities by filtering or the like as necessary. Here, when the ink contains a pigment, it is preferable to prepare the pigment in a state where it is uniformly dispersed in a solvent before mixing, since this makes handling easier. When preparing the pigment in a dispersed state beforehand, it is preferable to disperse it using a dispersant such as a dispersion resin.
[0137] The materials are preferably mixed by sequentially adding the materials to a vessel equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer, and stirring and mixing the materials. As a filtration method, for example, centrifugal filtration or filter filtration can be performed as necessary.
[0138] 1.9 Physical properties of ink-jet ink composition The surface tension of the ink composition at 25°C is preferably 20 to 50 mN / m, more preferably 20 to 40 mN / m. When the surface tension is within the above range, ejection stability tends to be good. The surface tension can be measured at a liquid temperature of 25°C by the Wilhelmy method using a surface tensiometer (such as the CBVP-Z surface tensiometer manufactured by Kyowa Interface Science Co., Ltd.).
[0139] The viscosity of the ink composition at 25°C is preferably 20 mPa·s or less, and more preferably 10 mPa·s or less. If the viscosity is within the above range, the ejection stability tends to be good. The viscosity can be measured using a viscometer.
[0140] The inkjet ink composition according to this embodiment may be an ink composition used in an inkjet recording method described below, or an ink composition used in an inkjet recording apparatus described below.
[0141] 2. Recording method A recording method according to one embodiment of the present invention includes an ink deposition step of ejecting the ink jet ink composition described above from an ink jet head and depositing it on a recording medium.
[0142]
[0046] According to the recording method of this embodiment, by using the inkjet ink composition described above, the abrasion resistance of the image recorded on the recording medium is improved, and the ability to recover from clogging of the nozzles of the inkjet head is also improved.
[0143] The recording medium, the recording device, and each process will be described below in that order.
[0144] 2.1 Recording medium The recording medium is not particularly limited, but examples thereof include absorbent recording media, low absorbent recording media, and non-absorbent recording media. According to the recording method of the present embodiment, a coating is formed on the surface of the image, thereby imparting abrasion resistance. Therefore, abrasion resistance is better when recording on a low absorbent recording medium into which ink is less likely to penetrate or a non-absorbent recording medium into which ink does not penetrate than on an absorbent recording medium into which ink is absorbed, so it is advantageous to use the recording method of the present embodiment.
[0145] Examples of the absorbent recording medium include, but are not limited to, plain paper such as electrophotographic paper having high ink composition permeability, inkjet paper, art paper used in general offset printing having relatively low ink composition permeability, coated paper, cast paper, etc. Examples of the inkjet paper include, but are not limited to, paper having an ink absorbing layer made of silica particles or alumina particles, or a hydrophilic polymer such as polyvinyl alcohol (PVA) or polyvinylpyrrolidone (PVP).
[0146] The low-absorbency recording medium is not particularly limited, but may be, for example, coated paper having a coating layer on the surface for receiving liquid. The coated paper is not particularly limited, but may be, for example, printing paper such as art paper, coated paper, and matte paper.
[0147] Non-absorbent recording media include, but are not limited to, plastic films and plates such as polyvinyl chloride, polyethylene, polypropylene, polyethylene terephthalate (PET), metal plates such as iron, silver, copper, aluminum, metal plates or plastic films produced by vapor deposition of these various metals, and alloy plates such as stainless steel and brass.
[0148] Here, a "low absorbency recording medium" and a "non-absorbency recording medium" are defined as recording media having a water absorption of 10 mL / m2 or less within 30 msec from the start of contact in the Bristow method. 2This refers to a recording medium that is as follows. The Bristow method is the most widely used method for measuring the amount of liquid absorbed in a short period of time, and is also adopted by the Japan Pulp and Paper Technical Association (JAPAN TAPPI). Details of the test method are described in Standard No. 51 "Paper and paperboard - Liquid absorbency test method - Bristow method" of the "JAPAN TAPPI Paper and Pulp Test Method 2000 Edition".
[0149] Non-absorbent recording media or low-absorbent recording media can also be classified according to the wettability of the recording surface to water. For example, a 0.5 μL water droplet is dropped onto the recording surface of the recording medium, and the contact angle drop rate (comparison of the contact angle at 0.5 milliseconds after impact with the contact angle at 5 seconds) is measured to characterize the recording medium. More specifically, in terms of the properties of the recording medium, the non-absorbency of a "non-absorbent recording medium" refers to a drop rate of less than 1%, and the low absorbency of a "low-absorbent recording medium" refers to a drop rate of 1% or more and less than 5%. Absorbency refers to a drop rate of 5% or more. The contact angle can be measured using a portable contact angle meter PCA-1 (manufactured by Kyowa Interface Science Co., Ltd.) or the like.
