Conductive paste composition, preparation method of solar cell and solar cell
By using conductive paste composition and laser enhanced contact technology in solar cells, the etching problem of silver aluminum paste on the passivation layer is solved, low carrier recombination and high efficiency metallization process is achieved, and solar cells are improved open circuit voltage and conversion efficiency.
Patent Information
- Application Number
- CN202411013592.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-27
- Publication Date
- 2024-11-12
AI Technical Summary
Prior Art In the metallization process of solar cells, the etching or damage of the passivation layer by silver aluminum paste causes carrier recombination to increase, affecting the open circuit voltage and efficiency.
By defining the cation of Pb+Bi in the glass frit with respect to B, using a conductive paste composition, including 0.5% to 4% of the frit, 80% to 92% of the conductive component, and 7% to 16% of the organic medium, the cation of Pb+Bi in the glass frit is defined. In combination with laser enhanced contact optimization technology, the passivation layer is etched and a conductive structure with low carrier composite is formed.
It significantly improves the open circuit voltage and photoelectric conversion efficiency of solar cells, reduces carrier recombination losses, and improves the contact effect and uniformity of the conductive structure.
Smart Images

Figure CN118942765A_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application number 202311265866.0, application date September 27, 2023, and name “Conductive paste composition, method for preparing solar cells and solar cells”. Technical Field
[0002] The present application belongs to the technical field of photovoltaic devices, and specifically relates to a conductive paste composition, a method for preparing a solar cell, and a solar cell. Background Art
[0003] Metallization is one of the important steps in the production process of photovoltaic solar cells, which achieves high photoelectric conversion efficiency by extracting photogenerated carriers. For N-type solar cells, silver-aluminum paste is usually used to achieve the metallization effect of forming an ohmic contact with the p-side under high-temperature sintering. Although the silver-aluminum paste can form an ohmic contact with the p-side with low resistivity, the higher carrier recombination will lead to a loss of open circuit voltage and efficiency. In addition, when the glass material in the silver-aluminum paste etches or damages the passivation film on the p-side during high-temperature sintering, the recombination loss will be further increased. Summary of the invention
[0004] Purpose of the invention: The embodiments of the present application provide a conductive paste composition, a method for preparing a solar cell, and a solar cell, so that the conductive paste composition can etch the surface passivation layer of the battery after sintering while achieving a low recombination effect, and is combined with laser enhanced contact optimization technology to achieve a significant increase in open circuit voltage and conversion efficiency.
[0005] Technical solution: A conductive paste composition described in an embodiment of the present application, according to the mass percentage of the composition, the conductive paste composition includes 0.5wt%-4wt% of glass frit, 80wt%-92wt% of conductive component, and 7wt%-16wt% of organic medium;
[0006] The glass frit includes an oxide, and according to the molar percentage of the oxide, the glass frit includes 20mol%-50mol% of B2O3; the glass frit also includes: 15mol%-50mol% of PbO; or, 15mol%-50mol% of Bi2O3; or, 15mol%-50mol% of a mixture of PbO and Bi2O3;
[0007] Wherein, the ratio of the sum of the cation contents of the PbO and the Bi2O3 to the cation content of the B2O3 is 0.30-1.25.
[0008] In some embodiments, the glass material further includes a first additive, measured by molar percentage of the oxide, wherein the content of the first additive is less than or equal to 18 mol %, and the first additive is selected from any one or more of Li2O, Al2O3, ZnO, SiO2, SeO2 and TeO2.
[0009] In some embodiments, the first additive satisfies at least one of the following conditions, based on the molar percentage of the oxide:
[0010] a) the first additive comprises Li2O, and the content of Li2O is less than or equal to 15 mol%;
[0011] b) the first additive comprises Al2O3, and the content of Al2O3 is less than or equal to 10 mol%;
[0012] c) the first additive comprises ZnO, and the content of ZnO is less than or equal to 18 mol%;
[0013] d) the first additive comprises SiO2, and the content of SiO2 is less than or equal to 15 mol%;
[0014] e) the first additive comprises SeO2, and the content of SeO2 is less than or equal to 15 mol%;
[0015] f) The first additive comprises TeO2, and the content of TeO2 is less than or equal to 15 mol%.
[0016] In some embodiments, the glass frit further comprises, in terms of molar percentage of the oxides: 0 to 15 mol % of Li2O; 0 to 10 mol % of Al2O3; 0 to 18 mol % of ZnO; and 0 to 15 mol % of SiO2.
[0017] In some embodiments, the glass material further includes a second additive, measured by molar percentage of the oxide, wherein the content of the second additive is less than or equal to 5 mol %, and the second additive is selected from any one or more of AgO2, Ag2O, AgO, Na2O, K2O, MgO, CaO and BaO.
[0018] In some embodiments, the conductive paste composition further comprises less than or equal to 1 wt % of a filler, measured by mass percentage of the composition; the filler comprises at least one of aluminum powder, silicon powder, and aluminum-silicon alloy powder.
[0019] In some embodiments, the mass percentage of the filler in the conductive paste composition is greater than 0 and less than or equal to 1 wt %.
[0020] In some embodiments, the filler has a D v 50 is 1-4μm; among them, D v 50 is the particle size corresponding to when the cumulative volume percentage of the filler reaches 50%.
[0021] In some embodiments, the conductive component is selected from any one or a mixture of silver, silver alloy, silver oxide and silver salt.
[0022] In some embodiments, a first conductive structure is formed in a solar cell, the solar cell comprising a substrate and a passivation layer located on at least one side of the substrate; when sintering the solar cell, the conductive paste composition can penetrate the passivation layer to form the first conductive structure.
[0023] In some embodiments, the substrate comprises an n-type doped semiconductor substrate.
[0024] In some embodiments, the present application also provides a method for preparing a solar cell, comprising the following steps:
[0025] Providing a substrate, the substrate comprising a substrate, a p-type doping layer, and a passivation layer, wherein the p-type doping layer is located between the substrate and the passivation layer;
[0026] Covering the conductive paste composition on the passivation layer;
[0027] Sintering the substrate coated with the conductive paste composition, so that the conductive paste composition etches the passivation layer during the sintering process to form a first conductive structure;
[0028] The substrate is subjected to laser enhanced contact optimization to obtain the solar cell.
[0029] In some embodiments, coating the conductive paste composition on the passivation layer comprises:
[0030] The conductive paste composition is applied to at least a portion of the surface of the passivation layer in a patterned form.
