Method for manufacturing structure comprising cavities
The method of vacuum welding and hot isostatic pressing diffusion welding addresses the challenges of complex cavity formation in structures by ensuring airtight, strong, and cost-effective assembly of diverse materials, achieving precise and complex geometries.
Patent Information
- Application Number
- JP2024049766
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for manufacturing structures with cavities, such as heat exchangers, face challenges in achieving complex geometries without deformation, displacement, or shearing, and often result in poor mechanical strength and high machining costs.
A method involving resistance welding, electron beam welding, or transparent laser welding under vacuum, followed by hot isostatic pressing diffusion welding, to form airtight cavities with complex shapes, using materials like copper, titanium, aluminum, or steel alloys, ensuring uniform welds and minimal residual stresses.
Enables the production of structures with complex cavities that are airtight, mechanically strong, and cost-effective, avoiding deformation and shearing, while allowing for precise assembly of materials with different chemical compositions.
Smart Images

Figure 2024139767000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of heat exchange, and more generally to structures comprising cavities, for example fluid circulation channels.
[0002] The present invention relates to a method for manufacturing a structure containing a cavity.
[0003] The present invention also relates to a structure including a cavity.
[0004] The present invention has applications in many industrial sectors, and in particular in the manufacture of heat exchangers.
[0005] The invention is of particular interest since it makes it possible to obtain elements that are provided with cavities, the cavities possibly having a simple or complex shape. [Background technology]
[0006] Currently, several methods are available for producing structures with recessed portions.
[0007] A first solution consists in producing components by additive manufacturing (or 3D printing). It is possible to obtain parts with complex geometries that have good mechanical properties. However, dimensional and geometric tolerances are often not respected.
[0008] A second solution consists in forming the channels by removing material in a solid basic part, but such machining techniques do not make it possible to obtain all the desired geometries, cross sections and lengths of the channels.
[0009] A third solution consists in assembling the elementary parts together by various techniques such as, for example, fusion welding, brazing or diffusion welding.
[0010] Diffusion welding is currently one of the most promising techniques, and more specifically Hot Isostatic Pressing (HIP) welding. Pressing is obtained by applying pressurized gas over all of the walls of the components to be assembled. There are three methods to create components with recessed parts with this technique:
[0011] The first method, shown in Figure 1, consists in using a tube 1 sandwiched between two grooved plates 2, 3. The shape of the grooves is identical to the tube. The tube can be pre-deformed to obtain different cross sections (e.g. square, rectangular) or to have different lengthwise curvatures.
[0012] However, this first method only results in recessed areas of simple geometric shapes.
[0013] A second method, shown in FIG. 2, consists in carrying out the assembly by two diffusion welding cycles. Such a method is described in document WO 2011 / 026925 A1. Several plates 4, 5, including at least one grooved plate, are superimposed. A bead is placed between the two plates. Processing steps are carried out to carry out welding by diffusion of the material bead on the plates 4, 5. A first cycle is carried out at low pressure. The recessed parts are closed at the ends. Diffusion welding is carried out, since gas does not penetrate the contact surfaces. The joint is gas-tight. However, large-sized pores remain and the assembly has low mechanical strength. The method therefore includes a step of joining the assembly by hot isostatic pressing in order to carry out diffusion welding of the elements of the assembly. This cycle is started at high pressure and the recessed parts are open to close the pores and hold down the joint.
[0014] The main drawback of this second method is that it is almost impossible to produce a recessed portion without deforming it: in fact, during the first cycle, the channel can be deformed, since there is no pressure inside it.
[0015] To avoid deformation / collapse of the channels, it is possible to insert a material into the channels that can later be eliminated or removed, for example chemically or mechanically. For example, such a solution is described in the document JP 2006 / 263746. However, it can be difficult not only to find a suitable filler material, but also to succeed in completely eliminating the filler material.
[0016] A third method consists in laser welding a thin-walled plate 6 onto a channel formed in a substrate 7 and then welding a cap 8 onto the resulting assembly. For example, this method is shown in FIG. 3. Such a method is also described in document WO2006 / 067349A1. More precisely, this method comprises the following steps: - providing a substrate 7 in which a groove is made to form the bottom of the recessed portion (FIG. 4A); - placing a thin-walled blade 6 on top of the groove to close the recessed portion (FIG. 4B); - welding the blade 6 to the substrate 7 by edge / edge laser welding to ensure gas tightness (FIG. 4C); - depositing a cap 8 onto the assembly formed by the substrate 7 and the blade 6 (FIG. 4D); - welding the substrate 7 and the cap 8 by hot isostatic pressing (FIG. 4E); Includes.
