composite
A composite structure with a glass base material and decorative film having controlled thermal expansion and a porous design addresses adhesion issues, improving structural integrity and impact resistance by buffering thermal expansion.
Patent Information
- Application Number
- JP2023051531
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
The difference in thermal expansion coefficients between the base material and decorative film leads to poor adhesion and potential cracking or peeling, compromising the integrity of the composite.
A composite structure is developed with a glass base material and a decorative film containing an inorganic pigment and a glass matrix with a specific thermal expansion coefficient difference and a porous design, achieving an average bonding ratio of 25% to 50%, enhancing adhesion through thermal expansion buffering.
The solution improves adhesion between the base material and decorative film, reducing the risk of cracking and peeling, while maintaining structural integrity and enhancing impact resistance.
Smart Images

Figure 2024140403000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a composite including a glass substrate and a decorative film provided on a surface of the substrate. [Background technology]
[0002] There is a technique for decorating inorganic substrates such as ceramics, ceramic tiles, and glass by drawing an image on the substrate by inkjet printing, screen printing, or the like using a composition containing a pigment and glass, and then baking the image. In this decoration, the pigment is fixed to the inorganic substrate by, for example, the glass.
[0003] In this regard, for example, Patent Document 1 discloses a light-shielding glass plate having a glass plate and a porous light-shielding layer provided on the surface of the glass plate. The glass plate is made of transparent low-expansion crystallized glass. The light-shielding layer is made of 40 to 90% by weight of inorganic pigment powder and 10 to 60% by weight of glass flux. In this light-shielding glass plate, adjacent inorganic pigment powder particles or the inorganic pigment powder and the glass plate are bonded together by glass formed by melting and solidifying the glass flux. This publication describes that the light-shielding glass plate having such a configuration is excellent in mechanical strength and thermal shock resistance.
[0004] In addition, the decorative glass substrate disclosed in Patent Document 2 has a pattern formed by painting a coloring composition on the surface of a low expansion glass substrate and firing it. This coloring composition contains a lead-free glass flux having a predetermined composition and a color pigment. This publication describes that the decorative glass substrate does not contain lead, is inhibited from generating cracks, and has excellent antifouling properties, acid resistance, and alkali resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-273342 [Patent Document 2] JP 2002-255584 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the thermal expansion coefficient of the base material and the thermal expansion coefficient of the decorative film may differ from each other. When there is a difference between the thermal expansion coefficient of the base material and the thermal expansion coefficient of the decorative film, it is required to improve the adhesion between the decorative film and the base material. [Means for solving the problem]
[0007] The composite disclosed herein includes a glass substrate and a decorative film provided on the surface of the substrate. The decorative film includes an inorganic pigment and a glass matrix made of glass having a glass transition point of 400°C or higher. The decorative film has a thermal expansion coefficient (CTE) of 30°C to 300°C of the substrate. B Thermal expansion coefficient CTE from 30℃ to 300℃ is greater than A It has a coefficient of thermal expansion (CTE) A and coefficient of thermal expansion (CTE) B The difference δCTE is 1.0×10 -6 / K or more 7.0×10 -6 / K or less. The decorative film is a porous film. Here, the average bonding ratio A ave is 25% or more and 50% or less. Average bonding ratio A ave is calculated by the following formula (1): Joint ratio A(%)=(total X) / (total X+total Y)×100 (1) In the composite body having such a configuration, the adhesion between the decorative film and the substrate is improved.
[0008] In a preferred embodiment of the composite disclosed herein, the decorative film contains 20% by volume or more and 70% by volume or less of the glass matrix when the entire decorative film is taken as 100% by volume. With this configuration, the adhesion between the decorative film and the substrate is further improved. In addition, the inorganic pigment is more stably held on the substrate.
[0009] In another preferred embodiment of the composite disclosed herein, the glass matrix is composed of glass containing at least three components selected from the group consisting of silicon, boron, aluminum, zinc, and alkali metal components, each of which is 10 mol % or more when the whole is taken as 100 mol % in terms of oxide molar ratio. With this configuration, the decorative film is given an appropriate strength and has improved adhesion to the substrate.
[0010] In another preferred embodiment of the composite disclosed herein, the glass matrix is composed of SiO2-B2O3-ZnO glass or Li2O-Al2O3-SiO2 glass. SiO2-B2O3-ZnO glass is glass containing 10 mol% or more of SiO2, 10 mol% or more of B2O3, and 10 mol% or more of ZnO when the whole is taken as 100 mol% in terms of oxide molar ratio. Li2O-Al2O3-SiO2 glass is glass containing 10 mol% or more of Li2O, 10 mol% or more of Al2O3, and 10 mol% or more of SiO2 when the whole is taken as 100 mol% in terms of oxide molar ratio. With this configuration, the effect of the technology disclosed herein is better realized.
[0011] In another preferred embodiment of the composite disclosed herein, the average bonding ratio A ave is 35% or less. With this configuration, the effects of the technology disclosed herein can be better realized.
[0012] In another preferred embodiment of the composite disclosed herein, the difference ΔCTE is ave The number obtained by multiplying is 25 x 10 -6 More than 60×10 -6According to this configuration, the impact resistance of the decorative film can be further improved.
[0013] The composite disclosed herein may further include an inorganic filler. ave This will make it easier to achieve this. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a cross-sectional view of the composite 1. [Diagram 2] FIG. 2 is an enlarged view of the frame A in FIG. [Diagram 3] FIG. 3 is a cross-sectional view of the agitator / pulverizer 100. [Figure 4] FIG. 4 is a schematic diagram of an inkjet device 1000 . [Diagram 5] FIG. 5 is a cross-sectional view of the ink-jet head 50. As shown in FIG. [Figure 6] FIG. 3 is an SEM observation image of Example 4. [Figure 7] FIG. 4 is an SEM observation image of Example 8. [Figure 8] FIG. 5 is an SEM observation image of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] An embodiment of the technology disclosed herein will be described below. The embodiment described herein is not intended to limit the technology disclosed herein. The technology disclosed herein is not limited to the embodiment described herein unless otherwise specified. The drawings are drawn typically and do not necessarily reflect the actual product. In addition, the same reference numerals are appropriately used for members and parts that perform the same function, and duplicated explanations are omitted. In addition, the notation "P~Q" indicating a numerical range means "P or more and Q or less" unless otherwise specified, and also includes the meaning of "greater than P and less than Q".
