Pyroelectric element and infrared sensor
The pyroelectric element with a perovskite structured metal oxide film and intermediate layers addresses sensitivity and stability issues in thin films, enabling efficient detection of temperature-induced polarization changes for improved infrared sensor performance.
Patent Information
- Application Number
- JP2023051734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional pyroelectric elements using bulk ceramics face challenges with high sensitivity requirements due to inferior ferroelectric properties and temperature-dependent pyroelectric current, especially in thin films, which are prone to rapid temperature changes and have a dead layer affecting performance.
A pyroelectric element design featuring a pyroelectric film with a specific hysteresis curve and coercive electric fields, containing a metal oxide with a perovskite structure, epitaxially grown with lattice stress to enhance polarization changes and detectability, and an intermediate layer to improve ferroelectricity and pyroelectricity.
The design enables easy detection of polarization value changes with temperature variations, enhancing pyroelectric coefficient and figure of merit, improving sensitivity and stability in infrared sensors.
Smart Images

Figure 2024140551000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a pyroelectric element and an infrared sensor. [Background technology]
[0002] The need for SDGs and energy conservation is growing due to the rise in global energy demand and environmental issues. Pyroelectric devices are widely used in various infrared sensors such as human presence sensors and motion sensors that consume little power and standby power (see Patent Documents 1 and 2 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-185982 A [Patent Document 2] JP 2014-187193 A Summary of the Invention [Problem to be solved by the invention]
[0004] With the development and spread of various technologies such as healthcare, wearable devices, smartphones, connected cars, smart cities, and smart homes, high sensitivity is required for pyroelectric elements applied to these technologies. In conventional pyroelectric elements, bulk materials (ceramics) of pyroelectrics have been widely used, but new pyroelectrics are required to improve the performance and reduce the size of pyroelectric elements. The volume of a thin film (pyroelectric film) formed from a pyroelectric body is smaller than the volume of the bulk material. Therefore, the heat capacity of the pyroelectric film is smaller than the heat capacity of the bulk material, and the temperature of the pyroelectric film is more likely to change than the temperature of the bulk material. As a result, in a pyroelectric element using a pyroelectric film, a pyrocurrent is likely to be generated with temperature changes, and high sensitivity of the voltage due to the pyrocurrent is expected. However, since a dead layer (non-ferroelectric layer, or low dielectric layer) exists near the surface of the pyroelectric film (near the interface between the pyroelectric film and the electrode), the ferroelectricity and therefore the pyroelectricity of the pyroelectric film are generally inferior to those of the bulk material.
[0005] An object of one aspect of the present invention is to provide a pyroelectric element in which the polarization value of a pyroelectric film is likely to change with temperature changes and in which the change in polarization value can be easily detected, and an infrared sensor including the pyroelectric element. [Means for solving the problem]
[0006] For example, as described in [1] to [7] below, one aspect of the present invention relates to a pyroelectric element and an infrared sensor.
[0007] [1] A semiconductor device comprising a first electrode, a second electrode, and a pyroelectric film; At least a portion of the pyroelectric film is disposed between the first electrode and the second electrode; The hysteresis curve of the pyroelectric film indicates the electric field applied to the pyroelectric film and the polarization value of the pyroelectric film when the electric field is applied, Ec1 is the polarization value of 0μC / cm on the hysteresis curve. 2 The absolute value of the coercive field is the larger of the two, Ec2 is the smaller absolute value of the two coercive fields, The residual polarization value Pr is 50μC / cm 2 That's all. The remanent polarization value Pr is the polarization value in the hysteresis curve at an electric field of (Ec1+Ec2) / 2, |Ec1| / |Ec1-Ec2| is 0.55 or more. Pyroelectric element.
[0008] [2] The pyroelectric film includes a metal oxide having a perovskite structure, Metal oxides include bismuth, potassium, and titanium; The pyroelectric element according to [1].
[0009] [3] The metal oxide further comprises at least one element selected from the group consisting of element M and iron; The element M is at least one element selected from the group consisting of magnesium and nickel; The pyroelectric element according to [2].
[0010] [4] Pyroelectric films contain tetragonal crystals of metal oxides. The pyroelectric film is polarized in a direction perpendicular to the (001) plane of the tetragonal crystal. The pyroelectric element according to [2] or [3].
[0011] [5] The first electrode comprises platinum crystals; The (002) plane of the platinum crystal is parallel to the (001) plane of the tetragonal crystal. The pyroelectric element according to [4].
[0012] [6] Pyroelectric films are epitaxial films. The pyroelectric element according to any one of [1] to [5].
[0013] [7] Further comprising at least one intermediate layer; the intermediate layer is disposed between the first electrode and the pyroelectric film; The intermediate layer contains at least one of LaNiO3 and SrRuO3. The pyroelectric element according to any one of [1] to [6].
[0014] [8] The temperature of the pyroelectric film during the measurement of the hysteresis curve is 25°C. The pyroelectric element according to any one of [1] to [7].
[0015] [9] A pyroelectric element according to any one of [1] to [8]. Infrared sensor. Effect of the Invention
[0016] According to one aspect of the present invention, there is provided a pyroelectric element in which the polarization value of a pyroelectric film is likely to change with a change in temperature and in which the change in polarization value can be easily detected, and an infrared sensor including the pyroelectric element. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic perspective view of a pyroelectric element according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic hysteresis curve of a pyroelectric film in a pyroelectric element according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a perspective view of a unit cell of a metal oxide (tetragonal crystal) having a perovskite structure, and shows the arrangement of each element in the perovskite structure. [Figure 4] FIG. 4 is a perspective view of a unit cell of a metal oxide (tetragonal crystal) having a perovskite structure, and shows each lattice plane of the tetragonal crystal and the orientation of each lattice plane. [Diagram 5] FIG. 5 is an example of a schematic circuit diagram of an infrared sensor including a pyroelectric element according to one embodiment of the present invention. [Figure 6] FIG. 6 shows hysteresis loops of the pyroelectric films of Example 4 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. In the drawings, equivalent components are given the same reference numerals. The present invention is not limited to the following embodiments. X, Y, and Z shown in FIG. 1 represent three coordinate axes that are orthogonal to each other. The direction of the Z axis is common to FIG. 1 and FIG. 4.
[0019] (Pyroelectric element) The pyroelectric element according to the present embodiment includes a first electrode, a second electrode, and a pyroelectric film. The pyroelectric film is made of a pyroelectric material. A pyroelectric is a dielectric material that is spontaneously polarized when no electric field is applied, and whose polarization value (surface charge per unit area of the surface) changes with temperature. The pyroelectric film may be a ferroelectric material. A ferroelectric is a type of pyroelectric material, and is a dielectric material in which the direction of polarization (electric dipole) (in other words, the positive and negative surface charges) is reversed in response to the reversal of the direction of the applied electric field.
[0020] A part or the whole of the pyroelectric film is disposed between the first electrode and the second electrode. In other words, the pyroelectric film directly or indirectly overlaps the first electrode, and the second electrode directly or indirectly overlaps the pyroelectric film. As long as a part or the whole of the pyroelectric film is disposed between the first electrode and the second electrode, the structure of the pyroelectric element is not limited. For example, as shown in FIG. 1, the pyroelectric element 10 according to the present embodiment may include a crystalline substrate 1, a first electrode 2 (lower electrode) overlapping the crystalline substrate 1, a pyroelectric film 3 overlapping the first electrode 2, a second electrode 4 (upper electrode) overlapping the pyroelectric film 3, and a detection unit 7 electrically connected to the first electrode 2 and the second electrode 4. The first electrode 2 may be referred to as a first electrode layer. The second electrode 4 may be referred to as a second electrode layer.
[0021] At least a part of the surface (e.g., the main surface) of the pyroelectric film 3 may be exposed as a light receiving section to which infrared rays IR are irradiated. The main surface is the surface with the largest area among the multiple surfaces of the polyhedron (pyroelectric film 3 which is a thin solid). However, the position of the light receiving surface in the pyroelectric film 3 is not limited. The pyroelectric element 10 may include an optical lens through which infrared rays are transmitted, and the optical lens may directly or indirectly overlap the surface (light receiving surface) of the pyroelectric film 3. For example, the optical lens through which infrared rays are transmitted may be formed of at least one material selected from the group consisting of germanium (Ge), chalcogenide glass, and silicon (Si). The pyroelectric element 10 may include an optical filter through which infrared rays are transmitted, and the optical filter may directly or indirectly overlap the surface (light receiving surface) of the pyroelectric film 3.
[0022] The pyroelectric element 10 may further include at least one intermediate layer. For example, the pyroelectric element 10 may include a first intermediate layer 5. The first intermediate layer 5 may be disposed between the crystalline substrate 1 and the first electrode 2. The first intermediate layer 5 may be directly overlapped on the surface of the crystalline substrate 1, and the first electrode 2 may be directly overlapped on the surface of the first intermediate layer 5. The pyroelectric element 10 may include a second intermediate layer 6. The second intermediate layer 6 may be disposed between the first electrode 2 and the pyroelectric film 3. The second intermediate layer 6 may be directly overlapped on the surface of the first electrode 2, and the pyroelectric film 3 may be directly overlapped on the surface of the second intermediate layer 6. The thicknesses of the crystalline substrate 1, the first intermediate layer 5, the first electrode 2, the second intermediate layer 6, the pyroelectric film 3, and the second electrode 4 may each be uniform. The thickness direction (Z-axis direction) of the pyroelectric film 3 may be approximately parallel to the normal direction to the surface of the first electrode 2. The thickness direction of the pyroelectric film 3 may be rephrased as the normal direction to the surface of the pyroelectric film 3. In other words, the surface of the pyroelectric film 3 may be approximately parallel to the surface of the first electrode 2. The thickness direction of the pyroelectric film 3 may be the polarization direction of the pyroelectric film 3.
