A conductive paste and its preparation method and application in high temperature porous back electrode
By adding a high-temperature binder to the conductive paste, the problems of poor mechanical properties and adhesion of high-temperature porous electrodes were solved, the mechanical properties and adhesion of porous electrodes were enhanced, and the performance of perovskite solar cells was improved.
Patent Information
- Application Number
- CN202310156507.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-02-23
AI Technical Summary
The poor mechanical properties and poor adhesion to the substrate of existing high-temperature porous electrodes affect the device performance of perovskite solar cells.
A high-temperature binder is added to the conductive paste. The high-temperature binder melts and penetrates into the bottom layer of the electrode during the high-temperature annealing process of the porous electrode, which enhances the mechanical properties and adhesion, and accumulates at the mesoporous spacer layer to block electron transfer.
This improved the mechanical properties and adhesion to the substrate of the porous electrode, thereby enhancing the device performance of perovskite solar cells, particularly power conversion efficiency and current density.
Smart Images

Figure CN116031015B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrode preparation of optoelectronic / electronic devices, and more specifically, to a conductive paste and a preparation method thereof and an application in a high-temperature porous back electrode, and in particular to a conductive paste that can be used to prepare a high-temperature porous electrode and an application thereof in preparing a porous electrode for a printable perovskite solar cell. Background Art
[0002] Nowadays, the development of optoelectronic / electronic devices has become one of the important indicators to measure the level of high-tech development of a country. The electrode preparation technology of optoelectronic / electronic devices is one of the core technologies that affect the performance of the device. The electrode must have good conductivity, processing stability, high efficiency and other characteristics. Common ones are metal electrodes based on gold, silver, platinum, and copper, and carbon electrodes based on graphite. Electrodes can be mainly prepared by direct high-temperature deposition or coating with conductive slurry. High-temperature deposition technology equipment is expensive and the process is complicated, while the method of preparing electrodes by coating conductive slurry is simple and conducive to the industrial production of electrodes.
[0003] Conductive paste can be divided into two types: low-temperature sintering and drying type and high-temperature sintering type. Low-temperature sintering and drying type conductive paste is cured at a temperature of <250°C. It generally uses synthetic resins such as acrylic, epoxy, and polyester as adhesives. It can be cured at low temperatures and is widely used in printed circuits and electronic packaging. High-temperature sintering conductive paste is usually sintered at a temperature of 350°C to 850°C. During the high-temperature calcination process, the low-temperature binder and pore-forming agent in the high-temperature sintering conductive paste will decompose and volatilize at high temperatures, leaving holes in the electrode, thereby forming a porous structure electrode, which is widely used in solar cells and other fields. Among them, perovskite solar cells have attracted widespread attention from researchers due to their excellent power conversion efficiency, solution preparation, and low material cost.
[0004] The porous electrodes in perovskite solar cells are mostly based on conductive carbon materials such as graphite, carbon black, carbon nanotubes, and graphene, which have the advantages of good stability and low price. The preparation of porous electrodes by coating the conductive slurry on the substrate through the screen printing process is conducive to the large-scale industrial preparation of battery devices. However, the loose porous structure of the electrode will lead to poor mechanical properties of the porous electrode and poor adhesion to the substrate, which will directly affect the conductivity of the electrode and the contact with the external circuit, thus affecting the device performance of the perovskite solar cell. Summary of the invention
[0005] In view of the defects and improvement needs of the prior art, the present invention provides a conductive paste and a preparation method thereof and an application in a high-temperature porous back electrode. The present invention improves the mechanical properties of the high-temperature porous electrode and the adhesion to the substrate by adding a high-temperature binder to the conductive paste. In addition, the porous back electrode of a printable perovskite solar cell is prepared with the conductive paste, which is beneficial to improving the device performance. Thus, the technical problems of poor mechanical properties and poor adhesion to the substrate of the high-temperature porous electrode in the prior art are solved.