[0031] In some embodiments, the step of performing laser enhanced contact optimization on the substrate further comprises:
[0032] A reverse voltage is applied to the substrate, and a laser is simultaneously scanned on the substrate to form an induced current in the first conductive structure.
[0033] In some embodiments, the preparation method satisfies at least one of the following conditions:
[0034] g) the solar cell has a breakdown voltage, and the reverse voltage is less than the breakdown voltage;
[0035] h) The laser scanning time is 1ms to 100ms;
[0036] i) The induced current is 100A to 1000A.
[0037] In some embodiments, the present application further provides a solar cell, the solar cell comprising a first conductive structure made of the conductive paste composition; or,
[0038] The solar cell is manufactured by adopting the manufacturing method.
[0039] In some embodiments, the solar cell is a solar cell having a tunnel oxide passivated contact structure.
[0040] Beneficial effect: Compared with the prior art, the conductive paste composition of the present application can be applied to the metallization of the p-side of a solar cell. After sintering, it can etch the passivation layer on the surface of the cell and simultaneously achieve the effect of low carrier recombination. By limiting the cation ratio of Pb+Bi relative to B in the glass material, the corrosion effect of the glass material on the passivation layer is further improved, and the excessive recombination loss caused by the conductive paste composition etching the passivation layer can be reduced.
[0041] The method for preparing solar cells provided in the present application achieves moderate corrosion of the passivation layer after sintering the conductive paste composition used, reduces the high recombination of carriers formed under excessive corrosion, and further combines laser enhanced contact optimization technology to guide a large number of carriers generated by laser scanning into the first conductive structure through the applied reverse voltage to form an induced current, and uses the energy generated by the current to improve the contact effect and uniformity of the first conductive structure, thereby achieving a significant increase in the open circuit voltage and conversion efficiency of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0043] Figure 1 A cross-sectional view of a solar cell provided in an embodiment of the present application;
[0044] Reference numerals: 10 - substrate, 20 - first conductive structure, 30 - second conductive structure, 101 - substrate, 102 - p-type doping layer, 103 - passivation layer, 104 - first passivation film, 105 - n +Polysilicon layer, 106 - second passivation film. DETAILED DESCRIPTION
[0045] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0046] In the description of the present application, it should be understood that the terms "upper", "lower", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In the description of the present application, "plurality" means two or more than two, and at least one means one, two or more than two, unless otherwise clearly and specifically defined.
[0047] The applicant has found that metallization is one of the important steps in the production process of photovoltaic solar cells, which can effectively extract photogenerated carriers to achieve high photoelectric conversion efficiency. Among them, screen printing is currently the most preferred method for metallization. For N-type solar cells, such as n-TOPCon and other cells containing tunneling oxide layer passivation contact structure, a metallization paste (silver-aluminum paste or Ag-Al paste) containing silver powder and aluminum powder is usually used under high temperature sintering to achieve the metallization effect on the p-side (or p-type doped layer) of the solar cell. The glass material in the silver-aluminum paste is etched during the sintering process and opens the SiN x 、SiNO x and AlO x The passivation film allows the metal in the paste to react with the p-type doped layer to form a silver-aluminum barb microstructure to achieve good ohmic contact. Although the silver-aluminum paste can form a low-resistivity ohmic contact with the p-type doped layer, the high carrier recombination loss leads to the loss of open-circuit voltage and efficiency of the battery, which is an important factor affecting the photoelectric conversion efficiency of N-type solar cells. In addition, because the surface passivation of the substrate has a significant effect on carrier recombination, the etching or damage of the passivation film by the glass material in the silver-aluminum paste during high-temperature sintering will further increase the recombination loss.
[0048] Based on this, it is necessary to provide a conductive paste composition, a method for preparing a solar cell and a solar cell, especially a conductive paste suitable for the p-side, so as to achieve the effect of low carrier recombination and enable the metallization method to achieve higher open circuit voltage and photoelectric conversion efficiency.
[0049] Some embodiments of the present application provide a conductive paste composition for forming an electrical connection with a p-type doped layer of a solar cell with low carrier recombination and low resistance.
[0050] Some embodiments of the present application provide a conductive paste composition, which includes, by mass percentage, 0.5wt%-4wt% of glass material, 80wt%-92wt% of conductive components, and 7wt%-16wt% of organic medium; the glass material includes oxides, and by molar percentage of oxides, the glass material includes 20mol%-50mol% of B2O3; the glass material also includes: 15mol%-50mol% of PbO; or, 15mol%-50mol% of Bi2O3; or, 15mol%-50mol% of a mixture of PbO and Bi2O3; wherein the ratio of the sum of the cation contents of PbO and Bi2O3 to the cation content of B2O3 is 0.30-1.25.
[0051] Among them, glass frit and conductive component are used as solid components in the conductive paste composition, and organic medium is used as dispersed phase in the conductive paste composition and provides printing performance. The sum of weight percentages of each component in the conductive paste composition is 100%. Cationic content refers to the number or proportion of cations in a chemical substance. In a chemical formula, cations are usually ions with positive charges.
[0052] Each component is described below.
[0053] Glass Frit
[0054] In some embodiments, glass frit refers to a composition containing one or more types of anions and cations. Glass frit has the ability to flow when heated, and the glass frit can be crystalline or partially or completely glassy or amorphous.
[0055] In some embodiments, the glass frit of the present embodiment can be understood as a composition having a glass component, and the mass percentage of the glass frit in the conductive paste composition is 0.5wt% to 4wt%; in some other embodiments, the mass percentage of the glass frit in the conductive paste composition is 1.0wt% to 3.8wt%, and can also be 1.5wt% to 3.5wt%; can further be 2.0wt% to 3.0wt%; can further be 2.2wt% to 2.8wt%. It can be understood that the adjustment of the proportion of the glass frit in the conductive paste composition needs to ensure that the sum of the weight percentages of the components in the conductive paste composition is 100%. The components of the glass frit directly affect its solubility, fluidity and etching properties, so the components of the glass frit need to be well balanced to achieve excellent carrier recombination effects.
[0056] In some embodiments, the glass frit contains at least the following components: in terms of molar percentages converted to oxides, including: 15 mol% or more and 50 mol% or less of PbO and / or Bi2O3, 20 mol% or more and 50 mol% or less of B2O3. In the following description, unless otherwise specified, the "mol%" of the content of each component of the glass frit represents the molar percentage converted to oxides. In addition, 15 mol% or more and 50 mol% or less can represent a corresponding range of greater than or equal to 15 mol% and less than or equal to 50 mol%, and the same applies to the others.
