Porous electrode material for SOEC / SOFC and manufacturing method thereof
A yttrium-doped ceria-zirconia solid solution with a specific pore structure is used to enhance electrode reaction efficiency in SOEC cathodes and SOFC anodes by improving substrate diffusivity, addressing the inefficiencies of conventional materials.
Patent Information
- Application Number
- JP2023052241
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Conventional electrode materials for SOEC cathodes and SOFC anodes exhibit insufficient electrode reaction efficiency, particularly in reduction reactions.
A porous ionic conductor made of a yttrium-doped ceria-zirconia solid solution with a pore diameter of 1 μm or less and a high pore volume is produced using a method involving a salt-containing aqueous solution, an alkaline dispersant, and a thermosetting resin precursor, followed by carbonization and firing, to enhance electrode reaction efficiency.
The resulting electrode material demonstrates improved reduction reaction efficiency at SOEC cathodes and oxidation reaction efficiency at SOFC anodes, with enhanced diffusivity of reaction substrates due to its porous structure.
Smart Images

Figure 2024140881000002 
Figure 2024140881000003 
Figure 2024140881000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a porous electrode material for solid oxide electrolysis cells (SOEC) / solid oxide fuel cells (SOFC) and a method for producing the same. [Background technology]
[0002] A solid oxide electrolysis cell (SOEC) is a water electrolysis device that uses a solid electrolyte. Carbon dioxide or water vapor is supplied to the cathode (hydrogen electrode) and a current is passed between the electrodes to generate carbon monoxide and hydrogen. A solid oxide fuel cell (SOFC) is a fuel cell that uses a solid electrolyte and has the same structure as an SOEC, but the electrode reaction is the opposite. That is, fuel such as hydrogen, carbon monoxide, or hydrocarbon is supplied to the anode (fuel electrode) and oxygen is supplied to the cathode (oxygen electrode), and the electrode reaction proceeds to generate carbon dioxide and water. Nickel-yttria stabilized zirconia (Ni-YSZ cermet), nickel-scandia stabilized zirconia (Ni-ScSZ cermet), and nickel-samaria doped ceria (Ni-SDC) are commonly used as electrode materials for the cathode of such SOECs and the anode of SOFCs.
[0003] Also, JP 2015-201428 A (Patent Document 1) describes a solid oxide fuel cell including a first inner electrode that acts as an anode and contains Ni and / or NiO and an oxide (excluding oxides containing Zr), and a second inner electrode that acts as an anode catalyst layer and contains Ni, NiO, and a cerium-containing oxide. Furthermore, Patent Document 1 describes the first inner electrode as containing Ni and / or NiO and Y2O3, and also describes a cerium-containing oxide (YDC) doped with yttrium (Y) as the cerium-containing oxide.
[0004] Furthermore, JP 2013-143189 A (Patent Document 1) describes an electrode-forming material used to form an electrode with a porous structure, the electrode-forming material including an electrode material having electronic conductivity and / or ionic conductivity and a pore-forming material made of a plant powder containing glutinous rice starch. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-201428 A [Patent Document 2] JP 2013-143189 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the electrode materials used in conventional SOEC cathodes and SOFC anodes, the electrode reaction efficiency (for example, reduction reaction efficiency in the SOEC cathode) was not necessarily sufficient.
[0007] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and aims to provide an electrode material for use in an SOEC cathode or an SOFC anode, which has excellent electrode reaction efficiency (e.g., reduction reaction efficiency in an SOEC cathode), and a manufacturing method thereof. [Means for solving the problem]
[0008] As a result of intensive research by the inventors in order to achieve the above object, the present inventors have discovered a method for producing a thermosetting resin precursor-containing slurry by mixing a salt-containing aqueous solution containing an yttrium salt, a cerium salt, and a zirconium salt, an alkaline aqueous solution containing a dispersant, and a thermosetting resin precursor, the thermosetting resin precursor in the thermosetting resin precursor-containing slurry is converted into a thermosetting resin to produce a thermosetting resin-containing slurry, the thermosetting resin precursor is dried to prepare a solid component containing the thermosetting resin, and the thermosetting resin precursor is then dried. The present inventors have found that an yttrium-doped ceria-zirconia solid solution, which is a porous ion conductor having a large pore volume and a pore diameter of 1 μm or less, can be obtained by carbonizing the thermosetting resin in a solid component to prepare a carbide-containing solid component and firing the carbide-containing solid component under an air atmosphere. They have also found that an electrode material containing this yttrium-doped ceria-zirconia solid solution has excellent electrode reaction efficiency (for example, reduction reaction efficiency at the cathode of an SOEC), and have thus completed the present invention.
[0009] That is, the present invention provides the following aspects.
[0010] [1] A porous ionic conductor is included, In the porous ionic conductor after heating in air at a temperature in the range of 1000 to 1500°C for 5 hours, the volume of pores having a pore diameter of 1 μm or less is 0.03 cm 3 / g or more, Porous electrode material for SOEC / SOFC.
[0011] [2] The porous electrode material for SOEC / SOFC according to [1], wherein the porous ionic conductor has an oxygen storage capacity.
[0012] [3] The porous electrode material for SOEC / SOFC according to [1] or [2], wherein the porous ionic conductor is a solid solution containing at least yttrium, cerium, and zirconium.
[0013] [4] The solid solution containing at least yttrium, cerium, and zirconium has the following composition formula (1): Yx Ce y Zr 1-x-y O 2-δ (1) (In formula (1), x and y each satisfy 0 < x < 0.2 and 0 < y < 0.2, and δ is a value that maintains electrical neutrality.) The porous electrode material for SOEC / SOFC according to [3], which is a yttrium-added ceria-zirconia solid solution represented by
[0014] [5] The porous electrode material for SOEC / SOFC according to [3] or [4], wherein nickel is supported on the solid solution containing at least yttrium, cerium, and zirconium.