[0017] However, this last method has many drawbacks: in particular, the engagement of the thin blade in the groove requires strict width tolerances (0.1 mm), which not only increases the machining costs but also complicates the method, since it remains difficult to engage and weld the thin blade in the engagement without deformation, displacement and / or misalignment, especially when the blade is brought into a recessed portion of complex shape. [Prior art documents] [Patent documents]
[0018] [Patent Document 1] International Publication No. 2011 / 026925 [Patent Document 2] JP 2006 / 263746 A [Patent Document 3] International Publication No. 2006 / 067349 Summary of the Invention [Problem to be solved by the invention]
[0019] The present invention aims to provide a method that overcomes the drawbacks of the prior art, in particular a method that makes it possible to form structures comprising cavities, possibly with simple or complex shapes, while avoiding the phenomena of deformation, displacement and / or slippage. [Means for solving the problem]
[0020] To this end, the invention relates to a method for manufacturing a structure comprising a cavity, comprising the following steps: a) forming a recessed area in a first surface of a substrate made of a first material; b) placing a plate made of a second material on the first surface of the substrate so as to cover the recessed area of the substrate; c) performing resistance welding, electron beam welding, or transparent laser welding, preferably under vacuum, around the recessed area, thereby welding the plate onto the substrate and forming a cavity; d) performing a step of hot isostatic pressing diffusion welding on the assembly obtained; The present invention provides a method comprising:
[0021] The present invention differs from the prior art essentially in placing a plate on the substrate and performing a step of penetration welding of the plate onto the substrate, preferably under vacuum, over the entire contour of the recessed area of the substrate to form an airtight cavity. The welding can consist of transparent resistance welding, transparent electron-beam welding or penetration laser welding. This step ensures airtightness at the substrate / plate joint. Thus, not only are the boundaries of the cavity sealed, but in addition, this step limits and possibly avoids contamination / oxidation of the enclosed surfaces.
[0022] The use of a vacuum environment makes it possible to obtain a thinner and more penetrating weld bead at the same beam power as under neutral gas. The weld is made through the plate at the plate / substrate interface.
[0023] Hot isostatic pressing diffusion welding makes it possible to complete the assembly.
[0024] Advantageously, during step c), a full laser weld is performed over the contour of the plate.
[0025] Since the weld bead is thin and the atmosphere is homogeneous under vacuum (it is not necessary to have a gaseous protection along with the melt, as when welding under neutral gases), it is possible to weld cavities of small width and / or weld at the bottom of narrow, deep wells.
[0026] Advantageously, after step c), a degassing step is carried out at the plate / substrate interface.
[0027] According to this advantageous variant, the method comprises, between steps c) and d), the following successive steps: - placing a cowl on the plate; - welding the cowl onto the plate; Includes.
[0028] Advantageously, after welding the cowl onto the plate, the method includes a step in which a degassing step is performed at the plate / cowl interface.
[0029] Advantageously, the cowl is welded onto the plate by through-hole laser welding, preferably under vacuum.
[0030] Advantageously, the first material and the second material are independently selected from copper and its alloys, titanium and its alloys, aluminum and its alloys, steel, and vanadium. The first material and the second material may be the same or different.
[0031] The method has many advantages, namely: - to obtain uniform welds (in terms of chemical composition and microstructure) with little residual stress, - assembling materials that are identical (steel, aluminum alloys, titanium alloys, copper alloys, etc.) with one another or that have very different chemical compositions (for example steel / copper, steel / vanadium assemblies, etc.); - has lower implementation costs, in particular lower machining costs, compared to prior art methods; - the ability to manufacture structures with cavities of complex shapes; - Avoid deformation phenomenon; - Do not carry out the bite alignment step has.
[0032] The invention also relates to a structure obtainable by such a method, the structure comprising: - a substrate made of a first material, the substrate having a recessed area on a first side thereof; - a plate made of a second material covering the recessed area of the substrate, the plate being welded onto the substrate around the recessed area by welds preferably obtained by transmission, resistance welding, laser welding and electron beam welding under vacuum, as well as by hot isostatic pressing diffusion, the recessed area being bounded by the substrate and the plate to form a cavity; - a cowl welded onto the plate; Equipped with.