[0150] 2.2 Recording Device The inkjet recording apparatus that can be used in the present embodiment preferably includes an inkjet head that ejects the ink composition onto a recording medium, a head heating unit that heats the inkjet head, and a drying unit that dries the recording medium to which the ink composition is attached.
[0151] Fig. 1 is a schematic cross-sectional view showing an inkjet recording apparatus. As shown in Fig. 1, the recording apparatus 1 includes an inkjet head 2, an IR heater 3, a platen heater 4, a curing heater 5, a cooling fan 6, a pre-heater 7, and a ventilation fan 8.
[0152] The drying means is for accelerating the drying of the ink attached to the recording medium around the inkjet head 2. This is the drying means in the ink attachment process. The drying means may be a means using heat or air. The drying means is not particularly limited, but may be, for example, a ventilation fan 8, an IR heater 3, a platen heater 4, a preheater 7, etc. The ventilation fan 8 may blow hot air or room temperature air. When the drying means is a heating means, the inkjet head 2 may be heated by the drying means. For example, the inkjet head 2 may be directly heated by hot air or the IR heater 3, or the inkjet head 2 may be heated via a recording medium heated by a platen heater 4. Alternatively, the recording apparatus may be provided with a heating means for heating the inkjet head 2 (head heating means). By heating the inkjet head 2, the viscosity of the ink composition in the inkjet head 2 decreases, and the ink composition can be ejected satisfactorily. On the other hand, when the inkjet head 2 is heated, the ink composition inside the inkjet head 2 is subjected to heat, which causes clogging to occur, which becomes an issue.
[0153] Note that when the IR heater 3 is used, the recording medium can be heated from the inkjet head 2 side. As a result, the inkjet head 2 is also likely to be heated at the same time, but compared to heating from the back side of the recording medium using the platen heater 4, the temperature can be increased without being affected by the thickness of the recording medium. Also, when the platen heater 4 is used, the recording medium can be heated from the side opposite the inkjet head 2. As a result, the inkjet head 2 is relatively less likely to be heated.
[0154] In the recording apparatus 1, when the ink composition is ejected and adhered to the recording medium, the surface temperature of the recording medium is preferably set to 20 to 70° C. When the above-mentioned drying means by heating is used, the surface temperature is the surface temperature of the heated recording medium. The drying means accelerates the drying of the ink adhered to the recording medium, improving image quality, while the drying means using heat dissolves the resin particles adhered to the recording medium more quickly, forming a uniform coating film.
[0155] The recording apparatus may be provided with a post-drying means. The post-drying means heats and dries the recording medium to which the ink composition is attached after the ink attachment step. The post-drying means is not particularly limited, but examples thereof include a curing heater 5, a hot air mechanism (not shown), and a thermostatic bath (not shown). When the drying means heats the recording medium on which an image is recorded, the moisture contained in the ink composition evaporates and dissipates more quickly, and a coating is formed by the resin particles contained in the ink composition. In this way, the dried ink is firmly fixed (adhered) on the recording medium, and a high-quality image with excellent abrasion resistance can be obtained in a short time.
[0156] It should be noted that the above phrase "heating the recording medium" refers to raising the temperature of the recording medium to a desired temperature, and is not limited to directly heating the recording medium.
[0157] The recording apparatus 1 may have a cooling fan 6. After drying, the ink composition on the recording medium is cooled by the cooling fan 6, which tends to form a coating with good adhesion on the recording medium.
[0158] The recording apparatus 1 may include a preheater 7 for heating (preheating) the recording medium before the ink composition is ejected onto the recording medium. Preheating the recording medium before ejecting the ink composition tends to form a high-quality image with less bleeding on the recording medium, particularly on a non-absorbent or low-absorbent recording medium. The preheating temperature is preferably 80 to 120°C.
[0159] The recording apparatus 1 may be provided with a ventilation fan 8 so that the ink composition deposited on the recording medium can be dried more efficiently.