[0006] According to a first aspect of the present invention, a conductive paste is provided, comprising conductive medium particles, a high temperature adhesive, a low temperature adhesive, a pore former and a solvent; the high temperature adhesive will not decompose and volatilize at 1000°C, thereby playing a role in bonding the conductive medium particles; the low temperature adhesive will decompose and volatilize at 300°C; the boiling point of the solvent is greater than 100°C;
[0007] When the low-temperature adhesive has a pore-forming effect, the low-temperature adhesive also functions as a pore-forming agent;
[0008] When the low-temperature adhesive does not have a pore-forming function, the conductive paste further includes a pore-forming agent.
[0009] Preferably, the initial melting temperature of the high-temperature adhesive is less than 400°C.
[0010] Preferably, the high temperature binder is one or more of low melting point glass powder, zirconium dioxide, silicone resin, epoxy resin, modified phenolic resin, polyurethane resin, silicate, phosphate and phosphazene salt;
[0011] The low-temperature binder is one or more of cellulose, polyethylene glycol, starch and polyvinyl pyrrolidone;
[0012] The pore-forming agent is one or more of cellulose, polystyrene and polyvinyl pyrrolidone.
[0013] Preferably, the conductive medium particles are one or more of graphite, carbon black, carbon nanotubes, graphene, fluorine-doped tin oxide, tin-doped indium oxide, aluminum-doped zinc oxide and antimony-doped tin oxide.
[0014] Preferably, the conductive paste further comprises an auxiliary agent;
[0015] Preferably, the auxiliary agent is at least one of a dispersant, a leveling agent and a defoaming agent.
[0016] Preferably, in the conductive paste, the mass ratio of the mass of the conductive medium particles, the mass of the high-temperature binder, and the sum of the mass of the low-temperature binder and the pore-forming agent is (10-20): (1-2): (2-3).
[0017] According to another aspect of the present invention, a method for preparing any one of the conductive pastes is provided.
[0018] The conductive medium particles, high temperature adhesive, low temperature adhesive, pore former and solvent are mixed, or the conductive medium particles, high temperature adhesive, low temperature adhesive and solvent are mixed, the boiling point of the solvent is greater than 100° C., and then a low boiling point solvent is added, and the low boiling point solvent is one or more of ethanol and isopropanol. After fully mixing, the low boiling point solvent is removed by heating or vacuuming to obtain the conductive paste.
[0019] According to another aspect of the present invention, there is provided a use of any one of the conductive pastes for preparing a porous back electrode;
[0020] Preferably, the back electrode is a porous back electrode of a mesoscopic perovskite solar cell;
[0021] Preferably, the application is specifically: coating the conductive paste to form a wet film, and heating to remove the solvent, pore former and low-temperature binder to form a porous back electrode.
[0022] According to another aspect of the present invention, a porous back electrode is provided, which is obtained by the application.
[0023] According to another aspect of the present invention, a mesoscopic perovskite solar cell is provided, comprising the porous back electrode.
[0024] In general, the above technical solutions conceived by the present invention can achieve the following beneficial effects compared with the prior art:
[0025] (1) The conductive paste for preparing a high-temperature porous electrode of the present invention comprises the following components: conductive medium particles, a high-temperature binder, a low-temperature binder, a pore former, and a solvent. The high-temperature binder is preferably a low-melting-point glass powder, which will melt when heated during the preparation of the high-temperature porous electrode, but will not decompose and volatilize, thereby playing the role of bonding the conductive medium particles in the electrode, and can enhance the mechanical properties of the porous electrode and the adhesion to the substrate. The present invention adds a high-temperature binder to the conductive paste, and can undergo a process of heating up, melting, penetrating into the bottom layer of the electrode, and then cooling down and solidifying during the high-temperature annealing of the porous electrode, thereby bonding the conductive medium particles in the electrode, and enhancing the mechanical properties of the high-temperature porous electrode and the contact with the substrate.