[0023] A modified example of the pyroelectric element 10 may not include the crystalline substrate 1. For example, the crystalline substrate 1 may be removed after the first electrode 2, the pyroelectric film 3, and the second electrode 4 are formed. When the crystalline substrate 1 functions as an electrode, the crystalline substrate 1 may be the first electrode 2. That is, when the crystalline substrate 1 functions as an electrode, a modified example of the pyroelectric element 10 may include the crystalline substrate 1 and the pyroelectric film 3 overlapping the crystalline substrate 1. The pyroelectric film 3 may directly overlap the crystalline substrate 1. The pyroelectric film 3 may overlap the crystalline substrate 1 via at least one of the first intermediate layer 5 and the second intermediate layer 6.
[0024] The change in the polarization value of the pyroelectric film 3 may be detected by the detection unit 7 through the following mechanism. The "first surface" described below refers to a portion of the surface of the pyroelectric film 3 that overlaps with the first electrode 2, and the "second surface" refers to a portion of the surface of the pyroelectric film 3 that overlaps with the second electrode 4. The "second surface" may be rephrased as the back side of the "first surface."
[0025] Due to the spontaneous polarization of the pyroelectric film 3, the first surface of the pyroelectric film 3 is positively charged, and the second surface of the pyroelectric film 3 is negatively charged. Naturally, the absolute value of the surface charge (positive charge) per unit area of the first surface of the pyroelectric film 3 is equal to the absolute value of the surface charge (negative charge) per unit area of the second surface of the pyroelectric film 3. The surface of the first electrode 2 facing the first surface of the pyroelectric film 3 is negatively charged, and the positive charges on the first surface of the pyroelectric film 3 are neutralized by the negative floating charges on the surface of the first electrode 2. In other words, the absolute value of the surface charge (positive charge) per unit area on the first surface of the pyroelectric film 3 is equal to the absolute value of the surface charge (negative charge) per unit area on the surface of the first electrode 2. The surface of the second electrode 4 facing the second surface of the pyroelectric film 3 is positively charged, and the negative charges on the second surface of the pyroelectric film 3 are neutralized by the positive floating charges on the surface of the second electrode 4. In other words, the absolute value of the surface charge (negative charge) per unit area on the second surface of the pyroelectric film 3 is equal to the absolute value of the surface charge (positive charge) per unit area on the surface of the second electrode 4. When the temperature of the pyroelectric film 3 is constant, the absolute values of the surface charge (positive charge) per unit area of the first surface of the pyroelectric film 3 and the surface charge (negative charge) per unit area of the second surface of the pyroelectric film 3 are constant. In other words, when the temperature of the pyroelectric film 3 is constant, the polarization value P of the pyroelectric film 3 is constant. As the temperature of the pyroelectric film 3 changes, the polarization value P (surface charge per unit area of the surface) of the pyroelectric film 3 changes. For example, as the temperature of the pyroelectric film 3 rises due to irradiation with infrared rays IR, the polarization value P of the pyroelectric film 3 decreases. That is, the positive charge on the first surface of the pyroelectric film 3 decreases, and the negative charge on the second surface of the pyroelectric film 3 also decreases. As a result, a part of the negative floating charge on the surface of the first electrode 2 (a part of the negative charge that was paired with the positive charge on the first surface of the pyroelectric film 3) becomes a negative free charge. A part of the positive floating charge on the surface of the second electrode 4 (a part of the positive charge that was paired with the negative charge on the second surface of the pyroelectric film 3) becomes a positive free charge. A pyrocurrent due to these free charges is generated, and the change in voltage due to the pyrocurrent is detected by the detection unit 7. Naturally, the above mechanism is valid even if the positive and negative charges are reversed.
[0026] 2, the horizontal axis of the hysteresis curve of the pyroelectric film 3 indicates the value of the electric field E (unit: kV / mm) applied to the pyroelectric film 3. The vertical axis of the hysteresis curve of the pyroelectric film 3 indicates the polarization value P (unit: μC / cm 2 ) in other words, the vertical axis represents the surface charge per unit area of the surface of the pyroelectric film 3. The hysteresis curve of the pyroelectric film 3 represents the dependency of the polarization value P on the value of the electric field E. The hysteresis curve of the pyroelectric film 3 may be a closed curve that loops with changes in the electric field E. The temperature of the pyroelectric film 3 during measurement of the hysteresis curve may be room temperature (e.g., 25°C). The electric field E applied to the pyroelectric film 3 may be rephrased as an electric field between the first electrode 2 and the second electrode 4. The electric field E applied to the pyroelectric film 3 may be approximately perpendicular to the main surface of the pyroelectric film 3. In other words, the electric field E applied to the pyroelectric film 3 may be approximately parallel to the thickness direction (Z-axis direction) of the pyroelectric film 3. As described later, the pyroelectric film 3 may include a tetragonal crystal of a metal oxide having a perovskite structure, and the electric field E applied to the pyroelectric film 3 may be approximately perpendicular to the (001) plane of the tetragonal crystal.
[0027] In one specific example of the hysteresis curve shown in Fig. 2, Ps and Pr are positive real numbers, Ec1 is a positive real number, and Ec2 is a negative real number. However, Ec1 and Ec2 may be positive or negative real numbers. Ec1 is the value at which the polarization value P is 0 μC / cm in the hysteresis curve. 2 Of the two coercive fields, Ec1 is the value of the coercive field with the larger absolute value. Of the two coercive fields, Ec2 is the value of the coercive field with the smaller absolute value. In other words, the absolute value of Ec1 is greater than the absolute value of Ec2. The remanent polarization value Pr is the polarization value P at an electric field E of (Ec1+Ec2) / 2 on the hysteresis curve. The saturation polarization value Ps is the maximum value of the polarization value P on the hysteresis curve. The remanent polarization value Pr is 50 μC / cm 2 is equal to or greater. |Ec1| / |Ec1-Ec2| is equal to or greater than 0.55. Needless to say, |Ec1| is the absolute value of Ec1, and |Ec1-Ec2| is the absolute value of the difference (Ec1-Ec2) between Ec1 and Ec2. The absolute value of the negative remanent polarization value Pr' in the hysteresis curve may be equal to the positive remanent polarization value Pr in the hysteresis curve. The absolute value of the negative saturation polarization value Ps' in the hysteresis curve may be equal to the positive saturation polarization value Ps in the hysteresis curve.
[0028] |Ec1| / |Ec1-Ec2| being 0.55 or more, i.e., the bias of the hysteresis curve with respect to the electric field E (imprint phenomenon), indicates that the crystal structure of the pyroelectric film 3 has high anisotropy due to large lattice stress. Since the pyroelectric film 3 has high anisotropy due to large lattice stress, spontaneous polarization of the pyroelectric film 3 is likely to occur without polarization treatment, and the pyroelectric film 3 has a large remanent polarization value Pr (50 μC / cm2 The pyroelectric film 3 can have a residual polarization value Pr) that is equal to or greater than the residual polarization value Pr. That is, due to the large lattice stress acting on the pyroelectric film 3, the pyroelectric film 3 has ferroelectricity and pyroelectricity. For example, the lattice stress is caused by the lattice mismatch between the pyroelectric film 3 and the first electrode 2. This lattice stress causes the crystal structure of the pyroelectric film 3 to elongate in the thickness direction (Z-axis direction) of the pyroelectric film 3. As a result, the thickness direction of the pyroelectric film 3 becomes the polarization direction. As the temperature of the pyroelectric film 3 and the first electrode 2 increases, the first electrode 2 thermally expands, reducing the lattice mismatch between the pyroelectric film 3 and the first electrode 2, and the lattice stress that causes the ferroelectricity and pyroelectricity is easily alleviated. Therefore, as the temperature of the pyroelectric film 3 and the first electrode 2 increases, the polarization value P of the pyroelectric film 3 decreases significantly. For the above reasons, the decrease in the polarization value P associated with the temperature increase of the pyroelectric film 3 can be easily detected. After the temperatures of the pyroelectric film 3 and the first electrode 2 rise, a large lattice stress is generated again as the temperatures of the pyroelectric film 3 and the first electrode 2 drop (natural cooling), and the spontaneous polarization of the pyroelectric film 3 caused by the lattice stress is restored. The temperature dependence of the polarization value P described above is a disadvantageous characteristic for the stability of the operation of the piezoelectric thin film element, but is an advantageous characteristic for the pyroelectric element 10.