[0016] FIG. 1 is a cross-sectional view of the composite 1. FIG. 1 shows a cross-sectional view along the thickness direction Z of the decorative film 12. As shown in FIG. 1, the composite 1 includes a base material 10 and a decorative film 12. In the embodiment shown in FIG. 1, the base material 10 is plate-shaped (substrate). However, the shape of the base material 10 is not particularly limited and can be appropriately changed as necessary. The base material 10 is made of, for example, glass. The base material 10 is preferably made of, for example, glass having high heat resistance and a low coefficient of thermal expansion. The base material 10 has, for example, a coefficient of thermal expansion of 1.0×10 from 30° C. to 300° C. -6 1 / K or less. Examples of such low expansion glass include quartz glass and crystallized glass. For the sake of convenience, the thermal expansion coefficient of the substrate 10 from 30° C. to 300° C. (i.e., the thermal expansion coefficient of the glass constituting the substrate 10) is referred to as the "thermal expansion coefficient CTE B ". In this specification, the "coefficient of thermal expansion" of the substrate 10 and the decorative film 12 refers to the coefficient of thermal expansion measured by a differential expansion method. For example, a commercially available analyzer is used to measure the coefficient of thermal expansion, as described in the test examples below. Here, a test piece molded into a predetermined shape (dimensions) is placed in a predetermined atmosphere (for example, in the air atmosphere) and heated in a temperature range from 30°C to 300°C, thereby measuring the coefficient of thermal expansion of the test piece. Alternatively, the nominal value of the manufacturer or the like may be used as the coefficient of thermal expansion, if necessary.
[0017] 1, the decorative film 12 is provided on the surface of the substrate 10. In this embodiment, the decorative film 12 is provided on one side of the substrate 10. The decorative film 12 may be provided on the entire one side of the substrate 10, or may be provided on only a part of the one side. Here, the decorative film 12 is a fired film provided by firing a decorating composition applied to the surface of the substrate 10.
[0018] Fig. 2 is an enlarged view of frame A in Fig. 1. Fig. 2 shows an enlarged cross-sectional structure of the boundary between the substrate 10 and the decorative film 12. The decorative film 12 can contain, for example, an inorganic pigment and a glass matrix.
[0019] The inorganic pigment may be, for example, a metal compound. Examples of the metal compound include metal compounds containing at least one of zirconium (Zr), titanium (Ti), praseodymium (Pr), chromium (Cr), antimony (Sb), nickel (Ni), cobalt (Co), aluminum (Al), and cadmium (Cd), or composite metal compounds. From the viewpoint of heat resistance, the inorganic pigment may be an oxide of the above-mentioned metals, and is preferably a Zr-based composite metal oxide containing zirconium (Zr). Examples of the Zr-based composite metal oxide include ZeSiO4.
[0020] In inkjet printing, for example, three colors of ink, cyan, yellow, and magenta, are combined to draw an image of a desired color. When Zr-based composite metal oxide is used as an inorganic pigment, for example, the three colors of inorganic pigment can be obtained by doping a Zr-based composite metal oxide with a predetermined metal element. An example of a cyan Zr-based composite metal oxide is ZrSiO4-V (vanadium). An example of a yellow Zr-based composite metal oxide is ZrSiO4-Pr (praseodymium). An example of a magenta Zr-based composite metal oxide is ZrSiO4-Fe (iron). In addition, black ink may be used. An example of an inorganic pigment used in black ink is an FeCr-based composite metal compound (e.g., spinel black). Note that, as the inorganic pigment, any conventionally used one may be used without any particular limitation.
[0021] The inorganic pigment may be, for example, particulate. The average particle size of the inorganic pigment is not particularly limited and may be appropriately set depending on, for example, the type of inkjet printer, the diameter of the ejection port, etc. The average particle size of the inorganic pigment is generally 0.01 μm to 2 μm, and preferably 0.1 μm to 1 μm. In this specification, the term "average particle size" refers to the particle size (D 50 This refers to the diameter.
[0022] There is no particular limitation on the proportion of the inorganic pigment in the decorative film 12. When the entire decorative film 12 is taken as 100 volume %, the proportion of the inorganic pigment is, for example, 10 volume % to 70 volume %, and preferably 20 volume % to 60 volume %.
[0023] The glass matrix has a function of, for example, making it easier to adhere inorganic pigments, inorganic fillers described later, and the like to the substrate 10, and can contribute to improving the durability of the decorative film. The decorative film 12 can be obtained by, for example, firing a printed film of a decorative composition under a temperature condition of 600°C to 1000°C (preferably, 700°C to 900°C). For this reason, the glass matrix is preferably composed of glass having a glass transition point (Tg) of 400°C or higher. The glass transition point of the glass constituting the glass matrix is preferably 425°C or higher, and more preferably 450°C or higher. On the other hand, such a glass transition point is, for example, 700°C or lower, preferably 600°C or lower, and more preferably 550°C or lower. In addition, the yield point (Ts) of the glass constituting the glass matrix is, for example, 450°C or higher, and preferably 500°C or higher. On the other hand, such a yield point is, for example, 750°C or lower, preferably 700°C or lower, more preferably 650°C or lower, and even more preferably 600°C or lower. In this specification, the glass transition point and the yield point are measured using a commercially available thermomechanical analysis (TMA). If necessary, the manufacturer's nominal value may be used.