[0015] [6] The porous electrode material for SOEC / SOFC according to any one of [1] to [5], wherein the pore volume of pores having a pore diameter of 1 μm or less is 0.04 cm 3 / g or more.
[0016] [7] A first step of mixing an aqueous salt-containing solution containing a yttrium salt, a cerium salt, and a zirconium salt, an alkaline aqueous solution containing a dispersant, and a thermosetting resin precursor to obtain a thermosetting resin precursor-containing slurry having a pH of 6.0 or more; A second step of converting the thermosetting resin precursor in the thermosetting resin precursor-containing slurry into a thermosetting resin to obtain a thermosetting resin-containing slurry; A third step of drying the thermosetting resin-containing slurry to obtain a solid component containing the thermosetting resin; A fourth step of carbonizing the thermosetting resin in the solid component to obtain a carbide-containing solid component; A fifth step of firing the carbide-containing solid component in an air atmosphere to obtain the porous electrode material according to any one of [3] to [6], which contains a solid solution containing at least yttrium, cerium, and zirconium. A method for manufacturing a porous electrode material for SOEC / SOFC, comprising
[0017] [8] The method for producing a porous electrode material for SOEC / SOFC according to [7], wherein in the first step, the salt-containing aqueous solution and the alkaline aqueous solution are mixed under high shear force to prepare a slurry, and then the thermosetting resin precursor is mixed into the slurry to obtain a slurry containing the thermosetting resin precursor.
[0018] [9] The method for producing a porous electrode material for SOEC / SOFC according to [7], wherein in the first step, the salt-containing aqueous solution, the alkaline aqueous solution, and the thermosetting resin precursor are mixed under high shear force to obtain a slurry containing the thermosetting resin precursor.
[0019]
[10] The high shear stress in the first step is a shear rate of 100,000 sec -1 The method for producing a porous electrode material for SOEC / SOFC according to [8] or [9], wherein the porous electrode material is subjected to a high shear force.
[0020]
[11] The method for producing a porous electrode material for SOEC / SOFC according to any one of [7] to
[10] , wherein in the second step, the thermosetting resin precursor is converted into the thermosetting resin by adjusting a pH of the thermosetting resin precursor-containing slurry to less than 6.0 to obtain the thermosetting resin-containing slurry.
[0021]
[12] The method for producing a porous electrode material for SOEC / SOFC according to any one of [7] to
[11] , wherein in the fifth step, the carbide-containing solid component is reduced and fired in an inert atmosphere, and then fired in an air atmosphere to obtain the porous electrode material containing the solid solution containing at least yttrium, cerium, and zirconium.
[0022] Although the reason why the porous electrode material of the present invention has excellent electrode reaction efficiency is not necessarily clear, the present inventors speculate as follows: That is, as shown in Figures 1A and 1B, the yttrium-doped ceria-zirconia solid solution (YCZ solid solution) (Figure 1A) used as a porous ion conductor in the present invention has a larger pore volume with a pore diameter of 1 μm or less inside the secondary particles than the conventional YCZ solid solution (Figure 1B), and therefore it is speculated that the diffusibility of reaction substrates (for example, carbon dioxide and water vapor in the cathode of an SOEC, and hydrogen, carbon monoxide, and hydrocarbons in the anode of an SOFC) into the YCZ solid solution is improved, resulting in improved electrode reaction efficiency. Effect of the Invention
[0023] According to the present invention, it is possible to obtain an electrode material that is used for the cathode of an SOEC or the anode of an SOFC and has excellent electrode reaction efficiency (for example, reduction reaction efficiency in the cathode of an SOEC). [Brief description of the drawings]
[0024] [Figure 1A] FIG. 2 is a schematic diagram showing the structure of secondary particles of the yttrium-doped ceria-zirconia solid solution used in the present invention. [Figure 1B] FIG. 2 is a schematic diagram showing the structure of secondary particles of a conventional yttrium-added ceria-zirconia solid solution. [Figure 2A] FIG. 1 is a schematic diagram showing a reduction reaction of water vapor in a conventional SOEC cathode. [Figure 2B] FIG. 2 is a schematic diagram showing a reduction reaction of water vapor in a cathode for SOEC containing the porous electrode material of the present invention. [Diagram 3] 1 is a graph showing the pore distribution of the yttrium-added ceria-zirconia solid solution powders obtained in Examples 1 to 3 and Comparative Example 1. [Figure 4] 1 is a graph showing the amount of H 2 produced by catalysts in which NiO is supported on each of the yttrium-added ceria-zirconia solid solution powders obtained in Examples 1 to 3 and Comparative Example 1. [Diagram 5]It is a graph showing the amount of oxygen released by the catalyst supporting Pt on each yttrium-added ceria-zirconia solid solution powder obtained in Examples 1 to 3 and Comparative Example 1. [Figure 6] It is a graph showing the relationship between the pore volume with a pore diameter of 1 μm or less and the amount of H2 generation in the catalyst supporting NiO on each yttrium-added ceria-zirconia solid solution powder obtained in Examples 1 to 3 and Comparative Example 1.
Mode for Carrying Out the Invention
[0025] Hereinafter, the present invention will be described in detail according to its preferred embodiments.