[0026] (2) The conductive paste of the present invention is used to prepare porous electrodes for printable mesoscopic perovskite solar cells. During the high-temperature annealing of the porous electrode, the high-temperature adhesive will melt and then penetrate into the bottom layer through the porous structure of the electrode. Most of it will gather at the contact point with the mesoporous spacer layer substrate, which can not only enhance the adhesion with the substrate, but the insulating high-temperature adhesive can also serve as a barrier layer to block the transfer of electrons in the perovskite to the porous back electrode, thereby reducing the non-radiative recombination of electrons and holes on the porous back electrode, thereby improving the performance of the printable mesoscopic perovskite solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the structure of a printable mesoscopic perovskite solar cell based on a porous electrode provided in an embodiment of the present invention.
[0028] Figure 2 This is the current-voltage diagram of the printable mesoscopic perovskite solar cell based on porous electrodes provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0030] The present invention discloses a conductive paste that can be used to prepare a high-temperature porous electrode, comprising the following components: conductive medium particles, a high-temperature binder, a low-temperature binder, a pore former, and a solvent; wherein the high-temperature binder will melt when heated during the preparation of the high-temperature porous electrode, but will not decompose and volatilize, thereby playing a role in bonding the conductive medium particles in the electrode, thereby enhancing the mechanical properties of the porous electrode and the adhesion to the substrate; the low-temperature binder is used to bond the solid phase components in the paste to facilitate wet coating processing, and the low-temperature binder will decompose and volatilize when heated during the preparation of the high-temperature porous electrode, thereby being removed; the pore former will decompose and volatilize when heated during the preparation of the high-temperature porous electrode, leaving holes in the electrode, thereby forming an electrode with a porous structure; the solvent will volatilize when heated during the preparation of the high-temperature porous electrode, thereby being removed;
[0031] In some embodiments, an auxiliary agent is also included, and the auxiliary agent includes a dispersant, a leveling agent, and a defoaming agent; the auxiliary agent can be volatilized and decomposed by heat, and can also be retained in the prepared high-temperature porous electrode.
[0032] In some embodiments, the conductive medium particles include one or more of graphite, carbon black, carbon nanotubes, graphene, fluorine-doped tin oxide, tin-doped indium oxide, aluminum-doped zinc oxide, and antimony-doped tin oxide powder.
[0033] In some embodiments, the high temperature binder has an initial melting temperature of less than 400° C. and includes low melting point glass powder.
[0034] In some embodiments, the low-temperature binder includes one or more of cellulose, polyethylene glycol, starch, and polyvinyl pyrrolidone.
[0035] In some embodiments, the pore-forming agent includes one or more of cellulose, polystyrene, and polyvinyl pyrrolidone.
[0036] In some embodiments, the solvent includes one or more of n-butanol, terpineol, and ethylene glycol.
[0037] In some embodiments, the conductive medium particles account for 5-30% by mass, the high temperature binder accounts for 0.5-5% by mass, the low temperature binder accounts for 1-10% by mass, the pore former accounts for 1-10% by mass, the auxiliary agent accounts for 0.5-5% by mass, and the rest is solvent.
[0038] The preparation method of the conductive paste of the present invention comprises the following steps: weighing each component according to a ratio; adding an appropriate amount of a low-boiling point solvent, including one or more of ethanol and isopropanol; mixing the raw materials mechanically or ultrasonically; and removing the low-boiling point solvent by heating or vacuuming to obtain a conductive paste that can be used to prepare a high-temperature porous electrode.
[0039] The conductive paste described in the present invention can be used to prepare porous electrodes for optoelectronic / electronic devices; the device includes a printable mesoscopic perovskite solar cell; the printable mesoscopic perovskite solar cell consists of a transparent conductive substrate, a hole blocking layer, a mesoporous electron transport layer, a mesoporous spacer layer, a porous electrode, and perovskite filled in the mesoporous layer; the porous electrode is formed by applying the conductive paste to form a wet film, and heating to 400°C to remove the solvent, pore-forming agent, and low-temperature adhesive.
