Perfect bound booklet and manufacturing method of perfect bound booklet

By employing thermoplastic adhesive layers with varying adhesive amounts and glass transition temperatures, the method addresses uneven adhesion in perfect bound booklets, enhancing sheet adhesion and preventing peeling failure and damage.

JP2024141014APending Publication Date: 2024-10-10FUJIFILM BUSINESS INNOVATION CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023052433
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing perfect bound booklets face issues with peeling failure and damage when sheets are peeled off due to uneven adhesion, particularly at the center of the booklet, where adhesion is either too weak or too strong, leading to tearing or poor peeling.

Method used

A method involving thermoplastic adhesive layers with varying adhesive amounts and glass transition temperatures is applied to the edges of sheets, ensuring higher adhesion between sheets, especially at the center, using a patterned adhesive layer to maintain uniform adhesion across the booklet.

Benefits of technology

The method provides a perfect bound booklet with enhanced adhesion between sheets, reducing peeling failure and damage, ensuring smooth peeling without tearing, even when multiple sheets are stacked.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141014000001_ABST
    Figure 2024141014000001_ABST
Patent Text Reader

Abstract

To provide a perfect bound booklet having high adhesion between sheets and hardly causing peeling failure (tear or breakage) when the sheets are peeled off.SOLUTION: A perfect bound booklet includes: a paper group in which a plurality of papers are stacked; and a plurality of adhesive layers provided at the ends of each paper of the paper group and interposed between each paper, releasably adhering each paper and including a thermoplastic adhesive. The amount of the thermoplastic adhesive in the plurality of adhesive layers varies from a first surface side and a second surface side of the booklet toward the center of the booklet in the thickness direction, respectively.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a perfect bound booklet and a method for manufacturing a perfect bound booklet. [Background technology]

[0002] Patent Document 1 proposes a method for binding a perfect bound booklet, comprising: a paper folding step of folding each sheet of paper in half to obtain a plurality of quires; a pressing step of applying pressure to the folds of the plurality of quires in the thickness direction of the plurality of quires; a paper aligning step of stacking a single bundle of books consisting of a predetermined number of quires, a cover and a back cover, or stacking a plurality of the single bundles of books to arrange the bundles of books; a first application step of applying a layer of a first adhesive, which becomes flexible when hardened, to a middle region excluding 5 to 10 mm from both top and bottom edges of a cross section of the spine side of the single bundle of books or the bundle of books; and a second application step of leaving the first adhesive layer for a predetermined drying time and then applying a layer of a second adhesive to the entire surface of the single bundle of books including the portions where the first adhesive is not applied.

[0003] Patent Document 2 proposes a method for producing a booklet, comprising: a pressure-phase-transition particle applying step of applying pressure-phase-transition particles to at least a part of the edge and folding part of a recording medium; an adhesion step of adhering the pressure-phase-transition particles to the recording medium; and a compression step of compressing a laminate of a plurality of recording media, each of which includes the recording medium to which the pressure-phase-transition particles are adhered, wherein the pressure-phase-transition particles include a styrene-based resin containing styrene and other vinyl monomers as polymerization components, and a (meth)acrylic acid ester-based resin containing at least two (meth)acrylic acid esters as polymerization components, the mass ratio of the (meth)acrylic acid esters to the total polymerization components being 90 mass % or more, the pressure-phase-transition particles have at least two glass transition temperatures, and the difference between the lowest glass transition temperature and the highest glass transition temperature among the glass transition temperatures exhibited by the pressure-phase-transition particles is 30° C. or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2018-503817 [Patent Document 2] Patent Publication No. 2021-133617 Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to provide a perfect bound booklet having a paper group in which a plurality of papers are stacked, and a plurality of adhesive layers that are provided at the ends of each paper of the paper group and interposed between each paper, and that releasably adhere each paper, the plurality of adhesive layers including a thermoplastic adhesive, wherein the amount of thermoplastic adhesive in the plurality of adhesive layers is the same from each of the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, and which has high adhesion between the papers and is less likely to cause peeling problems (tears or breakage) when the papers are peeled off, compared to a case in which the amount of thermoplastic adhesive in the plurality of adhesive layers is the same from each of the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet. [Means for solving the problem]

[0006] Means for solving the above problems include the following aspects. <1> A paper stack having a plurality of papers stacked thereon; a plurality of adhesive layers provided at the end of each sheet of the paper stack and interposed between each sheet of the paper stack, the adhesive layers including a thermoplastic adhesive, for releasably adhering the sheets of paper to each other; having A perfect bound booklet in which the amount of the thermoplastic adhesive in the plurality of adhesive layers varies from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet. <2> Among a plurality of adhesive layers interposed between the sheets of paper, the amount of the thermoplastic adhesive in the adhesive layer interposed between the sheets of paper at the center in the thickness direction of the booklet is 1.2 to 4.0 times the amount of the thermoplastic adhesive in the adhesive layer interposed between the sheets of paper on the first surface side and the second surface side of the booklet. <1> A perfect bound booklet as described above. <3> The amount of the thermoplastic adhesive in the adhesive layer changes from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, and the difference in the amount of adhesive on one sheet of paper out of five sheets of paper is 0.18 g / m 2 That's all. <1> or <2> A perfect bound booklet as described above. <4> The adhesive layer is configured with a linear pattern, a dotted pattern, or a combination of the linear pattern and the dotted pattern of the thermoplastic adhesive. <1> ~ <3> 2. A perfect bound booklet according to any one of claims 1 to 11. <5> The amount of the thermoplastic adhesive in the plurality of adhesive layers varies from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet by changing at least one of the line width of the linear pattern and the diameter of the dot pattern of the thermoplastic adhesive. <4> A perfect bound booklet as described above. <6> The thermoplastic adhesive is a pressure-induced phase-transition adhesive containing at least two resins having different glass transition temperatures, and the difference between the lowest glass transition temperature and the highest glass transition temperature of the at least two resins is 30° C. or more. <1> ~ <5> 2. A perfect bound booklet according to any one of claims 1 to 11. <7> The paper group is a paper group in which 10 to 100 sheets of paper are stacked as the plurality of sheets of paper. <1> ~ <6> 2. A perfect bound booklet according to any one of claims 1 to 11. <8> The paper has a basis weight of 200 gsm or less. <1> ~ <7> 2. A perfect bound booklet according to any one of claims 1 to 11. <9> applying particles of the thermoplastic adhesive to the edges of the plurality of sheets; fixing the particles of thermoplastic adhesive to the paper; a bonding process in which the plurality of sheets of paper having an adhesive layer containing the thermoplastic adhesive are stacked together so that the adhesive layer is interposed between each of the sheets of paper to obtain a paper group, and then pressure and heat are applied to the adhesive layer to bond each of the sheets of paper together with the adhesive layer; have <1> ~ <8> A method for manufacturing a perfect bound booklet according to any one of claims 1 to 5. <10> The applying step is a step of applying the thermoplastic adhesive particles to the ends of the plurality of sheets of paper by an electrophotographic method. <9> A method for manufacturing the perfect bound booklet described in claim 1. <11> The pressure bonding step is a step of applying a pressure of 0.01 MPa to 1 MPa and heat of 90° C. to 220° C. to the adhesive layer from the first surface side and the second surface side of the paper stack to bond the paper sheets with the adhesive layer. <9> or <10> A method for manufacturing the perfect bound booklet described in claim 1. Effect of the Invention

[0007] <1> , <4> or <5> According to the invention, there is provided a perfect bound booklet having a paper group in which a plurality of papers are stacked, and a plurality of adhesive layers that are provided at the ends of each paper in the paper group and interposed between each paper, and that removably adhere each paper, the plurality of adhesive layers including a thermoplastic adhesive, wherein the amount of thermoplastic adhesive in the plurality of adhesive layers is the same from each of the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, and a perfect bound booklet is provided in which the adhesion between the papers is higher and peeling problems (tears or breakage) are less likely to occur when the papers are peeled off, compared to a case in which the amount of thermoplastic adhesive in the plurality of adhesive layers is the same from each of the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet.

[0008] <2> According to the invention, a perfect bound booklet is provided in which the adhesion between the sheets is higher and peeling problems (tears or breakage) are less likely to occur when the sheets are peeled off, compared to when the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets on the first and second surface sides of the booklet, among the multiple adhesive layers interposed between the sheets, is less than 1.2 times or more than 4.0 times the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets at the center in the thickness direction of the booklet. <3> According to the invention, the amount of thermoplastic adhesive in the adhesive layer changes from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, and the difference in the amount of adhesive on one sheet of paper out of five sheets is 0.18 g / m 2 This provides a perfect bound booklet in which the adhesion between the sheets is high and peeling failure (tearing or damage) is unlikely to occur when the sheets are peeled off, as compared with a case in which the adhesion is less than 100%.

[0009] <6> According to the invention, a perfect bound booklet is provided in which the thermoplastic adhesive has higher adhesion between the sheets of paper than an adhesive containing one type of resin, and which is less likely to have peeling problems (tears or breakage) when the sheets are peeled away. <7> According to the invention, a perfect bound booklet is provided in which the adhesion between the sheets of paper is high and peeling failure (tearing or damage) is less likely to occur when the sheets are peeled off, compared to a paper group in which more than 100 sheets are stacked as multiple sheets of paper. <8> According to the present invention, a perfect bound booklet is provided in which the adhesion between the sheets is higher and peeling failure (tears or breakage) is less likely to occur when the sheets are peeled off, compared to when the basis weight of the sheets exceeds 200 gsm.