[0024] The glass matrix may be composed of glass containing at least three of the following components, each of which is 10 mol % or more when the whole is taken as 100 mol % in terms of oxide molar ratio: silicon component, boron component, aluminum component, zinc component, and alkali metal component. By forming the glass matrix from three or more of the above-mentioned components, it is possible to impart an appropriate strength to the decorative film 12, maintain the shape of the decorative film in a desired state, and increase the strength of the composite 1. In addition, the adhesion of the decorative film 12 to the substrate 10 can be improved.
[0025] The silicon component is, for example, silicon dioxide (SiO2). The silicon component is, for example, a component that constitutes the skeleton of the glass matrix, and has a function of increasing the thermal stability of the glass matrix, a function of increasing the softening point of the glass matrix, and the like. The boron component is, for example, boron oxide (B2O3). The boron component has, for example, a function of lowering the softening point of the glass matrix, and the like. The boron component can, for example, contribute to increasing the fluidity of the decorative composition during firing. Therefore, the boron component can increase the fixation of the decorative film 12 to the substrate 10. The aluminum component is, for example, aluminum oxide (alumina) (Al2O3). The aluminum component has, for example, a function of controlling the fluidity of the glass matrix, a function of increasing the adhesion stability of the glass matrix, and the like. The zinc component is, for example, zinc oxide (ZnO). The zinc component has, for example, a function of increasing the thermal stability of the glass matrix, a function of increasing the softening point of the glass matrix, and the like. The alkali metal component is, for example, at least one of lithium oxide (Li2O), sodium oxide (Na2O), and potassium oxide (K2O). The alkali metal component has a function of lowering the softening point of the glass matrix. For example, the alkali metal component can contribute to increasing the fluidity of the decorative composition during firing. Therefore, the alkali metal component can increase the fixation of the decorative film 12 to the substrate 10.
[0026] As the glass constituting the glass matrix, for example, SiO2-B2O3-ZnO-based glass can be preferably used. Here, SiO2-B2O3-ZnO-based glass refers to glass containing 10 mol% or more of SiO2, 10 mol% or more of B2O3, and 10 mol% or more of ZnO when the whole glass is taken as 100 mol% in terms of molar ratio of oxides. By using SiO2-B2O3-ZnO-based glass, it is possible to realize a decorative film 12 having SiO2 as a skeleton and realizing both the effect of improving the fixation to the substrate 10 by B2O3 and the effect of improving the thermal stability by ZnO.
[0027] Another preferred example of the glass constituting the glass matrix is Li2O-Al2O3-SiO2-based glass. The Li2O-Al2O3-SiO2-based glass refers to glass containing 10 mol% or more of Li2O, 10 mol% or more of Al2O3, and 10 mol% or more of SiO2 when the entire glass is taken as 100 mol% in terms of oxide molar ratio. By using the Li2O-Al2O3-SiO2-based glass, it is possible to realize a decorative film 12 having SiO2 as a skeleton and realizing both the effect of improving the fixation to the substrate 10 by Li2O and the effect of improving the adhesion stability to the substrate 10 by Al2O3.
[0028] In addition to the above-mentioned components, the glass matrix may further contain other components such as alkaline earth metal components such as BaO, MgO, CaO, SrO, etc.; transition metal components such as TiO2, ZrO2, Fe2O3, etc.; and noble metal components such as Au2O3.
[0029] The SiO2-B2O3-ZnO-based glass preferably used as the glass constituting the glass matrix has, for example, the following composition: Li2O 3mol%~5mol%; B2O3 20mol%~25mol%; Na2O 0mol%~0.15mol%; Al2O3 1.5mol%~3.5mol%; SiO2 37mol%~43mol%; K2O 0mol%~0.05mol%; ZnO 22mol%~28mol%; SrO 0mol%~0.05mol%; BaO 3 mol% to 5 mol%; and Au2O3 0.15mol%~0.35mol%; It consists of:
[0030] Another example of a SiO2-B2O3-ZnO-based glass preferably used as the glass constituting the glass matrix has the following composition: Li2O 4mol%~6mol%; B2O3 30mol%~35mol%; Na2O 0.05mol%~0.25mol%; Al2O3 3mol%~5mol%; SiO2 10mol%~15mol%; K2O 0mol%~0.2mol%; CaO 0mol%~0.1mol%; ZnO 35mol%~40mol%; SrO 0 mol% to 0.1 mol%; and BaO 5mol%~7mol%; It consists of:
[0031] The Li2O-Al2O3-SiO2-based glass preferably used as the glass constituting the glass matrix has, for example, the following composition: Li2O 14mol%~18mol%; B2O3 5mol%~10mol%; Na2O 0.2mol%~0.7mol%; Al2O3 13.5mol%~15.5mol%; SiO2 55mol%~60mol%; K2O 0.1mol%~0.4mol%; CaO 0.05 mol% to 0.25 mol%; and ZrO2 0.5mol%~0.7mol%; It consists of:
[0032] The proportion of the glass matrix in the decorative film 12 is not particularly limited. When the entire decorative film 12 is taken as 100 volume %, the proportion of the glass matrix is, for example, 20 volume % to 70 volume %, preferably 30 volume % to 67.5 volume %, and more preferably 40 volume % to 65 volume %. By setting the proportion of the glass matrix in the decorative film 12 within the above range, the adhesion of the decorative film 12 to the substrate 10 can be improved. In addition, inorganic pigments and the like can be more stably held in the decorative film 12.
[0033] Although not particularly limited, the decorative film 12 may contain an inorganic filler as necessary. By containing an inorganic filler, the bonding ratio between the decorative film 12 and the substrate 10 described later can be more easily adjusted to a desired range. This in turn increases the adhesion of the decorative film 12 to the substrate 10 and increases the strength of the composite 1. The type of inorganic filler is not particularly limited, and various inorganic fillers used in this type of application can be selected without particular restriction. Examples of such inorganic fillers include inorganic fillers made of silica, alumina, zirconia, titania, low thermal expansion crystallized glass, etc. The average particle size of the inorganic filler may be, for example, 0.1 μm to 1 μm (preferably, 0.15 μm to 0.5 μm).
