Honeycomb structure, electric heating carrier, and exhaust gas cleaning apparatus

By shortening cell lengths at the outer periphery of the honeycomb structure, the uneven temperature distribution and thermal stress issues in EHC systems are mitigated, enhancing thermal shock resistance and improving exhaust gas purification efficiency.

JP2024140914AInactive Publication Date: 2024-10-10NGK INSULATORS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052281
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing honeycomb structures used in electrically heated catalysts (EHC) face issues with uneven temperature distribution and thermal stress, leading to potential cracks due to differences in exhaust gas flow rates between the central and outer peripheral parts, which conventional methods have not adequately addressed.

Method used

The honeycomb structure is designed with shorter cell lengths at the outer periphery to promote even exhaust gas flow, reducing pressure loss and alleviating temperature distribution unevenness, thereby enhancing thermal shock resistance.

Benefits of technology

This design improves thermal shock resistance by ensuring uniform temperature distribution and reducing the likelihood of cracks, while maintaining effective exhaust gas purification performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140914000001_ABST
    Figure 2024140914000001_ABST
Patent Text Reader

Abstract

To provide a honeycomb structure capable of relaxing a flow rate difference of exhaust gas between center and outer peripheral parts.SOLUTION: A columnar honeycomb structure 110 comprises: a conductive columnar honeycomb structure part; and a pair of electrode layers 112a, 112b. In a vertical cross section where cells 115 extend, when a coordinate axis is arranged in a radial direction, a coordinate value of a centroid O is 0, and a coordinate value of an outer surface of an outer peripheral wall is 1.0R, an average length R1 of the honeycomb structure part in a direction where cells extend from a first end face 116 to a second end face in a range of 0 to 0.7 R (center), and an average length R2 of the honeycomb structure part in a range of 0.7 R to 1.0 R (outer peripheral part) satisfy 0.5≤R2 / R1<1.0. The average length R1 has a length of 99% or greater of a maximum value of the length of the honeycomb structure part where the cells extend from the first end face to the second end face in the center part, and the cells located on the center and the cells located on the outer peripheral part form a channel of fluid together.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a honeycomb structure. The present invention also relates to an electrically heated carrier having a honeycomb structure. The present invention also relates to an exhaust gas purification device having an electrically heated carrier. [Background technology]

[0002] Conventionally, catalysts supported on honeycomb structures made of cordierite or silicon carbide have been used to treat harmful substances in exhaust gases emitted from automobile engines. When treating exhaust gases with a catalyst supported on a honeycomb structure, the catalyst needs to be heated to a specified temperature. However, a problem has existed in the past where exhaust gases are not sufficiently purified at engine start-up because the catalyst temperature is low. To address this problem, a system called an electrically heated catalyst (EHC) has been developed in which electrodes are provided on a honeycomb structure made of conductive ceramics, and the honeycomb structure itself is heated by passing electricity through it, thereby heating the catalyst supported on the honeycomb structure to its activation temperature before or at engine start-up.

[0003] An EHC generally comprises an outer peripheral wall, a conductive honeycomb structure portion having partition walls disposed inside the outer peripheral wall to define a plurality of cells that form flow paths from a first end face to a second end face, and a pair of electrode layers disposed on the outer peripheral wall of the honeycomb structure portion. When an electric current is applied by connecting terminals to the pair of electrode layers and applying a voltage, the EHC generates heat by Joule heat caused by the electricity flowing inside the honeycomb structure portion, which is a conductive resistor.

[0004] In EHC, more exhaust gas tends to flow to the center than to the periphery. This causes uneven temperature distribution in the EHC when exhaust gas flows, and cracks may occur due to the expansion of the thermal expansion difference. For this reason, it is desirable to equalize the temperature distribution in the honeycomb structure of the EHC to prevent cracks from occurring due to thermal stress caused by the temperature difference between high and low temperature areas.

[0005] Under such circumstances, Patent Document 1 proposes that the aperture ratio of the central portion be 0.70 to 0.95 times that of the peripheral portion, which makes the electrical resistivity of the central portion lower than that of the peripheral portion, and thus when a voltage is applied to the honeycomb structure, a large current flows through the central portion, causing the central portion to heat up more quickly than before.

[0006] Furthermore, although Patent Document 2 is not an invention that aims to make the temperature distribution uniform, it describes that in order to securely grip the honeycomb structure with a metal case while shortening the axial length of the honeycomb structure, the axial length of the outer peripheral surface of the outer periphery is shorter than the axial length of the central portion, and the end face of the outer periphery forms a gripping end face for gripping the honeycomb structure. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2015 / 151823 [Patent Document 2] International Publication No. 2021 / 181758 Summary of the Invention [Problem to be solved by the invention]

[0008] As proposed in Patent Document 1, by making the aperture ratio of the central portion 0.70 to 0.95 times that of the peripheral portion, exhaust gas flows more easily to the peripheral portion than when the aperture ratio of the central portion is the same as that of the peripheral portion. This reduces the difference in the flow rate of exhaust gas between the central portion and the peripheral portion of the honeycomb structure, and reduces the bias in temperature distribution, thereby suppressing the occurrence of cracks due to thermal stress. However, there is a limit to how uniform the exhaust gas distribution can be achieved by the invention described in Patent Document 1, and further improvement in the thermal shock resistance of honeycomb structures is desired.

[0009] In the invention described in Patent Document 2, the axial length of the outer peripheral surface of the outer peripheral portion is shorter than the axial length of the central portion, but since the end face of the outer peripheral portion constitutes a gripping end face for gripping the honeycomb structure, exhaust gas does not flow to the outer peripheral portion, and therefore the effect of reducing the flow rate difference of exhaust gas between the central portion and the outer peripheral portion of the honeycomb structure cannot be obtained.

[0010] The present invention was created in consideration of the above-mentioned circumstances, and in one embodiment, an object of the present invention is to provide a honeycomb structure that can reduce the difference in exhaust gas flow rate between the center and the outer periphery using a method that is different from the conventional method. [Means for solving the problem]

[0011] The present inventors have conducted extensive research to solve the above problems and have found that it is advantageous to shorten the cell length of the outer peripheral portion that forms the fluid flow path so that exhaust gas can easily flow to the outer peripheral portion of the honeycomb structure. The present invention has been completed based on this finding and is exemplified below. [Aspect 1] an electrically conductive columnar honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form a fluid flow path from a first end surface to a second end surface; A pair of electrode layers are provided on the outer surface of the outer peripheral wall, extend in a band shape in the extending direction of the cells, and are provided so as to face each other across the central axis of the honeycomb structure section; Equipped with In a cross section perpendicular to the cell extension direction, coordinate axes are taken in the radial direction, the coordinate value of the center of gravity O is 0, and the coordinate value of the outer surface of the outer peripheral wall is 1.0R, an average length R1 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the central portion having a coordinate value in the range of 0 to 0.7R, and an average length R2 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the outer peripheral portion having a coordinate value in the range of 0.7R to 1.0R satisfy 0.5≦R2 / R1<1.0, The average length R1 is 99% or more of the maximum length of the honeycomb structure part in the cell extension direction from the first end face to the second end face in the central part, The plurality of cells located in the central portion and the plurality of cells located in the outer periphery together form a fluid flow path. Columnar honeycomb structure. [Aspect 2] 2. The pillar-shaped honeycomb structure according to embodiment 1, wherein 0.7≦R2 / R1<1.0. [Aspect 3] 3. The pillar-shaped honeycomb structure according to embodiment 1 or 2, wherein a difference between a maximum value and a minimum value of a length of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the central portion is 1 mm or less. [Aspect 4] 4. The pillar-shaped honeycomb structure according to any one of aspects 1 to 3, wherein the opening ratio in the central portion and the opening ratio in the peripheral portion are the same. [Aspect 5] 4. The pillar-shaped honeycomb structure according to any one of aspects 1 to 3, wherein the opening ratio in the central portion is 0.7 to 0.95 times the opening ratio in the peripheral portion. [Aspect 6] The pillar-shaped honeycomb structure according to any one of aspects 1 to 5, an electrode terminal joined to each outer surface of the pair of electrode layers; An electrically heated carrier comprising: [Aspect 7] An electrically heated carrier according to embodiment 6; a metal tube that houses the electrically heated carrier and that fits only with the outer circumferential wall of the electrically heated carrier; An exhaust gas purification device comprising: Effect of the Invention