[0160] 2.3 Each step of the recording method <Drying process> The recording method according to this embodiment may include a drying step in which the ink attached to the recording medium is dried by the drying means described above. This step is carried out during the ink application step described below, and the ink composition applied to the recording medium is immediately dried. It is also called the primary drying step. Preferably, the ink is applied to a heated recording medium. And / or the ink droplets applied to the recording medium start to be dried in this step within 0.5 seconds after the ink droplets are applied. In particular, a step of using a drying means by heating (heating step) may be provided and is preferable. A drying step by heating is also called a heating step. In the drying step, the recording medium is heated so that the upper limit of the surface temperature is preferably 70°C or less, more preferably 65°C or less, even more preferably 60°C or less, even more preferably 55°C or less, and particularly preferably 53°C or less. In particular, it is 50°C or less, even more preferably 45°C or less, and even more preferably 43°C or less. On the other hand, the recording medium is heated so that the lower limit of the surface temperature is preferably 20°C or more, more preferably 30°C or more, even more preferably 35°C or more, more preferably 37°C or more, even more preferably 38°C or more, and particularly preferably 40°C or more. By keeping the surface temperature of the recording medium at 70°C or less, the heating of the inkjet head is suppressed, the nozzles during printing are suppressed, and clogging recovery tends to be improved. In addition, by keeping the surface temperature of the recording medium at 20°C or more, it is possible to suppress the dots of the ink composition on the recording medium from gathering together, which causes deterioration of image quality, and the image quality tends to be improved. In addition, the filling property of the dots of the ink composition on the recording medium, particularly on a non-absorbent recording medium such as vinyl chloride, is further improved.
[0161] When the above-mentioned recording apparatus 1 is used, the surface temperature of the recording medium can be controlled by using at least one of the IR heater 3, the platen heater 4, the ventilation fan 8, a pre-heater, and the like.
[0162] <Ink application process> The recording method according to this embodiment includes a step of ejecting the inkjet ink composition from an inkjet head and depositing it on a recording medium (ink depositing step). For example, when the inkjet head 2 is heated by the head heating means, the viscosity of the ink composition in the inkjet head 2 is reduced, improving the ability to recover from clogging.
[0163] FIG. 2 is an enlarged cross-sectional view showing a schematic diagram of the ink-jet head 2. The head 2 includes a pressure chamber 21 and an element 23 that applies pressure to the ink composition in the pressure chamber 21 to eject it from a nozzle 22, and the element 23 is disposed in the pressure chamber 21 at a position other than the position facing the outlet through which the ink composition moves toward the nozzle 22. In terms of the force pushing the ink out of the nozzle, it is advantageous from the viewpoint of preventing the resin from sticking 24 if the element 23 is disposed directly above the nozzle, but this is not preferable for reasons of head design, and it is advantageous in terms of design to have the element 23 located at a position other than directly above the nozzle, and the present invention is particularly useful in such cases. The element 23 can be formed using an electromechanical conversion element such as a piezoelectric element that changes the volume of a cavity by mechanical deformation, or an electrothermal conversion element that generates heat to generate bubbles in the ink and eject it.
[0164] In the pressure chamber 21, the position facing the outlet 25 communicating with the nozzle 22 is the region enclosed by the extension lines if a line is extended from the wall of the outlet 25 upward in the figure in Fig. 2. For example, in the head of Fig. 2, the outlet 25 is a portion whose area in the direction perpendicular to the ink ejection direction is the same as that of the nozzle 22. When the element 23 is disposed in a location other than the relevant position, it means that at least a part of the element 23 is not present in at least a part of this region. This is preferable in that there is a high degree of freedom in the design of the piezoelectric element and the pressure chamber.
[0165] It is preferable to perform recording for 1 hour or more without performing a process of applying pressure from the outside to the inkjet head 2 to discharge the ink composition from the nozzle. Here, the pressure applied from the outside is suction (negative pressure) or applying positive pressure from the upstream of the head, and is not ink discharge (flushing) by the function of the head itself. Incidentally, as long as pressure is not applied from the outside to discharge the ink, recording does not have to be continuous and may be paused. In this case, the cumulative time of recording is 1 hour or more. The above recording time is preferably 1 to 4 hours, more preferably 2 to 3 hours. With such a recording method, the resin is in a state where it is relatively easy to fix, so that the effect of this embodiment can be more effectively exhibited. In addition, it is preferable not to perform a process of applying pressure from the outside to the inkjet head 2 to discharge the ink composition from the nozzle during recording in a single recording. Furthermore, it is also preferable to perform a process of applying pressure from the outside to the inkjet head 2 to discharge the ink composition from the nozzle at least either before or after recording. In the above case, it is preferable in that the recording speed can be increased, the effect of this embodiment can be more effectively exhibited, and the ejection stability can be further improved.