[0033] Advantageously, the first and second materials are independently selected from copper and its alloys, titanium and its alloys, aluminum and its alloys, steel, and vanadium. The first material may be the same as or different from the second material.
[0034] Advantageously, the structure is a heat exchanger comprising cavities arranged to cause a fluid circulation, the cavities forming channels for the circulation of a fluid, i.e. a gas or a liquid (for example a mixture of N2, water, molten metal).
[0035] Other features and advantages of the invention will become apparent from the following complementary description.
[0036] Of course, this complementary description is given merely as an illustration of the objectives of the present invention and should not be construed as limiting this objective in any way.
[0037] The invention will be better understood on reading the description of embodiments given purely for illustrative and non-limiting purposes with reference to the accompanying drawings, in which: [Brief description of the drawings]
[0038] [Figure 1] FIG. 1 is a diagram of the prior art embodiment previously described. [Diagram 2] FIG. 1 is a diagram of the prior art embodiment previously described. [Diagram 3] FIG. 1 is a diagram of the prior art embodiment previously described. [Figure 4A] FIG. 2 is a diagram of steps of the prior art method previously described. [Figure 4B] FIG. 2 is a diagram of steps of the prior art method previously described. [Figure 4C]FIG. 2 is a diagram of steps of the prior art method previously described. [Figure 4D] FIG. 2 is a diagram of steps of the prior art method previously described. [Figure 4E] FIG. 2 is a diagram of steps of the prior art method previously described. [Figure 5A] FIG. 2 is a diagram of method steps according to a particular embodiment of the invention. [Figure 5B] FIG. 2 is a diagram of method steps according to a particular embodiment of the invention. [Figure 5C] FIG. 2 is a diagram of method steps according to a particular embodiment of the invention. [Figure 5D] FIG. 2 is a diagram of method steps according to a particular embodiment of the invention. [Figure 6A] FIG. 4 is a diagram of method steps according to another particular embodiment of the invention. [Figure 6B] FIG. 4 is a diagram of method steps according to another particular embodiment of the invention. [Figure 6C] FIG. 4 is a diagram of method steps according to another particular embodiment of the invention. [Figure 6D] FIG. 4 is a diagram of method steps according to another particular embodiment of the invention. [Figure 6E] FIG. 4 is a diagram of method steps according to another particular embodiment of the invention. [Figure 7A] 1 is a schematic three-dimensional view of a substrate used to carry out a method according to a particular embodiment of the present invention; [Figure 7B] 1 is a schematic three-dimensional view of a substrate used to carry out a method according to a particular embodiment of the present invention; [Figure 8] Photographs of different substrates used to carry out a method according to another particular embodiment of the present invention. [Figure 9] 9 is a photograph of the different structures obtained after transparent laser-in-vacuum welding of the plate onto the different substrates of FIG. 8 according to another specific embodiment of the invention. [Figure 10]FIG. 10 is a metallographic cross-section of a weld in one of the structures shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] The various parts shown in the figures are not necessarily drawn to scale in order to make the figures more legible.
[0040] It should be understood that the various possibilities (variants and embodiments) are not mutually exclusive and can be combined with one another.
[0041] Additionally, in the following description, terms that depend on orientation, such as the "top" and "bottom" of a structure, are applied with respect to the structure being oriented in the manner shown in the figures.
[0042] Although this is in no way limiting, the invention finds particular application in the manufacture of structures including channels for the circulation of a fluid, particularly but not exclusively, intended for heat exchange between two fluids.
[0043] A method for manufacturing a structure with a cavity will now be described in more detail with reference to the accompanying Figures 5A to 5F, which comprises the following steps: a) forming a recessed area 110 on a first surface 101 of a substrate 100 made of a first material (FIG. 5A); b) placing a plate 200 made of a second material on the first side 101 of the substrate 100 so as to cover the recessed area of the substrate 100 (FIG. 5B); c) resistance welding, electron beam welding or penetration laser welding, preferably under vacuum, around the recessed area, thereby welding the plate 200 onto the substrate 100 and forming an airtight cavity (FIG. 5C); d) carrying out a step of hot isostatic pressing diffusion welding on the resulting assembly (FIG. 5D); Includes.