[0057] In some embodiments, further preferably, the glass material includes, in terms of molar percentage converted into oxides: 20 mol % or more and 40 mol % or less of PbO and / or Bi2O3, and 30 mol % or more and 40 mol % or less of B2O3.
[0058] In some embodiments, PbO, Bi2O3 or a combination of the two can form a low melting point glass phase and provide good fluidity, and both can corrode the passivation layer during the sintering process. This is because PbO and Bi2O3 are reactive with the passivation layer and have the function of improving the softening fluidity of the glass.
[0059] In some embodiments, B2O3, as a glass former, can form low-melting-point glass and provide good fluidity. B2O3 can form a network structure, which helps stabilize the glass and improves the ability of the glass to bond with the substrate after melting.
[0060] In some embodiments, in the glass frit, the ratio of the total cation content of PbO and Bi2O3 to the cation content of B2O3 is 0.30 to 1.25. For example, the value of the ratio can be any one of 0.30, 0.32, 0.34, 0.36, 0.38, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, 1.00, 1.05, 1.10, 1.15, 1.20, 1.21, 1.22, 1.23, 1.24, 1.25, or a range between any two values. By limiting the cation ratio of Pb+Bi relative to B, the corrosion effect of the glass material can be improved. This is because PbO is more corrosive than Bi2O3. Therefore, replacing part of PbO with Bi2O3 in the composition of the glass material can adjust the corrosion ability. Therefore, when the above cation ratio range is met, the corrosion properties and reaction ability of the glass material are controlled by adjusting the cation ratio of Pb+Bi relative to B to meet the effect of low carrier recombination, and the open circuit voltage and photoelectric conversion efficiency can be improved.
[0061] In some embodiments, the glass frit further comprises less than 18 mol% of a first additive, the first additive being selected from any one or more of Li2O, Al2O3, ZnO, SiO2, SeO2 and TeO2, in terms of molar percentage of oxide conversion. Further preferably, the glass frit further comprises more than 3 mol% and less than 15 mol% of the first additive, in terms of molar percentage of oxide conversion; and further preferably, the glass frit further comprises more than 6 mol% and less than 10 mol% of the first additive, in terms of molar percentage of oxide conversion.
[0062] In some embodiments, the first additive is used to modify the system of glass frit, and may further include a glass former or a glass modifier; during the preparation of glass frit, the glass former is used to form the initial network structure of the glass, and when the glass modifier is added to the glass network structure, the initial network structure formed by the glass former is changed, thereby changing the original thermal properties of the glass. The content of each component in the first additive can be adjusted accordingly depending on the desired glass properties.
[0063] In some embodiments, TeO2 or SeO2 is used as a glass former to increase the fluidity of the glass during molding. In terms of molar percentage of oxide conversion, the content of SeO2 in the glass material is less than 15 mol%; in terms of molar percentage of oxide conversion, the content of TeO2 in the glass material is less than 15 mol%. Further preferably, in terms of molar percentage of oxide conversion, the content of SeO2 in the glass material is greater than 5 mol% and less than 10 mol%. Further preferably, in terms of molar percentage of oxide conversion, the content of TeO2 or SeO2 in the glass material is greater than 5 mol% and less than 7.5 mol%.
[0064] In some embodiments, Li2O is used as a glass modifier. The addition of an appropriate amount can increase the fluidity of the glass. Li2O itself has a corrosive effect, and its addition amount needs to be controlled within a certain range. In terms of molar percentage converted as oxide, the content of Li2O in the glass material is less than 15 mol%. Further preferably, in terms of molar percentage converted as oxide, the content of Li2O in the glass material is greater than 5 mol% and less than 10 mol%. Within the above range, the fluidity and reactivity of the glass can be improved, and the electrical properties of the solar cell can be further improved.
[0065] In some embodiments, Al2O3, as a glass former, can stabilize the glass phase, increase the glass melting point and reduce fluidity, and can also be used as a component to improve the weather resistance of the glass. In terms of molar percentage converted as oxide, the content of Al2O3 in the glass material is 10 mol% or less. Further preferably, in terms of molar percentage converted as oxide, the content of Al2O3 in the glass material is 3 mol% or more and 7 mol% or less. Within the above range, the increase in the glass transition temperature can be suppressed, and excellent fluidity is exhibited during softening.
[0066] In some embodiments, ZnO is used as a glass modifier, and proper addition can improve electrical properties. In terms of molar percentage of oxide conversion, the content of ZnO in the glass material is 18 mol% or less. Further preferably, in terms of molar percentage of oxide conversion, the content of ZnO in the glass material is 6 mol% or more and 12 mol% or less. Within the above range, on the one hand, the melting temperature of the glass material can be reduced, the melting and melting properties of the glass material can be promoted, and it is helpful to prepare glass.
[0067] In some embodiments, SiO2 is used as a glass former, and proper addition can stabilize the glass phase, increase the melting point of the glass, and reduce fluidity. SiO2 can also improve the weather resistance of the glass and adjust the reactivity with the substrate. In terms of molar percentage converted as oxide, the content of SiO2 in the glass material is less than 15 mol%. Further preferably, in terms of molar percentage converted as oxide, the content of SiO2 in the glass material is greater than 3 mol% and less than 10 mol%. Within the above range, the glass transition temperature and the fluidity of the glass during sintering can be adjusted, and the etching property of the glass during sintering can be controlled.
[0068] In some embodiments, the glass material includes, in terms of molar percentage converted into oxides: 15 mol% to 50 mol% of PbO and / or Bi2O3; 20 mol% to 50 mol% of B2O3; 0 to 15 mol% of Li2O; 0 to 10 mol% of Al2O3; 0 to 18 mol% of ZnO; and 0 to 15 mol% of SiO2.
[0069] In some embodiments, the glass material includes, in terms of molar percentage converted into oxides: 15 mol% to 50 mol% of PbO and / or Bi2O3; 20 mol% to 50 mol% of B2O3; 0 to 15 mol% of Li2O; 0 to 10 mol% of Al2O3; 0 to 18 mol% of ZnO; 0 to 15 mol% of SiO2; and 0 to 15 mol% of SeO2 or TeO2.