[0010] <9> , <10> or <11> According to the invention, there is provided a method for manufacturing a perfect bound booklet, the method comprising the steps of: applying a pre-thermoplastic adhesive to the ends of a plurality of sheets of paper to form an adhesive layer containing a thermoplastic adhesive; and stacking the plurality of sheets of paper on which the adhesive layer containing the thermoplastic adhesive has been formed so that the adhesive layer is interposed between each sheet of paper to obtain a group of sheets of paper, and then applying pressure and heat to the adhesive layer to bond each sheet of paper with the adhesive layer. In this method, the adhesive layers are interposed between each sheet of paper, and the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets on the first surface side and the second surface side of the booklet is less than 1.2 times or more than 4.0 times the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets at the center of the booklet in the thickness direction, respectively, resulting in higher adhesion between the sheets of paper and less likely to cause peeling problems (tears or breakage) when the sheets are peeled off. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic plan view illustrating an example of a perfect bound booklet according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing an example of a perfect bound booklet according to an embodiment of the present invention. [Diagram 3] 1 is a schematic diagram showing an example of a profile of the amount of thermoplastic adhesive in a plurality of adhesive layers in a perfect bound booklet according to an embodiment of the present invention in the thickness direction of the booklet. FIG. [Figure 4] 3 is a schematic plan view showing an example of a linear pattern of a thermoplastic adhesive in a perfect bound booklet according to the present embodiment. FIG. [Diagram 5] 1 is a schematic plan view showing an example of a dot pattern of a thermoplastic adhesive in a perfect bound booklet according to the present embodiment. FIG. [Figure 6] 1 is a schematic diagram illustrating an example of a manufacturing system for a perfect bound booklet according to an embodiment of the present invention. [Figure 7] FIG. 11 is a schematic diagram showing another example of the booklet production system according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present invention will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0013] In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.

[0014] In this specification, the term "process" includes not only an independent process but also a process that is not clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0015] When an embodiment is described in this specification with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this.

[0016] In the present specification, each component may contain multiple types of the corresponding substance. When the amount of each component in the composition is mentioned in the present specification, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified.

[0017] In the present specification, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.

[0018] In this specification, the term "(meth)acrylic" means either "acrylic" or "methacrylic".

[0019] <Perfect bound booklet> The perfect bound booklet (hereinafter also referred to as "booklet") of this embodiment has a paper group in which multiple sheets of paper are stacked, and multiple adhesive layers that are provided at the ends of each sheet of the paper group and between each sheet of the paper group, releasably adhering each sheet, the multiple adhesive layers including a thermoplastic adhesive, and the amount of the thermoplastic adhesive in the multiple adhesive layers varies from the first surface side and second surface side of the booklet toward the center of the booklet in the thickness direction, respectively.

[0020] Here, a perfect bound booklet is made by forming multiple adhesive layers including a thermoplastic adhesive on the ends of each sheet of a paper group, and then applying heat and pressure to the first and second surface sides of the ends of the paper group to bond each sheet at its ends. However, it is more difficult to apply heat and pressure to the center of the paper-sheet stack (i.e., the booklet) in the thickness direction than to the first surface side and the second surface side of the paper-sheet stack (i.e., the booklet). Therefore, it is difficult to apply heat and pressure uniformly in the thickness direction of the paper stack (i.e., the booklet). As a result, the adhesive strength between the sheets of paper at the center in the thickness direction of the paper stack (i.e., the booklet) may be low. On the other hand, if the heat and pressure during adhesion are increased in order to increase the adhesive strength between the sheets of paper at the center in the thickness direction of the paper stack (i.e., the booklet), the adhesive strength between the sheets of paper at the first surface side and the second surface side of the paper stack (i.e., the booklet) may become excessively high, and peeling failure (tears or breakage) may occur when the sheets are peeled off.

[0021] In response to this, among the multiple adhesive layers interposed between the sheets of paper, the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets of paper at the center in the thickness direction of the sheet group (i.e., the booklet) is made greater than the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets of paper at the first and second surface sides of the sheet group (i.e., the booklet). This makes the adhesive strength between the sheets of paper at the center in the thickness direction of the sheet group (i.e., the booklet) due to heat and pressure during adhesion greater than the adhesive strength between the sheets of paper at the first and second surface sides of the sheet group (i.e., the booklet). This makes the adhesive strength between the sheets of paper nearly uniform between the first and second surface sides of the sheet group and the center in the thickness direction (i.e., across the thickness direction of the sheet group) even if less heat and pressure are applied to the center in the thickness direction of the sheet group (i.e., the booklet) than to the first and second surface sides of the sheet group (i.e., the booklet).

[0022] Here, the booklet obtained by bonding the edges of each sheet of the paper group together by applying heat and pressure may be used as a product as is, or may be divided into multiple pieces in the thickness direction. In other words, the booklet of this embodiment is produced as a product, and then divided, so that "the amount of thermoplastic adhesive in the multiple adhesive layers varies from the first surface side and the second surface side of the booklet toward the center of the booklet in the thickness direction."

[0023] Therefore, the booklet according to the present embodiment has high adhesion between the sheets of paper due to the above-mentioned configuration, and is a booklet in which peeling failure (tearing or damage) is unlikely to occur when the sheets are peeled off.

[0024] The booklet according to this embodiment will be described in detail below.

[0025] An example of a booklet according to this embodiment is a booklet having a paper group in which multiple sheets of paper having a rectangular planar shape are stacked on top of each other, and multiple adhesive layers that are provided at the ends of each sheet of the paper group and between each sheet of paper, releasably adhering each sheet, the multiple adhesive layers including a thermoplastic adhesive (see Figures 1 and 2). The average shape of the paper may be, for example, a polygon, a circle, or another shape (for example, a shape having a plurality of sides, the sides being straight and curved).

[0026] When rectangular, polygonal, or other shaped paper is applied, the adhesive layer is provided, for example, at the end of one side of the paper. When a circular paper is applied, the adhesive layer is provided, for example, on an end portion of the circular paper that is 1 / 2 to 1 / 6 of the circumference.

[0027] The width of the region where the adhesive layer is formed is, for example, within a range of 1 mm to 20 mm from the edge of each sheet of the booklet (see t1 in FIG. 2). However, for example, an area where no adhesive layer is provided may be provided within a range of more than 0 mm and not more than 3 mm from the edge of each sheet of the booklet (see t2 in FIG. 2). When the adhesive is formed in a pattern, the region where the adhesive layer is formed refers to the region connecting the outermost edges of the pattern located on the outside (see the region surrounded by dotted lines in Figs. 4 and 5). 1 and 2, 10 denotes a booklet, 10A denotes a first surface of the booklet, 10B denotes a second surface of the booklet, 10C denotes the center of the booklet in the thickness direction, 12 denotes a group of papers, 12A denotes paper, and 14 denotes an adhesive layer.

[0028] In the booklet according to the present embodiment, the amount of thermoplastic adhesive in the adhesive layers varies from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet. The change in the amount of thermoplastic adhesive may be either an increase or a decrease.

[0029] Here, the booklet according to this embodiment includes a booklet in which the individual sheets of paper are bonded together by adhesive layers using heat and pressure during bonding, with the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets of paper at the center of the thickness of the paper group (i.e., the booklet) being greater than the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets of paper on the first and second surface sides of the paper group (i.e., the booklet), out of the multiple adhesive layers interposed between each sheet of paper. Also includes a booklet in which the booklet is divided in the thickness direction.

[0030] Therefore, the profile of the amount of thermoplastic adhesive in the multiple adhesive layers in the thickness direction of the booklet may be, for example, as shown in FIG.

[0031] (1) An embodiment in which the amount of thermoplastic adhesive in multiple adhesive layers increases from each of the first and second surface sides of the booklet toward the center in the thickness direction of the booklet (the embodiment shown as A in Figure 3). (2) An embodiment in which the amount of thermoplastic adhesive in the multiple adhesive layers increases from the first surface side to the second surface side of the booklet (in FIG. 3, the embodiment shown as B1 divided by B in the embodiment (1), and the embodiment shown as C1 divided by C). (3) An embodiment in which the amount of thermoplastic adhesive in the multiple adhesive layers increases from the second surface side toward the first surface side of the booklet (in the embodiment (1) in Figure 3, the embodiment shown as B2 divided by B, and the embodiment shown as D2 divided by D). (4) An embodiment in which the amount of thermoplastic adhesive in a plurality of adhesive layers increases from the first surface side and the second surface side of the booklet toward any position in the thickness direction of the booklet except the center of the booklet in the thickness direction (the embodiment shown in C2 divided by C in the embodiment (1) in FIG. 3, and the embodiment shown in D1 divided by D).

[0032] Among the above embodiments, the embodiment (1) is preferable because it has a large number of sheets in the booklet. Here, the amount of thermoplastic adhesive in the multiple adhesive layers may be changed for each sheet of paper, or may be changed for multiple sheets (for example, 4 to 6 sheets).

[0033] Of the multiple adhesive layers interposed between the sheets of paper, the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets of paper at the center of the thickness of the booklet is preferably 1.2 to 4.0 times, and more preferably 1.7 to 2.3 times, the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets of paper on the first and second surface sides of the booklet. By setting the amount of thermoplastic adhesive in the adhesive layer between the sheets at the center of the thickness of the booklet within the above range, the adhesive strength between the sheets is easily made uniform while ensuring the adhesive strength between the first and second surface sides and the center of the thickness of the booklet. As a result, the adhesive strength between the sheets is high, and peeling failure (tears or breakage) is unlikely to occur when the sheets are peeled off.