[0166] <Post-drying process> The recording method according to the present embodiment may have a post-drying step of heating the recording medium by a post-drying means after the ink adhesion step. The post-drying step is also called a secondary drying step. The surface temperature of the recording medium in the post-drying step is preferably 50 to 110°C. This allows the resin particles contained in the ink composition on the recording medium to dissolve and form a recording material with good embedding properties. The surface temperature of the recording medium in the post-drying step is preferably 55°C or more and 100°C or less, more preferably 55°C or more and 90°C or less, more preferably 60°C or more and 80°C or less, and particularly preferably 65 to 75°C or less. It is also preferable that the maximum temperature of the recording medium in the post-heating step is within the above range. By setting the drying temperature within the above range, the abrasion resistance tends to be further improved.
[0167] 3. Working Example The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, "%" is based on mass unless otherwise specified.
[0168] 3.1 Manufacturing of composite resin particles <Production Example 1 of Resin Particles 1> A reaction vessel equipped with a stirrer, reflux condenser, dropping device, and thermometer was charged with ion-exchanged water. 350g and 0.25g of a surfactant shown in Table 1 below were charged, and the temperature was raised to 70°C while stirring and replacing with nitrogen. The internal temperature was kept at 70°C, and 2g of potassium persulfate was added as a polymerization initiator. After dissolving, an emulsion was prepared by adding 40g of ion-exchanged water, 0.25g of a surfactant shown in Table 1 below, 79g of methyl methacrylate, 8g of styrene, 11g of butyl acrylate, 1g of methacrylic acid, and 1g of acrylamide under stirring, and the emulsion was continuously dropped into the reaction solution over 3 hours (first resin). After the dropwise addition, aging was performed for 1 hour. After the aging, an emulsion was prepared by adding 80g of ion-exchanged water, 0.25g of a surfactant shown in Table 1 below, 81g of styrene, 15g of 2-ethylhexyl methacrylate, 2g of methacrylic acid, and 2g of acrylamide under stirring, and the emulsion was continuously dropped into the reaction solution over 4 hours (second resin). After the dropwise addition, aging was performed for 3 hours. The resulting aqueous emulsion was cooled to room temperature, and then ion-exchanged water and a neutralizing agent shown in Table 1 below were added to adjust the solid content to 30% by weight and the pH to 8. The resulting particles had a core-shell structure. <Production Example 2 of Resin Particles 26> Prepared with reference to WO2019143341(A1)Example 3. In a reaction vessel equipped with a stirrer, reflux condenser, dropping device, and thermometer, 470g of ion-exchanged water and 0.22g of Aqualon AR-10 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene styrenated propenyl phenyl ether sulfate ester ammonium salt) were charged, and the temperature was raised to 77°C while stirring and replacing with nitrogen. The internal temperature was kept at 77°C, and 0.6g of potassium persulfate was added as a polymerization initiator. After dissolution, an emulsion prepared by adding 30g of ion-exchanged water, 1g of Aqualon AR-10, 34.6g of methyl methacrylate, 64g of butyl acrylate, and 1.4g of methacrylic acid under stirring, and a solution prepared by adding 0.3g of potassium persulfate to 14g of ion-exchanged water were each dropped continuously into the reaction solution over 6 hours (first resin). After the dropping was completed, the mixture was aged for 1 hour. After the aging, an emulsion was prepared by adding 85g of ion-exchanged water, 1.2g of Aqualon AR-10, 140.5g of cyclohexyl methacrylate, 19.8g of cyclohexyl acrylate, 28.3g of 2-phenoxyethyl methacrylate, and 8.1g of methacrylic acid under stirring, and was continuously dropped into the reaction solution over 4 hours (second resin). After the dropping, the mixture was aged for 1 hour. The temperature was raised to 85°C, 3.3g of cyclohexyl acrylate was added, and the mixture was aged for 1 hour. After cooling to 70°C, 13g of 5% aqueous ascorbic acid solution and 26g of 5% aqueous tert-butyl hydroperoxide solution were added, and the mixture was aged for 1 hour. The obtained aqueous emulsion was cooled to room temperature, and then ion-exchanged water and an aqueous potassium hydroxide solution were added to adjust the solid content to about 30% by weight and the pH to 8. The obtained particles had a sea-island structure.
[0169] Based on Production Example 1 of the above-mentioned resin particle 1, the type and mass of each monomer used and the type of surfactant and neutralizer used were adjusted to produce core-shell structured resin particles having the physical properties of resin particles 2 to 20 and 22 to 25 in Table 1 below. Based on the first resin of Production Example 1 of the above-mentioned resin particle 1, single structured resin particles having the physical properties of resin particle 21 in Table 1 below were produced. Based on Production Example 2 of the above-mentioned resin particle 26, the mass of the surfactant used was adjusted to produce sea-island structured resin particles having the physical properties of resin particle 27 in Table 1 below. For each resin of the obtained composite resin particles, the glass transition temperature Tg (°C) was calculated as described above. The monomers used in the preparation of each resin particle are shown in Table 2.