[0026] 〔Porous Electrode Material for SOEC / SOFC〕 First, the porous electrode material for SOEC / SOFC of the present invention will be described. The porous electrode material for SOEC / SOFC of the present invention contains a porous ion conductor, and as the porous ion conductor, those having oxygen storage ability are preferable, and a solid solution containing at least yttrium, cerium, and zirconium is more preferable. The following composition formula (1): Y x Ce y Zr 1-x-y O 2-δ (1) (In formula (1), x and y each satisfy 0 < x < 0.2 and 0 < y < 0.2, and δ is a value that maintains electrical neutrality.) The yttrium-added ceria-zirconia solid solution (YCZ) represented by is particularly preferable. By using a porous ion conductor having oxygen storage ability, oxygen generated in the electrode reaction is stored in the porous ion conductor, so that deterioration due to oxidation of the electrode material is suppressed. Note that the "value that maintains electrical neutrality" means that the sum of the valences of Y x and Ce y and Zr 1-x-y is equal to the sum of the valences of O 2-δ , and is δ that satisfies the following formula: 3×x + 4×y + 4×(1 - x - y) = 2×(2 - δ) is δ that satisfies.
[0027] When a ceria-zirconia solid solution (CZ) without yttrium addition (i.e., x=0 in the composition formula (1)) is used as an electrode material for SOEC / SOFC, the oxide ion conductivity is insufficient, and the electrode characteristics are deteriorated. In addition, when yttrium-added zirconia (YZ) without ceria (i.e., y=0 in the composition formula (1)) is used as an electrode material for SOEC / SOFC, the oxidation of Ni during the electrode reaction cannot be suppressed, and the deterioration of the electrode progresses.
[0028] Furthermore, in the composition formula (1), if x exceeds the upper limit, the toughness of YCZ decreases, and the strength of the electrode decreases, while if y exceeds the upper limit, the lattice expansion of YCZ during the reduction reaction increases, and the durability of the electrode decreases.
[0029] In addition, in the porous ionic conductor, the volume of pores having a pore diameter of 1 μm or less (hereinafter, simply referred to as "pore volume having a pore diameter of 1 μm or less") after heating in air at a temperature in the range of 1000 to 1500° C. for 5 hours is 0.03 cm 3 The pore volume having a pore diameter of 1 μm or less is the total pore volume of pores having a pore diameter of 1 μm or less, calculated based on the pore distribution of the porous ionic conductor determined by mercury intrusion porosimetry using a mercury porosimeter.
[0030] When the volume of the pores having a pore diameter of 1 μm or less is less than the lower limit, the diffusibility of reaction substrates (e.g., carbon dioxide and water vapor in the cathode of an SOEC, and hydrogen, carbon monoxide, and hydrocarbons in the anode of an SOFC) into the inside of the secondary particles of the porous ionic conductor decreases, and the electrode reaction efficiency (e.g., reduction reaction efficiency in the cathode of an SOEC and oxidation reaction efficiency in the anode of an SOFC) decreases. From the viewpoint of improving the diffusibility of reaction substrates into the inside of the secondary particles of the porous ionic conductor and improving the electrode reaction efficiency, the volume of the pores having a pore diameter of 1 μm or less is preferably 0.04 cm. 3 / g or more is preferable, and 0.05 cm 3 / g or more is more preferable, and 0.07 cm 3 / g or more is more preferable, and 0.09 cm3 Although there is no particular upper limit to the volume of the pores having a diameter of 1 μm or less, it is preferable that the upper limit is 1.0 cm3 from the viewpoint of structural stability when an electrode is formed. 3 / g or less is preferable, and 0.7 cm 3 / g or less is more preferable. The lower limit of the pore diameter is equal to or greater than the detection limit of the pore diameter measurable by a mercury porosimeter (for example, 0.001 μm or more).
[0031] In the SOEC / SOFC porous electrode material of the present invention, nickel is preferably supported on the solid solution containing at least yttrium, cerium, and zirconium. The catalytic action of nickel supported on the solid solution promotes the reduction reaction in the SOEC cathode and promotes the oxidation reaction in the SOFC anode, thereby improving the electrode reaction efficiency. In addition, by supporting nickel on the solid solution, deterioration of the SOEC cathode due to the oxidation of nickel tends to be suppressed. The reason why deterioration of the SOEC cathode due to the oxidation of nickel is suppressed is not necessarily clear, but the present inventors speculate as follows. That is, in a conventional SOEC cathode in which nickel (Ni) is supported on a support such as yttria-stabilized zirconia (YSZ cermet), for example, oxygen generated by the reduction reaction of water vapor oxidizes the surface of Ni, as shown in FIG. 2A, so that the catalytic activity of Ni decreases and the SOEC cathode deteriorates. On the other hand, when Ni supported on a solid solution containing at least yttrium, cerium, and zirconium, such as YCZ, is supported on a support such as YSZ cermet, as shown in Figure 2B, oxygen generated by the reduction reaction of water vapor is stored in oxygen vacancies in the solid solution, such as YCZ, and it is presumed that this suppresses the oxidation of the Ni surface and thus the deterioration of the SOEC cathode.
[0032] The amount of nickel supported is preferably 5 to 70 mass %, more preferably 10 to 60 mass %, based on the total amount of the solid solution containing at least yttrium, cerium, and zirconium and nickel oxide, calculated as nickel oxide. If the amount of nickel supported is less than the lower limit, the effect of supporting nickel may not be fully exhibited, whereas if the amount of nickel supported is more than the upper limit, the performance tends to be saturated.