[0034] The amount of thermoplastic adhesive in the adhesive layer between the sheets on the first and second surface sides of the booklet is 2 ) per 0.4g / m 2 More than 1.5g / m 2 Less than 0.6 g / m is preferred. 2 More than 1.0g / m 2 The following is more preferred:

[0035] The amount of thermoplastic adhesive in the adhesive layer interposed between the sheets of paper on the first and second surface sides of the booklet, and the ratio of the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets of paper at the center of the booklet in the thickness direction are measured, for example, as follows. Ten booklets made under the same conditions are prepared, and one sheet of paper is taken out from each booklet from the first surface, the second surface, and the center in the thickness direction. The ten sheets of paper taken out from the same place are put together, and the weight of the ten sheets of paper at each place is measured. The weight of the paper without glue is subtracted from the weight, and the amount of adhesive at each place is calculated. Then, the ratio of the amount of adhesive on the 10 sheets of paper at the center in the thickness direction to the amount of adhesive on each of the 10 sheets of paper on the first surface and the second surface is calculated, and this ratio is defined as "the ratio of the amount of thermoplastic adhesive in the adhesive layer between the sheets of paper at the center in the thickness direction of the booklet to the amount of thermoplastic adhesive in the adhesive layer between the sheets of paper on the first surface side and the second surface side of the booklet." In addition, the unit area (m2) was calculated from the amount of adhesive on the first and second surfaces of each of the 10 sheets of paper and the total area of ​​the adhesive layer formation region of each of the 10 sheets of paper. 2 ) to determine the amount of adhesive on the first surface side and the second surface side.

[0036] The amount of thermoplastic adhesive in the adhesive layer changes from the first surface side and the second surface side of the booklet toward the center of the booklet in the thickness direction, and the difference in the amount of adhesive on one sheet per five sheets (hereinafter also referred to as the "adhesive change amount") is 0.18 g / m 2 More than 0.27 g / m is preferable. 2 More preferably, 0.36 g / m or more is preferable. 2 The above is even more preferable. By setting the change in the adhesive within the above range, the adhesive strength between the sheets is easily made uniform while ensuring the adhesive strength on the first and second surface sides and at the center in the thickness direction of the booklet. As a result, the adhesive strength between the sheets is high and peeling failure (tears or breakage) is unlikely to occur when the sheets are peeled off. However, from the viewpoint of uniformity of the force required for peeling, the change in adhesive force is, for example, 0.54 g / m 2 The following applies. Here, the difference in the amount of adhesive on one sheet of paper out of every five sheets of paper refers to the difference (absolute value) between the amount of adhesive on the Nth sheet of paper (e.g., the first sheet) peeled off and the amount of adhesive on the N+5th sheet of paper (e.g., the sixth sheet) peeled off when the sheets are peeled off.

[0037] The amount of change in the adhesive is measured, for example, as follows. Ten booklets made under the same conditions are prepared, and one sheet of paper is taken out from the first surface of the booklet to be measured. The ten sheets of paper taken out from the same place are put together, and the weight of the ten sheets of paper at each part is measured. This operation is carried out for every 5 sheets from the first surface to the second surface of the booklet, and the weight of the 10 sheets of paper at each location (i.e., the Nth sheet and the N+5th sheet) is calculated. The weight of the paper that does not have glue applied is subtracted from this to calculate the amount of adhesive at each location, and the amount of adhesive per unit of the adhesive layer is obtained from the area of ​​the adhesive layer formation region. Then, from the amount of adhesive per unit of the adhesive layer at each location, the difference in the amount of adhesive for one sheet of paper out of every 5 sheets of paper is calculated and the arithmetic average is taken.

[0038] The adhesive layer is preferably composed of a line pattern (see FIG. 4), a dot pattern (see FIG. 5), or a combination of line and dot patterns of a thermoplastic adhesive. The linear pattern of the thermoplastic adhesive may be, for example, a diagonal line pattern or a lattice line pattern. The dot pattern of the thermoplastic adhesive may be a circle, a polygon, a star, or the like dot pattern. 4 and 5, 14 denotes an adhesive layer, and 14A denotes a pattern of a thermoplastic adhesive.

[0039] Furthermore, it is preferable that the amount of thermoplastic adhesive in the multiple adhesive layers changes from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet due to a change in at least one of the line width of the linear pattern and the diameter of the dot pattern of the thermoplastic adhesive (see Figures 4 to 5). The adhesive layer is configured with a linear pattern, a dotted pattern, or a combination of a linear pattern and a dotted pattern of thermoplastic adhesive, making it easier to control the amount of change in the amount of thermoplastic adhesive in the multiple adhesive layers.

[0040] In addition to the pattern of the thermoplastic adhesive (i.e., the area of ​​the region where the adhesive is present), the amount of thermoplastic adhesive in the multiple adhesive layers may be changed by changing the thickness of the thermoplastic adhesive (i.e., the adhesive layer). In other words, by changing the thickness of the thermoplastic adhesive (i.e., the adhesive layer), the amount of thermoplastic adhesive in the multiple adhesive layers may be changed from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet.

[0041] Examples of the paper include coated paper, uncoated paper (ie, plain paper), and embossed paper. However, the basis weight of the paper is preferably 200 gsm or less, and more preferably 130 gsm or less. When the basis weight of the paper is within the above range, the heat and pressure applied to the paper stack during booklet production can be applied sufficiently to the center of the paper stack in the thickness direction. As a result, the adhesion between the sheets is high, and peeling failure (tears or breakage) is unlikely to occur when the sheets are peeled off. In order to ensure the strength of the paper, the basis weight of the paper is set to, for example, 50 gsm or more.

[0042] The basis weight of the paper is the value measured in accordance with JIS P8124:2011 for paper that has been left at 23°C and 50% RH for 24 hours.

[0043] The paper set (that is, the booklet) is preferably a paper set in which 10 to 100 sheets are stacked as a plurality of sheets, and more preferably 10 to 50 sheets. When the number of sheets in the paper stack (i.e., the booklet) is within the above range, the heat and pressure applied to the paper stack during booklet production can be applied sufficiently to the center of the paper stack in the thickness direction. As a result, the adhesion between the sheets is high, and peeling failure (tears or breakage) is unlikely to occur when the sheets are peeled off.

[0044] The booklet according to this embodiment is used by peeling the paper from the booklet (i.e., from the other paper directly underneath that is adhered with the adhesive layer). When the paper is peeled off, it is preferable that the adhesive layer is attached to the side of the paper that is peeled off. In other words, when the paper is peeled off, it is preferable that the paper is peeled off at the interface between the adhesive layer and the other paper directly underneath. When the paper is peeled off, the adhesive layer may remain on the side of the other paper directly below, or the adhesive layer may be divided in the thickness direction and attached to both the side of the paper being peeled off and the side of the other paper directly below.

[0045] <Manufacturing method of perfect bound booklets> The method for producing a perfect bound booklet according to the present embodiment is as follows: applying particles of a thermoplastic adhesive (hereinafter also referred to as "adhesive particles") to the ends of the plurality of sheets of paper; Fixing the adhesive particles to the paper; a bonding step in which a plurality of sheets of paper having an adhesive layer containing a thermoplastic adhesive are stacked together so that the adhesive layer is interposed between each sheet of paper to obtain a sheet group, and then pressure and heat are applied to the adhesive layer to bond each sheet of paper to the adhesive layer; has. In the manufacturing method of a perfect bound booklet according to this embodiment, the perfect bound booklet according to this embodiment is obtained through the above steps.

[0046] Here, in the manufacturing method for a perfect bound booklet according to this embodiment, in the application process, of the multiple adhesive layers interposed between each sheet of paper, the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets at the center in the thickness direction of the paper group (i.e., the booklet) is made greater than the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets on the first surface side and the second surface side of the paper group (i.e., the booklet).

[0047] In the manufacturing method of the perfect bound booklet according to the present embodiment,

[0048] The booklet manufacturing method according to this embodiment is performed by a booklet manufacturing system according to this embodiment, which will be described below. The booklet manufacturing system according to the present embodiment includes: an application section that stores adhesive particles and applies the adhesive particles to the ends of the plurality of sheets of paper; a fixing portion for fixing the adhesive particles to the paper; a bonding section that obtains a paper group by stacking a plurality of papers each having an adhesive layer containing a thermoplastic adhesive such that the adhesive layer is interposed between each of the papers, and then applies pressure and heat to the adhesive layer to bond each of the papers together with the adhesive layer; Equipped with.

[0049] Hereinafter, each step of the booklet manufacturing method according to this embodiment will be described together with each means of the booklet manufacturing system according to this embodiment.

[0050] <Application step and application unit> In the application step, the adhesive particles are applied to the edge of the paper by the application unit. The details of the adhesive particles will be described later. The adhesive particle application means in the application section is not particularly limited, and may be any means capable of applying adhesive particles in a desired amount and at a desired application position on the surface of the paper. Specifically, the adhesive particle application means may be a spraying method in which adhesive particles are sprayed, a coating method in which adhesive particles are applied, or an electrophotographic method in which adhesive particles are used as toner.

[0051] (Position where adhesive particles are applied) The adhesive particles are applied to the edges of the paper on at least one side of the paper. The adhesive particles are preferably applied to the edges of the paper on both sides of the paper in order to increase adhesive strength.

[0052] (Adhesive particle application state) The state in which the adhesive particles are applied may be such that the particle shape is retained, or the adhesive particles may be aggregated to form a layer, with a layered state being preferred from the viewpoint of obtaining sufficient peel strength (or adhesion by compression). The adhesive layer formed by the adhesive particles may be a continuous layer or a discontinuous layer.