[0170] The composite resin particles obtained above were then subjected to a Nanotrac WAVE II The average particle diameter (nm) of the composite resin particles was measured using a solubility tester (Microtrack Bell). Furthermore, the square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter for the composite resin particles, δph = √(δp 2 +δh 2 The mass ratio of the second resin to the first resin was determined from the mass of the monomers used in producing the composite resin particles.
[0171] [Table 1]
[0172] [Table 2]
[0173] The following provides additional explanation for Table 1 above. The "resin mass ratio w1 / w2" represents the mass ratio of the first resin to the second resin (first resin / second resin).
[0174] <Surfactant> Surfactant a: Adeka Reasoap SR-10 (trade name, manufactured by ADEKA Corporation, α-[2-[(allyloxy)-1-(alkyloxymethyl)]ethyl]-ω-polyoxyethylene sulfate ammonium salt), reactive surfactant Surfactant B: Sodium lauryl sulfate, a non-reactive surfactant Surfactant c: Aqualon AR-10 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene styrenated propenyl phenyl ether sulfate ester ammonium salt), reactive surfactant Surfactant d: Aqualon KH-10 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium salt), reactive surfactant Surfactant e: Aqualon KH-05 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium salt), reactive surfactant Surfactant f: LATEMURU PD-104 (product name, manufactured by Kao Corporation, polyoxyalkylene alkenyl ether ammonium sulfate, reactive surfactant
[0175] <Neutralizing agent> TEA: Triethanolamine NH3: Ammonia ·NaOH: Sodium hydroxide KOH: Potassium hydroxide In addition, "NH3 / NaOH" in Table 1 represents the combined use of ammonia and sodium hydroxide (a mixed solution with a molar ratio of 1:1). The monomers used in the preparation of each of the resin particles shown in Table 2 are shown below.
[0176] <First and second resins> MMA: Methyl methacrylate ST: Styrene ·BA: n-Butyl acrylate ·MAA: Methacrylic acid ·AAM: Acrylamide ·AN: Acrylonitrile 2EHMA: 2-Ethylhexyl methacrylate ·CHMA: Cyclohexyl methacrylate CHA: Cyclohexyl acrylate PHOEMA: Phenoxyethyl methacrylate
[0177] 3.2 Preparation of Inkjet Ink Composition Each material was mixed to obtain the composition shown in Tables 3 to 5 below, and thoroughly stirred to obtain a water-based inkjet ink composition. In the tables below, the units of values are % by mass, and the total is 100% by mass.
[0178] [Table 3]
[0179] [Table 4]
[0180] [Table 5]
[0181] The following provides additional explanations for Tables 3 to 5 above.
[0182] · CPL (ε-caprolactam, average molecular weight 113.16, solid at room temperature) 2P (2-pyrrolidone, average molecular weight 85.11, liquid at room temperature) DMPA (3-methoxy-N,N-dimethylpropanamide, average molecular weight 131.18, liquid at room temperature) ·PG (Propylene Glycol) 1,2HD (1,2-Hexanediol) 1,3PD (1,3-propanediol) HEP (N-hydroxyethyl-2-pyrrolidone) BYK-348 (BYK Japan Co., Ltd., silicone surfactant) AQUACER515 (manufactured by BYK Japan Co., Ltd., polyethylene wax emulsion)
[0183] 3.3 Evaluation method <Inkjet recording method> The recording device used was an inkjet printer (product name: modified SC-R5050, manufactured by Seiko Epson Corporation) equipped with a platen heater and the inkjet head shown in Fig. 2. Each of the inkjet ink compositions prepared above was filled into two adjacent nozzle rows (each nozzle row had 400 nozzles, 300 npi nozzle density) of the head of the recording device, and ejected onto Orajet 3165G-010 (Olafor Japan Co., Ltd., PVC film) to print a cyan solid pattern with a resolution of 1200 dpi vertical x 1200 dpi horizontal, with 8 scans, with an ink deposition amount of 12 mg / inch. 2 During this printing, the platen heater was operated to set the surface temperature of the recording medium to 40°C as the primary drying (drying process) of the recording medium at the location receiving the ink. In addition, the curing heater was set to a secondary drying temperature shown in Table 6 below as the surface temperature of the recording medium, and secondary drying (post-drying process) was performed. Note that a solid pattern refers to a pattern in which ink is uniformly applied to achieve the ink adhesion amount described below.