[0029] The above-mentioned effect of the pyroelectric element 10 can be rephrased as follows. Residual polarization value Pr is 50μC / cm 2 Since |Ec1| / |Ec1-Ec2| is 0.55 or more, the pyroelectric element 10 can have a large pyroelectric coefficient p and a large pyroelectric figure of merit Fv. Pyroelectric coefficient p (unit: C / cm 2 The polarization coefficient p (p / dT) is expressed as dP / dT. dT is the amount of change in temperature of the pyroelectric film 3. dP is the amount of change in the spontaneous polarization value (residual polarization value Pr) of the pyroelectric film 3 that accompanies the temperature change of the pyroelectric film 3. In other words, dP is the amount of change in the pyrocurrent that accompanies the temperature change of the pyroelectric film 3. The larger the pyroelectric coefficient p, the more easily the polarization value P of the pyroelectric film 3 changes with temperature change. For example, the pyroelectric coefficient p of the pyroelectric film 3 is 5.3×10 -8 C / cm 2 ℃ or higher 8.1×10 -8 C / cm 2 °C or less. The pyroelectric figure of merit Fv (unit: C cm / J) is calculated by p / (c V ε r ) where p is the pyroelectric coefficient. V is the specific heat at constant volume of the pyroelectric film 3 (unit: J / cm 3 ·℃). r is the relative dielectric constant (unit: no) of the pyroelectric film 3. The larger the pyroelectric figure of merit Fv is, the easier it is to detect a change in the polarization value P as a change in voltage. In other words, the larger the pyroelectric figure of merit Fv is, the higher the voltage sensitivity of the pyroelectric element 10 is. The larger the pyroelectric coefficient p is, the larger the pyroelectric figure of merit Fv is. Constant volume specific heat c V The smaller the dielectric constant, the larger the pyroelectric figure of merit Fv. r The smaller is the pyroelectric figure of merit Fv, the larger it is. Because the pyrocurrent is very weak, it is difficult to directly measure the pyrocurrent itself. However, with a pyroelectric element 10 having a large pyroelectric figure of merit Fv, the change in voltage caused by the pyrocurrent (change in polarization value P) can be easily detected. For example, the pyroelectric figure of merit Fv of the pyroelectric film 3 is 1.2×10 -10 C cm / J or more 3.1×10 -10 It may be less than C·cm / J.
[0030] Since the pyroelectric element 10 is likely to have a large pyroelectric coefficient p and a large pyroelectric figure of merit Fv, the residual polarization value Pr is 50 μC / cm 2 More than 120μC / cm 2 Below, 50μC / cm 2 More than 101μC / cm 2 or less than 60μC / cm 2 More than 101μC / cm 2 For the same reason, |Ec1| / |Ec1-Ec2| may be 0.55 or more and less than 1.00, 0.55 or more and 0.89 or less, or 0.56 or more and 0.89 or less.
[0031] The greater the lattice stress acting on the pyroelectric film 3, the greater the absolute value of the coercive electric field Ec1, and the greater the absolute value of the coercive electric field Ec1, the greater the temperature dependency of the polarization value P. Ec1 is not limited as long as |Ec1| / |Ec1-Ec2| is 0.55 or more. For example, Ec1 may be 40 kV / mm or more and 100 kV / mm or less, or 47 kV / mm or more and 75 kV / mm or less. Ec2 is not limited as long as |Ec1| / |Ec1-Ec2| is 0.55 or more. For example, Ec2 may be -40 kV / mm or more and -1 kV / mm or less, or -37 kV / mm or more and -9 kV / mm or less.
[0032] The pyroelectric film 3 may be an epitaxial film. When the pyroelectric film 3 is an epitaxial film, lattice stress caused by lattice mismatch between the pyroelectric film 3 and the first electrode 2 is likely to occur, and the lattice stress is likely to elongate the crystal structure of the pyroelectric film 3 in the thickness direction (Z-axis direction) of the pyroelectric film 3. As a result, the pyroelectric film 3 is likely to have anisotropy (in other words, ferroelectricity and pyroelectricity). For example, when the lattice constant of the crystal in the pyroelectric film 3 is larger than the lattice constant of the crystal in the first electrode 2, compressive stress caused by lattice mismatch acts on the pyroelectric film 3 in a direction parallel to the interface between the pyroelectric film 3 and the first electrode 2. As a result, the crystal structure of the pyroelectric film 3 is compressed in a direction parallel to the interface and elongated in a direction perpendicular to the interface (i.e., the thickness direction of the pyroelectric film 3).
[0033] The pyroelectric film 3 may contain a metal oxide having a perovskite structure. For example, the metal oxide may contain at least two elements selected from the group consisting of bismuth (Bi), lanthanum (La), yttrium (Y), potassium (K), sodium (Na), lithium (Li), titanium (Ti), zirconium (Zr), magnesium (Mg), nickel (Ni), zinc (Zn), iron (Fe), manganese (Mn), cobalt (Co), and potassium (Ga).
[0034] The metal oxide may contain bismuth, potassium, and titanium because the metal oxide is likely to become a tetragonal crystal having anisotropy (ferroelectricity and pyroelectricity) due to lattice stress, and the pyroelectric coefficient p and pyroelectric figure of merit Fv are likely to increase. For the same reason, the metal oxide may further contain at least one element of element M and iron in addition to bismuth, potassium, and titanium, and element M may be at least one element of magnesium and nickel. The metal oxide may contain all of bismuth, potassium, titanium, element M, and iron. The metal oxide is the main component of the pyroelectric film 3. In the pyroelectric film 3, the ratio of all elements constituting the above metal oxide may be 99% by mol or more and 100% by mol or less. The pyroelectric film 3 may be composed only of a metal oxide. As long as the pyroelectricity of the pyroelectric film 3 is not impaired, the pyroelectric film 3 may contain other elements in addition to Bi, K, Ti, element M, Fe, and O. The pyroelectric film 3 does not need to contain lead (Pb). For example, the pyroelectric film 3 does not need to contain oxides of lead, such as lead zirconate titanate.
[0035] The "perovskite oxide" described below means the above metal oxide having a perovskite structure. The pyroelectric film 3 may be made of a single crystal of a perovskite oxide. The pyroelectric film 3 may be made of a polycrystal of a perovskite oxide. A unit cell of a perovskite oxide is shown in FIG. 3. The element located at the A site of the unit cell uc may be Bi or K. The element located at the B site of the unit cell uc may be Ti, Mg, Ni or Fe. The unit cell uc shown in FIG. 3 is the same as the unit cell uc shown in FIG. 4. However, in FIG. 4, the B site and oxygen (O) in the unit cell uc are omitted in order to show the lattice plane. a is a lattice constant corresponding to the spacing of the (100) plane of the perovskite oxide. b is a lattice constant corresponding to the spacing of the (010) plane of the perovskite oxide. c is a lattice constant corresponding to the spacing of the (001) plane of the perovskite oxide.
[0036] The pyroelectric film 3 may contain a tetragonal crystal of a perovskite oxide at room temperature or at a temperature equal to or lower than the Curie temperature of the perovskite oxide. As described above, since the lattice stress is likely to act on the pyroelectric film 3, the pyroelectric film 3 is likely to shrink in a direction substantially perpendicular to the thickness direction (Z-axis direction). As a result, the lattice constants a and b of the perovskite oxide in the pyroelectric film 3 are each smaller than the lattice constant c of the perovskite oxide in the thickness direction (Z-axis direction) of the pyroelectric film 3, and the perovskite oxide becomes a tetragonal crystal. As a result, the pyroelectric film 3 is likely to have excellent pyroelectricity and ferroelectricity, and the pyroelectric coefficient p and pyroelectric figure of merit Fv are likely to increase. All of the perovskite oxides contained in the pyroelectric film 3 may be tetragonal crystals. The pyroelectric film 3 may further include one or both of cubic crystals of a perovskite type oxide and rhombohedral crystals of a perovskite type oxide in addition to tetragonal crystals of a perovskite type oxide.
[0037] The (001) plane of the tetragonal crystal may be oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3. In other words, the (001) plane of the tetragonal crystal may be oriented in the normal direction (Z-axis direction) of the main surface of the pyroelectric film 3. The orientation in which the perovskite oxide having the above-mentioned composition is likely to polarize is
[0001] . That is, the pyroelectric film 3 spontaneously polarizes in the direction perpendicular to the (001) plane of the tetragonal crystal (c-axis direction) without undergoing a polarization process. Due to the spontaneous polarization of the tetragonal crystal in the c-axis direction, the remanent polarization value Pr is likely to increase, and the absolute value of the coercive field Ec1 is likely to increase. That is, since the (001) plane of the tetragonal crystal is oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3, the pyroelectric film 3 is likely to have excellent pyroelectricity and ferroelectricity, and the pyroelectric coefficient p and pyroelectric figure of merit Fv are likely to increase. For the same reason, c / a of the tetragonal crystal may be 1.05 or more and 1.20 or less, or 1.05 or more and 1.14 or less. For example, the lattice constant a of the tetragonal crystal may be 0.375 Å or more and 0.395 Å or less. For example, the lattice constant c of the tetragonal crystal may be 0.430 Å or more and 0.450 Å or less. The lattice constant b of the tetragonal crystal is equal to the lattice constant a.