[0053] The amount of adhesive particles applied is set to 0.5 g / m from the viewpoint of obtaining sufficient adhesive strength through pressure bonding. 2 More than 8.0g / m 2 Preferably, the content is 1.0 g / m or less. 2 More than 6.0g / m 2 More preferably, it is 1.5 g / m or less. 2 More than 5.0g / m 2 It is even more preferable that:

[0054] (Addition of adhesive particles) The method of applying the adhesive particles is not particularly limited as long as the adhesive particles are applied to the desired application position, and specifically, a spraying method in which the adhesive particles are sprayed, a coating method in which the adhesive particles are applied, an electrophotographic method in which the adhesive particles are used as toner, etc. may be used. The adhesive particles may be applied directly to the adhesive layer forming area of ​​the paper by dropping or by roll coating. Examples of adhesive particle application means in the application section that applies adhesive particles onto paper include a particle application device that uses a spraying method to spray adhesive particles, a particle application device that uses a coating method to apply adhesive particles, and a particle application device that uses an electrophotographic method in which adhesive particles are used as toner.

[0055] The application process by spraying includes, for example, a step of preparing a dispersion liquid in which adhesive particles are dispersed, a step of spraying the dispersion liquid onto paper, and a step of drying the dispersion liquid sprayed onto the paper. The spray application unit includes, for example, a spraying unit that sprays a dispersion liquid in which adhesive particles are dispersed onto the paper, and a drying unit that dries the dispersion liquid sprayed onto the paper. The blowing means may be, for example, a spray, etc. The drying means may be, for example, a hot air blower, a near infrared heater, a laser irradiation device, etc.

[0056] The application step by the coating method may, for example, include a step of applying adhesive particles to paper. In the coating method, a coating liquid in which the adhesive particles are dispersed may be used. The application step by the coating method using a coating liquid may, for example, include a step of preparing a coating liquid in which the adhesive particles are dispersed, a step of applying the coating liquid to paper, and a step of drying the coating liquid applied to the paper. The application unit using a coating method may include, for example, a coating unit that applies adhesive particles to the paper. The application unit using a coating liquid may include, for example, a coating unit that applies the coating liquid to the paper, and a drying unit that dries the coating liquid applied to the paper. The coating means may be, for example, a roll.

[0057] The application process using the electrophotographic method includes, for example, a charging process for charging the surface of an image holder, an electrostatic image forming process for forming an electrostatic image on the charged surface of the image holder, a developing process for developing the electrostatic image formed on the surface of the image holder as an adhesive particle region using an electrostatic image developer containing adhesive particles, and a transfer process for transferring the adhesive particle region formed on the surface of the image holder to the surface of paper. In addition, the electrophotographic application unit includes, for example, an image holder, a charging means for charging the surface of the image holder, an electrostatic image forming means for forming an electrostatic image on the charged surface of the image holder, a developing means for containing an electrostatic image developer containing adhesive particles and developing the electrostatic image formed on the surface of the image holder as an adhesive particle area using the electrostatic image developer, and a transfer means for transferring the adhesive particle area formed on the surface of the image holder to the surface of a sheet of paper.

[0058] The electrophotographic application section may have a cartridge structure (so-called process cartridge) in which a section including a developing means is detachably attached to a particle application device. As the process cartridge, for example, a process cartridge that includes a developing means that contains an electrostatic charge image developer including adhesive particles and is detachably attached to a particle application device is preferably used. The electrophotographic application method and application unit may both use an electrophotographic image forming method and image forming apparatus, and may use known processes and means employed in the electrophotographic image forming method and image forming apparatus. The electrophotographic application method and application unit may employ an intermediate transfer method, in which, for example, an adhesive particle region formed on the surface of an image carrier is first transferred to the surface of an intermediate transfer body, and then finally transferred from the surface of the intermediate transfer body to the surface of a sheet of paper. Furthermore, the electrophotographic application method and application unit may include means and steps other than those described above, such as a step and means for cleaning the surface of the image carrier, or an apparatus equipped with a discharging means for irradiating the surface of the image carrier with discharging light to dissipate electricity.

[0059] When using paper on which an image has been formed, the adhesive particles may be applied to paper on which an image has been formed in advance, or the image forming step of forming an image on the paper and the application step may be carried out consecutively. Examples of the method of continuously performing the image forming step and the application step include a method of performing the application step after the image forming step using an inkjet recording method, a method of performing both the image forming step and the application step by an electrophotographic method, etc. Specifically, for example, there is a method of forming a composite image on the surface of a paper using both a color material for image formation (preferably a colored ink) in the image forming step and adhesive particles in the application step.

[0060] <Fixing process and fixing part> In the fixing step, for example, the adhesive particles applied to the paper are heated by a fixing unit. The means for heating the adhesive particles (particle heating means) is not particularly limited as long as it is a means capable of heating the adhesive particles applied onto the paper. The means for heating the adhesive particles (particle heating means) may be of a contact type or a non-contact type. Examples of the contact type particle heating means include a method in which a member such as a roll, belt, or pad is heated and the heated member is brought into contact with the adhesive particles. Non-contact particle heating means include, for example, a method in which paper to which adhesive particles have been applied is passed through an area heated by a heater or oven, or a method in which the adhesive particles are heated by irradiation light from a halogen lamp, xenon lamp, etc.

[0061] Among these, the fixing step preferably uses a contact type particle heating means from the viewpoint of being able to heat the adhesive particles and to suppress the movement, falling off, etc. of the adhesive particles. That is, the particle heating means is preferably a contact type particle heating means.

[0062] (Contact heating of adhesive particles) When the adhesive particles are heated by the contact method, the pressure applied to the paper group P2 by a member that contacts the adhesive particles (also called a contact member) is preferably 0.01 Mpa or more and 1 Mpa or less. When heating adhesive particles using a contact method, the set temperature of the member (also called the contact member) that comes into contact with the adhesive particles may be any temperature that can plasticize the adhesive particles, but from the standpoint of the heating efficiency of the adhesive particles, it is preferable that the set temperature be, for example, 120°C or higher and 250°C or lower. Here, the set temperature of the contact member refers to a target value of the surface temperature of the contact member that comes into contact with the adhesive particles. The contact member is not particularly limited as long as it has a surface heated to the above-mentioned set temperature, and examples thereof include a roll, a belt, a pad, and the like.

[0063] The fixing step is preferably a step of applying heat and pressure to the adhesive particles. By heating and pressurizing the adhesive particles, smoothness can be imparted to the surface to which the adhesive particles are applied (for example, the surface of the adhesive particle layer). The pressure applied to the adhesive particles in the fixing step may be, for example, a pressure applied by a fixing means in an electrophotographic system.

[0064] Examples of the means for heating and pressurizing the adhesive particles (also called a heating and pressurizing member) include the following. That is, examples of such devices include a heating and pressure roll pair consisting of two contacting rolls in which heat is applied from at least one of the rolls and the paper to which adhesive particles have been applied is passed between the pair of rolls to apply heat and pressure; a heating and pressure member consisting of a roll and a belt in contact with each other and in which heat is applied from at least one of the roll and the belt and the paper to which adhesive particles have been applied is passed between these members to apply heat and pressure; a heating and pressure belt pair consisting of two contacting belt pairs in which heat is applied from at least one of the belts and the paper to which adhesive particles have been applied is passed between the pair of belts to apply heat and pressure; and the like.

[0065] <Crimping process and crimping section> In the bonding process, the multiple sheets of paper each having an adhesive layer containing the thermoplastic adhesive formed thereon are stacked together so that the adhesive layer is interposed between each sheet of paper to obtain a group of sheets of paper, and then pressure and heat are applied to the adhesive layer to bond each sheet of paper to the adhesive layer.

[0066] The pressurization of the paper stack may be performed only on the end of the paper stack where the adhesive layer is formed, or may be performed on the entire paper stack. There are no particular limitations on the means for pressurizing the paper stack (paper stack pressurizing means), and any means capable of pressurizing the paper stack in the thickness direction may be used. For example, the means may be a means for passing the paper stack between a pair of spaced rolls, or a means for pressing the paper stack using a press, sealer, stapler, etc.

[0067] The paper group pressurizing means may be a commercially available device, such as PRESSLE LEADA, PRESSLE CORE, and PRESSLE Bee manufactured by Toppan Forms Co., Ltd., and PS-500H, PS-500, EX-4100WI, EX-4100W, EX-4100 / 4150, and PS-100 manufactured by Duplo Seiko Co., Ltd.

[0068] In the pressing process, it is preferable to apply a pressure of 0.01 MPa to 1 MPa (preferably 0.1 MPa to 0.5 MPa) and heat of 90°C to 220°C to the adhesive layer from the first surface side and the second surface side of the paper stack, thereby pressing each paper sheet with the adhesive layer. The pressure is the maximum pressure applied in the thickness direction of the paper stack, and the heat temperature is the surface temperature of the member that applies pressure and heat. By bonding each sheet of paper with the adhesive layer under the above conditions, the adhesive strength between the sheets of paper is easily made uniform while ensuring the adhesive strength between the first and second surfaces of the booklet and at the center in the thickness direction. As a result, the adhesive strength between the sheets of paper is high and peeling failure (tears or breakage) is unlikely to occur when the sheets are peeled off. The pressing pressure is measured using a commercially available pressure measuring film. A specific example of the pressure measuring film is the pressure measuring film Prescale manufactured by Fujifilm Corp. The maximum pressure refers to the maximum value of the change in pressure while pressure is being applied to the paper stack by the pressure applying means.

[0069] The booklet manufacturing method according to the present embodiment may include other steps in addition to the applying step, the fixing step, and the pressure bonding step. Examples of other steps include a step of cutting the paper stack after the fixing step or the booklet after the pressing step to a desired size, and a step of dividing the booklet after the pressing step in the thickness direction.