[0040] Example 1
[0041] The conductive paste used to prepare the high-temperature porous electrode in this embodiment includes the following components in parts by weight:
[0042] Graphite powder: 13 parts;
[0043] Carbon black: 4 parts;
[0044] Low melting point glass powder: 1.7 parts;
[0045] Ethyl cellulose: 2.5 parts;
[0046] Terpineol: 23 parts.
[0047] Preferably, the low-melting-point glass powder is mainly composed of Al, Si, B, K, and O elements, and has an initial melting point of 330°C.
[0048] The method for preparing a conductive slurry for preparing a high-temperature porous electrode in this embodiment includes the following steps: weighing the graphite powder and carbon black as conductive medium particles, low-melting point glass powder as a high-temperature binder, ethyl cellulose as a low-temperature binder and pore-forming agent, and pinene alcohol as a dispersant according to a ratio, and adding an appropriate amount of ethanol as a low-boiling point solvent; mechanically mixing by ball milling, the ball milling speed is 300r / min, and the ball milling time is 48h; then rotary evaporation is used to remove the ethanol to obtain a conductive slurry for preparing a high-temperature porous electrode.
[0049] The porous electrode of the printable mesoscopic perovskite solar cell of this embodiment is prepared by the conductive paste. Figure 1 The printable mesoscopic perovskite solar cell based on the porous electrode is composed of a transparent conductive substrate, a hole blocking layer, a mesoporous electron transport layer, a mesoporous spacer layer, a porous electrode, and a perovskite filled in the mesoporous layer. In addition, the low-melting point glass is used as a high-temperature binder, and most of it is concentrated at the bottom of the porous electrode after solidification.
[0050] The method for preparing a printable mesoscopic perovskite solar cell based on a porous electrode described in this embodiment specifically comprises the following steps:
[0051] (1) Spraying a thin dense layer of TiO2 on a fluorine-doped tin oxide transparent conductive glass substrate as a hole blocking layer;
[0052] (3) screen printing TiO2 slurry on the TiO2 dense layer and annealing at 500° C. to form a TiO2 mesoporous layer as an electron blocking layer;
[0053] (4) screen printing ZrO2 slurry on the TiO2 mesoporous layer and drying it at 75° C. to form a ZrO2 spacer layer;
[0054] (5) Screen printing the conductive paste on the ZrO2 spacer layer to form a wet film, heating it to 400°C and keeping it for 40 minutes, then cooling it naturally to remove the low boiling point solvent, dispersant, pore former, and low temperature adhesive to obtain a porous electrode.
[0055] (6) A methylamine formamidinium lead iodide perovskite precursor solution is dripped onto the surface of the porous electrode and annealed to crystallize, thereby finally obtaining a printable mesoscopic perovskite solar cell.
[0056] Preferably, the average thickness of the porous electrode is 10.5 microns.
[0057] Example 2
[0058] The conductive paste used to prepare the high-temperature porous electrode in this embodiment includes the following components in parts by weight:
[0059] Graphite powder: 13 parts;
[0060] Carbon black: 4 parts;
[0061] Low melting point glass powder: 1.7 parts;
[0062] Ethyl cellulose: 2.5 parts;
[0063] Terpineol: 23 parts.
[0064] Preferably, the low-melting-point glass powder is mainly composed of Al, Si, B, K, and O elements, and has an initial melting point of 330°C.
[0065] The method for preparing the conductive paste for preparing the high-temperature porous electrode in this embodiment includes the same steps as those in Embodiment 1.
[0066] The porous electrode of the printable mesoscopic perovskite solar cell of this embodiment is prepared by the conductive paste. Figure 1 The structure of the printable mesoscopic perovskite solar cell based on the porous electrode is exactly the same as that in Example 1.