[0038] The degree of orientation of each lattice plane of the perovskite oxide (tetragonal crystal) may be quantified by the degree of orientation. The degree of orientation of each lattice plane may be calculated based on the peak of the diffracted X-rays originating from each lattice plane. The peak of the diffracted X-rays originating from each lattice plane may be measured by out of plane measurement on the surface of the pyroelectric film 3. The degree of orientation of the (001) plane is 100×I (001) / ΣI (hkl) The orientation of the (110) plane can be expressed as 100×I (110) / ΣI (hkl) The orientation of the (111) plane can be expressed as 100×I (111) / ΣI (hkl) It may be expressed as: I (001) is the maximum value of the diffracted X-ray peak originating from the (001) plane. I (110) is the maximum value of the diffracted X-ray peak originating from the (110) plane. (111) is the maximum value of the diffracted X-ray peak originating from the (111) plane. ΣI (hkl) I (001) +I (110) +I (111) The orientation of the (001) plane is 100×S (001) / ΣS (hkl) The orientation of the (110) plane can be expressed as 100×S (110) / ΣS (hkl) The orientation of the (111) plane can be expressed as 100×S (111) / ΣS (hkl) It may be expressed as: S (001) is the area of the diffracted X-ray peak (peak integral) originating from the (001) plane. S (110) is the area of the diffracted X-ray peak (peak integral) originating from the (110) plane. S (111) is the area of the diffracted X-ray peak (peak integral) originating from the (111) plane. ΣS (hkl) is S (001) +S (110) +S (111) The degree of orientation of each lattice plane may be quantified by the degree of orientation based on the Lotgering method.
[0039] It is preferable that the (001) plane of the tetragonal crystal is preferentially oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3, since this tends to improve the pyroelectricity and ferroelectricity of the pyroelectric film 3 and tends to increase the pyroelectric coefficient p and the pyroelectric figure of merit Fv. In other words, it is preferable that the degree of orientation of the (001) plane is higher than the degrees of orientation of each of the (110) plane and the (111) plane. For example, the degree of orientation of the (001) plane may be 70% or more and 100% or less, preferably 80% or more and 100% or less, and more preferably 90% or more and 100% or less.
[0040] In contrast to the pyroelectric film 3, it is difficult to distort the bulk of a pyroelectric body having a cubic crystal structure or a pseudo cubic crystal structure to make the bulk of the pyroelectric body tetragonal. Therefore, the bulk of the pyroelectric body tends not to have the pyroelectricity and ferroelectricity due to the tetragonal crystal structure of a perovskite oxide.
[0041] The crystal orientation described below means that the (001) plane of the tetragonal crystal is oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3.
[0042] Since the pyroelectric film 3 is an epitaxial thin film formed by a vapor phase growth method or a solution method, the pyroelectric film 3 is likely to have the above-mentioned crystal orientation. On the other hand, the bulk of a pyroelectric body having the same composition as the pyroelectric film 3 tends to be less likely to have the above-mentioned crystal orientation than the pyroelectric film 3. This is because the bulk of a pyroelectric body is a sintered body (ceramic) of powder containing essential elements of the pyroelectric body, and it is difficult to control the structure and orientation of the many crystals that make up the sintered body. The specific resistance of the bulk of the pyroelectric body is lower than that of the pyroelectric film 3 due to the inclusion of Fe in the bulk of the pyroelectric body. As a result, leakage current is likely to occur in the bulk of the pyroelectric body. Therefore, it is difficult to polarize the bulk of the pyroelectric body by applying a high electric field, and it is also difficult for the bulk of the pyroelectric body to polarize spontaneously. For the above reasons, it is difficult for the bulk of the pyroelectric body to have the same pyroelectricity and ferroelectricity as the pyroelectric film 3.
[0043] The perovskite oxide contained in the pyroelectric film 3 may be represented by the following chemical formula 1. The following chemical formula 1 is substantially the same as the following chemical formula 1a. When the perovskite oxide is represented by the following chemical formula 1, the perovskite oxide is likely to become a tetragonal crystal having anisotropy (ferroelectricity and pyroelectricity) due to lattice stress, and the tetragonal crystal is likely to have the above-mentioned crystal orientation, and the pyroelectric coefficient p and pyroelectric figure of merit Fv are likely to increase. The Curie temperature of a conventional general ferroelectric is high, and the conventional general ferroelectric has poor temperature dependence of the polarization value P. However, the perovskite oxide represented by the following chemical formula 1 has excellent temperature dependence of the polarization value P despite having ferroelectricity. x(Bi α K 1-α )TiO3-yBi(M β Ti 1-β )O3‐zBiFeO3(1) (Bi α K 1-α ) x Bi y+z Ti x (M β Ti 1-β ) y Fe z O 3±δ (1a)
[0044] Each of x, y, and z in the above chemical formula 1 is a real number (unit: mole). x+y+z is 1. x in the above chemical formula 1 is greater than 0 and less than 1. y in the above chemical formula 1 is greater than 0 and less than 1. z in the above chemical formula 1 is greater than 0 and less than 1. α in the above chemical formula 1 is greater than 0 and less than 1. β in the above chemical formula 1 is greater than 0 and less than 1. For example, α may be 0.5 and β may be 0.5. M in the above chemical formula 1 is Mg γ Ni 1-γis expressed as follows. γ is 0 or more and 1 or less. The total number of moles of Bi and K in the perovskite oxide may be expressed as [A]. The total number of moles of Ti, Fe and element M in the perovskite oxide may be expressed as [B]. [A] / [B] may be 1.0. As long as the perovskite structure is maintained, [A] / [B] may be a value other than 1.0. That is, [A] / [B] may be less than 1.0 or may be greater than 1.0. δ in the above chemical formula 1a is 0 or more. As long as the perovskite structure is maintained, δ may be a value other than 0. For example, δ may be greater than 0 and 1.0 or less. δ may be calculated, for example, from the valence of each of the A-site ions and B-site ions of the perovskite structure. The valence of each ion may be measured by X-ray photoelectron spectroscopy (XPS).
[0045] In the following, (Bi α K 1-α )TiO3 is written as BKT. Bi(M β Ti 1-β )O3 is expressed as BMT. BiFeO3 is expressed as BFO. A metal oxide having a composition expressed as the sum of BKT and BMT is expressed as BKT-BMT. A metal oxide having a composition expressed by the above chemical formula 1 is expressed as xBKT-yBMT-zBFO. The crystals of BKT, BMT, BFO, BKT-BMT, BKT-BFO, and xBKT-yBMT-zBFO each have a perovskite structure.
[0046] The crystal of BKT is tetragonal at room temperature, and BKT is a ferroelectric. The crystal of BMT is rhombohedral at room temperature, and BMT is a ferroelectric. The crystal of BFO is rhombohedral at room temperature, and BFO bulk is a ferroelectric. A thin film made of BKT-BMT is tetragonal at room temperature. The c / a of the tetragonal crystal of BKT-BMT tends to be larger than the c / a of BKT. A thin film made of BKT-BMT has better ferroelectric properties than a thin film made of BKT and a thin film made of BMT. A thin film made of xBKT-yBMT-zBFO tends to be tetragonal at room temperature. The c / a of the tetragonal crystal of xBKT-yBMT-zBFO tends to be larger than the c / a of BKT-BMT. A thin film made of xBKT-yBMT-zBFO has better ferroelectric properties than a thin film made of BKT-BMT. The ferroelectricity of the pyroelectric film 3 is presumed to be due to the fact that the composition of xBKT-yBMT-zBFO has a morphotropic phase boundary (MPB). However, since the pyroelectric film 3 belongs to the tetragonal crystal system, it is presumed that the ferroelectricity of the pyroelectric film 3 is not simply due to the MPB. The ferroelectricity of the pyroelectric film 3 tends to increase the pyroelectric coefficient p and pyroelectric figure of merit Fv. In contrast to the pyroelectric film 3, the crystals contained in the bulk of xBKT-yBMT-zBFO are pseudocubic, and the bulk of xBKT-yBMT-zBFO tends to be less likely to have the above-mentioned crystal orientation and ferroelectricity compared to the pyroelectric film 3.
[0047] In the above chemical formula 1, x may be 0.25 or more and 1.00 or less, y may be 0.00 or more and 0.50 or less, and z may be 0.00 or more and 0.50 or less. x may be 0.100 or more and 0.450 or less, y may be 0.100 or more and 0.500 or less, and z may be 0.300 or more and 0.600 or less. x may be 0.100 or more and 0.400 or less, y may be 0.100 or more and 0.400 or less, and z may be 0.400 or more and 0.600 or less. x may be 0.150 or more and 0.350 or less, y may be 0.150 or more and 0.350 or less, and z may be 0.300 or more and 0.600 or less. x may be 0.250 or more and 0.300 or less, y may be 0.250 or more and 0.300 or less, and z may be 0.400 or more and 0.600 or less. When x, y, and z are in the above ranges and x+y+z is 1, the composition of xBKT-yBMT-zBFO is likely to have MPB, and the pyroelectricity and ferroelectricity of the pyroelectric film 3 are likely to be improved.
[0048] The thickness of the pyroelectric film 3 may be, for example, 10 nm to 10 μm, 0.3 μm to 10 μm, 0.3 μm to 5 μm, 0.5 μm to 5 μm, 0.3 μm to 3 μm, or 0.5 μm to 3 μm. 2 More than 500mm 2 The areas of the crystalline substrate 1, the first intermediate layer 5, the first electrode 2, the second intermediate layer 6, and the second electrode 4 may be the same as the area of the pyroelectric film 3.