[0070] <Example of manufacturing system and manufacturing method> An example of a booklet manufacturing system according to the present embodiment will be shown below, and a booklet manufacturing method according to the present embodiment will be described, but the present embodiment is not limited to this.

[0071] 6 is a schematic diagram showing an example of a booklet production system according to the present embodiment. The booklet production system shown in FIG. 6 includes a placement unit 150 and a pressing unit 200 disposed downstream of the placement unit 150. The placing means 150 has an application section for storing adhesive particles and applying the adhesive particles to the edge of the paper, and a fixing section for fixing the adhesive particles to the paper. The bonding means 200 includes a bonding section that overlaps a plurality of papers having an adhesive layer containing fixed adhesive particles so that the adhesive layer is interposed between each paper to form a group of papers, and applies pressure and heat to the adhesive layer to bond each paper with the adhesive layer. In FIG. 6, the arrow indicates the paper transport direction.

[0072] The placement means 150 is a device that uses a coating method to place and fix adhesive particles on the paper P. The paper P may have an image formed in advance on one or both sides, for example.

[0073] The placement means 150 has a particle applicator 518 that applies adhesive particles 516 to the surface of the paper P as an example of an applicator that applies adhesive particles to the edge of the paper.

[0074] The particle applying device 518 is a device that supplies adhesive particles 516 onto the surface of the paper P to form an adhesive particle area 516A on the surface of the paper P. The particle applicator 518 is provided with a supply roll 518A in a portion facing the paper P, and supplies the adhesive particles 516 only to a corresponding application area. In the particle applicator 518, the adhesive particles 516 are supplied to the supply roll 518A, and the amount of the adhesive particles 516 supplied to the supply roll 518A (i.e., the layer thickness when the adhesive particles 516 are supplied in a layer on the paper P) is adjusted.

[0075] The fixing device 564 includes a heating roll 564A incorporating a heat source, and a pressure roll 564B disposed opposite to the heating roll 564A.

[0076] The placement means 150 further includes a paper storage section (not shown) for storing paper P, a transport section (not shown) for transporting paper P stored in the paper storage section, a fixing device 564 for fixing the adhesive particles 516 applied to the paper P to the paper P, and a paper discharge section (not shown) from which the paper P to which the adhesive particles 516 have been fixed by the fixing device 564 is discharged.

[0077] The operation of the placing means 150 for placing and fixing the adhesive particles on the paper P will now be described. When the paper P is transported from the paper storage section by the transport section and reaches the position of the particle applicator 518, the particle applicator 518 applies adhesive particles 516 onto the paper P, forming an adhesive particle area 516A.

[0078] The paper P on which the adhesive particle region 516A has been formed is then transported to a fixing device 564 (an example of a fixing unit). Then, the fixing device 564 applies heat and pressure to the paper P, thereby fixing the adhesive particles to the paper P.

[0079] The paper P becomes a post-adhesive paper P1 having adhesive particles fixed to its edge by passing through the placement means 150. The post-adhesive paper P1 is transported towards the pressure bonding means 200.

[0080] In the booklet manufacturing system according to the present embodiment, the arrangement unit 150 and the pressing unit 200 may be in close proximity to each other or may be spaced apart from each other. When the arrangement unit 150 and the pressing unit 200 are spaced apart from each other, the arrangement unit 150 and the pressing unit 200 are connected to each other by, for example, a conveying unit (for example, a belt conveyor) that conveys the paper P1 after application.

[0081] The pressing means 200 includes a paper-sheet group forming device 220 and a pressure device 230, and is a means for pressing a paper-sheet group P2 in which paper sheets P1 are piled up after application.

[0082] The paper-sheet group forming device 220 creates a paper-sheet group P2 by stacking a plurality of post-adhesive paper sheets P1, which have passed through the device and have adhesive particles applied to their edges. The paper-sheet group P2 leaving the paper-sheet group forming device 220 is transported towards the pressure device 230.

[0083] The pressure device 230 includes a pair of pressure members (i.e., pressure rolls 231 and 232). The pressure rolls 231 and 232 come into contact with each other at their outer circumferential surfaces and push against each other to apply pressure to the passing paper group P2. The pair of pressure members included in the pressure device 230 is not limited to a combination of a pressure roll and a pressure roll, and may also be a combination of a pressure roll and a pressure belt, or a combination of a pressure belt and a pressure belt.

[0084] When pressure is applied to the paper stack P2 passing through the pressure device 230, the adhesive particles on the paper stack P2 become fluid due to the pressure and exhibit adhesive properties. The pressure device 230 has a heat source (for example, a halogen heater) (not shown) and heats the paper stack P2 when heated by the heat source.

[0085] As the group of sheets P2 passes through the pressure device 230, the overlapping surfaces are bonded together by fluidized adhesive particles to produce booklet P3.

[0086] The completed booklet P3 is conveyed out of the pressure device 230.

[0087] In the booklet manufacturing system according to this embodiment, the paper sheet group forming device 220 and the pressure device 230 may be in close proximity to each other or may be spaced apart. When the paper sheet group forming device 220 and the pressure device 230 are spaced apart, the paper sheet group forming device 220 and the pressure device 230 are connected by, for example, a conveying means (for example, a belt conveyor) that conveys the paper sheet group P2.

[0088] 7 is a schematic diagram showing another example of the booklet manufacturing system according to the present embodiment. The booklet manufacturing system shown in FIG. 7 includes a placement unit 100 and a pressing unit 200 disposed downstream of the placement unit 100. The placing means 100 has an application section that stores adhesive particles and applies the adhesive particles to the edge of the paper, and a fixing section that fixes the adhesive particles to the paper. The bonding means 200 includes a bonding section that overlaps a plurality of papers having an adhesive layer containing fixed adhesive particles so that the adhesive layer is interposed between each paper to form a group of papers, and applies pressure and heat to the adhesive layer to bond each paper with the adhesive layer. In FIG. 7, the arrows indicate the rotation direction of the photoconductor or the transport direction of the paper.

[0089] The placement means 100 is a direct transfer type device that uses a developer containing adhesive particles to place adhesive particles on the paper P by an electrophotographic method. The paper P may have an image formed in advance on one or both sides, for example.

[0090] The arrangement means 100 has a photoconductor 101. Around the photoconductor 101, there are sequentially arranged a charging roll (an example of a charging means) 102 that charges the surface of the photoconductor 101, an exposure device (an example of an electrostatic image forming means) 103 that exposes the charged surface of the photoconductor 101 to a laser beam to form an electrostatic image, a development device (an example of a development means) 104 that supplies adhesive particles to the electrostatic image to develop the electrostatic image and form an adhesive particle region, a transfer roll (an example of a transfer means) 105 that transfers the adhesive particle region formed by development onto paper P, and a photoconductor cleaning device (an example of a cleaning means) 106 that removes adhesive particles remaining on the surface of the photoconductor 101 after transfer.

[0091] The placement means 100 is provided with a fixing device 107 for fixing adhesive particles to the paper P. The fixing device 107 has, for example, a pair of fixing members (roll / roll, belt / roll). The fixing device 107 also has a heat source for heating the paper P (for example, a halogen heater).

[0092] The operation of the placing means 100 for placing and fixing the adhesive particles on the paper P will now be described. First, the surface of the photoconductor 101 is charged by the charging roll 102. The exposure device 103 irradiates the charged surface of the photoconductor 101 with a laser beam in accordance with image data sent from a control unit (not shown). As a result, an electrostatic charge image of the arrangement pattern of the adhesive particles is formed on the surface of the photoconductor 101.

[0093] The electrostatic image formed on the photoconductor 101 rotates to a development position as the photoconductor 101 travels. At the development position, the electrostatic image on the photoconductor 101 is developed by a developing device 104 and visualized to become an adhesive particle area.

[0094] The developing device 104 contains a developer containing at least adhesive particles and a carrier. The adhesive particles are triboelectrically charged by being stirred together with the carrier inside the developing device 104, and are held on a developer roll. As the surface of the photoconductor 101 passes through the developing device 104, the adhesive particles electrostatically adhere to the electrostatic charge image on the surface of the photoconductor 101, and the electrostatic charge image is developed by the adhesive particles to form an adhesive particle area. The photoconductor 101 with the adhesive particle area formed thereon continues to travel, and the adhesive particle area formed on the photoconductor 101 is transported to a transfer position.

[0095] When the adhesive particle area on the photoreceptor 101 is transported to the transfer position, a transfer bias is applied to the transfer roll 105, and an electrostatic force from the photoreceptor 101 to the transfer roll 105 acts on the adhesive particle area, causing the adhesive particle area on the photoreceptor 101 to be transferred onto the paper P.

[0096] The adhesive particles remaining on the photoreceptor 101 are removed and collected by the photoreceptor cleaning device 106. The photoreceptor cleaning device 106 is, for example, a cleaning blade, a cleaning brush, etc. The photoreceptor cleaning device 106 is preferably a cleaning brush from the viewpoint of suppressing the phenomenon in which the adhesive particles remaining on the surface of the photoreceptor are fluidized by pressure and adhere to the surface of the photoreceptor in the form of a film.

[0097] The paper P to which the adhesive particle regions have been transferred is transported to a fixing device (an example of a fixing unit) 107. Then, the fixing device 107 applies heat and pressure to the paper P, so that the adhesive particles are fixed to the paper P.

[0098] The paper P becomes a post-adhesive paper P1 having adhesive particles fixed to its edge by passing through the arrangement means 100. The post-adhesive paper P1 is transported toward the pressing means 200. As the pressing means 200 in the booklet production system shown in Fig. 7, a pressing means similar to the pressing means 200 in the booklet production system shown in Fig. 6 is used.