[0034] The proportion of the inorganic filler in the decorative film 12 is not particularly limited. When the entire decorative film 12 is taken as 100 volume %, the proportion of the inorganic filler may be, for example, more than 0 volume %, 3 volume % or more, 5 volume % or more, 10 volume % or more, or 30 volume % or less, or 25 volume % or less. By setting the proportion of the inorganic filler in the decorative film 12 within the above range, the bonding ratio of the decorative film 12 to the base material 10 can be more easily adjusted to a desired range. Note that it is not essential for the decorative film 12 to contain an inorganic filler. For this reason, the decorative film 12 may not contain an inorganic filler. In this case, the proportion of the inorganic filler in the decorative film 12 is 0 volume %.
[0035] The thermal expansion coefficient CTE of the decorative film 12 from 30°C to 300°C A ") is, for example, the thermal expansion coefficient CTE of the substrate B Also, the thermal expansion coefficient CTE A and coefficient of thermal expansion (CTE) B The difference δCTE is, for example, 1.0 × 10 -6 / K or more 7.0×10 -6 / K or less.
[0036] As described above, in a composite of a substrate and a decorative film, when there is a difference between the thermal expansion coefficient of the substrate and the thermal expansion coefficient of the decorative film, the present inventors have found that, for example, when a decorative composition applied to a substrate is fired to form a decorative film, the decorative film is likely to crack or peel off. Even if the decorative film does not crack or peel off, the composite is likely to be damaged from the joint between the substrate and the decorative film. Therefore, the present inventors have studied how to improve the adhesion between the substrate and the decorative film by buffering the expansion of the decorative composition during firing, thereby suppressing the occurrence of cracks and peeling in the decorative film.
[0037] The decorative film 12 here is a porous film. As shown in Fig. 2, voids 12s are formed in the decorative film 12. In the decorative film 12 shown in Fig. 2, the voids 12s are formed within the decorative film 12 (voids 12s1). Also, the voids 12s are formed at the interface between the base material 10 and the decorative film 12 (voids 12s2). Therefore, the region of the base material 10 where the decorative film is provided includes a region where the base material 10 and the decorative film 12 are bonded and a region where the base material 10 and the decorative film 12 are not bonded.
[0038] Average bonding ratio A between the decorative film 12 and the substrate 10 ave The average bonding ratio A may be, for example, 25% or more and 50% or less. aveBy being in the above range, even if the decorative composition expands during firing, the expansion can be absorbed by the gap (here, the portion at the interface between the substrate 10 and the decorative composition where the two are not bonded). This suppresses the occurrence of cracks and peeling in the decorative film 12, which in turn improves the adhesion between the substrate 10 and the decorative film 12, thereby increasing the strength of the composite 1. From the viewpoint of further improving the strength of the composite 1, the average bonding ratio A ave is preferably 45% or less, more preferably 40% or less, and even more preferably 35% or less.
[0039] In this specification, the average bonding ratio A between the substrate and the decorative film ave The average bonding ratio A is measured by observing the cross section of the decorative film in the thickness direction with an electron scanning microscope (SEM). ave is calculated by the following formula (1): Joint ratio A(%)=(total X) / (total X+total Y)×100 (1) This is the arithmetic average value of the joining ratio A calculated based on
[0040] As an example, the bonding ratio A between the base material 10 and the decorative film 12 in FIG. 2 is calculated as follows. In FIG. 2, there are four portions at the interface between the base material 10 and the decorative film 12 where the base material 10 and the decorative film 12 are bonded, and there are three portions where the base material 10 and the decorative film 12 are not bonded (i.e., portions where there is a gap 12s2). When the above formula (1) is used for this, the bonding ratio A is calculated by the formula (x1+x2+x3+x4) / {(x1+x2+x3+x4)+(y1+y2+y3)}×100. As shown in FIG. 2, x1 to x4 are the lengths of the portions where the base material 10 and the decorative film 12 are bonded along the surface of the base material 10. Moreover, y1 to y3 are the lengths of the portions along the surface of the base material 10 where the base material 10 and the decorative film 12 are not joined (that is, the portions that form the gaps 12s2).
[0041] The manufacturing method of the composite 1 may include, for example, inkjet printing a decorative composition for forming the decorative film 12 on the substrate 10. The decorative composition may be an inkjet ink. First, as materials for the decorative composition, glass powder, inorganic pigment, and, if necessary, inorganic filler, photocurable monomer, and any additives are prepared. As the glass powder, for example, glass powder having the characteristics of the glass matrix described above when the decorative film 12 is formed may be prepared. As the inorganic pigment and inorganic filler, the above-mentioned materials may be prepared. As the photocurable monomer, a photocurable monomer used for this type of application may be prepared.
[0042] FIG. 3 is a cross-sectional view of the agitation crusher 100. In the preparation of the decorative composition, for example, the agitation crusher 100 shown in FIG. 3 is used to agitate the slurry and crush the inorganic solids (glass powder, inorganic pigment, and inorganic filler). Here, after crushing beads (for example, zirconia beads with a diameter of 0.5 mm) are added to the decorative composition (slurry), the slurry is supplied from the supply port 110 into the stirring vessel 120. A shaft 134 having a plurality of stirring blades 132 is accommodated in the stirring vessel 120. One end of the shaft 134 is attached to a motor (not shown), and the motor is operated to rotate the shaft 134, thereby stirring the slurry while sending it downstream in the liquid sending direction P with the plurality of stirring blades 132. During this stirring, the inorganic solids are crushed by the crushing beads added to the slurry, and the finely divided inorganic solids are dispersed in the slurry.
[0043] The slurry sent to the downstream side in the liquid sending direction P passes through the filter 140. As a result, the grinding beads and inorganic solids that have not been atomized are collected by the filter 140, and the inkjet ink in which the atomized inorganic solids are sufficiently dispersed is discharged from the outlet 150. By adjusting the pore size of the filter 140 at this time, the maximum particle size of the inorganic solids in the inkjet ink can be controlled.