[0184] <Abrasion resistance> As described above, the modified SC-R5050 machine was filled with ink, and a solid pattern (ink deposition amount 12 mg / inch) was printed on the recording medium. 2 ) was printed on the paper. After leaving it at room temperature for 30 minutes, the ink-attached area was cut into a 30 x 150 mm rectangle and rubbed 50 times with a water-dampened plain-woven cloth using a Gakushin-type abrasion resistance tester (load 500 g). The degree of ink peeling was visually observed and evaluated according to the following criteria. A rating of C or higher indicates good abrasion resistance. (Evaluation Criteria) AA: No peeling. A: Less than 20% of the evaluation area has peeled off. B: Less than 50% of the evaluation area has peeled off. C: Peeling occurred on 50% to less than 80% of the evaluation area. D: More than 80% of the evaluation area has peeled off.
[0185] <Clogging recovery> After filling a modified SC-R5050 with ink, the nozzle surface was struck with a water-dampened Bemcot to intentionally cause nozzle clogs. In this state, the printer was left idle for two hours in an environment of 40°C and 15% relative humidity. After recording under the above recording conditions, cleaning was performed three times and the number of unrecovered nozzles was counted and evaluated according to the following evaluation criteria. For each cleaning, 1g of ink was discharged from the nozzle group. The nozzle group consists of two nozzle rows, each containing 800 nozzles. A rating of B or higher can be said to indicate good clogging recovery. (Evaluation Criteria) AA: No nozzle non-ejection. A: Less than 1% of nozzles fail. B: Nozzle non-discharge rate is 1% or more but less than 3%. C: Nozzle non-ejection rate 3% or more.
[0186] <Thermal deformation of substrate> As described above, the modified SC-R5050 machine was filled with ink, and a solid pattern (ink deposition amount 12 mg / inch) was printed on the recording medium. 2 The resulting print was visually inspected for substrate deformation and evaluated according to the following criteria. (Evaluation Criteria) A: No deformation of the recording medium occurs. B: Deformation of the recording medium occurs, but is tolerable. C: Deformation of the recording medium occurs and is unacceptable.
[0187] 3.4 Evaluation results The evaluation results are shown in Table 1 above and Table 6 below. The evaluation results in Table 1 are a portion of the evaluation results for Examples 1 to 20 and Comparative Examples 1 to 7, which have the same composition except that the resin particles contained in the ink are different in each example in Table 6.
[0188] [Table 6]
[0189] As a result of the evaluation, it was found that the water-based ink containing a coloring material, resin particles, and a water-soluble low-molecular-weight organic compound was an amide having a normal boiling point of 215 to 290°C. The ink composition contains 0.5 to 9.0% by mass of the resin particles, and the resin particles are composite resin particles made of a first resin and a second resin, which are acrylic resins. The first resin and the second resin are each a square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter δph=√(δp 2 +δh 2 ) but the δph1 of the first resin is 4.0 to 4.8 MPa 1 / 2 and δph2 of the second resin is more than 2.6 and less than 3.7 MPa. 1 / 2 It was found that all of the Examples, which were ink-jet ink compositions having the above-mentioned structure, were excellent in both abrasion resistance and clogging recovery properties, whereas all of the Comparative Examples, which were ink-jet ink compositions having the above-mentioned structure, were inferior in either abrasion resistance or clogging recovery properties.
[0190] Specifically, the results of Examples 1 to 20 show that various resin particles were excellent in both abrasion resistance and clogging recovery properties. It should be noted that, from the results of Examples 1 to 6, when the mass ratio of the first resin to the second resin (first resin / second resin) was within a predetermined range, the abrasion resistance and clogging recovery properties were particularly excellent. From the results of Examples 1 and 7 to 9, when Δph1 of the first resin and Δph2 of the second resin were within a predetermined range, and when the acid value was within a predetermined range, the abrasion resistance and clogging recovery properties were particularly excellent. The results of Examples 1, 10, and 11 show that when the resin particles were dispersed with a reactive surfactant, the abrasion resistance and clogging recovery properties were particularly excellent. The results of Examples 1, 12, and 13 show that when the volume average particle size of the resin particles was within a predetermined range, the abrasion resistance and clogging recovery properties were particularly excellent. The results of Examples 1 and 14 to 16 show that the resin particles neutralized with at least an organic amine or ammonia were particularly excellent in abrasion resistance and clogging recovery properties. The results of Examples 1 and 17 to 20 show that the resin particles using various reactive surfactants had excellent abrasion resistance and clogging recovery properties.