[0099] In the booklet manufacturing system according to the present embodiment, the arrangement means 100 and the pressing means 200 may be in close proximity to each other or may be spaced apart from each other. When the arrangement means 100 and the pressing means 200 are spaced apart from each other, the arrangement means 100 and the pressing means 200 are connected to each other by, for example, a conveying means (for example, a belt conveyor) that conveys the paper P1 after application.

[0100] The booklet manufacturing system according to the present embodiment may include a cutting means for cutting the paper to a predetermined size. The cutting means may be, for example, a cutting means arranged between the arrangement means and the pressing means for cutting off a part of the paper after application, a cutting means arranged between the paper group forming device and the pressure device for cutting off a part of the paper group, or a cutting means arranged downstream of the pressing means for cutting off a part of the booklet. The booklet manufacturing system according to the present embodiment may further include a dividing means arranged downstream of the pressing means for dividing the booklet in the thickness direction.

[0101] The booklet manufacturing system according to the present embodiment is not limited to a sheet-fed type device. The booklet manufacturing device according to the present embodiment may be a device that performs a placement process and a pressing process on long sheets to form a long booklet, and then cuts the long booklet to a predetermined size.

[0102] The booklet manufacturing system according to the present embodiment may further include a color image forming unit that forms a color image on paper using a colored coloring material. Examples of the color image forming unit include a unit that forms a color ink image on paper by an inkjet method using colored ink, and a unit that forms a color toner image on paper by an electrophotographic method using a colored electrostatic image developer.

[0103] The inkjet type color image forming means includes a liquid ejection head that ejects liquid, for example, ink. The inkjet type color image forming means may be of a direct ejection type in which the liquid ejection head ejects liquid directly onto paper, or of an intermediate transfer type in which the liquid ejection head ejects liquid onto an intermediate transfer body and transfers the liquid ejected onto the intermediate transfer body onto paper.

[0104] The electrophotographic color image forming means is, for example, A photoconductor; A charging means for charging the surface of the photoreceptor; an electrostatic image forming means for forming an electrostatic image on the charged surface of the photoreceptor; a developing means for storing a color electrostatic image developer and developing the electrostatic image formed on the surface of the photoconductor into a color toner image by the color electrostatic image developer; a transfer means for transferring the color toner image formed on the surface of the photoreceptor to a surface of a sheet of paper; and a heat fixing means for heat fixing the color toner image transferred onto the surface of the paper.

[0105] The manufacturing system having the above-described configuration implements a method for manufacturing a booklet according to the present embodiment, which further includes a color image forming process for forming a color image on paper using a colored coloring material. Specific examples of the color image forming process include a process for forming a color ink image on paper by an inkjet method using colored inks, and a process for forming a color toner image on paper by an electrophotographic method using a colored electrostatic image developer.

[0106] The color image forming process using the inkjet method includes, for example, a liquid ejection process of ejecting a liquid such as ink. The color image forming process using the inkjet method may be a direct ejection method in which the liquid is ejected directly onto a recording medium, or an intermediate transfer method in which the liquid is ejected onto an intermediate transfer body and the liquid ejected onto the intermediate transfer body is transferred onto paper.

[0107] The color image forming process using the electrophotographic method is, for example, a charging step of charging the surface of the photoconductor; an electrostatic image forming step of forming an electrostatic image on the charged surface of the photoreceptor; a developing step of developing the electrostatic image formed on the surface of the photoconductor into a color toner image by a color electrostatic image developer; a transfer step of transferring the color toner image formed on the surface of the photoreceptor onto a surface of a sheet of paper; and a heat fixing step of heat fixing the color toner image transferred onto the surface of the paper.

[0108] The color image forming means included in the booklet manufacturing system according to the present embodiment is, for example, a direct type device that forms a color image directly on a sheet of paper; an intermediate transfer type device that forms a color image on the surface of an intermediate transfer body and transfers the color image formed on the surface of the intermediate transfer body to the surface of a sheet of paper; a device equipped with a cleaning means that cleans the surface of a photoconductor before charging after the transfer of the color image when the color image is a color toner image; a device equipped with a discharging means that irradiates the surface of the photoconductor with discharging light to discharge the surface of the photoconductor before charging after the transfer of the color image when the color image is a color toner image. When the electrophotographic color image forming means is an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body on whose surface a color toner image is transferred, a primary transfer means that primarily transfers the color toner image formed on the surface of the photoconductor to the surface of the intermediate transfer body, and a secondary transfer means that secondarily transfers the color toner image transferred to the surface of the intermediate transfer body to the surface of a sheet of paper.

[0109] In the booklet manufacturing system according to this embodiment, if the adhesive particle placement means and the color image forming means adopt an intermediate transfer method, the placement means and the color image forming means may share the intermediate transfer body and transfer means.

[0110] In the booklet manufacturing system of this embodiment, when the color image forming means has a fixing device for adhering colored colorant to paper, the fixing device in the adhesive particle placement means and the fixing device in the color image forming means may share a single fixing device.

[0111] <Thermoplastic adhesive> Thermoplastic adhesives are applied which become plastic when heated. In particular, the thermoplastic adhesive is preferably a pressure phase transition adhesive. A pressure phase transition adhesive can bond by applying pressure together with heat, and the adhesive strength between the sheets is easily uniform while ensuring adhesive strength on the first and second surface sides and the center in the thickness direction of the booklet. As a result, the adhesive strength between the sheets is high, and peeling failure (tears or breakage) is unlikely to occur when the sheets are peeled off.

[0112] The pressure phase transition adhesive is an adhesive that undergoes a phase transition due to pressure, and specifically means an adhesive that satisfies the following formula 1. Formula 1...10℃≦T1-T2 In formula 1, T1 is the temperature at which the viscosity is 10,000 Pa s under a pressure of 1 MPa, and T2 is the temperature at which the viscosity is 10,000 Pa s under a pressure of 10 MPa. How to determine temperatures T1 and T2 will be described later.

[0113] Specifically, the thermoplastic adhesive preferably contains at least two types of resins having different glass transition temperatures, and is a pressure-induced phase transition adhesive in which the difference between the lowest and highest glass transition temperatures of the at least two types of resins is 30°C or more. By applying a pressure-sensitive phase transition adhesive having the above characteristics, the adhesive strength between the sheets of paper is easily made uniform while ensuring adhesive strength on the first and second surface sides and at the center in the thickness direction of the booklet. As a result, the adhesive strength between the sheets of paper is high and peeling failure (tears or breakage) is unlikely to occur when the sheets are peeled off.

[0114] An example of a pressure-induced phase transition adhesive having the above-described characteristics is an adhesive containing a styrene-based resin containing styrene and other vinyl monomers as polymerization components, and a (meth)acrylic acid ester-based resin containing at least two types of (meth)acrylic acid esters as polymerization components, with the mass proportion of (meth)acrylic acid esters in the total polymerization components being 90 mass% or more.

[0115] The thermoplastic adhesive will be described in detail below. In the following description, adhesive particles for forming an adhesive layer containing a thermoplastic adhesive (hereinafter, also referred to as "adhesive particles according to this embodiment") will be described. The composition and characteristics of the adhesive particles are the same as those of the adhesive.

[0116] The adhesive particles according to this embodiment contain at least base particles, and optionally contain an external additive. [Mother particle] (Binding resin) The base particles preferably contain, as binder resins, a styrene-based resin containing styrene and other vinyl monomers as polymerization components, and a (meth)acrylic acid ester-based resin containing at least two types of (meth)acrylic acid esters as polymerization components, with the mass ratio of the (meth)acrylic acid esters to the total polymerization components being 90 mass% or more. Hereinafter, "a styrene-based resin containing styrene and other vinyl monomers as polymerization components" is also referred to as "a specific styrene-based resin", and "a (meth)acrylic acid ester-based resin containing at least two types of (meth)acrylic acid esters as polymerization components, in which the mass ratio of (meth)acrylic acid esters in the total polymerization components is 90 mass% or more" is also referred to as "a specific (meth)acrylic acid ester-based resin".

[0117] From the viewpoint of maintaining adhesiveness by compression bonding, the base particles preferably have a specific styrene resin content greater than the specific (meth)acrylic acid ester resin content. The specific styrene resin content is preferably 55% by mass or more and 80% by mass or less, more preferably 60% by mass or more and 75% by mass or less, and even more preferably 65% ​​by mass or more and 70% by mass or less, based on the total content of the specific styrene resin and the specific (meth)acrylic acid ester resin.

[0118] -Specific styrene resin- The base particles constituting the specific particles contain a specific styrene-based resin containing styrene and other vinyl monomers as polymerization components.

[0119] The mass proportion of styrene in all the polymerization components of the specific styrene-based resin is preferably 60 mass% or more, more preferably 70 mass% or more, and even more preferably 75 mass% or more, from the viewpoint of suppressing fluidization of the specific particles in an unpressurized state. The mass proportion of styrene in all the polymerization components of the specific styrene-based resin is preferably 95 mass % or less, more preferably 90 mass % or less, and even more preferably 85 mass % or less, from the viewpoint of forming specific particles that are prone to phase transition under pressure. That is, the mass proportion of styrene in the total polymerization components of the specific styrene-based resin is preferably 60 mass % or more and 95 mass % or less.

[0120] Examples of vinyl monomers other than styrene contained in the polymerization components of the specific styrene-based resin (hereinafter also referred to as other vinyl monomers) include styrene-based monomers and acrylic-based monomers.

[0121] Examples of styrene-based monomers in the other vinyl monomers include vinylnaphthalene; alkyl-substituted styrenes such as α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene; aryl-substituted styrenes such as p-phenylstyrene; alkoxy-substituted styrenes such as p-methoxystyrene; halogen-substituted styrenes such as p-chlorostyrene, 3,4-dichlorostyrene, p-fluorostyrene, and 2,5-difluorostyrene; and nitro-substituted styrenes such as m-nitrostyrene, o-nitrostyrene, and p-nitrostyrene. These styrene-based monomers may be used alone or in combination of two or more.