[0067] The method for preparing a printable mesoscopic perovskite solar cell based on a porous electrode described in this embodiment specifically comprises the following steps:
[0068] (1) Spraying a thin dense layer of TiO2 on a fluorine-doped tin oxide transparent conductive glass substrate as a hole blocking layer;
[0069] (3) screen printing TiO2 slurry on the TiO2 dense layer and annealing at 500° C. to form a TiO2 mesoporous layer as an electron blocking layer;
[0070] (4) screen printing ZrO2 slurry on the TiO2 mesoporous layer and drying it at 75° C. to form a ZrO2 spacer layer;
[0071] (5) Screen printing the conductive paste on the ZrO2 spacer layer to form a wet film, heating it to 450°C and keeping it for 40 minutes, then cooling it naturally to remove the low boiling point solvent, dispersant, pore former, and low temperature adhesive to obtain a porous electrode.
[0072] (6) A methylamine formamidinium lead iodide perovskite precursor solution is dripped onto the surface of the porous electrode and annealed to crystallize, thereby finally obtaining a printable mesoscopic perovskite solar cell.
[0073] Preferably, the average thickness of the porous electrode is 9.6 microns.
[0074] Comparative Example 1
[0075] The conductive paste for preparing the high-temperature porous electrode, and the printable mesoscopic perovskite solar cell structure and preparation method based on the porous electrode in this comparative example are exactly the same as those in Example 1, with the only difference being that the conductive paste for preparing the high-temperature porous electrode does not contain a high-temperature binder.
[0076] Comparative Example 2
[0077] The conductive paste for preparing the high-temperature porous electrode, and the printable mesoscopic perovskite solar cell structure and preparation method based on the porous electrode in this comparative example are exactly the same as those in Example 1, with the only difference being that in the conductive paste for preparing the high-temperature porous electrode, 2.5 parts by weight of zirconium oxide powder is used instead of 1.7 parts by weight of low-melting-point glass powder.
[0078] Test Example
[0079] In order to verify the technical effect of the conductive paste for preparing high-temperature porous electrodes described in the present invention, the resistivity of high-temperature porous electrodes prepared with different conductive pastes was jointly tested by four-probe and step meter, and the open circuit voltage Voc, current density Jsc, fill factor FF, and power conversion efficiency PCE of printable perovskite solar cells based on different porous electrodes were tested by a solar simulator.
[0080] After experimentation, the results are as follows:
[0081]
[0082] From the table and Figure 2 The results show that in Example 1, the high-temperature porous electrode prepared by annealing at 400°C using a conductive paste with a low-melting-point glass powder as a high-temperature binder can improve the device performance of the printable mesoscopic perovskite solar cell. Compared with the use of high-temperature infusible ZrO2 as a binder in Comparative Example 2, after replacing the ZrO2 in the back electrode of the mesoscopic perovskite solar cell with a low-melting-point glass powder, the maximum power conversion efficiency of the battery device can be increased from 16.75% to 17.32%, with the open circuit voltage increased from 916mV to 948mV, and the current density increased from 22.84mAcm -2 Increased to 24.1mAcm -2. In addition, the porous electrode in Example 2 was annealed at 450°C, which changed the properties of the amorphous carbon black in the conductive medium particles, increased the resistivity of the porous electrode from 0.035Ω·cm to 0.041Ω·cm, and deteriorated the conductivity. The power conversion efficiency of the printable mesoscopic perovskite solar cell device based on the porous electrode was 16.41%, which was lower than the efficiency of 17.32% in Example 1. . At the same time, it can be seen from the results of Comparative Example 1 that when no high-temperature binder is added to the conductive paste, that is, ZrO2 and glass powder are not contained, the porous electrode prepared based on the conductive paste is not tightly connected to the mesoporous ZrO2 functional layer in the device, resulting in obstruction of carrier transport and a significant decrease in device performance. The power conversion efficiency of the device is reduced to 12.76%, and the current density is only 18.4mAcm -2 , the filling factor is 0.74.