[0049] The composition of the pyroelectric film 3 may be analyzed by, for example, X-ray fluorescence spectrometry (XRF) or inductively coupled plasma (ICP) optical emission spectroscopy. The crystal structure and crystal orientation of the pyroelectric film 3 may be identified by X-ray diffraction (XRD).
[0050] The pyroelectric film 3 may be formed, for example, by the following method.
[0051] A target having the same composition as that of the pyroelectric film 3 may be used as the raw material of the pyroelectric film 3. The target is produced as follows.
[0052] As the starting materials, for example, powders of bismuth oxide, potassium carbonate, titanium oxide, oxide of element M, and iron oxide may be used. The oxide of element M may be at least one of magnesium oxide and nickel oxide. Instead of the above oxides, substances that become oxides by sintering, such as carbonates or oxalates, may be used as the starting materials. After sufficiently drying these starting materials at 100° C. or higher, each starting material is weighed so that the mole numbers of Bi, K, Ti, element M, and Fe are within the ranges specified by the above chemical formula 1. In the vapor phase growth method described later, Bi and K in the target are more likely to volatilize than other elements. Therefore, the molar ratio of Bi in the target may be adjusted to a value higher than the molar ratio of Bi in the pyroelectric film 3. The molar ratio of K in the target may be adjusted to a value higher than the molar ratio of K in the pyroelectric film 3.
[0053] The weighed starting materials are thoroughly mixed in an organic solvent or water. The mixing time may be 5 hours or more and 20 hours or less. The mixing means may be a ball mill. After the mixed starting materials are thoroughly dried, the starting materials are molded in a press. The molded starting materials are calcinated to obtain a calcine. The calcine temperature may be 750°C or more and 900°C or less. The calcine time may be 1 hour or more and 3 hours or less. The calcine is pulverized in an organic solvent or water. The pulverization time may be 5 hours or more and 30 hours or less. The pulverization means may be a ball mill. After drying the pulverized calcine, the calcine to which a binder solution is added is granulated to obtain a calcine powder. The calcine powder is press molded to obtain a block-shaped molded body.
[0054] The block-shaped molded body is heated to volatilize the binder in the molded body. The heating temperature may be 400° C. or more and 800° C. or less. The heating time may be 2 hours or more and 4 hours or less. The molded body is then sintered. The sintering temperature may be 800° C. or more and 1100° C. or less. The sintering time may be 2 hours or more and 4 hours or less. The temperature increase rate and temperature decrease rate of the molded body during the sintering process may be, for example, 50° C. / hour or more and 300° C. / hour or less.
[0055] The target is obtained by the above steps. The average grain size of the metal oxide crystal grains contained in the target may be, for example, 1 μm or more and 20 μm or less.
[0056] The pyroelectric film 3 may be formed by a vapor phase growth method using the above target. In the vapor phase growth method, elements constituting the target are evaporated under a vacuum atmosphere. The evaporated elements are attached and deposited on the surface of any one of the second intermediate layer 6, the first electrode 2, or the crystalline substrate 1, thereby growing the pyroelectric film 3. The vapor phase growth method may be, for example, a sputtering method, an electron beam evaporation method, a chemical vapor deposition method, or a pulsed-laser deposition method. Hereinafter, the pulsed-laser deposition method is referred to as a PLD method. By using these vapor phase growth methods, it is possible to form a pyroelectric film 3 that is dense at the atomic level, and segregation of elements in the pyroelectric film 3 is suppressed. The excitation source differs depending on the type of vapor phase growth method. The excitation source of the sputtering method is Ar plasma. The excitation source of the electron beam evaporation method is an electron beam. The excitation source of the PLD method is a laser beam (for example, an excimer laser). When these excitation sources are irradiated onto a target, the elements that make up the target evaporate.
[0057] Among the above vapor phase growth methods, the PLD method is relatively superior in the following respects. In the PLD method, the elements constituting the target can be instantly and uniformly converted into plasma by a pulsed laser. Therefore, it is easy to form a pyroelectric film 3 having almost the same composition as the target. Furthermore, in the PLD method, the thickness of the pyroelectric film 3 can be easily controlled by changing the number of laser pulse shots.
[0058] As described above, the pyroelectric film 3 may be an epitaxial film. That is, the pyroelectric film 3 may be formed by epitaxial growth. By epitaxial growth, the perovskite oxide in the pyroelectric film 3 tends to become a tetragonal crystal having anisotropy due to lattice stress, and the pyroelectric film 3 having excellent crystal orientation is easily formed. When the pyroelectric film 3 is formed by the PLD method, the pyroelectric film 3 is easily formed by epitaxial growth.
[0059] In the PLD method, the pyroelectric film 3 may be formed while heating the crystalline substrate 1 and the first electrode 2 in a vacuum chamber. The temperature (film formation temperature) of the crystalline substrate 1 and the first electrode 2 may be, for example, 300°C to 800°C, 500°C to 700°C, or 500°C to 600°C. The higher the film formation temperature, the more improved the cleanliness of the surface of the crystalline substrate 1 or the first electrode 2 is, and the more likely the crystallinity of the pyroelectric film 3 is to be enhanced, leading to an increased degree of orientation of the lattice plane. If the film formation temperature is too high, Bi or K is likely to be desorbed from the pyroelectric film 3, making it difficult to control the composition of the pyroelectric film 3.
[0060] In the PLD method, the oxygen partial pressure in the vacuum chamber may be, for example, greater than 10 mTorr and less than 400 mTorr, greater than 15 mTorr and less than 300 mTorr, or greater than 20 mTorr and less than 200 mTorr. In other words, the oxygen partial pressure in the vacuum chamber may be, for example, greater than 1 Pa and less than 53 Pa, greater than 2 Pa and less than 40 Pa, or greater than 3 Pa and less than 30 Pa. By maintaining the oxygen partial pressure within the above range, Bi, K, Ti, element M, and Fe deposited on the crystalline substrate 1 are likely to be sufficiently oxidized. If the oxygen partial pressure is too high, the growth rate of the pyroelectric film 3 is likely to decrease, and the orientation degree of the lattice plane of the pyroelectric film 3 is likely to decrease.
[0061] Other parameters controlled in the PLD method include, for example, the laser oscillation frequency and the distance between the substrate and the target. By controlling these parameters, it is easy to control the crystal structure and crystal orientation of the pyroelectric film 3. For example, when the laser oscillation frequency is 10 Hz or less, the degree of orientation of the lattice plane of the pyroelectric film 3 is easy to increase.
[0062] After the pyroelectric film 3 is grown, the pyroelectric film 3 may be annealed (heated). The temperature of the pyroelectric film 3 in the annealing (annealing temperature) may be, for example, 300° C. or higher and 1000° C. or lower, 600° C. or higher and 1000° C. or lower, or 850° C. or higher and 1000° C. or lower. The annealing of the pyroelectric film 3 tends to further improve the pyroelectricity and ferroelectricity of the pyroelectric film 3. In particular, the annealing at 850° C. or higher and 1000° C. or lower tends to improve the pyroelectricity and ferroelectricity of the pyroelectric film 3. However, the annealing is not essential.
[0063] The crystalline substrate 1 may be, for example, a substrate made of a single crystal of Si, or a substrate made of a single crystal of a compound semiconductor such as GaAs. The crystalline substrate 1 may be a substrate made of a single crystal of an oxide such as MgO or a perovskite oxide (for example, SrTiO3). The thickness of the crystalline substrate 1 may be, for example, 10 μm or more and 1000 μm or less. When the crystalline substrate 1 has conductivity, the crystalline substrate 1 functions as an electrode, so that the first electrode 2 may not be required. The crystalline substrate 1 having conductivity may be, for example, a single crystal of SrTiO3 doped with niobium (Nb). The crystalline substrate 1 may be an SOI (Silicon-on-Insulator) substrate.
[0064] The crystal orientation of the crystalline substrate 1 may be the same as the normal direction of the surface of the crystalline substrate 1. In other words, the surface of the crystalline substrate 1 may be parallel to a lattice plane in the crystalline substrate 1. The crystalline substrate 1 may be a uniaxially oriented substrate. For example, one lattice plane selected from the group consisting of the (100) plane, the (001) plane, the (110) plane, the (101) plane, and the (111) plane may be parallel to the surface of the crystalline substrate 1. When the (100) plane of the crystalline substrate 1 (e.g., Si) is parallel to the surface of the crystalline substrate 1, the (001) plane of the perovskite oxide in the pyroelectric film 3 is likely to be oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3.
[0065] As described above, the first intermediate layer 5 may be disposed between the crystalline substrate 1 and the first electrode 2. The first intermediate layer 5 may contain at least one selected from the group consisting of titanium (Ti), chromium (Cr), titanium oxide (TiO2), silicon oxide (SiO2), and zirconium oxide (ZrO2). The first intermediate layer 5 facilitates adhesion of the first electrode 2 to the crystalline substrate 1. The first intermediate layer 5 may be crystalline. The lattice plane of the first intermediate layer 5 may be oriented in the normal direction to the surface of the crystalline substrate 1. Both the lattice plane of the crystalline substrate 1 and the lattice plane of the first intermediate layer 5 may be oriented in the normal direction to the surface of the crystalline substrate 1. The first intermediate layer 5 may be formed by a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method.