[0122] The acrylic monomer in the other vinyl monomer is preferably at least one acrylic monomer selected from the group consisting of (meth)acrylic acid and (meth)acrylic acid esters. Examples of the (meth)acrylic acid esters include (meth)acrylic acid alkyl esters, (meth)acrylic acid carboxy-substituted alkyl esters, (meth)acrylic acid hydroxy-substituted alkyl esters, (meth)acrylic acid alkoxy-substituted alkyl esters, and di(meth)acrylic acid esters. These acrylic monomers may be used alone or in combination of two or more.

[0123] Examples of other vinyl monomers contained in the polymerization components of the specific styrene-based resin include, in addition to styrene-based monomers and acrylic-based monomers, (meth)acrylonitrile; vinyl ethers such as vinyl methyl ether and vinyl isobutyl ether; vinyl ketones such as vinyl methyl ketone, vinyl ethyl ketone and vinyl isopropenyl ketone; and olefins such as isoprene, butene and butadiene.

[0124] The mass ratio of the (meth)acrylic acid ester in the entire polymerization components of the specific styrene-based resin is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less from the viewpoint of suppressing fluidization of the specific particles in a non-pressurized state, and is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more from the viewpoint of forming specific particles that are prone to phase transition by pressure. As the (meth)acrylic acid ester here, a (meth)acrylic acid alkyl ester is preferred, a (meth)acrylic acid alkyl ester having 2 to 10 carbon atoms in the alkyl group is more preferred, and a (meth)acrylic acid alkyl ester having 4 to 8 carbon atoms in the alkyl group is even more preferred.

[0125] It is particularly preferable that the specific styrene-based resin contains at least one of n-butyl acrylate and 2-ethylhexyl acrylate as a polymerization component, and the total amount of n-butyl acrylate and 2-ethylhexyl acrylate in all the polymerization components of the styrene-based resin is preferably 40 mass% or less, more preferably 30 mass% or less, and even more preferably 25 mass% or less, from the viewpoint of suppressing fluidization of the particles in an unpressurized state, and is preferably 5 mass% or more, more preferably 10 mass% or more, and even more preferably 15 mass% or more, from the viewpoint of forming adhesive particles that are prone to phase transition due to pressure.

[0126] The weight average molecular weight of the specific styrene-based resin is preferably 3,000 or more, more preferably 4,000 or more, and even more preferably 5,000 or more, from the viewpoint of suppressing fluidization of the adhesive particles in an unpressurized state, and is preferably 60,000 or less, more preferably 55,000 or less, and even more preferably 50,000 or less, from the viewpoint of forming adhesive particles that are prone to phase transition due to pressure.

[0127] The weight average molecular weight of the resin is measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh HLC-8120GPC as the GPC device, a Tosoh TSKgel SuperHM-M (15 cm) as the column, and tetrahydrofuran as the solvent. The weight average molecular weight of the resin is calculated using a molecular weight calibration curve created using monodisperse polystyrene standard samples.

[0128] The glass transition temperature of the specific styrene-based resin is preferably 30°C or higher, more preferably 40°C or higher, and even more preferably 50°C or higher, from the viewpoint of preventing the adhesive particles from fluidizing in an unpressurized state; and is preferably 110°C or lower, more preferably 100°C or lower, and even more preferably 90°C or lower, from the viewpoint of forming adhesive particles that are prone to phase transition when subjected to pressure.

[0129] The glass transition temperature of a resin is determined from a differential scanning calorimetry (DSC) curve obtained by performing differential scanning calorimetry (DSC). More specifically, it is determined according to the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."

[0130] The glass transition temperature of a resin is controlled by the type and polymerization ratio of the polymerization components. The higher the density of flexible units such as methylene groups, ethylene groups, and oxyethylene groups contained in the main chain, the lower the glass transition temperature tends to be, and the higher the density of rigid units such as aromatic rings and cyclohexane rings contained in the main chain, the higher the glass transition temperature tends to be. In addition, the higher the density of aliphatic groups in the side chain, the lower the glass transition temperature tends to be.

[0131] The mass proportion of the specific styrene-based resin in the entire mother particle is preferably 55 mass% or more, more preferably 60 mass% or more, and even more preferably 65 mass% or more, from the viewpoint of suppressing fluidization of the adhesive particles in an unpressurized state, and is preferably 80 mass% or less, more preferably 75 mass% or less, and even more preferably 70 mass% or less, from the viewpoint of forming adhesive particles that are prone to phase transition due to pressure.

[0132] -Specific (meth)acrylic acid ester resin- The base particles constituting the adhesive particles preferably contain a (meth)acrylic acid ester-based resin that contains at least two types of (meth)acrylic acid esters as polymerization components, and in which the mass ratio of the (meth)acrylic acid esters to the total polymerization components is 90 mass% or more.

[0133] The mass proportion of (meth)acrylic acid ester in all the polymerization components of the (meth)acrylic acid ester resin is 90 mass % or more, more preferably 95 mass % or more, even more preferably 98 mass % or more, and still more preferably 100 mass %.

[0134] Examples of the (meth)acrylic acid ester include (meth)acrylic acid alkyl ester, (meth)acrylic acid carboxy-substituted alkyl ester, (meth)acrylic acid hydroxy-substituted alkyl ester, (meth)acrylic acid alkoxy-substituted alkyl ester, and di(meth)acrylic acid ester.

[0135] The mass ratio of the (meth)acrylic acid alkyl ester to the entire polymerization components of the specific (meth)acrylic acid ester resin is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 98 mass% or more, and even more preferably 100 mass% from the viewpoint of forming adhesive particles that are easily phase-transferred by pressure and have excellent adhesiveness by compression bonding. As the (meth)acrylic acid alkyl ester here, a (meth)acrylic acid alkyl ester having an alkyl group with 2 to 10 carbon atoms is preferable, and a (meth)acrylic acid alkyl ester having an alkyl group with 4 to 8 carbon atoms is more preferable.

[0136] The mass ratio of the two (meth)acrylic esters having the largest mass ratios among the at least two (meth)acrylic esters contained as polymerization components in the specific (meth)acrylic ester-based resin is preferably 80:20 to 20:80, more preferably 70:30 to 30:70, and even more preferably 60:40 to 40:60, from the viewpoint of forming adhesive particles that are easily phase-transformed by pressure and have excellent adhesiveness when pressed.

[0137] Of the at least two (meth)acrylic esters contained as polymerization components in the specific (meth)acrylic ester-based resin, the two with the largest mass ratios are preferably (meth)acrylic acid alkyl esters. The (meth)acrylic acid alkyl esters herein are preferably (meth)acrylic acid alkyl esters having an alkyl group with 2 to 10 carbon atoms, and more preferably (meth)acrylic acid alkyl esters having an alkyl group with 4 to 8 carbon atoms.

[0138] When the two (meth)acrylic acid esters having the largest mass proportions among the at least two (meth)acrylic acid esters contained as polymerization components in the specific (meth)acrylic acid ester-based resin are (meth)acrylic acid alkyl esters, the difference in the number of carbon atoms in the alkyl groups of the two (meth)acrylic acid alkyl esters is preferably 1 or more and 4 or less, more preferably 2 or more and 4 or less, and even more preferably 3 or 4, from the viewpoint of forming adhesive particles that are easily rearranged by pressure and have excellent adhesiveness when pressed.

[0139] From the viewpoint of forming adhesive particles that easily undergo phase transition under pressure and have excellent adhesiveness by compression bonding, the specific (meth)acrylic acid ester resin preferably contains n-butyl acrylate and 2-ethylhexyl acrylate as polymerization components, and it is particularly preferable that the two types of (meth)acrylic acid esters that have the largest mass ratios among the at least two types of (meth)acrylic acid esters contained as polymerization components in the (meth)acrylic acid ester resin are n-butyl acrylate and 2-ethylhexyl acrylate. The total amount of n-butyl acrylate and 2-ethylhexyl acrylate in the total polymerization components of the (meth)acrylic acid ester resin is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 98 mass% or more, and even more preferably 100 mass%.

[0140] The specific (meth)acrylic acid ester resin may contain a vinyl monomer other than the (meth)acrylic acid ester as a polymerization component. Examples of vinyl monomers other than (meth)acrylic acid esters include (meth)acrylic acid, styrene, styrene-based monomers other than styrene, (meth)acrylonitrile, vinyl ethers such as vinyl methyl ether and vinyl isobutyl ether, vinyl ketones such as vinyl methyl ketone, vinyl ethyl ketone and vinyl isopropenyl ketone, and olefins such as isoprene, butene and butadiene. These vinyl monomers may be used alone or in combination of two or more.

[0141] When the specific (meth)acrylic acid ester resin contains a vinyl monomer other than (meth)acrylic acid ester as a polymerization component, the vinyl monomer other than (meth)acrylic acid ester is preferably at least one of acrylic acid and methacrylic acid, and more preferably acrylic acid.

[0142] The weight average molecular weight of the specific (meth)acrylic acid ester resin is preferably 100,000 or more, more preferably 120,000 or more, and even more preferably 150,000 or more, from the viewpoint of suppressing fluidization of the particles in the absence of pressure, and is preferably 250,000 or less, more preferably 220,000 or less, and even more preferably 200,000 or less, from the viewpoint of forming particles that are prone to phase transition due to pressure.