[0033] [Manufacturing method of porous electrode material for SOEC / SOFC] Next, a method for producing the porous electrode material for SOEC / SOFC of the present invention will be described. The method for producing the porous electrode material for SOEC / SOFC of the present invention includes the following steps: a first step of mixing a salt-containing aqueous solution containing a yttrium salt, a cerium salt, and a zirconium salt, an alkaline aqueous solution containing a dispersant, and a thermosetting resin precursor to obtain a thermosetting resin precursor-containing slurry having a pH of 6.0 or more; a second step of converting the thermosetting resin precursor in the thermosetting resin precursor-containing slurry into a thermosetting resin to obtain a thermosetting resin-containing slurry; a third step of drying the thermosetting resin-containing slurry to obtain a solid component containing the thermosetting resin; a fourth step of carbonizing the thermosetting resin in the solid component to obtain a char-containing solid component; A fifth step of sintering the carbide-containing solid component in an air atmosphere to obtain a porous electrode material comprising a solid solution containing at least yttrium, cerium, and zirconium; The method includes:
[0034] <First step> In the first step, a salt-containing aqueous solution containing an yttrium salt, a cerium salt, and a zirconium salt, an alkaline aqueous solution containing a dispersant, and a thermosetting resin precursor are mixed together to obtain a thermosetting resin precursor-containing slurry having a pH of 6.0 or more.
[0035] Examples of the yttrium salt include yttrium nitrate, yttrium chloride, yttrium sulfate, and yttrium acetate. Examples of the cerium salt include ammonium cerium nitrate, cerium nitrate, cerium chloride, cerium sulfate, and cerium acetate. Examples of the zirconium salt include zirconium nitrate, zirconyl oxynitrate, zirconium chloride, zirconium sulfate, and zirconium acetate.
[0036] The salt-containing aqueous solution can be prepared by dissolving the yttrium salt, the cerium salt, and the zirconium salt in water. In the salt-containing aqueous solution, the ratio of the yttrium salt, the cerium salt, and the zirconium salt is appropriately adjusted so that the yttrium (Y), cerium (Ce), and zirconium (Zr) in the YCZ satisfy the composition formula (1).
[0037] Examples of the dispersant include alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, and ethylenediamine; and ammonium salts of carboxylic acids such as ammonium polyacrylate (molecular weight 2000 to 6000).
[0038] In the method for producing a porous electrode material for SOEC / SOFC of the present invention, the aqueous solution containing the dispersant must be alkaline. When the aqueous solution containing the dispersant is alkaline, all of the yttrium (Y) precipitates and can be uniformly dissolved in the solid solution containing at least yttrium, cerium, and zirconium. On the other hand, if the aqueous solution containing the dispersant is acidic, precipitation of yttrium (Y) does not occur, and only a portion of it is incorporated into the solid solution, which causes segregation of yttrium oxide.
[0039] The alkaline aqueous solution containing the dispersant (dispersant-containing alkaline aqueous solution) can be prepared by dissolving the dispersant in water. If the resulting aqueous solution is alkaline, it can be used as is. On the other hand, if the resulting aqueous solution is acidic, a basic compound is added to adjust the aqueous solution to alkaline. Examples of the basic compound include ammonia water, ammonium carbonate, sodium hydroxide, potassium hydroxide, sodium carbonate, etc. In addition, the aqueous solution can be adjusted to alkaline by increasing the amount of the alkanolamine dispersant added.
[0040] Examples of the thermosetting resin precursor include a urea resin precursor (a mixture of urea and formaldehyde), a melamine resin precursor (melamine and formaldehyde, or commercially available methylol melamine), and other resin precursors that react with formaldehyde to form a methylol group.
[0041] In the method for producing the porous electrode material for SOEC / SOFC of the present invention, the method for mixing the salt-containing aqueous solution, the dispersant-containing alkaline aqueous solution, and the thermosetting resin precursor is not particularly limited as long as it is a method that can obtain a slurry containing the solid solution containing at least yttrium, cerium, and zirconium and the thermosetting resin precursor (slurry containing a thermosetting resin precursor). For example, the salt-containing aqueous solution and the dispersant-containing alkaline aqueous solution are mixed to prepare a slurry containing the solid solution containing at least yttrium, cerium, and zirconium, and then the thermosetting resin precursor is mixed with this slurry (first method); the salt-containing aqueous solution is mixed with an alkaline aqueous solution containing the dispersant and the thermosetting resin precursor (second method), etc. Among these methods, the first method is more preferable from the viewpoint that the pore volume having a pore diameter of 1 μm or less is increased in the obtained solid solution.
[0042] When the salt-containing aqueous solution is mixed with the dispersant-containing alkaline aqueous solution, or when the salt-containing aqueous solution is mixed with the alkaline aqueous solution containing the dispersant and the thermosetting resin precursor, the mixing is performed under high shear force (preferably at a shear rate of 10,000 sec -1 More preferably, the shear rate is 15,000 sec -1 It is preferable to carry out the mixing under high shearing force (above 10 ...
[0043] In the thermosetting resin precursor-containing slurry thus obtained, the content ratio of the solid solution containing at least yttrium, cerium, and zirconium to the thermosetting resin precursor is preferably 1:4 to 1:10 by mass, more preferably 1:5 to 1:8 by mass, and particularly preferably 1:6 to 1:7 by mass. If the ratio of the thermosetting resin precursor is less than the lower limit, the predetermined pore volume tends to be insufficient, while if the ratio of the thermosetting resin precursor exceeds the upper limit, the production efficiency decreases, and the resin component is wasted, which is undesirable from the viewpoint of carbon neutrality. The mixing ratio of the salt-containing aqueous solution, the dispersant-containing alkaline aqueous solution, and the thermosetting resin precursor, and the mixing ratio of the salt-containing aqueous solution and the alkaline aqueous solution containing the dispersant and the thermosetting resin precursor are appropriately adjusted so that the content ratio of the solid solution and the thermosetting resin precursor is within the above range.