[0066] The first intermediate layer 5 may contain ZrO2 and an oxide of a rare earth element. When the first intermediate layer 5 contains ZrO2 and an oxide of a rare earth element, the first electrode 2 made of platinum crystals is easily formed on the surface of the first intermediate layer 5, the (002) plane of the platinum crystals is easily oriented in the normal direction (Z-axis direction) of the surface of the first electrode 2, and the (200) plane of the platinum crystals is easily oriented in the in-plane direction of the surface of the first electrode 2. The rare earth element may be at least one selected from the group consisting of scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu). The first intermediate layer 5 may be made of yttria-stabilized zirconia (ZrO2 with added Y2O3). Since the first intermediate layer 5 is made of yttria-stabilized zirconia, the first electrode 2 made of platinum crystals is easily formed on the surface of the first intermediate layer 5, the (002) plane of the platinum crystals is easily oriented in the normal direction (Z-axis direction) of the surface of the first electrode 2, and the (200) plane of the platinum crystals is easily oriented in the in-plane direction of the surface of the first electrode 2. For the same reason, the first intermediate layer 5 may have a first layer made of ZrO2 and a second layer made of Y2O3. The first layer may be laminated directly on the surface of the crystalline substrate 1, the second layer may be laminated directly on the surface of the first layer, and the first electrode 2 may be laminated directly on the surface of the second layer.
[0067] The first electrode 2 may be made of at least one metal selected from the group consisting of, for example, Pt (platinum), Pd (palladium), Rh (rhodium), Au (gold), Ru (ruthenium), Ir (iridium), Mo (molybdenum), Ti (titanium), Ta (tantalum), and Ni (nickel). The first electrode 2 may be made of, for example, a conductive metal oxide such as strontium ruthenate (SrRuO3), lanthanum nickelate (LaNiO3), or lanthanum strontium cobaltate ((La,Sr)CoO3). The first electrode 2 may be crystalline. The lattice plane of the first electrode 2 may be oriented in the normal direction to the surface of the crystalline substrate 1. The lattice plane of the first electrode 2 may be approximately parallel to the surface of the crystalline substrate 1. Both the lattice plane of the crystalline substrate 1 and the lattice plane of the first electrode 2 may be oriented in the normal direction to the surface of the crystalline substrate 1. The lattice plane of the first electrode 2 may be approximately parallel to the lattice plane of the perovskite oxide oriented in the pyroelectric film 3. The thickness of the first electrode 2 may be, for example, 1 nm or more and 1.0 μm or less. The method for forming the first electrode 2 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method. In the case of the printing method, the spin coating method, or the sol-gel method, the first electrode 2 may be subjected to a heat treatment (annealing) in order to enhance the crystallinity of the first electrode 2.
[0068] The first electrode 2 may include platinum crystals. The first electrode 2 may be composed of platinum crystals only. When the first electrode 2 includes platinum crystals, the pyroelectric coefficient p and the pyroelectric figure of merit Fv tend to increase. The platinum crystals are cubic crystals having a face-centered cubic lattice structure. The (002) plane of the platinum crystals may be oriented in the normal direction (Z-axis direction) of the surface of the first electrode 2, and the (200) plane of the platinum crystals may be oriented in the in-plane direction of the surface of the first electrode 2. In other words, the (002) plane of the platinum crystals may be approximately parallel to the surface of the first electrode 2, and the (200) plane of the platinum crystals may be approximately perpendicular to the surface of the first electrode 2. The (002) plane of the platinum crystals may be approximately parallel to the (001) plane of the tetragonal crystals in the pyroelectric film 3. When the (002) and (200) planes of the platinum crystals constituting the first electrode 2 have the above-mentioned orientation, the pyroelectric film 3 is likely to grow epitaxially on the surface of the first electrode 2, and the lattice stress caused by the lattice mismatch between the perovskite oxide (pyroelectric film 3) and the platinum crystals (first electrode 2) is likely to act on the pyroelectric film 3. As a result, the pyroelectric film 3 is likely to contain tetragonal crystals of the perovskite oxide, and the (001) plane of the tetragonal crystals is likely to be preferentially oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3, and the pyroelectricity and ferroelectricity of the pyroelectric film 3 are likely to be improved. As the temperature of the perovskite oxide and the platinum crystals increases, the platinum crystals thermally expand. As a result, the lattice mismatch between the perovskite oxide and the platinum crystals is reduced, and the lattice stress that causes the ferroelectricity and pyroelectricity is easily alleviated. Therefore, as the temperature of the perovskite oxide and the platinum crystal increases, the polarization value P decreases significantly. After the temperature of the perovskite oxide and the platinum crystal increases, as the temperature of the perovskite oxide and the platinum crystal decreases, a large lattice stress is generated again, and the spontaneous polarization of the perovskite oxide due to the lattice stress is restored.
[0069] The second intermediate layer 6 may be disposed between the first electrode 2 and the pyroelectric film 3. The second intermediate layer 6 may contain at least one compound selected from the group consisting of, for example, LaNiO3, SrRuO3, and (La,Sr)CoO3. The resistivity between the first electrode 2 and the second electrode 4 is likely to increase due to the second intermediate layer 6. The pyroelectric film 3 is likely to adhere to the first electrode 2 through the second intermediate layer 6. The second intermediate layer 6 may be crystalline. When the second intermediate layer 6 contains at least one of LaNiO3 and SrRuO3, lattice stress due to lattice mismatch between the second intermediate layer 6 and the pyroelectric film 3 is likely to act on the pyroelectric film 3. As a result, the pyroelectric film 3 is likely to contain tetragonal crystals of a perovskite-type oxide, and the (001) plane of the tetragonal crystals is likely to be preferentially oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3. The lattice plane of the second intermediate layer 6 may be oriented in the normal direction (Z-axis direction) to the surface of the first electrode 2. Both the lattice plane of the crystalline substrate 1 and the lattice plane of the second intermediate layer 6 may be oriented in the normal direction (Z-axis direction) to the surface of the first electrode 2. The method for forming the second intermediate layer 6 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method.
[0070] The second electrode 4 may be made of at least one metal selected from the group consisting of, for example, Pt, Pd, Rh, Au, Ru, Ir, Mo, Ti, Ta, and Ni. The second electrode 4 may be a transparent conductive film such as indium tin oxide (ITO). The second electrode 4 may be made of at least one conductive metal oxide selected from the group consisting of, for example, LaNiO3, SrRuO3, and (La,Sr)CoO3. The second electrode 4 may be crystalline. The lattice plane of the second electrode 4 may be oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3. The lattice plane of the second electrode 4 may be approximately parallel to the surface of the pyroelectric film 3. The lattice plane of the second electrode 4 may be approximately parallel to the (001) plane oriented in the pyroelectric film 3. The thickness of the second electrode 4 may be, for example, 1 nm or more and 1.0 μm or less. The method for forming the second electrode 4 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method. In the case of the printing method, the spin coating method, or the sol-gel method, the second electrode 4 may be subjected to a heat treatment (annealing) in order to enhance the crystallinity of the second electrode 4.
[0071] A third intermediate layer may be disposed between the pyroelectric film 3 and the second electrode 4. The third intermediate layer tends to increase the resistivity between the first electrode 2 and the second electrode 4. The second electrode 4 tends to adhere to the pyroelectric film 3 due to the third intermediate layer. The lattice mismatch between the crystalline third intermediate layer and the pyroelectric film 3 tends to cause the above-mentioned lattice stress to act on the pyroelectric film 3. As a result, the pyroelectric film 3 tends to contain tetragonal crystals of a perovskite-type oxide, and the (001) plane of the tetragonal crystals tends to be preferentially oriented in the thickness direction (Z-axis direction) of the pyroelectric film 3. The composition, crystal structure, and formation method of the third intermediate layer may be the same as those of the second intermediate layer 6.
[0072] At least a part or the entire surface of the pyroelectric element 10 may be covered with a protective film. By covering the pyroelectric element 10 with a protective film, for example, the moisture resistance of the pyroelectric element 10 is improved.
[0073] (Infrared sensor) The infrared sensor according to the present embodiment includes the pyroelectric element 10 described above. The application of the infrared sensor is not limited. The infrared sensor may be applied to various technologies such as healthcare, wearable devices, smartphones, connected cars, smart cities, and smart homes. For example, the application of the infrared sensor may be a blood glucose sensor, a human sensor, a motion sensor, an infrared image sensor, an in-vehicle sensor, a flame detection sensor, or a gas detection sensor. The infrared sensor may include an infrared irradiation device to irradiate infrared rays within a predetermined wavelength range to a detection target and receive infrared rays reflected from the detection target. For example, the blood glucose sensor irradiates infrared rays to a part of the human body, and glucose in the blood flowing through the human body absorbs infrared rays within a specific wavelength range. Infrared rays not absorbed by glucose are reflected from the human body and detected by the blood glucose sensor. The infrared sensor such as the blood glucose sensor may be a non-invasive sensor. The infrared sensor such as the blood glucose sensor may be a wearable sensor or a portable sensor.