[0012] According to one embodiment of the present invention, the cell length of the outer periphery of the honeycomb structure is made shorter than that of the central portion, so that the pressure loss in the outer periphery is relatively low. This promotes the flow of exhaust gas to the outer periphery, and the difference in the flow rate of exhaust gas between the central portion and the outer periphery can be alleviated. As a result, the bias of the temperature distribution during heating is alleviated, and it is possible to improve the thermal shock resistance of the honeycomb structure. By combining this with other conventionally known methods, further improvement in thermal shock resistance can be expected. In addition, an electrically heated carrier can be produced by joining electrode terminals to this honeycomb structure. The electrically heated carrier can be suitably used, for example, as a catalyst carrier for an exhaust gas purification device. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic diagram of an electrically heated carrier according to an embodiment of the present invention, as viewed from a first end surface. [Figure 2A] 1 is a schematic cross-sectional view of an example of a honeycomb structure section, observed in a cross section passing through a central axis O and parallel to a cell extension direction. [Figure 2B] FIG. 2 is a schematic cross-sectional view of another example of a honeycomb structure portion, observed in a cross section passing through the central axis O and parallel to the cell extension direction. [Figure 2C] FIG. 11 is a schematic cross-sectional view of still another example of a honeycomb structure portion, observed in a cross section passing through the central axis O and parallel to the cell extension direction. [Diagram 3] 1 is a schematic cross-sectional view showing an exhaust gas purification device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0015] (1. Electrically heated carrier) Fig. 1 is a schematic diagram of an electrically heated carrier 100 according to one embodiment of the present invention, observed from a first end face 116. Figs. 2A to 2C are schematic cross-sectional views of several examples of honeycomb structure parts.

[0016] The electrically heated carrier 100 includes a honeycomb structure 110 and electrode terminals 130a, 130b. By supporting a catalyst on the electrically heated carrier 100, the electrically heated carrier 100 can be used as a catalyst body. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts and oxidation catalysts in which precious metals such as platinum (Pt), palladium (Pd), and rhodium (Rh) are supported on the surface of alumina pores and contain co-catalysts such as ceria and zirconia, or alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts). x Examples of the catalyst include selective catalytic reduction catalysts (SCR catalysts). Two or more catalysts selected from these catalysts may be used. There is no particular limitation on the method of supporting the catalyst, and any known method for supporting a catalyst on a honeycomb structure may be used.

[0017] (1-1. Honeycomb structure) In one embodiment, the honeycomb structure 110 is a honeycomb structure having an outer peripheral wall 114 and partition walls 113 disposed inside the outer peripheral wall 114 and partitioning a plurality of cells 115 that form flow paths from a first end surface 116 to a second end surface 118; a first electrode layer 112a provided on the outer surface of the outer peripheral wall 114 and extending in a strip shape in the extension direction of the cells 115; and A second electrode layer 112b is provided on the outer surface of the outer peripheral wall 114, extends in a strip shape in the extending direction of the cells 115, and is provided so as to face the first electrode layer 112a across the central axis O of the honeycomb structure portion. Equipped with.

[0018] <Honeycomb structure> The honeycomb structure portion has a higher volume resistivity than the electrode layers 112a and 112b, but is conductive. The volume resistivity of the honeycomb structure portion is not particularly limited as long as it can generate heat by Joule heat when current is applied, and may be set appropriately according to the voltage to be applied. For example, when measured at 25°C by a four-terminal method, the volume resistivity may be 0.001 to 100 Ω·cm. For high voltages of more than 60V, the volume resistivity may be 2 to 100 Ω·cm, typically 5 to 100 Ω·cm. For low voltages of 60V or less, such as 48V, the volume resistivity may be 0.001 to 2 Ω·cm, typically 0.001 to 1 Ω·cm, and more typically 0.01 to 1 Ω·cm.

[0019] The outer shape of the honeycomb structure is not particularly limited, and may be, for example, a cylinder whose end face is round, such as a circular, oval, elliptical, racetrack, or oval shape, a cylinder whose end face is polygonal, such as a triangular or rectangular shape, or a cylinder whose end face has other irregular shapes. The honeycomb structure in FIG. 1 has a circular end face shape.

[0020] There is no particular limit to the height of the honeycomb structure part (the length from one end face to the other end face) and it may be set appropriately depending on the application and required performance. There is also no particular limit to the relationship between the height of the honeycomb structure part and the maximum diameter of each end face (the maximum length of the diameters passing through the center of gravity of each end face of the honeycomb structure). Therefore, the height of the honeycomb structure part may be longer than the maximum diameter of each end face, or the height of the honeycomb structure part may be shorter than the maximum diameter of each end face.

[0021] However, it is advantageous for the length in the direction in which the cells extend from the first end face 116 to the second end face (cell length) to be shorter in the peripheral portion than in the central portion in order to reduce the difference in exhaust gas flow rate between the central portion and the peripheral portion. This is because, when the cell length is shorter in the peripheral portion than in the central portion, the peripheral portion experiences relatively low pressure loss, and the flow of exhaust gas to the peripheral portion is promoted. As a result, the bias in temperature distribution during heating is reduced, and it is possible to improve the thermal shock resistance of the honeycomb structure.

[0022] Specifically, in a cross section perpendicular to the cell extension direction, coordinate axes are taken in the radial direction, the coordinate value of the center of gravity O is 0, and the coordinate value of the outer surface of the outer peripheral wall is 1.0R, it is preferable that the average length R1 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the central portion where the coordinate value is in the range of 0 to 0.7R, and the average length R2 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the outer peripheral portion where the coordinate value is in the range of 0.7R to 1.0R satisfy 0.5≦R2 / R1<1.0.

[0023] The smaller R2 / R1 is, the more effective it is in reducing the difference in the flow rate of exhaust gas between the central portion and the outer periphery. Therefore, R2 / R1 is more preferably 0.95 or less, and even more preferably 0.90 or less. However, if R2 / R1 is too small, the area of ​​the outer periphery wall that can be fitted with the metal pipe becomes small, and the canning retention property decreases, so R2 / R1 is preferably 0.7 or more, more preferably 0.75 or more, and even more preferably 0.80 or more. Therefore, for example, it is preferable to satisfy 0.7≦R2 / R1<1.0, more preferably to satisfy 0.75≦R2 / R1≦0.95, and even more preferably to satisfy 0.80≦R2 / R1≦0.90.

[0024] The average length R1 can be obtained, for example, by dividing the volume of the central part of the honeycomb structure (including the volume of the cells and pores) by the cross-sectional area perpendicular to the extension direction of the cells in the central part. The average length R2 can be obtained, for example, by dividing the volume of the outer periphery of the honeycomb structure part (including the volume of the cells and pores) by the cross-sectional area perpendicular to the extension direction of the cells in the outer periphery.