[0070] In some embodiments, the glass frit further comprises less than 5 mol% of a second additive in terms of molar percentage of oxide, and the second additive is selected from any one or more of AgO2, Ag2O, AgO, Na2O, K2O, MgO, CaO and BaO. It is understood that the second additive, as a glass modifier, can further change and adjust the melting point and fluidity of the glass frit in combination with the first additive during the preparation of the glass frit.
[0071] Conductive components
[0072] In some embodiments, the conductive component serves as a conductive source of the conductive paste composition. The conductive component in this embodiment can use metal powders commonly used in electrodes formed on circuit substrates such as semiconductor substrates without particular limitation. Exemplary metals include, but are not limited to, silver, gold, copper, nickel, palladium, platinum, aluminum, and alloys and mixtures thereof. Alternatively, the conductive component is substantially composed of silver, depending on its excellent processability and high conductivity.
[0073] In some embodiments, the mass percentage of the conductive component in the conductive paste composition is 80wt% to 92wt%; in some other embodiments, the mass percentage of the conductive component in the conductive paste composition is 82wt% to 90wt%, and can also be 85wt% to 88wt%; and can further be 86wt% to 87wt%. It is understood that the adjustment of the proportion of the conductive component in the conductive paste composition needs to ensure that the sum of the weight percentages of the components in the conductive paste composition is 100%. The conductive component is used to play a conductive role after forming a solar cell.
[0074] In some embodiments, the conductive component may be directly combined in the conductive paste composition of the present invention by selecting metal powder; or a mixture of two or more such metals or alloys; the metal is provided by a metal oxide or salt, which decomposes to form a metal when exposed to the heat of firing. When the metal powder is silver powder, it should be understood to refer to elemental silver metal, silver alloys, silver oxides or silver salts and mixtures thereof, and may further include silver oxide (Ag2O or AgO) or silver salts such as AgCl, AgNO3, AgOOCCH3 (silver acetate), AgOOCF3 (silver trifluoroacetate), Ag3PO4 (silver orthophosphate), or mixtures thereof.
[0075] In some embodiments, the conductive component may be provided as finely dispersed particles having a morphology such as powder form, flake form, spherical form, rod form, granular form, nodular form, layered or coated form, other irregular forms, or mixtures thereof.
[0076] In some embodiments, the median particle size of the conductive component is in the range of 0.5-3.5 μm. A further preferred conductive component uses spherical silver powder with a median particle size of 1-3 μm; a further preferred conductive component uses spherical silver powder with a median particle size of 1.5-2.5 μm; a further preferred spherical silver powder with a median particle size of 2 μm. The main function of the silver powder is to form a high-density silver body after sintering to improve good conductivity. The spherical silver powder with a median particle size of 2 μm can also inhibit agglomeration and ensure uniform dispersion of the silver powder.
[0077] Organic medium
[0078] In some embodiments, the organic medium is used as a liquid phase in the conductive paste composition to disperse the solids composed of the conductive components and glass frits to form a paste with a certain viscosity. The viscosity and rheology of the paste can not only allow the conductive components and glass frits to be dispersed therein with long-term stability, but also allow the conductive paste composition to be dispersed on the printing screen, and the desired pattern can be applied to the passivation layer of the substrate by screen printing.
[0079] In some embodiments, the organic medium may include a polymer and an organic solvent. The polymer may include cellulose, resin, esters, etc. Cellulose includes cellulose resins such as methyl cellulose, ethyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, benzyl cellulose, propyl cellulose, nitrocellulose, or mixtures thereof. Resins include wood rosin, phenolic resins, acrylic resins, or mixtures thereof. Esters include polymethacrylates of lower alcohols, etc. The organic solvent may include terpineol, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, propylene glycol diacetate, α-terpene, β-terpene, dibutyl phthalate, butyl carbitol, butyl carbitol acetate, hexylene glycol, etc.
[0080] In some embodiments, the organic medium has a consistency and rheology that makes it suitable for printing methods, including but not limited to screen printing. The organic medium may also include other additives such as non-ionic surfactants, thixotropic agents, dispersants, rheological agents, etc. to adapt the organic medium to different needs.
[0081] filler
[0082] In some embodiments, the mass percentage of the filler in the conductive paste composition is greater than 0 and less than or equal to 1 wt %; wherein the filler is selected from at least one of aluminum powder, silicon powder and aluminum-silicon alloy powder.
[0083] In some embodiments, unlike the aluminum powder added to the commercially available silver aluminum paste for TOPCon cells to improve the contact, the aluminum powder added as a filler in this embodiment can further control the etching property of the glass powder to achieve a higher open circuit voltage. It is understandable that the reason why the above-mentioned effect of improving the open circuit voltage can be achieved is affected by the amount of aluminum powder added. This is because a small amount of aluminum powder is added to the slurry, and the melted glass powder can further incorporate a small amount of aluminum oxide during the high-temperature sintering process. The increase of aluminum oxide in the melted glass material will reduce its fluidity and corrosiveness, thereby forming smaller damage to the passivation film, and the effect is that lower recombination brings an increase in open circuit voltage, but too much aluminum powder added during sintering will cause the melted glass material to incorporate too much aluminum powder and greatly reduce the corrosiveness, resulting in a negative impact on the fill factor.
[0084] More preferably, the mass percentage of the filler in the conductive paste composition is greater than 0 and less than or equal to 0.75 wt %.
[0085] More preferably, the mass percentage of the filler in the conductive paste composition is any one of 0.25 wt %, 0.50 wt %, 0.75 wt %, 1.0 wt % or a range between any two of them.
[0086] In some embodiments, the filler D v 50 is 1-4μm; among them, D v50 is the particle size corresponding to when the cumulative volume percentage of the filler reaches 50%. v 50 is 1-3 μm. Further preferably, the filler D v 50 is 2μm.
[0087] In some embodiments, the preparation method of glass powder can be produced by the method conventionally used in the field of glass manufacturing. For example, the oxides corresponding to the composition ratio of the glass powder described in the embodiment are batched, mixed, added to a crucible (e.g., platinum or ceramic crucible), heated to a peak temperature (e.g., 800°C to 1400°C) and kept for a period of time to melt the oxides inside together. The molten material can then be quenched in any suitable manner, including but not limited to passing it between counter-rotating stainless steel rollers to form a sheet 0.25 to 0.50 mm thick, by pouring it on a thick stainless steel plate, or by pouring it into water. The resulting glass material is then subjected to conventional grinding techniques to form a powder with a particle size of 0.5-2 μm.