[0044] The pH of the thermosetting resin precursor-containing slurry thus obtained is usually 6.0 or more, preferably 6.2 or more, more preferably 6.4 or more, and usually 8.0 or less, preferably pH 7.5 or less, more preferably pH 7.0 or less. When preparing a thermosetting resin precursor-containing slurry by the first method, the pH of the slurry containing the solid solution obtained by mixing the salt-containing aqueous solution and the dispersant-containing alkaline aqueous solution is adjusted to preferably 9.0 or more, more preferably 9.5 or more, in order to form the solid solution. There is no particular limit to the upper limit of the pH of the slurry containing the solid solution, but a pH of 10 or less is preferred. Then, by mixing the thermosetting resin precursor with the slurry containing the solid solution having such a pH, a thermosetting resin precursor-containing slurry having a pH within the above range is obtained.
[0045] <Second step> In the second step, the thermosetting resin precursor in the slurry containing the thermosetting resin precursor obtained in the first step is converted into a thermosetting resin, thereby obtaining a slurry containing a thermosetting resin.
[0046] The method of converting the thermosetting resin precursor into the thermosetting resin is not particularly limited, but may be, for example, a method of adjusting the pH of the thermosetting resin precursor-containing slurry to less than 6.0, preferably 5.8 or less, more preferably 5.5 or less. The method of adjusting the pH of the thermosetting resin precursor-containing slurry to the above range may be, for example, a method of adding an acid to the thermosetting resin precursor-containing slurry. The acid may be, for example, an organic carboxylic acid such as maleic acid, citric acid, malic acid, or acetic acid.
[0047] <Third process> In the third step, the thermosetting resin-containing slurry obtained in the second step is dried, thereby obtaining a solid component containing the thermosetting resin.
[0048] The drying conditions for the thermosetting resin-containing slurry are not particularly limited as long as the water in the slurry can be removed. For example, the drying temperature is preferably 110 to 180° C., and more preferably 140 to 160° C., and the drying time is preferably 7 to 15 hours, and more preferably 10 to 12 hours.
[0049] <Fourth step> In the fourth step, the thermosetting resin in the solid component obtained in the third step is carbonized, thereby obtaining a char-containing solid component.
[0050] The heating conditions for carbonizing the thermosetting resin are not particularly limited, but for example, the heating temperature is preferably 200 to 350° C., more preferably 280 to 320° C., and the heating time is preferably 1 to 5 hours, more preferably 2 to 4 hours.
[0051] <The fifth step> In the fifth step, the carbide-containing solid component obtained in the fourth step is sintered in an air atmosphere, thereby obtaining a porous electrode material containing a solid solution containing at least yttrium, cerium, and zirconium, the pore volume of which is within a predetermined range and has a pore diameter of 1 μm or less.
[0052] The conditions for firing the carbide-containing solid component are not particularly limited, but for example, the firing temperature is preferably 1250 to 1400° C., more preferably 1300 to 1350° C., and the firing time is preferably 3 to 10 hours, more preferably 4 to 6 hours.
[0053] In the fifth step, the carbide-containing solid component is preferably reduced and fired in an inert atmosphere, and then fired in an air atmosphere. This increases the volume of pores with a pore diameter of 1 μm or less in the obtained solid solution. The reduction and firing in an inert atmosphere suppresses excessive sintering between oxide particles in the solid solution while keeping the carbon contained, and grows necks between the oxide particles, thereby increasing the oxygen ion conductivity of the solid solution while maintaining a porous state.
[0054] The inert atmosphere is not particularly limited, and examples thereof include an argon gas atmosphere, a nitrogen gas atmosphere, and a helium gas atmosphere. The reduction firing conditions are not particularly limited, and examples thereof include a reduction firing temperature of preferably 800 to 1000°C, more preferably 850 to 950°C, and a reduction firing time of preferably 3 to 10 hours, more preferably 4 to 6 hours. If the reduction firing temperature is below the lower limit, the formation of necks is likely to be insufficient, while if the reduction firing temperature exceeds the upper limit, the carbon (carbide) derived from the thermosetting resin and the zirconia in the solid solution may form a carbide (ZrC), destroying the porous structure. EXAMPLES
[0055] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0056] Example 1 <Preparation of aqueous solution A-1> 10.34 g of yttrium nitrate hexahydrate (Y(NO3)3·6H2O, manufactured by Kanto Chemical Co., Ltd.), 10.96 g of ammonium cerium nitrate (Ce(NH4)2(NO3)6, manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.), and 104.74 g of an aqueous solution of zirconium oxynitrate (Zr(NO3)2, 18% by mass aqueous solution, "Zircosol" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.) were mixed, and ion-exchanged water was further added to prepare a total of 400 ml of aqueous solution A-1. The pH of this aqueous solution A-1 was 1.29.
[0057] <Preparation of aqueous solution B-1> 57.04 g of 2-aminoethanol (monoethanolamine, Fujifilm Wako Pure Chemical Industries, Ltd.) and 253.16 g of ammonium polyacrylate (Aron A30SL, Toagosei Co., Ltd.) were added to ion-exchanged water to prepare a total of 400 ml of aqueous solution B-1. The pH of this aqueous solution B-1 was 10.3.