[0025] As long as R2 / R1 satisfies the above condition, there is no particular restriction on the shape of the central part and the outer periphery. For example, the outer periphery of the honeycomb structure part may have a tapered part that narrows in diameter toward the first end face 116 and the second end face 118 when observed in a cross section passing through the central axis O and parallel to the cell extension direction. The contour of the tapered part may be linear as shown in FIG. 2A, or curved as shown in FIG. 2B. The tapered part may be provided only on the outer periphery, or a part of the tapered part may reach the central part. Also, as shown in FIG. 3, the outer periphery of the honeycomb structure part may narrow in diameter in a step-like manner. Also, the part where the diameter narrows in a step-like manner may be in the central part. Other shapes are also possible.

[0026] The length (cell length) of the honeycomb structure part in the cell extension direction from the first end face to the second end face in the central part does not need to be constant and can vary. However, there is little point in varying the cell length in the central part. Rather, if there is a part with a shortened cell length in the central part, it may have an adverse effect on thermal shock resistance. For this reason, it is preferable that the average length R1 is 99% or more of the maximum length of the honeycomb structure part in the cell extension direction from the first end face to the second end face in the central part, and more preferably has the same length. According to a typical embodiment, the difference between the maximum and minimum values ​​of the cell length in the central part can be 1 mm or less.

[0027] The shape of the honeycomb structure part is preferably symmetrical about the central axis O (center of gravity) when observed in a cross section passing through the central axis O and parallel to the cell extension direction. Furthermore, the shape of the honeycomb structure part is preferably symmetrical about a line segment L that is orthogonal to the central axis O (center of gravity) and passes through a point (midpoint M) on the central axis O (center of gravity) that bisects the length in the cell extension direction from the first end face 116 to the second end face 118.

[0028] Since the multiple cells located in the center and the multiple cells located in the outer periphery must form a fluid flow path together, they should not be blocked by the metal tube. Therefore, when accommodating a honeycomb structure in the metal tube, it is preferable that the metal tube is fitted only with the outer periphery wall. The concept of the metal tube fitting with the outer periphery wall includes the direct fitting of the inner surface of the metal tube with the outer surface of the outer periphery wall, and the indirect fitting of the inner surface of the metal tube with the outer surface of the outer periphery wall via other members such as an electrode layer or a mat.

[0029] In addition, the size of the honeycomb structure is set so that the area of ​​one end face is 2,000 to 20,000 mm2 in order to increase heat resistance (suppress cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm. 2 It is more preferable that:

[0030] There is no limitation on the opening shape of the cells in a cross section perpendicular to the extension direction of the cells 115, and the cell may be, for example, a polygonal shape, preferably a square, a hexagon, an octagon, or a combination of these. Among these, square and hexagonal shapes are preferable. By making the cell shape like this, the pressure loss when exhaust gas flows through the honeycomb structure 110 is reduced, and the purification performance of the catalyst is improved. Even if these cells have arc-shaped corners, they are considered to be polygonal cells.

[0031] The cells 115 may penetrate from the first end face 116 to the second end face 118. Moreover, the cells 115 may be arranged such that first cells, each having a plugged first end face 116 and an opening on the second end face 118, and second cells, each having an opening on the first end face 116 and a plugged second end face 118, are alternately adjacent to each other with the partition wall 113 interposed therebetween.

[0032] The material of the outer peripheral wall 114 and the partition walls 113 is not particularly limited as long as it can generate heat by Joule heat when electricity is applied, and ceramics (particularly conductive ceramics) can be used alone or in combination. The material of the outer peripheral wall 114 and the partition walls 113 is not limited, and one or more of oxide ceramics such as alumina, mullite, zirconia, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride can be used. In addition, silicon carbide-silicon composites, silicon carbide / graphite composites, and the like can also be used. Among these, from the viewpoint of achieving both heat resistance and conductivity, the material of the outer peripheral wall 114 and the partition walls 113 is preferably a silicon-silicon carbide composite or a silicon carbide composite as the main component, and more preferably a silicon-silicon carbide composite or silicon carbide. When the material of the outer peripheral wall 114 and the partition wall 113 is said to be mainly composed of silicon-silicon carbide composite, it means that the outer peripheral wall 114 and the partition wall 113 each contain 80 mass% or more of silicon-silicon carbide composite (total mass) as a whole, and preferably contain 90 mass% or more. Here, the silicon-silicon carbide composite contains silicon carbide particles as aggregates and silicon as a binder for binding the silicon carbide particles, and it is preferable that a plurality of silicon carbide particles are bound by silicon so as to form pores between the silicon carbide particles. When the material of the outer peripheral wall 114 and the partition wall 113 is said to be mainly composed of silicon carbide, it means that the outer peripheral wall 114 and the partition wall 113 each contain 80 mass% or more of silicon carbide (total mass) as a whole, and preferably contain 90 mass% or more.

[0033] When the outer peripheral wall 114 and the partition walls 113 contain a silicon-silicon carbide composite material, the ratio of the "mass of silicon as a binder" contained in the outer peripheral wall 114 and the partition walls 113 to the sum of the "mass of silicon carbide particles as aggregate" contained in the outer peripheral wall 114 and the partition walls 113 and the "mass of silicon as a binder" contained in the outer peripheral wall 114 and the partition walls 113 is preferably 10 to 40 mass%, and more preferably 15 to 35 mass%. When it is 10 mass% or more, the strength of the outer peripheral wall 114 and the partition walls 113 is sufficiently maintained. When it is 40 mass% or less, the shape is easily maintained during firing.

[0034] The partition walls 113 of the honeycomb structure may be dense, such as in the form of Si-impregnated SiC, but are preferably porous. If the porosity of the partition walls 113 is 30% or more, deformation during firing is more easily suppressed. If the porosity of the partition walls 113 is 60% or less, the strength of the honeycomb structure is sufficiently maintained. Therefore, the porosity of the partition walls 113 is preferably, for example, 30% or more, more preferably 35 to 60%, and more preferably 35 to 45%. The porosity is a value measured by a mercury porosimeter. Note that dense refers to a porosity of 5% or less.

[0035] The thickness of the partition walls 113 that define the cells 115 is preferably 0.1 to 0.3 mm, and more preferably 0.1 to 0.2 mm. When the thickness of the partition walls 113 is 0.1 mm or more, it is possible to suppress a decrease in the strength of the honeycomb structure section. When the thickness of the partition walls 113 is 0.3 mm or less, it is possible to suppress an increase in pressure loss when exhaust gas is passed through the honeycomb structure section when the honeycomb structure section is used as a catalyst carrier to support a catalyst. In this specification, the thickness of the partition walls 113 is defined as the length of a portion that passes through the partition walls 113, of a line segment that connects the centers of gravity of adjacent cells 115 in a cross section perpendicular to the extension direction of the cells 115.

[0036] Providing the outer peripheral wall 114 on the honeycomb structure portion is useful from the viewpoint of ensuring the structural strength of the honeycomb structure portion and suppressing leakage of the fluid flowing through the cells 115 from the outer peripheral wall 114. In this respect, the thickness of the outer peripheral wall 114 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the outer peripheral wall 114 is made too thick, the strength becomes too high, and the strength balance with the partition walls 113 is lost, and the thermal shock resistance is reduced. Therefore, the thickness of the outer peripheral wall 114 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Therefore, the thickness of the outer peripheral wall 114 is preferably, for example, 0.1 to 1.0 mm, more preferably 0.15 to 0.7 mm, and even more preferably 0.2 to 0.5 mm. Here, the thickness of the outer peripheral wall 114 is defined as the thickness in the normal direction to the tangent to the outer surface of the outer peripheral wall 114 at the measurement point when the portion of the outer peripheral wall 114 where the thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cells 115. preferable.