[0088] In some embodiments, the preparation method of the conductive paste composition may include: preparing the paste components described in the embodiments, stirring and dispersing, and then grinding with a three-roll mill to a fineness of less than 10 μm, and then further filtering. The amount of glass frit and aluminum powder added in some embodiments may be different. In these cases, silver powder is replaced in equal amounts, and the amount of other components such as organic medium remains unchanged. The adjustment of the ratio of glass frit, conductive component, organic medium and filler needs to ensure that the sum of the mass percentages of each component in the conductive paste composition is 100%.
[0089] In some embodiments, the conductive paste composition of this embodiment is used to form a first conductive structure 20 in a solar cell, wherein the solar cell includes a substrate 101, the substrate 101 has a main surface and at least one passivation layer 103 disposed on the main surface, wherein the conductive paste composition can penetrate at least one passivation layer 103 during sintering to form the first conductive structure 20.
[0090] It is understood that the first conductive structure 20 can form an electrical connection with the p-type semiconductor in the substrate 101 with low carrier recombination. The p-type semiconductor can preferably be a p-type doped layer, and the substrate 101 can be an n-type doped semiconductor substrate. In addition, in the TOPCon cell, the p-type doped layer is also called a p-type emitter.
[0091] Solar Cells
[0092] like Figure 1As shown, some embodiments of the present application provide a solar cell, which is a solar cell containing a tunnel oxide passivated contact structure (Tunnel Oxide Passivated Contacts), and the above-mentioned conductive paste composition is used in its preparation.
[0093] In some embodiments, a solar cell with a tunnel oxide passivated contact structure is called a TOPCon solar cell (Tunnel Oxide Passivated Contact Solar Cell). This solar cell uses a tunnel oxide layer as a charge transfer channel and a surface passivation layer to improve the efficiency and performance of the cell. The TOPCon solar cell structure has lower electron reflection and surface recombination, as well as higher photoelectric conversion efficiency and lower electron defects.
[0094] In some embodiments, a TOPCon solar cell includes a substrate 10 and a first conductive structure 20, wherein the substrate 10 includes a substrate 101, a p-type doping layer 102 formed on one side of the substrate 101, and a passivation layer 103 formed on a side of the p-type doping layer 102 away from the substrate 101; Figure 1 For example, the substrate 101 is located in the middle of the TOPCon solar cell, and the substrate 101 can be an n-type doped semiconductor substrate; the p-type doped layer 102 is located on the front side of the n-type doped semiconductor substrate, and the passivation layer 103 is located on the surface of the p-type doped layer 102; the conductive structure 20 penetrates at least a portion of the passivation layer 103 and forms an electrical connection with the p-type doped layer 102.
[0095] In some embodiments, see Figure 1 The substrate 10 further includes: a first passivation film 104, which is located on the back side of the n-type doped semiconductor substrate; + The polysilicon layer 105 is located on the surface of the first passivation film 104 away from the n-type doped semiconductor substrate; the second passivation film 106 is deposited on the n-type doped semiconductor substrate. + The polysilicon layer 105 is separated from the surface of the first passivation film 104 .
[0096] In some embodiments, see Figure 1 The TOPCon solar cell further includes a second conductive structure 30, which penetrates at least a portion of the second passivation film 106 and is connected to the n + The polysilicon layer 105 forms an electrical connection.
[0097] In some embodiments, the front side refers to the light-exposed side of the solar cell, which is also the working side of the solar cell. The back side is the back side of the solar cell, which usually does not directly receive light.
[0098] In some embodiments, the first passivation film 104 and the n + Polysilicon layer 105 .
[0099] In some embodiments, the first conductive structure 20 is formed by using the conductive paste composition of this embodiment. The conductive paste composition is applied to at least a portion of the surface of the passivation layer 103 in a desired patterned form, and during the sintering process, the conductive paste composition penetrates the passivation layer 103 to obtain the first conductive structure 20 that is electrically connected to the p-type doped layer 102 to form a low carrier recombination.
[0100] In some embodiments, the second conductive structure 30 can use a metallization silver paste used in P-type or N-type crystalline silicon cells on the market, such as a silver paste containing Pb-Te-O glass powder. The conductive paste composition is applied to at least a portion of the surface of the second passivation film 106 in a desired patterned form. During the sintering process, the silver paste containing Pb-Te-O glass powder etches and penetrates the second passivation film 106, thereby contacting the n-type crystalline silicon cell. + The polysilicon layer 105 forms an electrical contact to facilitate forming a second conductive structure 30 in the form of a conductive metal contact.
[0101] The present application provides a method for preparing a solar cell, comprising:
[0102] 1) providing a substrate 10, the substrate 10 comprising a substrate 101, a p-type doping layer 102 formed on one side of the substrate 101, and a passivation layer 103 formed on a side of the p-type doping layer 102 away from the substrate 101; wherein a trivalent element (such as boron or gallium) is doped on the front side of the substrate 101, thereby forming the p-type doping layer 102 on the front side of the n-type doped semiconductor substrate; and depositing the passivation layer 103 on the surface of the p-type doping layer 102 by a deposition method;
[0103] 2) applying the conductive paste composition provided in this embodiment to the passivation layer 103; specifically, applying the conductive paste composition to at least a portion of the surface of the passivation layer 103 in a patterned form; the patterning method can be screen printing; it can be understood that the conductive paste composition involved in this embodiment is used as a fine grid for the P surface of a solar cell containing a tunneling oxide layer passivation contact structure, and is passed through four screen printers corresponding to the back main grid, the back fine grid, the front main grid, and the front fine grid respectively; the conductive paste composition of this embodiment is used for the fine grid of the P surface, usually the fourth front fine grid;
[0104] 3) sintering the substrate 10 and the conductive paste composition, so that the conductive paste composition etches the passivation layer 103 during the sintering process to form the first conductive structure 20; in addition, the preparation of the second conductive structure 30 is the same as the preparation of the first conductive structure 20;
[0105] 4) Performing laser enhanced contact optimization on the substrate 10 to prepare a solar cell.
[0106] The serial numbers of the above steps are not to be construed as limiting the order of the steps.