[0058] <Preparation of Slurry C-1> The aqueous solution A-1 and the aqueous solution B-1 were mixed using the "Apparatus for Producing Ultrafine Particles and Porous Body Precursors" described in Japanese Patent No. 6658564 at a rotor rotation speed of 8000 rpm, a liquid delivery speed of 5 ml / min, and a shear rate of 15000 sec. -1 The mixture was mixed under the above conditions to prepare slurry C-1. As the SA (Shear-Agitation) reactor of the manufacturing apparatus, an outer nozzle type SA reactor of the type shown in Figures 5A and 5B of the above patent publication was used, and during mixing, nozzles 15B and 15C and flow paths 16B and 16C were used instead of nozzle 15A and flow path 16A. The pH of the obtained slurry C-1 was 9.72.
[0059] <Preparation of Slurry D-1> 52.74 g of urea (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was added to water to prepare a total of 250 ml of urea aqueous solution. In addition, 128.30 g of formaldehyde (36-38% aqueous solution, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was added to ion-exchanged water to prepare a total of 250 ml of formaldehyde aqueous solution. The urea aqueous solution and the formaldehyde aqueous solution were each dropped into the slurry C-1 at a liquid delivery rate of 10 ml / min using a cassette tube pump and mixed to prepare a slurry D-1 containing a urea resin precursor. The pH of this slurry D-1 was 6.52.
[0060] <Preparation of Slurry E-1> 29.05g of maleic anhydride was added to ion-exchanged water, and the mixture was stirred with a magnetic stirrer to prepare a total of 200ml of maleic acid aqueous solution. The pH of this maleic acid aqueous solution was 1.59. The maleic acid aqueous solution was dropped into the slurry D-1 at a liquid delivery rate of 10ml / min using a cassette tube pump, and mixed, and the urea resin precursor was converted into urea resin to prepare a slurry E-1 containing the urea resin. The pH of this slurry E-1 was 5.45.
[0061] <Drying> First, the slurry E-1 was stirred overnight using a magnetic stirrer, and then divided into two 1 L glass beakers, which were then placed in a hot air dryer and dried at 150° C. for 12 hours.
[0062] <Carbonization> Next, the obtained solid component was heated at 300° C. for 4 hours using a hot air dryer to carbonize the urea resin.
[0063] <Firing> Next, the solid component after carbonization was transferred from the glass beaker to a carbon container and placed in a small vacuum pressure sintering furnace (FVPS-R-150, manufactured by Fuji Electric Industrial Co., Ltd.) and reduced and fired at 900°C for 5 hours under an argon gas atmosphere. The solid component after reduction and firing was transferred from the carbon container to an alumina crucible and placed in a Kanthal Super electric furnace (NE-3550G, manufactured by Motoyama Co., Ltd.) and heated to 1340°C at a heating rate of 134°C / h in an air atmosphere, and then held at this temperature for 5 hours to obtain Y-added CeO2-ZrO2 solid solution powder (YCZ powder). The atomic ratio of this YCZ powder was Y / Ce / Zr=13.5 / 10.0 / 76.5.
[0064] Example 2 <Preparation of aqueous solution B-2> 57.04 g of 2-aminoethanol (monoethanolamine, Fujifilm Wako Pure Chemical Industries, Ltd.), 253.16 g of ammonium polyacrylate (Toagosei Co., Ltd. "Aron A30SL"), 52.74 g of urea (Fujifilm Wako Pure Chemical Industries, Ltd.), and 128.30 g of formaldehyde (36-38% aqueous solution, Fujifilm Wako Pure Chemical Industries, Ltd.) were added to ion-exchanged water to prepare a total of 400 ml of aqueous solution B-2. The pH of this aqueous solution B-2 was 8.96.
[0065] <Preparation of Slurry D-2> The aqueous solution A-1 and the aqueous solution B-2 prepared in the same manner as in Example 1 were mixed in a rotor at a rotation speed of 8000 rpm, a liquid feed rate of 5 ml / min, and a shear rate of 15000 sec using the "Apparatus for Producing Ultrafine Particles and Porous Body Precursors" described in Japanese Patent No. 6658564. -1The mixture was mixed under the above conditions to prepare a slurry D-2 containing a urea resin precursor. As the SA (Shear-Agitation) reactor of the manufacturing apparatus, an outer nozzle type SA reactor of the type shown in Figures 5A and 5B of the above patent publication was used, and during mixing, nozzles 15B and 15C and flow paths 16B and 16C were used instead of nozzle 15A and flow path 16A. The pH of the obtained slurry D-2 was 7.12.
[0066] <Preparation of Slurry E-2> The maleic acid aqueous solution prepared in the same manner as in Example 1 was added dropwise to the slurry D-2 at a liquid delivery rate of 10 ml / min using a cassette tube pump, and mixed to convert the urea resin precursor to urea resin, thereby preparing a slurry E-2 containing the urea resin. The pH of this slurry E-2 was 5.75.
[0067] <Drying, carbonization and firing> A Y-added CeO2-ZrO2 solid solution powder (YCZ powder) was obtained in the same manner as in Example 1, except that the slurry E-2 was used instead of the slurry E-1. The atomic ratio of this YCZ powder was Y / Ce / Zr=13.5 / 10.0 / 76.5.
[0068] Example 3 <Firing> The carbonized solid component prepared in the same manner as in Example 1 was transferred from the glass beaker to an alumina crucible and placed in a Kanthal Super electric furnace ("NE-3550G" manufactured by Motoyama Corporation), where it was heated to 1340°C at a heating rate of 134°C / h in an air atmosphere, and then held at this temperature for 5 hours to obtain a Y-added CeO2-ZrO2 solid solution powder (YCZ powder). The atomic ratio of this YCZ powder was Y / Ce / Zr=13.5 / 10.0 / 76.5.