[0037] In one embodiment, the honeycomb structure part can have the same opening ratio in the central part and the same opening ratio in the peripheral part. As described above, the honeycomb structure part has a shorter cell length in the peripheral part than in the central part, which promotes the flow of exhaust gas to the peripheral part, and can reduce the flow rate difference of exhaust gas between the central part and the peripheral part. In addition, since the cell length has a relatively high degree of freedom, the magnitude of the reduction effect of the flow rate difference can be easily adjusted. Therefore, even if a structure that provides a difference in the opening rate between the central part and the peripheral part as proposed in the past is not adopted, a desired reduction effect regarding the flow rate difference can be obtained. Note that the term "same" here is a concept that includes substantially the same, and for example, when the opening rate in the central part is more than 0.95 times and less than 1.05 times the opening rate in the peripheral part, it is considered to be the same.

[0038] In one embodiment, the honeycomb structure may have an aperture ratio in the center portion smaller than that in the outer peripheral portion. For example, the aperture ratio in the center portion may be 0.7 to 0.95 times that in the outer peripheral portion. If the cell length in the outer peripheral portion is too short, problems other than the effect of mitigating the flow rate difference between the center portion and the outer peripheral portion may occur, such as a decrease in canning retention. For this reason, by making the cell length in the outer peripheral portion shorter than that in the center portion and making the aperture ratio in the center portion smaller than that in the outer peripheral portion, it is possible to achieve both canning retention and thermal shock resistance at a high level.

[0039] In this specification, the opening ratio of the central portion is a value obtained by dividing the total cell opening area in the central portion by the sum of the partition wall area and the cell opening area in the central portion in a cross section perpendicular to the cell extension direction (total cell opening area / (total cell opening area+total partition wall area)), expressed as a percentage. Also, in this specification, the opening ratio of the peripheral portion is a value obtained by dividing the total cell opening area in the peripheral portion by the sum of the partition wall area (excluding the peripheral wall) and the cell opening area in the peripheral portion in a cross section perpendicular to the cell extension direction (total cell opening area / (total cell opening area+total partition wall area)), expressed as a percentage.

[0040] One method for changing the opening ratio of a honeycomb structure between the peripheral portion and the central portion is to use a die having a structure in which the opening ratio changes between the peripheral region and the central region during the process of producing a honeycomb molded body by extrusion molding, as described below.

[0041] The opening ratios of the outer peripheral portion and the central portion are not limited, but may be, for example, 50 to 80%, preferably 55 to 75%, and more preferably 60 to 70%. By setting the opening ratios of the outer peripheral portion and the central portion in such ranges, the purification performance of the catalyst can be improved while reducing the pressure loss when exhaust gas flows through the honeycomb structure portion.

[0042] The honeycomb structure has a cell density of 40 to 150 cells / cm in a cross section perpendicular to the extension direction of the cells 115. 2Preferably, the cell density is 70 to 100 cells / cm. 2 By setting the cell density in this range, it is possible to increase the purification performance of the catalyst while reducing the pressure loss when exhaust gas flows through the honeycomb structure. 2 If the cell density is 150 cells / cm or more, the catalyst carrying area is sufficiently secured. 2 When the honeycomb structure 110 is used as a catalyst carrier to support a catalyst, the pressure loss caused by the exhaust gas flowing therethrough is prevented from becoming too large if the honeycomb structure 110 is used as a catalyst carrier to support a catalyst, and the cell density is a value obtained by dividing the number of cells by the area of ​​one end face of the honeycomb structure part on the inner peripheral side than the outer peripheral wall 114.

[0043] Although there is no limitation on the shape of the cells in a cross section perpendicular to the extension direction of the cells 115, a rectangle, a hexagon, an octagon, or a combination of these is preferable. Among these, a rectangle and a hexagon are preferable. By using such a cell shape, the pressure loss when exhaust gas flows through the honeycomb structure 110 is reduced, and the purification performance of the catalyst is excellent. From the viewpoint of easily achieving both structural strength and heating uniformity, a hexagon is particularly preferable.

[0044] The cells 115 may penetrate from the first end face 116 to the second end face 118. In this case, the cells 115 may be open at both the first end face 116 and the second end face 118. Alternatively, a first cell having a plugged first end face 116 and an opening at the second end face 118 and a second cell having an opening at the first end face 116 and a plugged second end face 118 may be alternately arranged adjacent to each other with the partition wall 113 in between.

[0045] <Electrode layer> A first electrode layer 112a and a second electrode layer 112b facing the first electrode layer 112a across the central axis O of the honeycomb structure part can be provided on the outer surface of the outer peripheral wall 114. By disposing the electrode layers 112a and 112b having a lower volume resistivity than the outer peripheral wall 114, the current spreads easily in the circumferential direction of the honeycomb structure 110 and in the extending direction of the cells 115, so that the uniform heat generation of the honeycomb structure 110 can be improved. Referring to FIG. 1, in a cross section perpendicular to the extending direction of the cells 115, the angle θ (0°≦θ≦180°) formed by two line segments extending from the circumferential centers of the pair of electrode layers 112a and 112b to the central axis O (center of gravity) of the honeycomb structure 110 is preferably 150°≦θ≦180°, more preferably 160°≦θ≦180°, even more preferably 170°≦θ≦180°, and most preferably 180°.

[0046] Although there is no particular restriction on the formation region of the pair of electrode layers 112a, 112b, from the viewpoint of improving the uniform heat generation of the honeycomb structure 110, it is preferable that the pair of electrode layers 112a, 112b are each provided in a band shape extending in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115 on the outer surface of the outer peripheral wall 114. Specifically, in a cross section perpendicular to the extension direction of the cells 115, the central angle α formed by two line segments connecting both side ends in the circumferential direction of each electrode layer 112a, 112b and the central axis O (center of gravity) is preferably 30° or more, more preferably 40° or more, and even more preferably 60° or more from the viewpoint of spreading the current in the circumferential direction and improving the uniform heat generation (see FIG. 1). However, if the central angle α is too large, the current passing through the inside of the honeycomb structure 110 decreases, and the current passing through the vicinity of the outer peripheral wall 114 increases. Therefore, from the viewpoint of uniform heat generation of the honeycomb structure 110, the central angle α is preferably 140° or less, more preferably 130° or less, and even more preferably 120° or less. Moreover, it is desirable that each of the electrode layers 112a and 112b extends over 80% or more of the length between both end faces of the honeycomb structure 110, preferably over 90% or more, and more preferably over the entire length. The electrode layers 112a and 112b may be composed of a single layer, or may have a laminated structure in which multiple layers are laminated.

[0047] The thickness of the electrode layers 112a, 112b is preferably 0.01 to 5 mm, and more preferably 0.01 to 3 mm. By setting the thickness in this range, the uniform heat generation can be improved. When the thickness of the electrode layers 112a, 112b is 0.01 mm or more, the electrical resistance is appropriately controlled, and the heat can be generated more uniformly. When the thickness of the electrode layers 112a, 112b is 5 mm or less, the risk of damage to the canning retention is reduced. The thickness of the electrode layers 112a, 112b is defined as the thickness in the normal direction to the tangent of the outer surface of the electrode layers 112a, 112b at the measurement point when the part of the electrode layers 112a, 112b to be measured for thickness is observed in a cross section perpendicular to the extension direction of the cell 115.