[0044] According to one variant, the method further comprises, between steps c) and d), the steps of placing a cowl 300 on the plate 200 and welding the cowl 300 to the plate 200. Thus, according to this variant, for example illustrated in figures 6A to 6E, the method comprises the following steps: a) forming a recessed area 110 on a first surface 101 of a substrate 100 made of a first material (FIG. 6A); b) placing a plate 200 made of a second material on the first side 101 of the substrate 100 so as to cover the recessed area 110 of the substrate 100 (FIG. 6B); c) resistance welding, laser welding or electron beam welding, preferably under vacuum, around the recessed area 110, thereby welding the plate 200 onto the substrate 100 and forming an airtight cavity (FIG. 6C); - placing the cowl 300 on the plate 200; - welding the cowl 300 onto the plate 200 (FIG. 6D); d) carrying out a step of hot isostatic compression diffusion welding on the resulting assembly (FIG. 6E); Includes.
[0045] The substrate 100 comprises a first side 101 and a second side 102. The first side 101 can be parallel to the second side 102. The first side 101 may not be parallel to the second side 102. For example, the first side 101 may be planar (FIG. 7A) or contoured (FIG. 7B).
[0046] During step a), the substrate 100 is machined to form recessed regions. The recessed regions 110 may have a simple shape (e.g., a longitudinal shape). For example, the recessed regions consist of grooves (i.e., longitudinal cutouts that may be narrow). The recessed regions may also have a complex shape (e.g., may have turns, zigzags).
[0047] The recessed regions 110 may have a wide variety of cross-sections and paths. Specifically, the recessed regions 110 may have rectangular, polygonal, or semicircular cross-sections. The recessed regions 110 may also have cross-sections that vary along their length. The paths of the recessed regions 110 may or may not be linear. The paths may feature back and forth segments and / or tight turns.
[0048] The recessed regions may be made in 2D (ie in the same plane (x, y)) or in 3D (ie their position may vary within the plane (x, y, z)).
[0049] Advantageously, each recessed area 110 is open at least at one of its ends. Preferably, the recessed area has two ends, the two ends being open in communication.
[0050] In a particular embodiment, recessed regions 110 can be formed on the first side 101 and the second side 102 of the substrate 100. Another plate can then be placed on the second side 102 of the substrate 100, such that the substrate is sandwiched between the two plates. This embodiment allows for a compact structure to be formed.
[0051] Advantageously, all surfaces to be assembled are cleaned and / or pretreated (e.g. by chemical pickling or light machining) to obtain clean surfaces and to improve the properties (e.g. mechanical or electrical properties) of the joints.
[0052] The plate 200 used during step b) is selected so that it is possible to weld it onto the substrate by penetration welding. The plate 200 is placed on the substrate 100 and aligned. Since the plate 200 is a solid plate, this adjustment is easy to perform. The surface of the plate 200 covers at least all of the recessed area 110. The surface of the plate 200 preferably covers the entire first side 101 of the substrate 100.
[0053] Advantageously, the plate 200 and the substrate 100 are cleaned and / or machined before being assembled in order to remove surface oxides that may be present on the surfaces of those parts and / or to have a good roughness. Thus, the cleanliness of the joint to be assembled is guaranteed. This step leads to an improvement of the mechanical properties at the joint.
[0054] According to a first variant, the plate 200 can function as a cap. This makes it possible to reduce the number of steps and elements necessary for the implementation of the method. The costs are therefore reduced. The thickness of the plate 200 is chosen to be small enough to obtain a tight weld with the substrate 100.
[0055] According to another variant, a cowl 300 is then welded onto the plate 200. The cowl 300 acts as a cap. The surface of the cowl 300 corresponds at least to the surface of the plate 200. The cowl 300 is of counter-form, which allows adding material if necessary.
[0056] According to this variant, plate 200 may also include a recessed area. The recessed area of the plate may be blocked by cowl 300. Cowl 300 may have no recessed area or may have a recessed area.
[0057] According to this variant, the thickness of the plate 200 may be less than in the variant in which the plate also functions as a cap.
[0058] The first material of the substrate 100 and the second material of the plate 200 may be the same (ie, comprised of a homogenous mass).