[0069] Comparative Example 1 49.1g of cerium nitrate solution with a concentration of 28% by mass in terms of CeO2, 418.2g of zirconium nitrate aqueous solution with a concentration of 18% by mass in terms of ZrO2, 99.8g of 30% hydrogen peroxide solution, and yttrium nitrate aqueous solution (41.4g of yttrium nitrate dissolved in 50ml of pure water) were mixed. The resulting mixed solution was added to diluted ammonia water (145.9g of 25% ammonia water diluted with 400ml of pure water) while stirring with a propeller stirrer, and further stirred at 1000 rpm for 10 minutes using a homogenizer to generate a precipitate. The solution containing this precipitate was distributed into three 1L beakers and placed in a degreasing furnace, dried in air at 150°C for 7 hours, and then calcined at 400°C for 5 hours. The calcined powder was placed in a Kanthal Super electric furnace ("NE-3550G" manufactured by Motoyama Corporation) and heated to 1340°C at a rate of 134°C / h in an air atmosphere, and then held at this temperature for 5 hours to obtain Y-added CeO2-ZrO2 solid solution powder (YCZ powder). The atomic ratio of this YCZ powder was Y / Ce / Zr=13.5 / 10.0 / 76.5.
[0070] [Pore distribution measurement] The pore distribution of the obtained YCZ powder was measured by mercury intrusion method using a mercury porosimeter ("PoreMaster 60GT" manufactured by Anton Paar). The results are shown in Figure 3. In addition, based on the obtained pore distribution, the pore volume with a pore diameter of 1 μm or less was calculated. The results are shown in Table 1.
[0071] [Catalyst preparation] The obtained YCZ powder was impregnated with nickel (II) nitrate so that the amount of NiO supported was 10 mass%, and then evaporated to dryness. The obtained dried product was calcined in air at 400°C for 3 hours to prepare a powder in which NiO was supported on the YCZ (NiO-supported YCZ powder). This NiO-supported YCZ powder was then heated in air at 1340°C for 5 hours to obtain a catalyst powder. 3 g of this catalyst powder and 1 g of γ-alumina powder were mixed in a mortar, and the resulting mixed powder was subjected to a pressure of 1000 kgf / cm. 2 After cold isostatic pressing (CIP) at a pressure (molding pressure) of (98 MPa) for 1 minute, the catalyst powder for evaluating hydrogen generation capacity was obtained by crushing the catalyst into pellets having a diameter of 0.5 to 1 mm.
[0072] The obtained YCZ powder was heated in air at 1,340°C for 5 hours to obtain a heat-treated YCZ powder, which was then impregnated with a dinitrodiammineplatinum(II) acid solution and evaporated to dryness. The dried product was then calcined at 300°C for 3 hours to obtain a catalyst powder for oxygen release measurement in which platinum (Pt) was supported on the YCZ powder (Pt loading: 1% by mass).
[0073] [Hydrogen generation ability evaluation test] 1 g of the catalyst powder for evaluating hydrogen generation capacity prepared as described above was packed into a reaction tube and set in a fixed-bed flow-type catalytic reaction evaluation device (Best Sokki Co., Ltd. "CATA-5000-SP7"). While flowing O2 (5%)-containing gas (balance: N2) at a gas flow rate of 5 L / min, the catalyst bed was heated from room temperature to 700°C over 14 minutes (Step 1), and then held at 700°C for 10 minutes (Step 2). Next, while holding the catalyst bed at 700°C, N2 was flowed at a gas flow rate of 5 L / min for 5 minutes. After passing the catalyst bed through the catalyst bed (Step 3), a gas containing H2 (1%) (balance: N2) was passed through the catalyst bed for 10 minutes (Step 4), N2 was passed through the catalyst bed for 10 minutes again (Step 5), and then a gas containing water vapor (20%) (balance: N2) was passed through the catalyst bed for 20 minutes (Step 6). After that, the catalyst bed was held at 700°C for 1 minute while passing N2 at a gas flow rate of 5 L / min (Step 7), and then cooled to room temperature (Step 8). The amount of H2 generated in Step 6 was measured. The results are shown in FIG. 4 and Table 1.
[0074] <Oxygen release measurement> 15 mg of the catalyst powder for measuring the amount of oxygen released prepared as described above was placed in a thermogravimetric measuring device (Shimadzu Corporation's "TGA-50"), and a reducing gas (H2 (5% by volume) + N2 (balance)) and an oxidizing gas (O2 (5% by volume) + N2 (balance)) were passed through the catalyst powder at a gas flow rate of 100 ml / min at a temperature of 700°C while being alternately switched every 5 minutes, and the increase or decrease in the mass of the catalyst powder during this period was measured. The amount of mass loss of the catalyst powder during the third reduction gas pass was determined and this was taken as the amount of oxygen released. The results are shown in Figure 5 and Table 1.
[0075] [Table 1]
[0076] As shown in Table 1, it was confirmed that the catalysts (Examples 1 to 3) using as a support YCZ powder prepared by heating a solid component consisting of a mixture of YCZ powder and a resin component to carbonize the resin component had a larger pore volume with a pore diameter of 1 μm or less than the catalyst (Comparative Example 1) using as a support YCZ powder prepared by coprecipitation.
[0077] Furthermore, as shown in FIG. 4 and Table 1, the catalysts (Examples 1 to 3) using as a support YCZ powder prepared by heating a solid component consisting of a mixture of YCZ powder and a resin component to carbonize the resin component produced more H2 and were superior in hydrogen generation ability compared to the catalyst (Comparative Example 1) using as a support YCZ powder prepared by coprecipitation.