[0048] By making the volume resistivity of the electrode layers 112a, 112b lower than that of the partition walls 113 and the outer peripheral wall 114, electricity flows preferentially through the electrode layers 112a, 112b, and electricity spreads easily in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115 when electricity is applied. The volume resistivity of the electrode layers 112a, 112b is preferably 1 / 10 or less, more preferably 1 / 30 or less, and even more preferably 1 / 50 or less of the volume resistivity of the partition walls 113 and the outer peripheral wall 114. However, if the difference between the volume resistivities of the two becomes too large, current is concentrated between the ends of the opposing electrode layers 112a and 112b, and heat generation in the honeycomb structure 110 is biased, so that the volume resistivities of the electrode layers 112a and 112b are preferably 1 / 350 or more, more preferably 1 / 250 or more, and even more preferably 1 / 150 or more of the volume resistivities of the partition walls 113 and the outer peripheral wall 114. Therefore, the volume resistivities of the electrode layers 112a and 112b are, for example, preferably 1 / 350 to 1 / 10, more preferably 1 / 250 to 1 / 30, and even more preferably 1 / 150 to 1 / 50 of the volume resistivities of the partition walls 113 and the outer peripheral wall 114. The volume resistivities of the electrode layers, partition walls, and outer peripheral wall here are values ​​measured at 25°C by a four-terminal method.

[0049] The material of the electrode layers 112a and 112b is not limited, but a composite material (cermet) of metal and ceramic (particularly conductive ceramic) can be used. Examples of metals include, for example, simple metals such as Cr, Fe, Co, Ni, Si, or Ti, or alloys containing at least one metal selected from these metals. Examples of ceramics include, but are not limited to, silicon carbide (SiC), as well as metal compounds such as metal silicides such as tantalum silicide (TaSi2) and chromium silicide (CrSi2). Specific examples of composite materials (cermets) of metal and ceramics include composite materials of silicon and silicon carbide, composite materials of metal silicides such as tantalum silicide and chromium silicide, and silicon and silicon carbide, and composite materials in which one or more of the above metals are added with one or more insulating ceramics such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride from the viewpoint of reducing thermal expansion. As the material for the electrode layers 112a, 112b, among the various metals and ceramics mentioned above, a composite material of a metal silicide such as tantalum silicide or chromium silicide, silicon, and silicon carbide is preferable because it can be fired simultaneously with the partition wall and the outer peripheral wall, which contributes to simplifying the manufacturing process.

[0050] (1-2. Electrode terminal) The electrode terminals 130a and 130b can be directly or indirectly joined to the outer surfaces of the pair of electrode layers 112a and 112b. When a voltage is applied to the honeycomb structure 110 via the electrode terminals 130a and 130b, electricity is passed through the honeycomb structure 110, and the honeycomb structure 110 can generate heat by Joule heat. Therefore, the honeycomb structure 110 can be suitably used as a heater. This makes it possible to improve the uniform heat generation of the honeycomb structure 110. The voltage to be applied is preferably 12 to 900 V, more preferably 48 to 600 V, but the voltage to be applied can be changed as appropriate.

[0051] The electrode terminals 130a, 130b and the electrode layers 112a, 112b may be directly bonded to each other, but in order to improve the bonding reliability of the electrode terminals 130a, 130b by reducing the thermal expansion difference between the electrode layers 112a, 112b and the electrode terminals 130a, 130b, they may be bonded to each other via one or more base layers 120. Therefore, in a preferred embodiment, the honeycomb structure 110 has a first electrode layer 112a and a second electrode layer 112b disposed on the outer peripheral wall 114 so as to face each other across the central axis O of the honeycomb structure 110, and one or more electrode terminals 130a, 130b are bonded to each of the electrode layers 112a, 112b via the base layer 120.

[0052] From the viewpoint of improving the bonding reliability, it is preferable that the thermal expansion coefficient gradually decreases in the order of the electrode terminals 130a, 130b → (underlying layer 120) → electrode layers 112a, 112b → outer peripheral wall 114. Note that the "thermal expansion coefficient" here means the linear expansion coefficient measured according to JIS R1618:2002 when the temperature is changed from 25°C to 800°C.

[0053] The material of the electrode terminals 130a and 130b is not particularly limited as long as it is a metal, and a single metal or an alloy can be adopted. However, from the viewpoint of corrosion resistance, volume resistivity, and linear expansion coefficient, for example, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, and Ti is preferable, and stainless steel and an Fe-Ni alloy are more preferable. In addition to metals, ceramics may be used. When ceramics are used, it is preferable to use conductive ceramics. Furthermore, it is also possible to use a composite material (cermet) of metal and ceramics (especially conductive ceramics). The number, shape, and size of the electrode terminals 130a and 130b are not particularly limited, and can be appropriately designed according to the size and current carrying performance of the honeycomb structure 110. The volume resistivity of the electrode terminals 130a and 130b measured at 25°C by a four-terminal method is not limited, but is preferably the same as or less than the volume resistivity of the electrode layers 112a and 112b.

[0054] The material of the underlayer 120 is not limited, but may be a composite material (cermet) of metal and ceramics (particularly conductive ceramics). The thermal expansion coefficient of the underlayer 120 can be controlled by adjusting the compounding ratio of the metal and ceramics, for example.

[0055] The underlayer 120 preferably contains, but is not limited to, one or more metals selected from a Ni-based alloy, an Fe-based alloy, a Ti-based alloy, a Co-based alloy, silicon, and Cr.

[0056] The underlayer 120 preferably contains one or more ceramics selected from oxide ceramics such as alumina, mullite, zirconia, glass, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride, although this is not limited thereto.

[0057] The thickness of the underlayer 120 is not particularly limited, but is preferably 0.1 to 1.5 mm, and more preferably 0.3 to 0.5 mm, from the viewpoint of crack suppression. The thickness of the underlayer 120 is defined as the thickness in the normal direction to the tangent of the outer surface of the underlayer 120 at the measurement point when the underlayer 120 whose thickness is to be measured is observed in a cross section perpendicular to the cell extension direction.

[0058] The method for joining the electrode terminals 130a, 130b to the electrode layers 112a, 112b or the base layer 120 is not particularly limited, and examples thereof include thermal spraying, welding, and brazing.

[0059] (2. Exhaust gas purification equipment) The electrically heated carrier according to one embodiment of the present invention can be used in an exhaust gas purification device. Referring to FIG. 3, an exhaust gas purification device 200 has an electrically heated carrier 100 and a metal tube 220 that houses the electrically heated carrier 100. In this exhaust gas purification device, the metal tube 220 is fitted only with the outer peripheral wall 114 of the electrically heated carrier. Therefore, the metal tube 220 is not fitted with the first end face and the second end face of the honeycomb structure part including the reduced diameter part, and the cells 115 in the center part and the outer peripheral part are not blocked by the inner surface of the metal tube 220 and can function as a flow path for exhaust gas. In addition, since the cell length in the outer peripheral part is shortened compared to the center part, exhaust gas easily flows to the outer peripheral part of the honeycomb structure. As a result, the bias of the temperature distribution during heating is mitigated, and it is possible to improve the thermal shock resistance of the honeycomb structure.