[0083] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. Application of conductive paste for preparing porous back electrode, characterized in that: The conductive paste includes conductive medium particles, a high temperature adhesive, a low temperature adhesive and a solvent; the high temperature adhesive is a low melting point glass powder; the conductive medium particles are one or more of graphite, carbon black, carbon nanotubes, graphene, fluorine-doped tin oxide, tin-doped indium oxide, aluminum-doped zinc oxide and antimony-doped tin oxide; the high temperature adhesive will not decompose and volatilize at 1000°C, thereby playing a role in bonding the conductive medium particles; the low temperature adhesive will decompose and volatilize at 300°C; the boiling point of the solvent is greater than 100°C; The low temperature adhesive has a pore-forming effect, and the low temperature adhesive also acts as a pore-forming agent; The conductive paste is screen-printed on the zirconium dioxide spacer layer to form a wet film, and the film is heated and kept warm before being cooled naturally to remove the solvent and the low-temperature adhesive to obtain a porous electrode.
2. Application of the conductive paste for preparing a porous back electrode, characterized in that: The conductive paste includes conductive medium particles, a high temperature adhesive, a low temperature adhesive, a pore former and a solvent; the high temperature adhesive is a low melting point glass powder; the conductive medium particles are one or more of graphite, carbon black, carbon nanotubes, graphene, fluorine-doped tin oxide, tin-doped indium oxide, aluminum-doped zinc oxide and antimony-doped tin oxide; the high temperature adhesive will not decompose and volatilize at 1000°C, thereby playing the role of bonding the conductive medium particles; the low temperature adhesive will decompose and volatilize at 300°C; the boiling point of the solvent is greater than 100°C; The low-temperature adhesive does not have a pore-forming effect; The conductive paste is screen-printed on the zirconium dioxide spacer layer to form a wet film, and the film is heated and kept warm before being cooled naturally to remove the solvent, pore-forming agent and low-temperature adhesive to obtain a porous electrode.
3. The use according to claim 1 or 2, characterized in that: The back electrode is a porous back electrode of a mesoscopic perovskite solar cell.
4. The use according to claim 1 or 2, characterized in that: The initial melting temperature of the high temperature adhesive is less than 400 o C.
5. The use according to claim 2, characterized in that The pore-forming agent is one or more of cellulose, polystyrene and polyvinyl pyrrolidone.
6. The use according to claim 1 or 2, characterized in that: The conductive paste further includes an auxiliary agent.
7. The use according to claim 6, characterized in that The auxiliary agent is at least one of a dispersant, a leveling agent and a defoaming agent.
8. The use according to claim 2, characterized in that The mass ratio of the mass of the conductive medium particles, the mass of the high-temperature binder, and the sum of the mass of the low-temperature binder and the pore-forming agent is (10-20): (1-2): (2-3).
9. The use according to claim 1, characterized in that The conductive medium particles, high temperature binder, low temperature adhesive and solvent are mixed, the boiling point of the solvent is greater than 100° C., and then a low boiling point solvent is added, the low boiling point solvent is one or more of ethanol and isopropanol, and after fully mixing, the low boiling point solvent is removed by heating or vacuuming to obtain the conductive paste.
10. The use according to claim 2, characterized in that The preparation method of the conductive paste is: mixing the conductive medium particles, high-temperature binder, low-temperature adhesive, pore-forming agent and solvent, wherein the boiling point of the solvent is greater than 100° C., adding a low-boiling point solvent, wherein the low-boiling point solvent is one or more of ethanol and isopropanol, and after fully mixing, heating or vacuuming to remove the low-boiling point solvent to obtain the conductive paste.
11. A porous back electrode, characterized in that: The method is obtained by applying any one of claims 1 to 10. arrive.
12. A mesoscopic perovskite solar cell, characterized in that: Comprising the porous back electrode as claimed in claim 11.
Citation Information
Cited By
Porous electrode based on organic polymer binder and preparation method and application thereof
CN120417726A