[0044] Next, the inkjet ink (decorative composition) is applied to the substrate 10. In this specification, "applying the inkjet ink (decorative composition) to the substrate (substrate 10)" includes not only an embodiment in which the inkjet ink (decorative composition) is directly applied to the substrate (substrate 10), but also an embodiment in which the inkjet ink (decorative composition) is indirectly applied to the substrate (substrate 10) using transfer paper or the like. In the following, a method for manufacturing transfer paper for glass substrates using the inkjet ink (a printing method for drawing an image on the surface of transfer paper) will be described. FIG. 4 is a schematic diagram of an inkjet device 1000. FIG. 5 is a cross-sectional view of an inkjet head 50.
[0045] Inkjet ink is stored in an inkjet head 50 of an inkjet device 1000 shown in FIG. 4. The inkjet device 1000 includes four inkjet heads 50. Each inkjet head 50 stores four different colors of ink: black (K), cyan (C), yellow (Y), and magenta (M). The inkjet ink is stored in the inkjet heads 50 of black (K), cyan (C), yellow (Y), and magenta (M). Each inkjet head 50 is accommodated inside a print cartridge 40. The print cartridge 40 is inserted into a guide shaft 20 and is configured to reciprocate along an axial direction X of the guide shaft 20. Although not shown, the inkjet device 1000 also includes a moving means for moving the guide shaft 20 in a vertical direction Y. This allows ink to be ejected from the inkjet head 50 toward a desired position on a backing sheet W of a transfer paper.
[0046] For example, a piezoelectric inkjet head as shown in Fig. 5 is used for the inkjet head 50 shown in Fig. 4. The piezoelectric inkjet head 50 is provided with a storage section 53 for storing ink in a case 52, and the storage section 53 is connected to a discharge section 56 via a liquid transfer path 55. The discharge section 56 is provided with a discharge port 57 that opens to the outside of the case 52, and a piezoelectric element 58 is arranged to face the discharge port 57. In the inkjet head 50, the piezoelectric element 58 is vibrated, so that the ink in the discharge section 56 is discharged from the discharge port 57 toward the backing paper W (see Fig. 3).
[0047] A UV irradiation means 30 is attached to the guide shaft 20 of the inkjet device 1000 shown in Fig. 4. The UV irradiation means 30 is disposed adjacent to the print cartridge 40, and moves with the reciprocating movement of the print cartridge 40, irradiating the mount W with ink attached with ultraviolet light. This causes the ink to harden immediately after it is attached to the surface of the mount W. This allows a sufficient thickness of ink to be fixed on the surface of the transfer paper (mount W).
[0048] Next, the inkjet ink is applied to the surface of the substrate 10. Here, the inkjet ink is applied to the substrate 10 via the above-mentioned transfer paper. In another embodiment, when the inkjet ink is applied directly to the surface of the substrate 10 using an inkjet device, the inkjet ink may be ejected onto the surface of the substrate 10 in the same manner as described above.
[0049] Next, the substrate 10 with the inkjet ink applied thereto is baked under conditions in which the maximum baking temperature is set within the range of 450°C to 1200°C (preferably 500°C to 1000°C, more preferably 550°C to 850°C). As a result, the resin component formed by hardening the monomer is burned off, and the glass powder in the inorganic solid content melts. Then, by cooling after baking, the melted glass powder solidifies, and the inorganic pigment is fixed to the surface of the substrate 10. In this manner, the decorative film 12 is formed on the substrate 10, and the composite 1 is manufactured.
[0050] The composite 1 can be used as an article having a decorative portion formed of a decorative film, such as, but not limited to, various tableware, various cooking utensils, and various decorative utensils.
[0051] As described above, the composite 1 disclosed herein includes a glass substrate 10 and a decorative film 12 provided on the surface of the substrate 10. The decorative film 12 includes an inorganic pigment and a glass matrix made of glass having a glass transition point of 400° C. or higher. The decorative film 12 has a thermal expansion coefficient (CTE) of 1000° C. or more. B CTE greater than A It has a coefficient of thermal expansion (CTE) A and coefficient of thermal expansion (CTE) B The difference δCTE is 1.0×10 -6 / K or more 7.0×10 -6 / K or less. The decorative film 12 is a porous film. Here, for the interface between the substrate 10 and the decorative film 12 in a cross section in the thickness direction Z of the decorative film 12, in each of the SEM images in randomly selected multiple visual fields, the total length X of the bonded portion between the substrate 10 and the decorative film 12 and the total length Y of the non-bonded portion between the substrate 10 and the decorative film 12 are used to calculate the thickness of the decorative film 12. The following formula (1): Joint ratio A(%)=(total X) / (total X+total Y)×100 (1) The average bonding ratio A between the substrate 10 and the decorative film 12 is the arithmetic average value of the bonding ratio A calculated based on ave is between 25% and 50%.
[0052] In the composite 1, the decorative film 12 contains an inorganic pigment and a glass matrix made of glass with a glass transition point of 400° C. or higher. With this, when the precursor of the composite 1 is fired under predetermined firing conditions, the glass material that constitutes the glass matrix melts to form a glass matrix, and the inorganic pigment is appropriately held on the substrate 10. In addition, the decorative film 12 has a thermal expansion coefficient CTE of 400° C. or higher than that of the substrate 10. B CTE greater than A The difference δCTE is 1.0×10 -6 / K or more 7.0×10 -6 The decorative film 12 is a porous film, and the average bonding ratio A ave is formed so that the ratio of the thickness of the decorative film 12 to the thickness of the base material 10 is 25% or more and 50% or less. As a result, when the precursor of the composite 1 is fired, the decorative film 12 is formed with an appropriate gap between the base material 10 and the decorative composition. In other words, when the precursor of the composite 1 is fired, the decorative composition thermally expands, but the decorative film 12 is formed while this thermal expansion is buffered by the gap formed between the base material 10 and the decorative composition. Therefore, the risk of the decorative film 12 being formed with cracks or peeling due to firing of the precursor of the composite 1 is reduced, and as a result, the adhesion between the base material 10 and the decorative film 12 in the composite 1 can be improved.