[0191] The results of Examples 1, 21 to 24, and 27 to 29 show that when the content of the water-soluble low molecular weight organic compound was a predetermined amount or less relative to the total mass of the ink, and the amount of the water-soluble low molecular weight organic compound having a normal boiling point of 210°C or less was a predetermined amount or more relative to the total mass of the water-soluble low molecular weight organic compound, the abrasion resistance and clogging recovery properties were particularly excellent.
[0192] The results of Examples 1, 25, and 26 show that by using various amides having normal boiling points of 215 to 290° C., excellent abrasion resistance and clogging recovery could be achieved. From the results of Examples 21 and 22, the lower the temperature in the post-drying step, the better the suppression of thermal deformation of the substrate. This shows that the ink composition of the present embodiment is superior in that it can provide excellent abrasion resistance even when the temperature in the post-drying step is relatively low. Although not shown in the table, Example 21 was performed in the same manner as Example 21 except that the surface temperature of the recording medium in the primary drying step was 35° C., and the clogging recovery was rated A, and some deterioration in image quality was observed in the pattern. This demonstrates that the ink composition of the present embodiment is superior in that it can provide excellent clogging recovery even when the temperature in the primary drying step is relatively high.
[0193] In contrast to this, in Comparative Examples 1 to 7, since Δph1 of the first resin and Δph2 of the second resin in the composite resin particles were outside the specified range, either the abrasion resistance or the clogging recovery property was poor. In addition, it is presumed that in Comparative Example 4, the Δph2 of the second resin exceeded the specified range, which promoted dissolution of the resin particles and resulted in poor clogging recovery. In Comparative Example 5, the Δph2 of the second resin was below the specified range, which resulted in too low hydrophilicity, poor dispersion stability in water, and poor clogging recovery.
[0194] In Comparative Examples 8 to 11, the content of the amides having a normal boiling point of 215 to 290° C. was outside the specified range, and therefore at least either the abrasion resistance or the clogging recovery property was poor.
[0195] The following can be derived from the above-described embodiment.
[0196] One embodiment of the inkjet ink composition comprises: A water-based ink containing a color material, resin particles, and a water-soluble low-molecular-weight organic compound, the water-soluble low-molecular-weight organic compound contains an amide having a normal boiling point of 215 to 290° C. in an amount of 0.5 to 9.0% by mass relative to the total mass of the ink composition; the resin particles are composite resin particles composed of a first resin and a second resin, each of which is an acrylic resin; The first resin and the second resin are the square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter δph=√(δp 2 +δh 2 ) wherein Δph1 of the first resin is 4.0 to 4.8 MPa 1 / 2 and Δph2 of the second resin is more than 2.6 and less than 3.7 MPa. 1 / 2 It is.
[0197] In one embodiment of the inkjet ink composition, The composite resin particles may have a phase-separated structure in which a phase made of the first resin and a phase made of the second resin are separated, and the phase made of the first resin may be encapsulated in the phase made of the second resin.
[0198] In any of the embodiments of the ink-jet ink composition described above, The composite resin particles may have a mass ratio of the first resin to the second resin (first resin / second resin) of 0.5 to 2.
[0199] In any of the embodiments of the ink-jet ink composition described above, The content of the water-soluble low molecular weight organic compound may be 30 mass % or less relative to the total mass of the ink, and the water-soluble low molecular weight organic compound having a normal boiling point of 210°C or less may be 50 mass % or more relative to the total mass of the water-soluble low molecular weight organic compounds.
[0200] In any of the embodiments of the ink-jet ink composition described above, The composite resin particles may be resin particles dispersed with a reactive surfactant.
[0201] In any of the embodiments of the ink-jet ink composition described above, The reactive surfactant may be anionic.
[0202] In any of the embodiments of the ink-jet ink composition described above, The reactive surfactant may have an oxyalkylene group.
[0203] In any of the embodiments of the ink-jet ink composition described above, The composite resin particles may be soap-free type resin particles.
[0204] In any of the embodiments of the ink-jet ink composition described above, The composite resin particles may have a volume average particle diameter of 90 to 250 nm.
[0205] In any of the embodiments of the ink-jet ink composition described above, The composite resin particles may be resin particles neutralized with at least an organic amine or ammonia.
[0206] In any of the embodiments of the ink-jet ink composition described above, The composite resin particles may have an acid value of 5 to 35 mgKOH / g.