[0107] In some embodiments, in step 4), laser enhanced contact improvement optimization is a method of using laser to improve the electrical contact of metallization paste during the manufacturing process of solar cells. The basic principle of laser enhanced contact improvement technology is to use a large number of carriers generated by laser, use bias to guide these carriers through the formed metallization contact points, and use the heat energy generated by current to improve the contact effect and uniformity, which can improve the uniformity of electrical contact and reduce contact defects, thereby improving the efficiency and reliability of solar cells. In this technology, the amount of carrier injection can be controlled by parameters such as laser power and time to achieve better contact uniformity and improvement effect.
[0108] In some embodiments, the step of performing laser enhanced contact optimization on the substrate 10 further includes: applying a reverse voltage to the substrate 10 and simultaneously performing laser scanning on the substrate 10 to form an induced current in the first conductive structure 20. Using laser enhanced contact optimization technology to process the conductive structure can reduce contact resistance, which is more conducive to increasing the open circuit voltage and improving efficiency.
[0109] In some embodiments, the reverse voltage is less than the breakdown voltage of the solar cell, which can avoid breakdown damage, extend the life of the solar cell, improve battery safety and protect battery performance.
[0110] In some embodiments, the laser scanning time is 1 ms to 100 ms, for example, any value among 1 ms, 2 ms, 3 ms, 5 ms, 10 ms, 20 ms, 30 ms, 40 ms, 50 ms, 60 ms, 70 ms, 80 ms, 90 ms, 100 ms, or a range between any two values.
[0111] In some embodiments, the induced current is 100A to 1000A. For example, it can be any value among 100A, 150A, 200A, 250A, 300A, 350A, 400A, 450A, 500A, 550A, 600A, 650A, 700A, 750A, 800A, 850A, 900A, 950A, 1000A or a range between any two values.
[0112] The technical solution of the present application is further described below in conjunction with specific embodiments.
[0113] The contents of the components of the glass frits of Examples 1 to 13 and Comparative Examples 1 to 4 are shown in Table 1. The sum of the components in the glass frits of the Examples and Comparative Examples is 100%. The values in Table 1 are molar percentages (mol%). In the glass frits of Comparative Examples 1-2, the cation ratio of (Pb+Bi) / B is not within the range of 0.30-1.25, and the content of the first additive TeO2 added in Comparative Examples 3-4 is too high.
[0114] Table 1
[0115]
[0116]
[0117] The glass frits of Examples 1 to 13 and Comparative Examples 1 to 4 in Table 1 were prepared into conductive paste compositions and made into solar cells to obtain corresponding Examples 14 to 26 and Comparative Examples 5 to 8. The performance of the cells of Examples 14 to 26 and Comparative Examples 5 to 8 was tested, and the quality test data is shown in Table 2.
[0118] Among them, in the conductive paste compositions of Examples 14 to 26 and Comparative Examples 5 to 8, the mass percentage of glass frit is 1.5wt%; the conductive component adopts spherical silver powder with a median particle size of 2μm, and the mass percentage of the conductive component glass frit is 89.5wt%; the mass percentage of the organic medium is 9wt%, wherein the organic medium specifically includes: 1.5wt% of ethyl cellulose, 1.5wt% of polyvinyl alcohol butyral copolymer (PVB), 1.6wt% of diethylene glycol butyl ether acetate, 0.3wt% of silicone oil, 0.15wt% of Duomeen TDO (non-ionic surfactant, which belongs to the amine oxide category), 0.15wt% of Brij L4 (non-ionic surfactant, which belongs to the polyoxyethylene alcohol category), 0.4wt% of Thixotrol plus (rheological agent), 2.8wt% of ester alcohol dodecahydrate (Ethoxylated Alcohol C12), and 0.6wt% of dibasic acid ester. The specific preparation process of the conductive paste composition is: the above components are mixed, stirred and dispersed, and then grinded with a three-roll mill to a fineness of less than 10um, and then further filtered to obtain.
[0119] The preparation process is as follows: first prepare the blue film of the TOPCon battery, and pass it through four screen printing machines corresponding to the back main grid, back fine grid, front main grid, and front fine grid respectively; apply the conductive paste composition to the front fine grid of the P surface; sinter the substrate and the conductive paste composition, so that the conductive paste composition etches the passivation layer during the sintering process to obtain a conductive structure formed on the p-side of the substrate; perform laser enhanced contact optimization on the conductive structure to prepare a solar cell.
[0120] Among them, the test data in Table 2 are measured by the following method:
[0121] a) Suns-Voc test: Sinton WCT120 tester is used for testing. Suns-Voc is tested after sintering. The tested Voc is used to characterize and compare the carrier recombination performance of different conductive pastes after sintering.
[0122] b) IV test: The photovoltaic conversion efficiency of the cell was tested using a commercially available IV tester. The test items included efficiency (Eff), open circuit voltage (Voc), fill factor (FF) and current (Isc). The experimental data were expressed in the form of difference values, ΔEff, ΔVoc, ΔFF, ΔIsc, to describe the electrical performance of the embodiment and the comparative example.
[0123] Table 2
[0124] Suns-Voc mV ΔEff% ΔVoc mV ΔIsc mA ΔFF% Embodiment 14 723 0.00 0.00 0.00 0.00 Embodiment 15 727 0.06 2.5 -6.1 0.0 Example 16 731 0.12 4.5 15.2 -0.2 Embodiment 17 727 0.10 3.5 13.8 -0.1 Embodiment 18 729 -0.05 1.1 -11.9 -0.2 Embodiment 19 723 -0.07 -2.4 -16.1 0.1 Embodiment 20 722 -0.07 -0.7 -5.9 -0.1 Embodiment 21 728 0.03 2.6 -0.2 -0.20 Embodiment 22 727 0.05 2.1 2.8 -0.08 Embodiment 23 723 -0.06 0.3 -2.1 -0.20 Embodiment 24 724 -0.03 0.8 10.8 -0.24 Embodiment 25 724 -0.01 1.3 16.7 -0.30 Embodiment 26 728 0.05 2.4 9.7 -0.20 Comparative Example 5 719 -0.20 -3.9 -14.7 -0.13 Comparative Example 6 725 -0.18 1.1 -16.7 -0.62 Comparative Example 7 721 -0.33 -2.8 -19.2 -0.68 Comparative Example 8 718 -0.59 -5.5 -15.9 -1.30
[0125] As can be seen from Table 2, the batteries of Examples 14 to 26 achieve an efficiency performance of ±0.1%. Compared with Comparative Examples 5-8, the conductive paste composition of the embodiments of the present application can achieve a significant improvement in open circuit voltage and conversion efficiency after laser enhanced contact improvement, indicating that the conductive paste composition provided by the present application can significantly improve the effect of p-side metallization composite of TOPCon structure batteries. Among them, the effects of Comparative Examples 5 and 6 are worse than those of the embodiments. This is because the cation ratio of (Pb+Bi) / B in the glass powder corresponding to Comparative Example 5 is too high, resulting in too strong corrosion of the glass powder and loss of opening voltage; the cation ratio of (Pb+Bi) / B in Comparative Example 6 is too low, and the corrosion of the glass powder is too weak to form a good ohmic contact, resulting in a significant reduction in FF. In addition, in Comparative Examples 7 and 8, due to the high addition of TeO2 in the glass material, the fluidity of the glass is too strong, which causes excessive damage to the passivation film during sintering, resulting in a loss of opening voltage.