[0053] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.
[0054] <Preparation of Decorative Composition> As starting materials for the decorative composition (here, the decorative inkjet ink), glass powders A to D, inorganic pigments A to G, and inorganic fillers A and B were prepared. The compositions of the glass powders A to D are shown in Table 1. Table 1 shows the ratio (mol%) of each oxide when the entire glass powder is taken as 100 mol% in terms of the molar ratio of oxide. In Table 1, the notation "-" indicates that the oxide is not contained. The average particle diameters of the glass powders A to D were all 0.4 μm to 0.5 μm. The glass powder A had a glass transition point of 537°C and a deformation point of 570°C. The glass powder B had a glass transition point of 506°C and a deformation point of 535°C. The glass powder C had a glass transition point of 458°C and a deformation point of 506°C. The glass powder D had a glass transition point of 520°C and a deformation point of 637°C.
[0055] [Table 1]
[0056] The inorganic pigments A to G are as follows. Inorganic pigment A: Tin-sphene pink pigment Inorganic pigment B: Zircon-based cyan pigment Inorganic pigment C: Iron oxide red iron oxide pigment 1 (D50>0.25μm) Inorganic pigment D: Rutile-type titania yellow pigment Inorganic pigment E: Spinel-based black pigment Inorganic pigment F: Titania-based white pigment Inorganic pigment G: Iron oxide-based red iron oxide pigment 2 (D50≦0.25μm) The inorganic pigments A to G all had average particle sizes of 0.1 μm to 1 μm.
[0057] Regarding the inorganic filler, silica having an average particle size of 0.2 μm was prepared as inorganic filler A. As inorganic filler B, a high-melting-point glass filler having an average particle size of 0.4 μm and a melting point of 850° C. or higher was prepared.
[0058] Example 1 A material containing inorganic pigment A, glass powder A, a photocurable monomer, a photopolymerization initiator, and additives was prepared. The materials were then mixed using a commercially available bead mill (manufactured by IMEX Co., Ltd.) to prepare the decorative composition of this example. Zirconia beads with a diameter of 0.5 mm were used when mixing the materials. When the total volume of the inorganic solid components was taken as 100 volume %, the proportion of glass powder A was 65 volume %, and the proportion of inorganic pigment A was 35 volume %. In this test example, the "inorganic solid components" refers to components consisting of inorganic pigments, glass powders, and, if necessary, inorganic fillers.
[0059] The photocurable monomer is a mixture of a monofunctional acrylate monomer, a monofunctional N-vinyl compound monomer, a polyfunctional acrylate monomer, and a polyfunctional vinyl ether monomer in a predetermined volume ratio. As the monofunctional acrylate monomer, a mixture of isobornyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.), benzyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.), phenoxyethyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.), and cyclic trimethylolpropane formal acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.) was used. As the monofunctional N-vinyl compound monomer, N-vinyl caprolactam (manufactured by Tokyo Chemical Industry Co., Ltd.) was used. As the polyfunctional acrylate monomer, 1,9-nonanediol diacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.) was used. As the polyfunctional vinyl ether monomer, a mixture of triethylene glycol divinyl ether (manufactured by Nippon Carbide Corporation), diethylene glycol divinyl ether (manufactured by Nippon Carbide Corporation), and 1,4-cyclohexanedimethanol divinyl ether (manufactured by Nippon Carbide Corporation) was used.
[0060] As the photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator (IGMRESINS: Omnirad 819) was used. The additives used in this example were a dispersant (BYK Japan: DISPERBYK-2013) and a polymerization inhibitor (FUJIFILM Wako Pure Chemical Industries: Q-1301 (N-nitroso-N-phenylhydroxylamine aluminum)).
[0061] --Examples 2 to 11, Comparative Examples 1 to 5-- The glass powder shown in the corresponding column in Table 2, the inorganic pigment shown in the corresponding column in Table 2, and the inorganic filler shown in the corresponding column in Table 2 were used. The proportion (volume %) of each component when the total volume of the inorganic solid components was 100 volume % was as shown in the corresponding column in Table 2. The decorative composition of each example was prepared using the materials and procedures used in Example 1 except for the above. In Table 2, the notation "-" in the corresponding column indicates that the decorative composition does not contain that component.
[0062] [Table 2]
[0063] <Measurement of thermal expansion coefficient> The decorative compositions of Examples 1 to 11 and Comparative Examples 1 to 5 were fired at 800°C and processed to have dimensions of approximately 3 mm x 3 mm x 15 mm to prepare test pieces for measurement. The glass substrate used in producing the composite described below was processed to have the same dimensions as the processed decorative composition of each example to prepare test pieces for measurement. Two test pieces were prepared for each decorative composition and glass substrate. Next, the thermal expansion coefficient of the test pieces was measured by a differential expansion method using a thermomechanical analyzer (TMA8310, manufactured by Rigaku Corporation). The test pieces were heated in an air atmosphere in a temperature range from 30°C to 300°C to obtain the thermal expansion coefficient CTE of the test pieces for the decorative composition of each example. A and the thermal expansion coefficient CTE for the glass substrate BThe difference ΔCTE was calculated from the obtained thermal expansion coefficient. The obtained value is shown in Table 3 as "ΔCTE (×10 -6 / K) column. For Comparative Example 5, the glass was not sufficiently melted by the above-mentioned firing, so the measurement of the thermal expansion coefficient and the following evaluations were not performed. The entry "-" in the corresponding column in Table 3 indicates that no evaluation was performed.
[0064] <Preparation of Complex> The decorative compositions (here, inkjet inks) of Examples 1 to 11 and Comparative Examples 1 to 5 were printed on a glass substrate using an inkjet printer (Material Printer DMP-2831, manufactured by Fujifilm Corporation). -7 A low-thermal expansion glass substrate of 1000 nm or less was used. Next, the glass substrate on which the decorative composition of each example was printed was fired at 800° C. In this way, a composite of each example was produced.