[0060] An electric wire 240 for power supply can be connected to the electrode terminals 130a, 130b of the electrically heated carrier 100. The metal constituting the metal tube 220 is not limited to, but may include various stainless steels such as chromium-based stainless steel. By using these metals, the exhaust gas purification device has high heat resistance and corrosion resistance.

[0061] In the exhaust gas purification device 200, the electrically heated carrier 100 can be installed in the middle of a flow path of a fluid such as automobile exhaust gas. The electrically heated carrier 100 can be fixed in the metal tube 220 by, for example, push-in canning, in which the electrically heated carrier 100 is pushed into the metal tube 220 and fitted in a positional relationship in which the extension direction of the cells and the extension direction of the metal tube 220 coincide. It is preferable to dispose a retaining material (mat) 260 between the metal tube 220 and the electrically heated carrier 100. The material constituting the retaining material (mat) 260 is not limited, but examples thereof include ceramics such as alumina fiber, mullite fiber, and ceramic fiber mainly composed of alumina-silica.

[0062] (3. Manufacturing method) Next, a method for manufacturing a honeycomb structure according to an embodiment of the present invention will be described by way of example. The honeycomb structure can be manufactured by a manufacturing method including a step 1 of manufacturing a honeycomb molded body, a step 2 of applying a pair of electrode layer forming pastes to the outer surface of the outer peripheral wall so as to extend in a band shape in the cell extension direction across the central axis of the honeycomb molded body, to manufacture a honeycomb molded body with the electrode layer forming paste, a step 3 of firing the honeycomb molded body with the electrode layer forming paste to manufacture a honeycomb fired body, and a step 4 of processing the honeycomb fired body so that the cell length of the outer peripheral part is shorter than that of the central part.

[0063] (Process 1) Step 1 is a step of producing a honeycomb formed body, which is a precursor of a honeycomb structure. The honeycomb formed body can be produced in accordance with a method for producing a honeycomb formed body in a known method for producing a honeycomb structure. For example, first, silicon powder (silicon), a binder, a surfactant, a pore former, water, and the like are added to silicon carbide powder (silicon carbide) to produce a forming raw material. It is preferable that the mass of the silicon powder is 10 to 40 mass% with respect to the total mass of the silicon carbide powder and the silicon powder. The average particle diameter of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 μm, more preferably 3 to 40 μm. The average particle diameter of the silicon particles in the silicon powder is preferably 2 to 35 μm. The average particle diameters of the silicon carbide particles and the silicon particles refer to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size is measured by a laser diffraction method. The silicon carbide particles are fine particles of silicon carbide constituting the silicon carbide powder, and the silicon particles are fine particles of silicon constituting the silicon powder. Note that this is the blending of the forming raw material when the material of the honeycomb structure is a silicon-silicon carbide composite material, and when the material of the honeycomb structure is silicon carbide, silicon is not added.

[0064] Examples of the binder include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass.

[0065] The surfactant may be ethylene glycol, dextrin, fatty acid soap, polyalcohol, etc. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass.

[0066] The pore-forming material is not particularly limited as long as it becomes pores after firing, and examples thereof include graphite, starch, foamed resin, water-absorbent resin, silica gel, etc. The content of the pore-forming material is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass. The average particle diameter of the pore-forming material is preferably 10 to 30 μm. The average particle diameter of the pore-forming material refers to the arithmetic mean diameter based on volume when the frequency distribution of particle size is measured by a laser diffraction method. When the pore-forming material is a water-absorbent resin, the average particle diameter of the pore-forming material refers to the average particle diameter after water absorption.

[0067] The content of water is preferably 20 to 60 parts by mass when the total mass of the silicon carbide powder and the silicon powder is taken as 100 parts by mass.

[0068] Next, the obtained forming raw material is kneaded to form a clay, and the clay is then extruded to produce a columnar honeycomb formed body having an outer peripheral wall and partition walls. A die having a desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used during extrusion molding. Next, it is preferable to dry the obtained honeycomb formed body. If the length of the honeycomb formed body in the cell extension direction is not the desired length, both ends of the honeycomb formed body can be cut to the desired length. The honeycomb formed body after drying is called a honeycomb dried body.

[0069] The honeycomb formed body may be fired once as a modified example of step 1. That is, in this modified example, the honeycomb formed body is fired to prepare a honeycomb fired body, and step 2 is then carried out on the honeycomb fired body.

[0070] (Process 2) Step 2 is a step of applying an electrode layer forming paste to the outer surface of the outer wall of the honeycomb molded body to obtain a honeycomb molded body with an electrode layer forming paste. The electrode layer forming paste can be formed by appropriately adding various additives to raw material powders (metal powders, ceramic powders, etc.) mixed according to the required characteristics of the electrode layer, and kneading the mixture. The average particle diameter of the raw material powders is not limited, but is preferably, for example, 5 to 50 μm, and more preferably 10 to 30 μm. The average particle diameter of the raw material powders refers to the arithmetic mean diameter based on volume when the frequency distribution of particle sizes is measured by a laser diffraction method.

[0071] Next, the obtained electrode layer forming paste is applied to a required portion of the side surface of a honeycomb molded body (typically a dried honeycomb body) to obtain a honeycomb molded body with the electrode layer forming paste. The method of preparing the electrode layer forming paste and the method of applying the electrode layer forming paste to the honeycomb molded body can be performed in accordance with a known manufacturing method of a honeycomb structure, but in order to give the electrode layer a lower volume resistivity than the outer peripheral wall and the partition wall, the metal content ratio can be made higher than that of the outer peripheral wall and the partition wall, or the particle size of the metal particles in the raw material powder can be made smaller. After application, it is preferable to dry the electrode layer forming paste. Also, care should be taken not to block the cells, particularly the cells in the outer peripheral portion, with the electrode layer forming paste.

[0072] (Step 3) Step 3 is a step of firing the honeycomb molded body with the electrode layer forming paste to obtain a honeycomb structure. Before firing, degreasing may be performed to remove binders and the like. The method of degreasing and firing is not particularly limited, and firing can be performed using an electric furnace, a gas furnace, or the like. The firing conditions vary depending on the material of the honeycomb structure, but are preferably heated at 1400 to 1500°C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon.

[0073] (Step 4) Step 4 is a process for shortening the cell length of the outer periphery of the honeycomb fired body compared to the central part. As described above, there is no particular limitation on the shape of the central part and the outer periphery as long as R2 / R1 satisfies a predetermined condition. There is no particular limitation on the processing method, and examples include cutting and polishing.

[0074] An electrically heated carrier can be manufactured by joining an electrode terminal to the electrode layer of the honeycomb structure thus obtained. The joining method is not particularly limited, and examples thereof include thermal spraying, welding, and brazing. In order to improve the joining property between the electrode layer and the electrode terminal, a base layer may be formed by a method such as thermal spraying.

[0075] An appropriate catalyst may be supported on the electrically heated carrier depending on the application. An example of a method for supporting a catalyst on a honeycomb structure is a method in which a catalyst slurry is introduced into cells by a conventionally known suction method or the like, and is attached to the surfaces and pores of the partition walls, and then a high-temperature treatment is performed to bake the catalyst contained in the catalyst slurry onto the partition walls and support the catalyst. EXAMPLES

[0076] The following examples are provided to better understand the present invention and its advantages, but the present invention is not limited to these examples.