[0059] Alternatively, the first material and the second material may be different (ie, comprised of a heterogeneous mass).
[0060] The first and second materials may be selected independently from copper and its alloys, titanium and its alloys, aluminum and its alloys, steel, and vanadium. During step c), the face of the plate 200 placed opposite the first face 101 of the substrate 100 and the first face 101 of the substrate 100 form contact surfaces to be welded by diffusion.
[0061] The plate 200 is welded onto the substrate 100. The weld is made over the entire contour of the recessed area 110. The resulting weld 210 follows the contour of the recessed area 110 (FIGS. 5C, 6C). The periphery of the contact surfaces is welded in an airtight and degassed manner.
[0062] With welding, the use of brazing is not necessary, and therefore the maximum temperature at which the resulting element can be used is increased.
[0063] The penetration welding can be performed by laser welding, electron beam welding or resistance welding. Advantageously, in the case of resistance welding, the thickness of the elements to be welded is typically less than 3 mm. Resistance welding can be performed under air, under a controlled atmosphere or under vacuum.
[0064] This step is preferably performed by laser welding, and more preferably consists of vacuum penetration laser welding.
[0065] It is possible to form two weld beads for each recessed area 110. Nonetheless, if the recessed areas are very close to each other, a single weld bead may be sufficient.
[0066] The welding conditions are selected to achieve a gas tightness at the substrate / plate joint.
[0067] Thus, the pressurized gas applied during the hot isostatic pressing (HIP) cycle and penetrating the recessed portions is not present at the substrate 100 / plate 200 interface between the two laser weld beads.
[0068] Advantageously, as defined in standard NF EN ISO 13919, a metallographic cross section can be carried out on the inspection specimen to verify the complete penetration of the bead and the absence of prohibitive defects in the weld bead, however this control is destructive.
[0069] Advantageously, in order to ensure good tightness of the through vacuum welding of each channel of the base material 100, a 1x10 -10 mbar.ls -1 A helium leak-tight test with a leak detection limit of 1000 m / s may be performed. This control is non-destructive.
[0070] Advantageously, X-ray fluoroscopy or X-ray tomography can be carried out to verify the absence of redhibitory defects in the weld bead, as defined in the standard NF EN ISO 13919. This control is non-destructive.
[0071] Advantageously, during step c), the contour of the substrate 100 / plate 200 interface is also welded. Welds 220 make it possible to make the assembly gas-tight (FIG. 5D). If appropriate, the contour of the cowl 300 / plate 200 interface is also welded. Welds 310 make it possible to make the assembly gas-tight (FIG. 6D). The welding of the contour is preferably carried out by vacuum welding.
[0072] After completion of step c), the formed cavity is airtight.
[0073] To carry out step d), the cavities are open at least at one of their ends so that gas can circulate inside the recessed portion. Thus, during step d), the pressure inside the cavities can increase and there is no deformation of the channels during the carrying out of this step. This opening can be provided during a step of machining of the substrate 100 prior to the HIP cycle.
[0074] Advantageously, prior to step d), the substrate 100 / plate 200 interface and / or the cowl 300 / plate 200 interface are degassed under a secondary vacuum.
[0075] During step d), HIP diffusion welding is performed. The sealing of the recessed area 110 by the plate 200 welded during step c) allows HIP diffusion welding without significant deformation of the formed channels.
[0076] This diffusion welding is carried out in the solid phase: a temperature of about 0.5 to 0.9xTf, the melting point of the material, and high pressure are applied to the components to be assembled.
[0077] For steels and nickel alloys, the welding temperature is typically selected between 900°C and 1,250°C. The pressure is typically between 700 and 1,500 bar (i.e. 8x10 7 Pa to 1.5x10 8 For example, the welding time is comprised between 1 hour and 10 hours, preferably between 2 hours and 5 hours.
[0078] In the first step, contact is made at the coarse material spike. Then, various diffusion mechanisms and the movement of the grain seals close the pores. Thus, the contact surface between the two parts to be assembled disappears.
[0079] If the vacuum for the laser welding in step c) is not sufficient, it is possible to carry out a step before the HIP diffusion welding step in which holes are formed, for example by means of a drilling nozzle and a pump nozzle (i.e. a tube making it possible to draw a vacuum at the substrate / plate interface and / or the plate / cowl interface). The higher the vacuum at the interface to be welded, the better the mechanical properties of the joint will be.