[0074] The structure of the infrared sensor is not limited. The infrared sensor may include one pyroelectric element 10. The infrared sensor may include multiple pyroelectric elements 10. The infrared sensor may be an array sensor including multiple pyroelectric elements 10 arranged in an array. FIG. 5 is an example of a circuit diagram of an infrared sensor 100 used in a human detection sensor. The infrared sensor 100 is a dual-type sensor including two pyroelectric elements 10a and 10b. Each of the two pyroelectric elements 10a and 10b includes a first electrode, a second electrode, and a pyroelectric film disposed between the first electrode and the second electrode. The two pyroelectric elements 10a and 10b are connected in series. The polarization direction of the pyroelectric film in one pyroelectric element 10a is opposite to the polarization direction of the pyroelectric film in the other pyroelectric element 10b. The gate resistor R and the pair of pyroelectric elements 10a and 10b are connected in parallel between the gate (GATE) and ground (GND) of a field effect transistor (FET). A gate resistor R is connected to the gate for impedance conversion. A power supply (not shown) applies a constant voltage to the drain (DRAIN) of the field effect transistor. When a human body moves near the infrared sensor 100, infrared rays IR originating from the heat of the human body are received by the pyroelectric films of the pyroelectric elements 10a and 10b. As a result, the temperature of each pyroelectric film rises, and the polarization value of each pyroelectric film decreases. Since the amount of infrared rays received by each of the pyroelectric elements 10a and 10b due to the movement of the human body is not uniform, a pyroelectric current is generated. The voltage across the gate resistor R associated with the pyrocurrent controls the current between the drain and the source (SOURCE), and the voltage of the source changes. A source resistor (not shown) is installed between the source and ground, and the voltage generated at the source resistor associated with the pyrocurrent is measured. In other words, a weak pyrocurrent is measured as a change in voltage at the source resistor due to impedance conversion. According to the above principle, the infrared sensor 100 detects the change in the amount of infrared rays associated with the movement of the human body. Since the pyroelectric element according to this embodiment has a large pyroelectric figure of merit Fv, the voltage generated across the source resistor in association with the pyrocurrent can be easily measured.
[0075] The present invention is not necessarily limited to the above-described embodiment. Various modifications of the present invention are possible without departing from the spirit of the present invention, and these modifications are also included in the present invention. For example, the change in electrical resistance of the pyroelectric film accompanying the change in temperature of the pyroelectric film may be measured in the pyroelectric element. EXAMPLES
[0076] The present invention will be described in detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0077] Example 1 A single crystal substrate (Si wafer) made of Si was used to fabricate the pyroelectric element of Example 1. The (100) plane of Si was parallel to the surface of the single crystal substrate. The diameter φ of the single crystal substrate was 3 inches. The thickness of the single crystal substrate was 400 μm.
[0078] In a vacuum chamber, a crystalline first intermediate layer made of ZrO2 and Y2O3 was formed on the entire surface of the single crystal substrate. The first intermediate layer was formed by a sputtering method. The first intermediate layer had a first layer made of ZrO2 and a second layer made of Y2O3. The first layer was laminated directly on the surface of the crystalline substrate 1. The second layer was laminated directly on the surface of the first layer. The first layer made of ZrO2 had a thickness of 20 nm. The second layer made of Y2O3 had a thickness of 45 nm.
[0079] In the vacuum chamber, a first electrode layer made of Pt crystals was formed on the entire surface of the first intermediate layer. The first electrode layer was formed by a sputtering method. The thickness of the first electrode layer was 50 nm. The temperature of the single crystal substrate during the formation of the first electrode layer (film formation temperature) was maintained at 500°C.
[0080] The laminate produced by the above method was cut (diced) to produce a plurality of rectangular laminates each consisting of a single crystal substrate, a first intermediate layer, and a first electrode layer. That is, a plurality of laminates were produced as samples for the analysis and measurement described below. The dimensions of each laminate in the direction perpendicular to the stacking direction were adjusted to 10 mm x 10 mm.
[0081] The X-ray diffraction (XRD) pattern of the first electrode layer was measured by out-of-plane measurement on the surface of the first electrode layer. The XRD pattern of the first electrode layer was measured by in-plane measurement on the surface of the first electrode layer. An X-ray diffractometer (SmartLab) manufactured by Rigaku Corporation was used to measure these XRD patterns. Measurement conditions were set so that each peak intensity in the XRD pattern was at least three orders of magnitude higher than the background intensity. The out-of-plane measurement detected a diffracted X-ray peak of the (002) plane of the Pt crystal. That is, the (002) plane of the Pt crystal was approximately parallel to the surface of the first electrode layer. The in-plane measurement detected a diffracted X-ray peak of the (200) plane of the Pt crystal. That is, the (200) plane of the Pt crystal was approximately perpendicular to the surface of the first electrode layer.
[0082] In a vacuum chamber, a second intermediate layer made of crystalline LaNiO3 was formed on the entire surface of the first electrode layer. The second intermediate layer was formed by a sputtering method. The thickness of the second intermediate layer was 20 nm.
[0083] In the vacuum chamber, an epitaxial pyroelectric film was formed on the entire surface of the second intermediate layer. The pyroelectric film was formed by the PLD method. The thickness of the pyroelectric film in Example 1 was adjusted to 2 μm. The temperature (film formation temperature) of the single crystal substrate during the formation of the pyroelectric film was maintained at 500° C. The oxygen partial pressure in the vacuum chamber during the formation of the pyroelectric film was maintained at 10 Pa. A target (sintered body of raw material powder) was used as the raw material of the pyroelectric film. When the target was produced, the compounding ratio of the raw material powder (bismuth oxide, potassium carbonate, titanium oxide, magnesium oxide, and iron oxide) was adjusted according to the composition of the desired pyroelectric film. The composition of the desired pyroelectric film in Example 1 is represented by the following chemical formula 1b. That is, the composition of the target, which is the raw material of the pyroelectric film, is represented by the following chemical formula 1b. In the case of Example 1, x in chemical formula 1b was 1.00, and y and z in chemical formula 1b were each 0.00. That is, the target of Example 1 is (Bi 0.5 K 0.5 ) It consisted only of TiO3. x(Bi 0.5 K 0.5 )TiO3-yBi(Mg 0.5 Ti 0.5 )O3‐zBiFeO3(1b)
[0084] In the following Table 1, xBKT-yBMT-zBFO means the above chemical formula 1b. That is, "BKT" in the following Table 1 means (Bi 0.5 K 0.5 )TiO3. In Table 1 below, "BMT" stands for Bi(Mg 0.5 Ti 0.5 )O3. In Table 1 below, "BFO" means BiFeO3.
[0085] Using the above method, a laminate was produced including a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, a second intermediate layer overlapping the first electrode layer, and a pyroelectric film overlapping the second intermediate layer.
[0086] <Analysis of composition> The composition of the pyroelectric film was analyzed by X-ray fluorescence analysis (XRF method). For the analysis, a PW2404 apparatus manufactured by Philips Japan, Ltd. was used. The composition of the pyroelectric film of Example 1 determined by the analysis was consistent with the composition of the target.
[0087] <Crystal structure analysis> The XRD pattern of the pyroelectric film was measured by out-of-plane measurement on the surface of the pyroelectric film. The XRD pattern of the pyroelectric film was measured by in-plane measurement on the surface of the pyroelectric film. The measuring device and measuring conditions for the XRD pattern were the same as above. The XRD pattern of the pyroelectric film showed that it was composed of perovskite oxide. Out-of-plane measurement detected a diffracted X-ray peak of the (001) plane of the perovskite oxide. In other words, the (001) plane of the perovskite oxide was approximately parallel to the surface (principal surface) of the pyroelectric film and approximately perpendicular to the thickness direction of the pyroelectric film. The out-of-plane measurements yielded the lattice constant c of the perovskite oxide in the thickness direction of the pyroelectric film (the normal direction to the surface of the pyroelectric film). Lattice constant c can be rephrased as the spacing between the crystal planes in the thickness direction of the pyroelectric film. The in-plane measurements yielded the lattice constant a of the perovskite oxide in the direction parallel to the surface of the pyroelectric film. Lattice constant a can be rephrased as the spacing between the crystal planes perpendicular to the surface of the pyroelectric film. a was smaller than c. In other words, the perovskite oxide contained in the pyroelectric film was tetragonal.
[0088] <Hysteresis curve measurement> A second electrode layer made of Pt was formed directly on the surface of the pyroelectric film constituting the laminate, thereby obtaining a sample (pyroelectric element) for measuring the hysteresis curve. The second electrode layer was formed by a sputtering method in a vacuum chamber. The temperature of the single crystal substrate during the formation of the second electrode layer was maintained at 500°C. The thickness of the second electrode layer was 200 nm. The sample (pyroelectric element) for measuring the hysteresis curve included a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, a second intermediate layer overlapping the first electrode layer, a pyroelectric film overlapping the second intermediate layer, and a second electrode layer overlapping the pyroelectric film.