[0077] <Comparative Example 1> (1. Making a cylindrical clay pot) A ceramic raw material was prepared by mixing silicon carbide (SiC) powder and silicon (Si) powder in a mass ratio of 80:20. Hydroxypropyl methylcellulose as a binder and a water-absorbent resin as a pore former were added to the ceramic raw material, and water was added to prepare a molding raw material. The molding raw material was kneaded by a vacuum clay kneader to prepare a cylindrical clay. The binder content was 7 parts by mass when the total of silicon carbide (SiC) powder and silicon (Si) powder was 100 parts by mass. The pore former content was 3 parts by mass when the total of silicon carbide (SiC) powder and silicon (Si) powder was 100 parts by mass. The water content was 42 parts by mass when the total of silicon carbide (SiC) powder and silicon (Si) powder was 100 parts by mass. The average particle diameter of the silicon carbide powder was 20 μm, and the average particle diameter of the silicon powder was 6 μm. The average particle diameter of the pore former was 20 μm. The average particle size of the silicon carbide powder, silicon powder and pore-forming material refers to the arithmetic mean size based on volume when the frequency distribution of particle sizes is measured by a laser diffraction method.

[0078] (2. Preparation of dried honeycomb body) The obtained cylindrical clay was molded using an extrusion molding machine with a predetermined die structure to obtain a cylindrical honeycomb molded body in which each cell shape in a cross section perpendicular to the cell extension direction is hexagonal. This honeycomb molded body was dried by high-frequency dielectric heating, and then dried at 120°C for 2 hours using a hot air dryer, and both end faces were cut by a predetermined amount to produce a dried honeycomb body.

[0079] (3. Preparation of electrode layer forming paste) Silicon (Si) powder, silicon carbide (SiC) powder, methyl cellulose, glycerin, and water were mixed with a centrifugal mixer to prepare an electrode layer forming paste. The Si powder and the SiC powder were mixed so that the volume ratio of the Si powder:SiC powder was 40:60. In addition, when the total of the Si powder and the SiC powder was 100 parts by mass, the amount of the methyl cellulose was 0.5 parts by mass, the amount of the glycerin was 10 parts by mass, and the amount of the water was 38 parts by mass. The average particle diameter of the silicon powder was 6 μm. The average particle diameter of the silicon carbide powder was 35 μm. These average particle diameters refer to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size was measured by the laser diffraction method.

[0080] (4. Application of electrode layer forming paste) The electrode layer forming paste was applied to two locations on the outer surface of the outer peripheral wall of the honeycomb dried body by a curved surface printer so as to face each other across the central axis. Each application was formed in a strip shape over the entire length of the outer peripheral wall of the honeycomb dried body in the cell extension direction (angle θ=180°, central angle α=127°). Next, the electrode layer forming paste applied to the honeycomb dried body was dried to obtain a honeycomb dried body with an electrode layer. The drying temperature was 70°C.

[0081] (5. Firing) The dried honeycomb body with the electrode layer forming paste was degreased in an air atmosphere at 550°C for 3 hours. Next, the degreased dried honeycomb body with the electrode layer forming paste was fired in an air atmosphere at 1450°C for 2 hours to obtain a cylindrical honeycomb structure. The honeycomb structures were produced in the number required for the following tests.

[0082] (6. Specifications of honeycomb structure)

[0083] The honeycomb structure obtained under the above manufacturing conditions had a circular end face with a diameter of 80 mm (excluding the electrode layer) and a height (length in the cell extension direction) of 65 mm. The cell density was 93 cells / cm. 2 The thickness of the outer peripheral wall was 0.3 mm, the thickness of the partition wall was 0.14 mm, and the porosity of the partition wall was 45%. The thickness of the electrode layer was 0.23 mm. The aperture ratio in the central part and the aperture ratio in the outer peripheral part were the same, 73%.

[0084] For the honeycomb structure obtained under the above manufacturing conditions, in a cross section perpendicular to the cell extension direction, coordinate axes are taken in the radial direction, and the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.0R, the average length R1 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the central part where the coordinate value is in the range of 0 to 0.7R, and the average length R2 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the outer peripheral part where the coordinate value is in the range of 0.7R to 1.0R are measured. The results are shown in Table 1 together with R2 / R1. The average length R1 was obtained by dividing the volume of the central part of the honeycomb structure (including the volume of the cells and pores) by the cross-sectional area perpendicular to the extension direction of the cells in the central part. The average length R2 was obtained by dividing the volume of the outer periphery of the honeycomb structure part (including the volume of the cells and pores) by the cross-sectional area perpendicular to the extension direction of the cells in the outer periphery.

[0085] <Example 1> After obtaining the same honeycomb structure as in Comparative Example 1, the honeycomb structure was polished to perform external processing to shorten the cell length of the outer periphery compared to the central part. The honeycomb structure after external processing had a cross-sectional shape as shown in FIG. 2C, and the cell length was shortened by 50% in the region of 0.7R to 1.0R. The shape of the honeycomb structure part was made to be a shape that was line-symmetrical with the central axis O as the axis of symmetry when observed in a cross section passing through the central axis O and parallel to the cell extension direction, and further, was made to be a shape that was line-symmetrical with the line segment L that was perpendicular to the central axis O and passed through a point (midpoint M) on the central axis O that divided the length of the cell in the extension direction from the first end face to the second end face in half. The honeycomb structures that were externally processed in this way were produced in the number required for the following tests.

[0086] For the honeycomb structure obtained under the above manufacturing conditions, R1 and R2 were measured and R2 / R1 was calculated in the same manner as in Comparative Example 1. The results are shown in Table 1.

[0087] <Example 2> After obtaining the same honeycomb structure as in Comparative Example 1, the honeycomb structure was polished to perform external processing to shorten the cell length of the outer periphery compared to the central part. The honeycomb structure after external processing had a cross-sectional shape as shown in FIG. 2C, and the cell length was shortened by about 15% in the region of 0.7R to 1.0R. The shape of the honeycomb structure part was made to be a shape that was line-symmetrical with the central axis O as the axis of symmetry when observed in a cross section passing through the central axis O and parallel to the cell extension direction, and further, was made to be a shape that was line-symmetrical with the line segment L that was perpendicular to the central axis O and passed through a point (midpoint M) on the central axis O that divided the length of the cell in the extension direction from the first end face to the second end face in half. The honeycomb structures that were externally processed in this way were produced in the number required for the following tests.

[0088] For the honeycomb structure obtained under the above manufacturing conditions, R1 and R2 were measured and R2 / R1 was calculated in the same manner as in Comparative Example 1. The results are shown in Table 1.

[0089] <Example 3> After obtaining the same honeycomb structure as in Comparative Example 1, the honeycomb structure was polished to perform external processing to shorten the cell length of the outer periphery compared to the central part. The dried honeycomb body after external processing had a cross-sectional shape as shown in FIG. 2C, and the cell length was shortened by about 15% in the region of 0.85R to 1.0R. The shape of the honeycomb structure part was made to be a shape that was line-symmetrical with the central axis O as the axis of symmetry when observed in a cross section passing through the central axis O and parallel to the cell extension direction, and further, was made to be a shape that was line-symmetrical with the line segment L that was perpendicular to the central axis O and passed through a point (midpoint M) on the central axis O that divided the length of the cell extension direction from the first end face to the second end face in half. The honeycomb structures that were externally processed in this way were produced in the number required for the following tests.

[0090] For the honeycomb structure obtained under the above manufacturing conditions, R1 and R2 were measured and R2 / R1 was calculated in the same manner as in Comparative Example 1. The results are shown in Table 1.