[0126] Examples 27 to 30 and comparative example 9 are provided, wherein the process of preparing solar cells in examples 27 to 30 is exactly the same as that in example 14, except that the conductive paste compositions of examples 27 to 30 also contain fillers, and the fillers are aluminum powders with a median particle size of 2 μm. Among them, since aluminum powder is added to the components, it is necessary to adjust the content of the silver powder of the conductive component to ensure that the overall mass content is 100%. Comparative example 9 is similar to example 27, except that the amount of aluminum powder added exceeds 1wt%. See Table 3 for specific dosage and test data.
[0127] Table 3
[0128]
[0129] It can be seen from Table 3 that the addition of a small amount of aluminum powder can further reduce the composite to improve the open circuit voltage. This is because a small amount of aluminum powder forms a small amount of aluminum oxide during the high-temperature sintering process, which can be melted into the glass material in a small amount. The increase of aluminum oxide in the melted glass material will reduce its fluidity and corrosiveness, thereby causing smaller damage to the passivation layer. However, aluminum powder is not suitable for adding in large quantities because it will greatly reduce the filling factor and thus reduce the efficiency. In Table 3, when matched with the glass material of Example 1, since the aluminum powder of Comparative Example 9 is higher than 1wt%, the loss of FF increases, which is insufficient to compensate for the increase in open circuit voltage. Since the aluminum content that can be melted after melting different glass materials will be somewhat different, the addition of aluminum powder in an amount of 0-1wt% can further reduce the composite to improve the open voltage.
[0130] Example 31 and comparative examples 10 to 11 are provided, wherein the process of preparing the solar cell in Example 31 is exactly the same as that in Example 14, except that the content of the glass material in Example 31 is 3wt%; the content of the glass material in Comparative Example 10 exceeds the prescribed range and is 4.5wt%; Comparative Example 11 is a commercially available silver aluminum paste (containing 3-7wt% of glass material, 1-2wt% of aluminum powder, and about 10% of an organic vehicle, and the rest is silver powder). See Table 4 for specific dosage and test data.
[0131] Table 4
[0132]
[0133]
[0134] As shown in Table 4, compared with the commercially available high-efficiency silver-aluminum paste, the conductive paste composition used in this embodiment can significantly reduce the composite after sintering, as shown in Suns-Voc in Table 4. The effect is that after the laser enhanced contact improvement treatment after sintering, a significant open circuit voltage and an efficiency improvement of more than 0.3% can be achieved. From the data of Comparative Example 10, it can be seen that increasing the amount of glass powder to 4.5wt% will increase the damage to the passivation layer and cause the loss of Suns-Voc, so the content of glass material should be in the range of 0.5wt% to 4wt%.
[0135] Furthermore, two groups of data comparison were conducted using commercially available high-efficiency silver-aluminum paste. The preparation of the two groups was the same as in Example 14, but the difference was that the process was different. The test results are shown in Table 5.
[0136] Table 5
[0137]
[0138] It can be seen from Table 5 that the commercially available high-efficiency silver-aluminum paste does not have further efficiency improvement after sintering when combined with the laser enhanced contact improvement technology. This shows that the laser enhanced contact improvement technology requires the improved conductive paste composition of the present application to achieve higher battery conversion efficiency.
[0139] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0140] The conductive paste composition, the method for preparing a solar cell and the solar cell provided in the embodiments of the present application are introduced in detail above, and the principles and implementation modes of the present application are explained by using specific examples. The description of the above embodiments is only used to help understand the technical solution and core idea of the present application. A person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. These modifications or replacements do not cause the essence of the corresponding technical solution to deviate from the scope of the technical solution of the embodiments of the present application.
Claims
1. A conductive paste composition, It is characterized in that According to the mass percentage of the conductive paste composition, the conductive paste composition includes 0.5wt%-4wt% of glass frit, 80wt%-92wt% of conductive component, and 7wt%-16wt% of organic medium; The glass material comprises oxides, and the glass material comprises 20 mol% to 50 mol% of B in terms of molar percentage of the oxides. 2 O 3 The glass material further comprises: 15mol%-50mol% PbO; or, 15mol%-50mol% Bi 2 O 3 ; or, 15mol%-50mol% of PbO and Bi 2 O 3 A mixture of both; The glass material further comprises a first additive, the content of which is less than or equal to 18 mol%, according to the molar percentage of the oxide. The first additive is selected from SeO 2 and TeO 2 Any one or more of the following; Wherein, the PbO and the Bi 2 O 3 The sum of the cation contents of B 2 O 3 The ratio of the cation content is 0.30-1.
25.
2. The conductive paste composition according to claim 1, It is characterized in that The first additive is also selected from Li 2 O、Al 2 O 3 、ZnO、SiO 2 Any one or more of .
3. The conductive paste composition according to claim 2, It is characterized in that In terms of molar percentage of the oxide, the first additive satisfies at least one of the following conditions: a) The first additive comprises Li 2 O, Li 2 The content of O is less than or equal to 15 mol%; b) The first additive comprises Al 2 O 3 , the Al 2 O 3 The content is less than or equal to 10 mol%; c) the first additive comprises ZnO, and the content of ZnO is less than or equal to 18 mol %; d) The first additive comprises SiO 2 , the SiO 2 The content is less than or equal to 15 mol%; e) The first additive comprises SeO 2 , the SeO 2 The content is less than or equal to 15 mol%; f) The first additive comprises TeO 2 , the TeO 2 The content is less than or equal to 15 mol%.