[0207] In any of the embodiments of the ink-jet ink composition described above, The first resin and the second resin may have a glass transition temperature of 60 to 95°C.
[0208] In any of the embodiments of the ink-jet ink composition described above, The inkjet ink composition may contain 1% by mass or less of a surfactant that is not a dispersant for the resin particles.
[0209] One aspect of the recording method is The method includes an ink deposition step of ejecting the ink-jet ink composition from an ink-jet head and depositing it on a recording medium.
[0210] In one embodiment of the recording method, The ink application step may be followed by a post-drying step of heating the recording medium at 50 to 110°C.
[0211] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the present invention includes a configuration that is substantially the same as the configuration described in the embodiment, for example, a configuration that has the same function, method, and result, or a configuration that has the same purpose and effect. The present invention also includes a configuration in which non-essential parts of the configuration described in the embodiment are replaced. The present invention also includes a configuration that has the same action and effect as the configuration described in the embodiment, or a configuration that can achieve the same purpose. The present invention also includes a configuration in which publicly known technology is added to the configuration described in the embodiment. [Explanation of symbols]
[0212] Reference Signs List 1: Recording device, 2: Inkjet head, 3: IR heater, 4: Platen heater, 5: Curing heater, 6: Cooling fan, 7: Preheater, 8: Ventilation fan, 21: Pressure chamber, 22: Nozzle, 23: Element, 24: Resin adhesion, 25: Outlet
Claims
1. A water-based ink containing a color material, resin particles, and a water-soluble low-molecular-weight organic compound, the water-soluble low-molecular-weight organic compound contains amides having a normal boiling point of 215 to 290° C. in an amount of 0.5 to 9.0% by mass relative to the total mass of the ink composition; the resin particles are composite resin particles made of a first resin and a second resin, each of which is an acrylic resin; The first resin and the second resin are the square root of the polar component δp and the hydrogen bond component δh of the Hansen solubility parameter δph = √(δp 2 + δ h 2 ) The δph1 of the first resin is 4.0 to 4.8 MPa. 1/2 The second resin has a δph2 of more than 2.6 and less than 3.7 MPa. 1/2 The ink-jet ink composition according to claim 1,
2. 2. The ink-jet ink composition according to claim 1, wherein the composite resin particles have a phase-separated structure in which a phase composed of the first resin and a phase composed of the second resin are separated, and the phase composed of the first resin is encapsulated in the phase composed of the second resin.
3. 2. The ink-jet ink composition according to claim 1, wherein the composite resin particles have a mass ratio of the first resin to the second resin (first resin / second resin) of 0.5 to 2.
4. 2. The ink-jet ink composition according to claim 1, wherein a content of the water-soluble low-molecular-weight organic compound is 30% by mass or less relative to the total mass of the ink, and a content of the water-soluble low-molecular-weight organic compound having a normal boiling point of 210° C. or less is 50% by mass or more relative to the total mass of the water-soluble low-molecular-weight organic compounds.
5. The ink-jet ink composition according to claim 1 , wherein the composite resin particles are resin particles dispersed with a reactive surfactant.
6. The ink-jet ink composition of claim 5 , wherein the reactive surfactant is anionic.
7. The ink-jet ink composition according to claim 5 , wherein the reactive surfactant has an oxyalkylene group.
8. The ink-jet ink composition according to claim 1 , wherein the composite resin particles are soap-free type resin particles.
9. 2. The ink-jet ink composition according to claim 1, wherein the composite resin particles have a volume average particle diameter of 90 to 250 nm.
10. The ink-jet ink composition according to claim 1 , wherein the composite resin particles are resin particles neutralized with at least an organic amine or ammonia.
11. 2. The ink-jet ink composition according to claim 1, wherein the composite resin particles have an acid value of 5 to 35 mgKOH / g.
12. 2. The ink-jet ink composition according to claim 1, wherein the first resin and the second resin have a glass transition temperature of 60 to 95.degree.
13. The ink-jet ink composition according to claim 1 , further comprising 1% by mass or less of a surfactant that is not a dispersant for the resin particles.
14. A recording method comprising an ink depositing step of ejecting the ink-jet ink composition according to claim 1 from an ink-jet head and depositing the ink-jet ink composition on a recording medium.
15. The recording method according to claim 14, further comprising a post-drying step of heating the recording medium at 50 to 110° C. after the ink application step.
Citation Information
Patent Citations
Ink composition and recording method
JP2017203077A
Cited By
Aqueous ink, ink cartridge and ink jet recording method
EP4806961A1