[0065] <Evaluation test> -Dropping ball test- In order to evaluate the impact resistance of each composite, a ball drop test was carried out in accordance with JIS R3212:1998. Specifically, a commercially available ball drop tester was used to drop a steel ball weighing 535 g onto the surface of the composite on which no decorative film was formed, and it was evaluated whether the steel ball would damage the composite. In this case, the height from which the steel ball was dropped was changed, and the minimum height at which damage occurred in the composite (hereinafter also referred to as "damage height H") was investigated. In this test, if the steel ball penetrated the composite or if the composite was fragmented, it was evaluated as "damage occurred." The "height (mm)" column in Table 3 shows the damage height H.
[0066] Based on the breakage height H obtained for each example, the impact resistance of each example was evaluated according to the following items. The evaluation results are shown in the corresponding columns in Table 3. "E (Excellent impact resistance)": Breaking height H of 600 mm or more "G (good impact resistance)": Breaking height H between 300mm and 600mm "P (poor impact resistance)": Breaking height H of less than 300 mm
[0067] -Scratch hardness test- In order to evaluate the adhesion of the decorative film in each composite, a scratch hardness test (pencil method) was performed in accordance with JIS K 5600-5-4:1999. Using a commercially available scratch hardness tester, the decorative film was scratched with a pencil to evaluate whether the decorative film was scratched. In this case, the maximum hardness at which the decorative film was not scratched was examined while changing the hardness of the pencil. The "Hardness" column in Table 3 shows the minimum hardness at which the decorative film was scratched. Note that the entry "6H≦" in Table 3 indicates that the decorative film was not scratched with a pencil of at least 6H hardness. Also, the entry "≦B" in Table 3 indicates that the decorative film was scratched with a pencil of B or a hardness lower than B (softer than B).
[0068] -Adhesion test- A test was conducted to evaluate the adhesion of the decorative film in the composite of each example. For each composite, cellophane tape was attached to the glass substrate and the decorative film, and when the cellophane tape was pulled up at 90 degrees, it was checked whether the decorative film peeled off. When the peeling rate of the decorative film was 0 to less than 50%, it was evaluated as "○ (good adhesion)", and when the peeling rate of the decorative film was 50% or more, it was evaluated as "× (poor adhesion)". The evaluation results are shown in the "Tape" column of Table 3.
[0069] Based on the results of the scratch hardness test and the adhesion test, the adhesion of the decorative film in each example was evaluated as follows. The evaluation results are shown in the corresponding columns in Table 3. "E (Excellent adhesion): The maximum pencil hardness at which the decorative film was not scratched was H or higher, and the test using cellophane tape resulted in a rating of "○" "P (poor adhesion)": The maximum pencil hardness that did not cause scratches on the decorative film is less than H, or the test using cellophane tape resulted in an evaluation of "X"
[0070] - Measurement of bonding ratio - The bonding ratio between the glass substrate and the decorative film in each example composite was measured based on SEM observation. First, for each example composite, an SEM (JSM-IT510 manufactured by JEOL Ltd.) was used to randomly obtain observation images of 10 fields of view for a cross section along the thickness direction of the decorative film. The observation magnification was 3000 times. Next, for each observation image, image software was used to calculate the total length X of the portion where the glass substrate and the decorative film were bonded and the total length Y of the portion where the glass substrate and the decorative film were not bonded. Using the totals X and Y obtained here, the bonding ratio A in each observation image was calculated based on the above formula (1). Then, the arithmetic mean value (i.e., the average bonding ratio A) for the observation images of the 10 fields of view was calculated. ave The results are shown in the corresponding columns of Table 3. In addition, the average bonding ratio A was calculated based on the thermal expansion coefficient measured as described above. ave The numerical values obtained are shown in the corresponding columns of Table 3. Examples of the observation images are shown in Figs. 6 to 8. Fig. 6 is an SEM observation image of Example 4. The observation image shown in Fig. 6 shows the interface between the glass substrate and the decorative film in the cross section in the thickness direction of the decorative film for Example 4. The observation image shown in Fig. 6 was acquired at an observation magnification of 3000 times. Fig. 7 is an SEM observation image of Example 8. The observation image shown in Fig. 7 shows the interface between the glass substrate and the decorative film in the cross section in the thickness direction of the decorative film for Example 8. The observation image shown in Fig. 7 was acquired at an observation magnification of 3000 times. Fig. 8 is an SEM observation image of Comparative Example 2. The observation image shown in Fig. 8 shows the interface between the glass substrate and the decorative film in the cross section in the thickness direction of the decorative film for Comparative Example 2. The observation image shown in Fig. 8 was acquired at an observation magnification of 5000 times. The scale bars in Figs. 6 to 8 all indicate 5 μm.
[0071] [Table 3]
[0072] In the composite including the glass substrate and the decorative film, in Examples 1 to 11, the decorative film contains an inorganic pigment and a glass matrix made of glass having a glass transition point of 400° C. or more. In addition, the decorative film has a thermal expansion coefficient CTE of the glass substrate. B CTE greater than A It has a coefficient of thermal expansion (CTE) A and coefficient of thermal expansion (CTE) B The difference δCTE is 1.0×10 -6 / K or more 7.0×10 -6 / K or less. The decorative film is a porous film. The average bonding ratio A ave is 25% or more and 50% or less. In Examples 1 to 11, as shown in Table 3, the average bonding ratio A ave It was found that, compared with Comparative Examples 1 to 5 which did not satisfy the average bonding ratio A of 25% or more and 50% or less, the adhesiveness and impact resistance were excellent. ave In Examples 5 to 11, in which the difference was 35% or less, the impact resistance was higher.
[0073] In addition, from the results shown in Tables 2 and 3, it can be seen that, for inorganic pigments and inorganic fillers, the more particles with an average particle size of 0.25 μm or more and 0.4 μm or less are present, the greater the average bonding ratio A ave In addition, it was found that the average bonding ratio A of inorganic pigments and inorganic fillers increases as the number of particles with an average particle size exceeding 0.4 μm increases. ave was found to tend to be smaller.