4. The conductive paste composition according to claim 1, It is characterized in that According to the molar percentage of the oxide, the glass material also includes: 0-15 mol% Li 2 O; 0-10 mol% Al 2 O 3 ; 0 to 18 mol% ZnO; 0 to 15 mol% SiO 2 .
5. The conductive paste composition according to claim 1, It is characterized in that The glass material further comprises a second additive according to the molar percentage of the oxide, the content of the second additive is less than or equal to 5 mol%, and the second additive is selected from AgO 2 、Ag 2 O, AgO, Na 2 O.K 2 Any one or more of O, MgO, CaO and BaO.
6. The conductive paste composition according to claim 1, It is characterized in that The conductive paste composition further comprises less than or equal to 1 wt % of filler in terms of mass percentage of the composition; the filler comprises at least one of aluminum powder, silicon powder and aluminum-silicon alloy powder.
7. The conductive paste composition according to claim 6, It is characterized in that The mass percentage of the filler in the conductive paste composition is greater than 0 and less than or equal to 1 wt %.
8. The conductive paste composition according to claim 6, It is characterized in that The D of the filler v 50 is 1-4μm, D v 50 is the particle size corresponding to when the cumulative volume percentage of the filler reaches 50%.
9. The conductive paste composition according to claim 1, It is characterized in that The conductive component is selected from any one or a mixture of silver, silver alloy, silver oxide and silver salt.
10. The conductive paste composition according to claim 1, It is characterized in that Used to form a first conductive structure (20) in a solar cell, the solar cell comprising a substrate (101) and a passivation layer (103) located at least on one side of the substrate (101); when sintering the solar cell, the conductive paste composition can penetrate the passivation layer (103) to form the first conductive structure (20).
11. The conductive paste composition according to claim 10, It is characterized in that The substrate (101) comprises an n-type doped semiconductor substrate.
12. A conductive paste composition, It is characterized in that According to the mass percentage of the conductive paste composition, the conductive paste composition includes 0.5wt%-4wt% of glass frit, 80wt%-92wt% of conductive components, 7wt%-16wt% of organic medium and less than or equal to 1wt% of filler; The glass material comprises oxides, and the glass material comprises 20 mol% to 50 mol% of B in terms of molar percentage of the oxides. 2 O 3 The glass material further comprises: 15mol%-50mol% PbO; or, 15mol%-50mol% Bi 2 O 3 ; or, 15mol%-50mol% of PbO and Bi 2 O 3 A mixture of both; Wherein, the PbO and the Bi 2 O 3 The sum of the cation contents of B 2 O 3 The ratio of the cation content is 0.30-1.25; the filler includes at least one of aluminum powder, silicon powder and aluminum-silicon alloy powder.
13. The conductive paste composition according to claim 12, It is characterized in that The glass material further comprises a first additive, the content of which is less than or equal to 18 mol%, according to the molar percentage of the oxide. The first additive is selected from Li 2 O、Al 2 O 3 、ZnO、SiO 2 , SeO 2 and TeO 2 Any one or more of .
14. The conductive paste composition according to claim 13, It is characterized in that In terms of molar percentage of the oxide, the first additive satisfies at least one of the following conditions: a) The first additive comprises Li 2 O, Li 2 The content of O is less than or equal to 15 mol%; b) The first additive comprises Al 2 O 3 , the Al 2 O 3 The content is less than or equal to 10 mol%; c) the first additive comprises ZnO, and the content of ZnO is less than or equal to 18 mol %; d) The first additive comprises SiO 2 , the SiO 2 The content is less than or equal to 15 mol%; e) The first additive comprises SeO 2 , the SeO 2 The content is less than or equal to 15 mol%; f) The first additive comprises TeO 2 , the TeO 2 The content is less than or equal to 15 mol%.
15. The conductive paste composition according to claim 12, It is characterized in that The glass material further comprises a second additive according to the molar percentage of the oxide, the content of the second additive is less than or equal to 5 mol%, and the second additive is selected from AgO 2 、Ag 2 O, AgO, Na 2 O.K 2 Any one or more of O, MgO, CaO and BaO.
16. The conductive paste composition according to claim 12, It is characterized in that The D of the filler v 50 is 1-4μm, D v 50 is the particle size corresponding to when the cumulative volume percentage of the filler reaches 50%.
17. A method for preparing a solar cell, It is characterized in that The following steps are involved: Providing a substrate (10), the substrate (10) comprising a substrate (101), a p-type doping layer (102), and a passivation layer (103), wherein the p-type doping layer (102) is located between the substrate (101) and the passivation layer (103); Applying the conductive paste composition according to any one of claims 1 to 11 on the passivation layer (103); Sintering the substrate (10) coated with the conductive paste composition, so that the conductive paste composition etches the passivation layer (103) during the sintering process to form a first conductive structure (20); Laser enhanced contact optimization is performed on the substrate (10) to obtain the solar cell.
18. The method for preparing a solar cell according to claim 17, It is characterized in that The conductive paste composition is coated on the passivation layer (103), comprising: The conductive paste composition is applied to at least a portion of the surface of the passivation layer (103) in a patterned form.
19. The method for preparing a solar cell according to claim 17, It is characterized in that The step of performing laser enhanced contact optimization on the substrate (10) comprises: A reverse voltage is applied to the substrate (10), and at the same time, a laser is scanned on the substrate (10) to form an induced current in the first conductive structure (20).
20. The method for preparing a solar cell according to claim 19, It is characterized in that The preparation method satisfies at least one of the following conditions: g) the solar cell has a breakdown voltage, and the reverse voltage is less than the breakdown voltage; h) The laser scanning time is 1ms to 100ms; i) The induced current is 100A to 1000A.
21. A solar cell, It is characterized in that The solar cell comprises a first conductive structure (20) made of the conductive paste composition according to any one of claims 1 to 11; or, A first conductive structure (20) made of the conductive paste composition according to any one of claims 12 to 16; or The solar cell is manufactured by the manufacturing method according to any one of claims 17 to 20.
22. The solar cell according to claim 21, It is characterized in that The solar cell is a solar cell having a tunneling oxide layer passivation contact structure.
Citation Information
Patent Citations
Method of manufacturing a solar cell electrode
CN105261669A
Cited By
Electric field enhanced light injection method and device and battery piece production method and system
CN119153589A
Conductive paste, conductive electrode and preparation method therefor, and crystalline silicon solar cell
WO2026171159A1