[0091] <Comparative Example 2> After obtaining the same honeycomb structure as in Comparative Example 1, the honeycomb structure was polished to perform external processing to shorten the cell length of the outer periphery compared to the central part. The honeycomb structure after external processing had a cross-sectional shape as shown in FIG. 2C, and the cell length was shortened by about 85% in the region of 0.7R to 1.0R. The shape of the honeycomb structure part was made to be a shape that was line-symmetrical with the central axis O as the axis of symmetry when observed in a cross section passing through the central axis O and parallel to the cell extension direction, and further, was made to be a shape that was line-symmetrical with the line segment L that was perpendicular to the central axis O and passed through a point (midpoint M) on the central axis O that divided the length of the cell extension direction from the first end face to the second end face in half. The honeycomb structures that were externally processed in this way were produced in the number required for the following tests.

[0092] For the honeycomb structure obtained under the above manufacturing conditions, R1 and R2 were measured and R2 / R1 was calculated in the same manner as in Comparative Example 1. The results are shown in Table 1.

[0093] <Comparative Example 3> After obtaining the same honeycomb structure as in Comparative Example 1, the honeycomb structure was polished to perform external processing to shorten the cell length of the outer periphery compared to the central part. The honeycomb structure after external processing had a cross-sectional shape as shown in FIG. 2C, and the cell length was shortened by about 15% in the region of 0.25R to 1.0R. The shape of the honeycomb structure part was made to be a shape that was line-symmetrical with the central axis O as the axis of symmetry when observed in a cross section passing through the central axis O and parallel to the cell extension direction, and further, was made to be a shape that was line-symmetrical with the line segment L that was perpendicular to the central axis O and passed through a point (midpoint M) on the central axis O that divided the length of the cell extension direction from the first end face to the second end face in half. The honeycomb structures that were externally processed in this way were produced in the number required for the following tests.

[0094] For the honeycomb structure obtained under the above manufacturing conditions, R1 and R2 were measured and R2 / R1 was calculated in the same manner as in Comparative Example 1. The results are shown in Table 1.

[0095] <Thermal shock resistance> A thermal shock resistance test was carried out on the honeycomb structures corresponding to each test number, and the crack initiation temperature was determined. The thermal shock resistance test was carried out in the following manner. The honeycomb structure was canned in a cylindrical metal case with an inner diameter of 88 mm of a propane gas burner tester, with an alumina mat sandwiched between them. At this time, the metal case was fitted only to the outer peripheral wall of the honeycomb structure. Gas (combustion gas) heated by a propane gas burner was supplied into the metal case, and the temperature conditions (inlet gas temperature conditions) of the heated gas flowing into the metal case so that the gas passes through the honeycomb structure were set as follows:

[0096] First, the temperature is raised to the designated temperature in 5 minutes, and held at the designated temperature for 10 minutes. After that, the temperature is cooled to 100°C in 5 minutes, and held at 100°C for 10 minutes. This series of operations of raising the temperature, holding, cooling, and holding is called the "heating and cooling operation." After that, the honeycomb structure is cooled to room temperature and checked for cracks under a microscope. The above "heating and cooling operation" is repeated while raising the designated temperature from 800°C in increments of 50°C. The designated temperature is raised in increments of 50°C until cracks appear in the honeycomb structure. The results are shown in Table 1.

[0097] <Canning retention> A test for evaluating the canning retention was carried out for the honeycomb structures having each test number. The test for evaluating the canning retention was carried out in the following manner. The honeycomb structure was housed in a metal case with an inner diameter of 88 mm, sandwiching an alumina mat. At this time, the metal case was fitted only to the outer peripheral wall of the honeycomb structure. Next, a heating vibration test was carried out using a device (manufactured in-house) with a vibrator attached to a burner. The canning retention was evaluated based on whether or not the honeycomb structure was misaligned within the metal case after repeatedly heating and cooling the honeycomb structure and the metal case while applying vibration with the vibrator. Specifically, gas (combustion gas) heated by a propane gas burner was supplied into a metal case, and the gas was passed through the honeycomb structure, heating it to 900°C under inlet gas temperature conditions for 5 minutes, and then cooling it to 100°C in 5 minutes. After this heating and cooling process was carried out for 16 hours, the positional deviation of the honeycomb structure was investigated. The vibration conditions were 40G and 150Hz. The flow rate of gas flowing into the honeycomb structure by the burner was 2Nm 3 / min. The honeycomb structures were evaluated according to the state of misalignment as follows. The results are shown in Table 1. ×: The positional deviation is 4 mm or more in the cell extension direction. △: The positional deviation is 2 mm or more and less than 4 mm in the cell extension direction. ◯: The positional deviation is less than 2 mm in the cell extension direction.

[0098] [Table 1]

[0099] <Consideration> Comparative Example 1 is a conventional example in which the cell length is the same in the central part and the outer periphery. The crack initiation temperature in Comparative Example 1 was 800°C. In contrast, in Examples 1 to 3 in which the cell length in the outer periphery was shortened, the crack initiation temperature increased, and it was confirmed that the thermal shock resistance was improved. In addition, Examples 2 and 3 in which R2 / R1 was more appropriate also had excellent canning retention. [Explanation of symbols]

[0100] 100: Electrically heated carrier 110: Honeycomb structure 112a: First electrode layer 112b: Second electrode layer 113: Bulkhead 114:Outer wall 115: Cell 116: First end surface 118: Second end face 120: Base layer 130a: Electrode terminal 130b: Electrode terminal 200: Exhaust gas purification equipment 220:Metal tube 240: Electric wire

Claims

1. an electrically conductive columnar honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form a fluid flow path from a first end surface to a second end surface; A pair of electrode layers are provided on the outer surface of the outer peripheral wall, extend in a band shape in the extending direction of the cells, and are provided so as to face each other across the central axis of the honeycomb structure section; Equipped with In a cross section perpendicular to the cell extension direction, coordinate axes are taken in the radial direction, and the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.0R, an average length R1 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the central portion having a coordinate value in the range of 0 to 0.7R, and an average length R2 of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the outer peripheral portion having a coordinate value in the range of 0.7R to 1.0R satisfy 0.5≦R2 / R1<1.0, The average length R1 has a length of 99% or more of the maximum length of the honeycomb structure part in the cell extension direction from the first end face to the second end face in the central part, The plurality of cells located in the central portion and the plurality of cells located in the outer periphery together form a fluid flow path. Columnar honeycomb structure.

2. 2. The pillar-shaped honeycomb structure according to claim 1, wherein 0.7≦R2 / R1<1.

0.

3. 3. The pillar-shaped honeycomb structure according to claim 1, wherein the difference between the maximum and minimum lengths of the honeycomb structure portion in the cell extension direction from the first end face to the second end face in the central portion is 1 mm or less.

4. 3. The pillar-shaped honeycomb structure according to claim 1, wherein an opening ratio in the central portion and an opening ratio in the peripheral portion are the same.

5. 3. The pillar-shaped honeycomb structure according to claim 1, wherein the opening ratio in the central portion is 0.7 to 0.95 times the opening ratio in the peripheral portion.

6. The columnar honeycomb structure according to claim 1 or 2, an electrode terminal joined to each outer surface of the pair of electrode layers; An electrically heated carrier comprising:

7. An electrically heated carrier according to claim 6; a metal tube that houses the electrically heated carrier and that fits only with the outer circumferential wall of the electrically heated carrier; An exhaust gas purification device comprising:

Citation Information

Patent Citations

  • Honeycomb structure

    WO2015151823A1

  • Electrically heated carrier and exhaust gas purification device

    WO2021181758A1