[0078] Furthermore, as shown in FIG. 5 and Table 1, it was found that the catalysts (Examples 1 to 3) using as a support YCZ powder prepared by heating a solid component consisting of a mixture of YCZ powder and a resin component to carbonize the resin component released more oxygen and had superior oxygen storage capacity than the catalyst (Comparative Example 1) using as a support YCZ powder prepared by coprecipitation.
[0079] Based on the results shown in Table 1, the amount of H2 generated was plotted against the volume of pores with a pore diameter of 1 μm or less. The results are shown in FIG. 6. As shown in FIG. 6, it was found that the amount of H2 generated increased as the volume of pores with a pore diameter of 1 μm or less increased. This result indicates that the increase in the volume of pores with a pore diameter of 1 μm or less inside the secondary particles of YCZ improved the diffusibility of water vapor into the inside of the secondary particles of YCZ, and the reduction reaction of water vapor by YCZ proceeded efficiently. Therefore, it was confirmed that the electrode material of the present invention is an electrode with excellent electrode reaction efficiency because it can efficiently reduce water vapor. [Industrial Applicability]
[0080] As described above, according to the present invention, it is possible to obtain an electrode material having excellent electrode reaction efficiency. Therefore, the porous electrode material of the present invention is useful as an electrode material for use in the cathode of an SOEC or the anode of an SOFC.
Claims
1. Contains a porous ionic conductor, In the porous ionic conductor after heating in air at a temperature in the range of 1000 to 1500°C for 5 hours, the volume of pores having a pore diameter of 1 μm or less is 0.03 cm 3 / g or more; A porous electrode material for SOEC / SOFC, characterized in that:
2. 2. The porous electrode material for SOEC / SOFC according to claim 1, wherein the porous ionic conductor has an oxygen storage capacity.
3. 2. The porous electrode material for SOEC / SOFC according to claim 1, wherein the porous ionic conductor is a solid solution containing at least yttrium, cerium, and zirconium.
4. The solid solution containing at least yttrium, cerium, and zirconium has the following composition formula (1): Y x Ce y Zr 1-x-y O 2-δ (1) (In formula (1), x and y satisfy 0<x<0.2 and 0<y<0.2, respectively, and δ is a value that maintains electrical neutrality.) 4. The porous electrode material for SOEC / SOFC according to claim 3, which is a yttrium-doped ceria-zirconia solid solution represented by the formula:
5. 4. The porous electrode material for SOEC / SOFC according to claim 3, wherein nickel is supported on the solid solution containing at least yttrium, cerium and zirconium.
6. The pore volume of the pores having a diameter of 1 μm or less is 0.04 cm 3 2. The porous electrode material for SOEC / SOFC according to claim 1, wherein the porous electrode material for SOEC / SOFC has a molecular weight of 1 / g or more.
7. a first step of mixing a salt-containing aqueous solution containing a yttrium salt, a cerium salt, and a zirconium salt, an alkaline aqueous solution containing a dispersant, and a thermosetting resin precursor to obtain a thermosetting resin precursor-containing slurry having a pH of 6.0 or more; a second step of converting the thermosetting resin precursor in the thermosetting resin precursor-containing slurry into a thermosetting resin to obtain a thermosetting resin-containing slurry; a third step of drying the thermosetting resin-containing slurry to obtain a solid component containing the thermosetting resin; a fourth step of carbonizing the thermosetting resin in the solid component to obtain a char-containing solid component; A fifth step of calcining the carbide-containing solid component in an air atmosphere to obtain the porous electrode material according to claim 3, which contains a solid solution containing at least yttrium, cerium, and zirconium; A method for producing a porous electrode material for SOEC / SOFC, comprising:
8. 8. The method for producing a porous electrode material for SOEC / SOFC according to claim 7, wherein in the first step, the salt-containing aqueous solution and the alkaline aqueous solution are mixed under high shear force to prepare a slurry, and then the thermosetting resin precursor is mixed into the slurry to obtain a slurry containing the thermosetting resin precursor.
9. 8. The method for producing a porous electrode material for SOEC / SOFC according to claim 7, characterized in that in the first step, the salt-containing aqueous solution, the alkaline aqueous solution, and the thermosetting resin precursor are mixed under high shear force to obtain a slurry containing the thermosetting resin precursor.
10. The high shear stress in the first step is a shear rate of 100,000 sec -1 10. The method for producing a porous electrode material for SOEC / SOFC according to claim 8 or 9, wherein the porous electrode material is subjected to a high shearing force of at least 100%.
11. 8. The method for producing a porous electrode material for SOEC / SOFC according to claim 7, characterized in that in the second step, the thermosetting resin precursor is converted into the thermosetting resin by adjusting the pH of the thermosetting resin precursor-containing slurry to less than 6.0 to obtain the thermosetting resin-containing slurry.
12. 8. The method for producing a porous electrode material for SOEC / SOFC according to claim 7, characterized in that in the fifth step, the carbide-containing solid component is reduced and fired in an inert atmosphere, and then fired in an air atmosphere to obtain a porous electrode material containing a solid solution containing at least yttrium, cerium, and zirconium.
Citation Information
Patent Citations
Solid oxide fuel cell and its manufacturing method
JP2007242429A
Solid electrolyte material
JP2016150892A
Anode for solid oxide fuel cell
JP2020155349A
Anode for solid oxide fuel cell
JP2020170607A
Hydrogen electrode for water vapor electrolysis
JP2022181976A