[0089] The hysteresis curve of the pyroelectric film was measured using the above sample (pyroelectric element). For the measurement, an apparatus combining an atomic force microscope (AFM) and a ferroelectric evaluation system was used. The atomic force microscope was an SPA-400 manufactured by Seiko Instruments Inc. The ferroelectric evaluation system was an FCE manufactured by Toyo Corporation. The frequency of the AC voltage used for measuring the hysteresis curve was 5 Hz. The maximum voltage applied to the pyroelectric thin film during the measurement was 20 V. The temperature of the pyroelectric film during the measurement of the hysteresis curve was maintained at room temperature (25°C). The remanent polarization value Pr of Example 1 is shown in the following Table 1. The remanent polarization value Pr is the polarization value P at an electric field E that is (Ec1+Ec2) / 2 on the hysteresis curve. The Ec1 of Example 1 is shown in Table 1 below. Ec1 is the value when the polarization value P in the hysteresis curve is 0 μC / cm 2 Of the two coercive electric fields, this is the value with the larger absolute value. The Ec2 of Example 1 is shown in the following Table 1. Of the two coercive fields, Ec2 is the value of the coercive field with the smaller absolute value. |Ec1| / |Ec1-Ec2| for Example 1 is shown in Table 1 below.
[0090] <Measurement of pyroelectric coefficient p> A sample (pyroelectric element) for measuring the pyroelectric coefficient p was prepared in the same manner as the sample for measuring the hysteresis curve. The sample after the polarization treatment was placed on a heat stage. The pyrocurrent generated in the sample was continuously measured at each temperature while the temperature of the sample was increased by the heat stage. The temperature of the sample was continuously increased from room temperature to 180°C. The change in pyrocurrent (spontaneous polarization value) per 1°C change in temperature corresponds to the pyroelectric coefficient. The pyroelectric coefficient p of Example 1 is shown in Table 1 below. The pyroelectric coefficient p shown in Table 1 below is the average value of the pyroelectric coefficient in the range from 50°C to 80°C. A homemade device (not for sale) including a pA meter B2987A manufactured by Keysight Technologies, Inc. was used to measure the pyroelectric coefficient p.
[0091] <Relative permittivity ε r Measurements > A sample (pyroelectric element) for measuring the capacitance C was obtained by directly forming a plurality of dot-shaped electrodes (second electrodes) arranged in a lattice pattern on the surface of the pyroelectric film constituting the laminate. Each dot-shaped electrode was made of silver. The diameter φ of each dot-shaped electrode was 100 μm. The interval between the dot-shaped electrodes was 300 μm. The sample (pyroelectric element) for measuring the capacitance C included a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, a second intermediate layer overlapping the first electrode layer, a pyroelectric film overlapping the second intermediate layer, and a second electrode overlapping the pyroelectric film. The capacitance C of the sample was measured. The details of the measurement of the capacitance C were as follows. Measurement equipment: LCR meter (E4980A) manufactured by Agilent Technologies, Inc. Frequency: 10kHz Electric field: 1V / μm Based on the following formula A, the relative dielectric constant ε of the pyroelectric film is calculated from the measured capacitance C. r was calculated. ε0 in formula A is the dielectric constant of a vacuum (8.854×10 -12 Fm -1 ) In formula A, S is the surface area of the pyroelectric film. In other words, S is the total area of the dot-shaped electrodes (silver electrodes) that overlap the surface of the pyroelectric film. In formula A, T is the thickness of the pyroelectric film. C = ε0 × ε r ×(S / T) (A)
[0092] <Calculation of pyroelectric figure of merit Fv> Pyroelectric coefficient p and relative dielectric constant ε r From each of the measured values, the pyroelectric figure of merit Fv of Example 1 was calculated. The pyroelectric figure of merit Fv is p / (c V ε r ) Generally, the constant volume specific heat of pyroelectrics, which are perovskite oxides, is expressed as V is approximately 3.0J / cm 3 ·℃. Therefore, in calculating the pyroelectric figure of merit Fv, the constant volume specific heat c V As a result, it is 3.0 J / cm 3 The pyroelectric figure of merit Fv of Example 1 is shown in Table 1 below.
[0093] (Examples 2 to 6 and Comparative Examples 1 to 5) In Comparative Example 1, the pyroelectric film was PbZr 0.5 Ti 0.5 A thin film consisting of O3 was formed.
[0094] The pyroelectric films of Examples 2 to 6 and Comparative Examples 2 to 5 were formed using targets having the compositions shown in Table 1 below.
[0095] The pyroelectric film of Comparative Example 4 was produced using the same target as in Example 2. However, the configuration of the substrate of Comparative Example 4 was different from that of Example 1. The Pt crystals constituting the first electrode layer of Comparative Example 4 had a (111) plane oriented approximately parallel to the surface of the first electrode layer, but did not have in-plane orientation of the lattice plane. As a result, the pyroelectric film of Comparative Example 4 was not an epitaxial film and did not have crystallinity.
[0096] The pyroelectric film of Comparative Example 5 was produced using the same target as that of Example 4. However, the configuration of the substrate of Comparative Example 5 was different from that of Example 1. The Pt crystals constituting the first electrode layer of Comparative Example 5 had a (111) plane oriented approximately parallel to the surface of the first electrode layer, but did not have in-plane orientation of the lattice plane. As a result, the pyroelectric film of Comparative Example 5 was not an epitaxial film and did not have crystallinity.
[0097] Except for the above points, the pyroelectric elements of Examples 2 to 6 and Comparative Examples 1 to 5 were each produced in the same manner as in Example 1.
[0098] The composition of the pyroelectric film in each of Examples 2 to 6 and Comparative Examples 2 to 5 was analyzed by the same method as in Example 1. In each of Examples 2 to 6 and Comparative Examples 2 to 5, the composition of the pyroelectric film matched the composition of the target (xBKT-yBMT-zBFO in Table 1 below).
[0099] The XRD patterns of the pyroelectric films of Examples 2 to 6 and Comparative Examples 1 to 5 were measured by the same method as in Example 1. The XRD patterns of Examples 2 to 6 and Comparative Examples 1 to 3 all showed that the pyroelectric films were composed of metal oxides having a perovskite structure. In the cases of Examples 2 to 6 and Comparative Examples 1 to 3, the perovskite oxides contained in the pyroelectric films were tetragonal. In the cases of Examples 2 to 6 and Comparative Examples 1 to 3, the (001) plane of the tetragonal crystal was approximately parallel to the surface (principal surface) of the pyroelectric film and approximately perpendicular to the thickness direction of the pyroelectric film. The pyroelectric films of Examples 2 to 6 and Comparative Examples 1 to 3 were epitaxial films.
[0100] Measurements were carried out using the pyroelectric elements of Examples 2 to 6 and Comparative Examples 1 to 5 in the same manner as in Example 1. The results of the measurements of Examples 2 to 6 and Comparative Examples 1 to 5 are shown in Table 1 below. However, in the case of Comparative Example 2, no pyroelectricity was obtained. The hysteresis curves of Example 4 and Comparative Example 1 are shown in FIG.
[0101] [Table 1] [Industrial Applicability]
[0102] For example, a pyroelectric element according to one aspect of the present invention may be used in an infrared sensor such as a blood glucose sensor. [Explanation of symbols]
[0103] Reference Signs List 1: crystalline substrate, 2: first electrode, 3: pyroelectric film, 4: second electrode, 5: first intermediate layer, 6: second intermediate layer, 7: detection portion, 10, 10a, 10b: pyroelectric element, 100: infrared sensor.
Claims
1. A first electrode, a second electrode, and a pyroelectric film, At least a portion of the pyroelectric film is disposed between the first electrode and the second electrode, The hysteresis curve of the pyroelectric film indicates an electric field applied to the pyroelectric film and a polarization value of the pyroelectric film when the electric field is applied, Ec1 is the polarization value in the hysteresis curve of 0 μC / cm 2 The absolute value of the coercive field is larger than that of the two coercive fields, Ec2 is the value of the coercive field having a smaller absolute value of the two coercive fields, the remanent polarization value Pr is the polarization value in the hysteresis curve at the electric field that is (Ec1+Ec2) / 2; The residual polarization value Pr is 50 μC / cm 2 That's all. |Ec1| / |Ec1-Ec2| is 0.55 or more, Pyroelectric element.
2. the pyroelectric film includes a metal oxide having a perovskite structure, The metal oxide includes bismuth, potassium, and titanium. The pyroelectric element according to claim 1 .
3. The metal oxide further comprises at least one element selected from the group consisting of element M and iron; The element M is at least one element selected from the group consisting of magnesium and nickel. The pyroelectric element according to claim 2 .
4. the pyroelectric film contains tetragonal crystals of the metal oxide, The pyroelectric film is polarized in a direction perpendicular to the (001) plane of the tetragonal crystal. The pyroelectric element according to claim 2 or 3.
5. the first electrode comprises platinum crystals; The (002) plane of the platinum crystal is parallel to the (001) plane of the tetragonal crystal. The pyroelectric element according to claim 4.
6. The pyroelectric film is an epitaxial film. The pyroelectric element according to claim 4.
7. Further comprising at least one intermediate layer, the intermediate layer is disposed between the first electrode and the pyroelectric film, The intermediate layer is LaNiO 3 and SrRuO 3 At least one of the following is included: The pyroelectric element according to claim 1 .
8. The temperature of the pyroelectric film during the measurement of the hysteresis curve is 25° C. The pyroelectric element according to claim 1 .
9. The pyroelectric element according to claim 1 , Infrared sensor.
Citation Information
Patent Citations
Infrared sensor and thermal detector element
JP2014185982A
Infrared sensor and thermoelectric conversion element
JP2014187193A
Cited By
Switchable nonvolatile pyroelectric device
US12787645B2
Switchable nonvolatile pyroelectric device
US20240260472A1