[0080] Diffusion welding does not result in deformation of the channel.
[0081] In a particular variant, after the diffusion welding step, it is possible to reduce the thickness of the various elements of the structure in order to obtain the desired dimensions of the part to be made.
[0082] Illustrative and Non-Limiting Example of One Embodiment In this example, a substrate 100 was manufactured that includes a zigzag-like recessed region 110, more specifically an M-shaped recessed region (FIG. 8). The substrate 100 is made of steel.
[0083] A plate 200 made of steel is placed on the structure. The following steps are then carried out: - a through-hole laser welding is performed in a vacuum in order to weld the plate 200 onto the substrate 100 by means of a weld 210, thus forming an airtight cavity, the contour of the substrate 100 and the contour of the plate 200 also being welded by the through-hole laser welding; - hot isostatic pressing diffusion welding of the resulting assembly; will be carried out.
[0084] FIG. 9 shows the resulting part after the through-vacuum laser welding step.
[0085] A helium test was performed to verify the tightness of the laser welds. The test was as described in paragraph A.3 of the standard ISO20485:2018 ("Non-destructive testing - Leak tests - Tracer gas method"). The parts have good tightness.
[0086] A metallographic cross section confirms that the weld 210 penetrates into the substrate 100 (FIG. 10). [Explanation of symbols]
[0087] 1 tube 2 Grooved Plate 3 Grooved Plate 4 Plate 5 Plate 6 Plates, Blades 7 Base material 8 Cap 100 Base material 101 First Side 102 Second Side 110 Concave area 200 plates 210 Welding 220 Welding 300 Cowl 310 Welding
Claims
1. A method for manufacturing a structure comprising a cavity, comprising the following steps: a) forming a recessed area (110) on a first surface (101) of a substrate (100) made of a first material; b) placing a plate (200) made of a second material on the first surface (101) of the substrate (100) so as to cover the recessed area (110) of the substrate (100); c) performing resistance penetration welding under vacuum or penetration laser welding in vacuum around the recessed area, thereby welding the plate (200) onto the substrate (100) and forming a cavity; d) performing a step of hot isostatic pressing diffusion welding on the resulting assembly; A method comprising:
2. 2. The method according to claim 1, characterized in that during step c) a through laser weld is performed over the contour of the plate (200).
3. 3. Method according to claim 1 or 2, characterized in that after step c) a step of degassing is performed at the plate (200) / substrate (100) interface.
4. Between steps c) and d), the following successive steps are carried out: - placing a cowl (300) on said plate (200); - welding said cowl (300) onto said plate (200); 4. The method according to claim 1, further comprising:
5. 5. The method of claim 4, further comprising the step of: after welding the cowl (300) onto the plate (200), a degassing step is performed at the plate (200) / cowl (300) interface.
6. Method according to claim 4 or 5, characterized in that the cowl (300) is welded onto the plate (200) by laser welding, preferably under vacuum.
7. 7. The method according to claim 1, wherein the first material and the second material are independently selected from among copper and its alloys, titanium and its alloys, aluminum and its alloys, steel, and vanadium, and the first material and the second material are possibly the same or different.
8. a substrate (100) made of a first material and comprising a recessed area (110) on its first side (101); a plate (200) made of a second material covering said recessed area (110) of said substrate (100) and welded onto said substrate (100) around said recessed area (110) by means of welds (210) obtained by vacuum penetration, resistance welding or laser welding and hot isostatic pressing diffusion, said recessed area bounded by said substrate (100) and said plate (200) forming a cavity; - optionally a cowl (300) welded onto said plate (200); A structure comprising:
9. 9. The structure of claim 8, wherein the first material and the second material are independently selected from copper and its alloys, titanium and its alloys, aluminum and its alloys, steel, and vanadium, and the first material is optionally the same as or different from the second material.
10. 10. A structure according to claim 8 or 9, characterized in that the structure is a heat exchanger comprising cavities arranged to cause a fluid circulation, the cavities forming channels for the circulation of a fluid, such as a gas or a liquid.
Citation Information
Patent Citations
Production method of heat exchanger
JP2006263746A
Method for production of an element comprising fluid circulation channels
WO2006067349A1
Method for manufacturing a module having hollow area, preferably for the circulation of fluid
WO2011026925A1