[0074] -Modes included in the technology disclosed herein- The technology disclosed herein encompasses the following aspects 1 to 7.
[0075] Although specific examples of the technology disclosed herein have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. Section 1: A glass substrate; A decorative film provided on a surface of the base material; A composite comprising: The decorative film is The composition includes an inorganic pigment and a glass matrix made of glass having a glass transition temperature of 400° C. or higher. The coefficient of thermal expansion (CTE) of the substrate from 30°C to 300°C B Thermal expansion coefficient CTE from 30℃ to 300℃ is greater than A and the coefficient of thermal expansion CTE A and the coefficient of thermal expansion CTE B The difference δCTE is 1.0×10 -6 / K or more 7.0×10 -6 / K or less, It is a porous membrane, Here, for the interface between the substrate and the decorative film in a cross section in the thickness direction of the decorative film, in each of the observation images by an electron microscope for a plurality of randomly selected visual fields, the total length X of the bonded portion between the substrate and the decorative film and the total length Y of the non-bonded portion between the substrate and the decorative film are used to calculate the following formula (1): Bonding ratio A (%) = (the total X) / (the total X + the total Y) × 100 (1) The average bonding ratio A between the substrate and the decorative film is the arithmetic average value of the bonding ratio A calculated based on ave is 25% or more and 50% or less, a composite. Section 2: Item 2. The composite according to item 1, wherein the decorative film contains 20% by volume or more and 70% by volume or less of the glass matrix when the entire decorative film is taken as 100% by volume. Section 3: Item 3. The composite according to item 1 or 2, wherein the glass matrix is composed of glass containing at least three components selected from a silicon component, a boron component, an aluminum component, a zinc component, and an alkali metal component in an amount of 10 mol % or more, when the whole is taken as 100 mol % in terms of a molar ratio of oxides. Section 4: The glass matrix is SiO2-B2O3-ZnO-based glass containing 10 mol% or more of SiO2, 10 mol% or more of B2O3, and 10 mol% or more of ZnO when the whole is taken as 100 mol% in terms of molar ratio of oxides, or Li2O-Al2O3-SiO2-based glass containing 10 mol% or more of Li2O, 10 mol% or more of Al2O3, and 10 mol% or more of SiO2 when the whole is taken as 100 mol% in terms of molar ratio of oxides; Item 4. The complex according to any one of Items 1 to 3, comprising: Section 5: The average bonding ratio A ave 5. The complex according to any one of Items 1 to 4, wherein the ratio of the total number of molecules to the total number of molecules is 35% or less. Item 6: The difference δCTE is the average bonding ratio A ave The number obtained by multiplying is 25 x 10 -6 More than 60×10 -6 6. The complex according to any one of Items 1 to 5, which is: Section 7: Item 7. The composite according to any one of items 1 to 6, further comprising an inorganic filler. [Explanation of symbols]
[0076] 1. Complex 10 Base material 12 Decorative film 12s void 20 Guide shaft 30 UV irradiation means 40 Print Cartridge 50 Inkjet head 52 cases 53 Storage 55 Liquid delivery path 56 Discharge part 57 Discharge port 58 Piezoelectric element 100 Stirring mill 110 Supply port 120 Mixing vessel 132 Stirring blade 134 Shaft 140 Filters 150 Outlet P Flow direction X Guide shaft axial direction Y guide axis vertical direction 1000 Inkjet device
Claims
1. A glass substrate; A decorative film provided on a surface of the base material; A composite comprising: The decorative film is The composition includes an inorganic pigment and a glass matrix made of glass having a glass transition point of 400° C. or higher, The coefficient of thermal expansion (CTE) of the substrate from 30°C to 300°C B A coefficient of thermal expansion (CTE) from 30° C. to 300° C. is greater than A and said coefficient of thermal expansion CTE A and the thermal expansion coefficient CTE B The difference δCTE is 1.0 × 10 -6 / K or more 7.0×10 -6 / K or less, It is a porous membrane, Here, for the interface between the substrate and the decorative film in a cross section in the thickness direction of the decorative film, in each of the observation images by an electron microscope for a plurality of randomly selected visual fields, the total length X of the bonded portion between the substrate and the decorative film and the total length Y of the non-bonded portion between the substrate and the decorative film are used to calculate the following formula (1): Bonding ratio A (%) = (the total X) / (the total X + the total Y) × 100 (1) The average bonding ratio A between the substrate and the decorative film is the arithmetic average value of the bonding ratio A calculated based on ave is 25% or more and 50% or less.
2. 2. The composite according to claim 1, wherein the decorative film contains 20% by volume or more and 70% by volume or less of the glass matrix when the entire decorative film is taken as 100% by volume.
3. 2. The composite according to claim 1, wherein the glass matrix is composed of glass containing at least three components selected from a silicon component, a boron component, an aluminum component, a zinc component, and an alkali metal component in an amount of 10 mol % or more each, when the whole is taken as 100 mol % in terms of a molar ratio of oxides.
4. The glass matrix is When the whole is taken as 100 mol % in terms of molar ratio of oxides, 10 mol % or more of SiO 2 and 10 mol% or more of B 2 O 3 and SiO containing 10 mol % or more of ZnO. 2 -B 2 O 3 ZnO-based glass, or When the whole is taken as 100 mol % in terms of oxide molar ratio, 10 mol % or more of Li 2 O and 10 mol % or more of Al 2 O 3 and 10 mol % or more of SiO 2 and Li 2 O-Al 2 O 3 -SiO 2 Glasses, The complex of claim 3, comprising:
5. The average bonding ratio A ave The composite of claim 1 , wherein the β-
6. The difference δCTE is the average bonding ratio A ave The number obtained by multiplying is 25 x 10 -6 Above 60 x 10 -6 6. The complex of claim 5, wherein:
7. The composite according to any one of claims 1 to 6, further comprising an inorganic filler.
Citation Information
Patent Citations
Shading glass plate
JP1998273342A
Glass flux, coloring composition, and decorative glass substrate
JP2002255584A