[0143] The glass transition temperature of the specific (meth)acrylic acid ester resin is preferably 10° C. or lower, more preferably 0° C. or lower, and even more preferably −10° C. or lower, from the viewpoint of forming particles that easily undergo phase transition due to pressure, and is preferably −90° C. or higher, more preferably −80° C. or higher, and even more preferably −70° C. or higher, from the viewpoint of preventing the particles from fluidizing in an unpressurized state.

[0144] In this embodiment, the mass proportion of the specific (meth)acrylic acid ester resin in the entire mother particle is preferably 20 mass% or more, more preferably 25 mass% or more, and even more preferably 30 mass% or more, from the viewpoint of forming particles that are prone to phase transition due to pressure, and is preferably 45 mass% or less, more preferably 40 mass% or less, and even more preferably 35 mass% or less, from the viewpoint of suppressing fluidization of the particles in an unpressurized state.

[0145] In this embodiment, the total amount of the specific styrene-based resin and the specific (meth)acrylic acid ester-based resin contained in the base particle is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and even more preferably 100 mass% based on the entire base particle.

[0146] The base particles may contain, as necessary, for example, polystyrene; non-vinyl resins such as epoxy resin, polyester resin, polyurethane resin, polyamide resin, cellulose resin, polyether resin, and modified rosin; and the like. These resins may be used alone or in combination of two or more.

[0147] [Other ingredients] The base particles may contain other components as necessary. Other components include colorants (e.g., pigments, dyes), release agents (e.g., hydrocarbon waxes; natural waxes such as carnauba wax, rice wax, candelilla wax, etc.; synthetic or mineral / petroleum waxes such as montan wax; ester waxes such as fatty acid esters, montan acid esters, etc.), and charge control agents.

[0148] The base particles may contain a colorant as long as the visibility of the image is not impaired. The content of the colorant in the base particle is preferably as small as possible from the viewpoint of increasing the transparency of the adhesive particle. Specifically, the content of the colorant is preferably 1.0% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.01% by mass or less, based on the total mass of the base particle, and particularly preferably none is contained.

[0149] The base particles may be transparent. "Transparent" means that the average transmittance of light in the visible range (400 nm or more and 700 nm or less) in the area to which the adhesive particles are applied is 10% or more, preferably 50% or more, more preferably 80% or more, and even more preferably 90% or more. The average transmittance is measured using a spectrophotometer V700 (manufactured by JASCO Corporation).

[0150] - Structure of the mother particle - The internal structure of the base particle is preferably an island-in-a-sea structure. The sea-island structure is preferably a sea-island structure having a sea phase containing one of two or more binder resins and an island phase containing the other of the two or more binder resins dispersed in the sea phase. More specifically, from the viewpoint of facilitating phase transition by pressure, a sea-island structure is preferably a sea phase containing a specific styrene-based resin and an island phase containing a specific (meth)acrylic acid ester-based resin dispersed in the sea phase. Details of the specific styrene-based resin contained in the sea phase and the (meth)acrylic acid ester-based resin contained in the island phase are as described above. Note that an island phase not containing a (meth)acrylic acid ester-based resin may be dispersed in the sea phase.

[0151] The base particles may be base particles of a single layer structure, or base particles of a core-shell structure having a core and a shell layer covering the core. From the viewpoint of suppressing fluidization of the adhesive particles in a non-pressurized state, the base particles preferably have a core-shell structure.

[0152] When the base particles have a core-shell structure, the core preferably contains a specific styrene resin and a specific (meth)acrylic acid ester resin from the viewpoint of facilitating phase transition by pressure, and the shell preferably contains a specific styrene resin from the viewpoint of suppressing fluidization of the adhesive particles in a non-pressurized state.

[0153] When the base particle has a core-shell structure, the core preferably has a sea phase containing a specific styrene resin and an island phase containing a specific (meth)acrylic acid ester resin dispersed in the sea phase. The average diameter of the island phase is preferably within the above-mentioned range. Furthermore, in addition to the above-mentioned core structure, the shell layer preferably contains a specific styrene resin. In this case, the sea phase and the shell layer of the core are in a continuous structure, and the base particle is easily subjected to phase transition due to pressure.

[0154] Examples of the resin contained in the shell layer include polystyrene; and non-vinyl resins such as epoxy resin, polyester resin, polyurethane resin, polyamide resin, cellulose resin, polyether resin, and modified rosin. These resins may be used alone or in combination of two or more.

[0155] From the viewpoint of ease of handling of the mother particles, the volume average particle size (D50v) of the mother particles is preferably 4 μm or more, more preferably 5 μm or more, and even more preferably 6 μm or more, and is preferably 15 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less.

[0156] The volume average particle size (D50v) of the parent particles is measured using a Coulter Multisizer II (Beckman Coulter, Inc.) with an aperture of 100 μm diameter. 0.5 mg to 50 mg of parent particles are added and dispersed in 2 mL of 5 mass % aqueous solution of sodium alkylbenzene sulfonate, then mixed with 100 mL to 150 mL of electrolyte (ISOTON-II, Beckman Coulter, Inc.), dispersed for 1 minute with an ultrasonic disperser, and the resulting dispersion is used as the sample. The particle size of 50,000 particles with a particle size of 2 μm to 60 μm in the sample is measured. The particle size at which the cumulative 50% of the particle size distribution on a volume basis calculated from the small diameter side is the volume average particle size (D50v).

[0157] [External additives] The external additive may be, for example, inorganic particles. Examples of inorganic particles include SiO 2 , TiO 2 , Al 2 O 3 , CuO, ZnO, SnO 2 , CEO 2 , Fe 2 O 3 , MgO, BaO, CaO, K 2 O, Na 2 O, ZrO 2 , CaO SiO 2 , K 2 O (TiO 2 )n, Al 2 O 3 2SiO 2 , CaCO 3 , MgCO 3 , BaSO 4 , MgSO 4etc.

[0158] The surface of the inorganic particles as an external additive may be hydrophobized. The hydrophobization may be performed, for example, by immersing the inorganic particles in a hydrophobizing agent. The hydrophobizing agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is, for example, 1 part by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the inorganic particles.

[0159] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate, and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles), and the like.

[0160] The amount of the external additive added is preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the base particles.

[0161] [Characteristics of adhesive particles] The adhesive particles (their base particles) preferably contain at least two types of resins having different glass transition temperatures. The adhesive particles may contain three or more resins with different glass transition temperatures, but preferably contain two types of resins. As described above, the two types of resins are preferably the specific styrene resin and the specific (meth)acrylic acid ester resin. Other resins than the specific styrene resin and the specific (meth)acrylic acid ester resin may be included. However, the content of the other resins is preferably 5% by mass or less based on the entire adhesive particles (their mother particles).

[0162] Of the glass transition temperatures of at least two resins, the difference between the lowest glass transition temperature and the highest glass transition temperature is preferably 30° C. or more. From the viewpoint of facilitating phase transition of the particles due to pressure, the difference between the lowest glass transition temperature and the highest glass transition temperature is more preferably 40° C. or more, even more preferably 50° C. or more, and even more preferably 60° C. or more. The upper limit of the difference between the lowest glass transition temperature and the highest glass transition temperature is, for example, 140° C. or less, 130° C. or less, or 120° C. or less.

[0163] From the viewpoint of allowing the particles to easily undergo phase transition due to pressure, the lowest glass transition temperature is preferably 10°C or lower, more preferably 0°C or lower, and even more preferably -10°C or lower, and from the viewpoint of preventing the particles from fluidizing in the absence of pressure, it is preferably -90°C or higher, more preferably -80°C or higher, and even more preferably -70°C or higher.

[0164] From the viewpoint of suppressing fluidization of the particles in the absence of pressure, the highest glass transition temperature is preferably 30° C. or higher, more preferably 40° C. or higher, and even more preferably 50° C. or higher, and from the viewpoint of facilitating phase transition of the particles due to pressure, the highest glass transition temperature is preferably 70° C. or lower, more preferably 65° C. or lower, and even more preferably 60° C. or lower.

[0165] The glass transition temperature can be determined from the adhesive particles. The adhesive particles are compressed to prepare a plate-shaped sample, and the differential scanning calorimetry (DSC) is performed to obtain a differential scanning calorimetry curve (DSC curve). More specifically, the glass transition temperature is determined according to the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."

[0166] The adhesive particles are preferably particles that undergo a phase transition due to pressure, and preferably satisfy the following formula 1. Formula 1...10℃≦T1-T2 In formula 1, T1 is the temperature at which the viscosity is 10,000 Pa s under a pressure of 1 MPa, and T2 is the temperature at which the viscosity is 10,000 Pa s under a pressure of 10 MPa. How to determine T1 and T2 will be described later.

[0167] The temperature difference (T1-T2) is preferably 10°C or more, more preferably 15°C or more, and more preferably 20°C or more, from the viewpoint of facilitating phase transition of the particles due to pressure, and is preferably 120°C or less, more preferably 100°C or less, and even more preferably 80°C or less, from the viewpoint of suppressing fluidization of the particles in an unpressurized state.

[0168] The value of T1 is preferably 140° C. or less, more preferably 130° C. or less, even more preferably 120° C. or less, and still more preferably 115° C. or less. The lower limit of the temperature T1 is preferably 80° C. or more, and more preferably 85° C. or more. The value of T2 is preferably 40° C. or more, more preferably 50° C. or more, and even more preferably 60° C. or more. The upper limit of the temperature T2 is preferably 85° C. or less.

[0169] An index showing the ease with which adhesive particles undergo phase transition due to pressure is the temperature difference (T1-T3) between the temperature T1 at which the adhesive shows a viscosity of 10,000 Pa s under a pressure of 1 MPa and the temperature T3 at which the adhesive shows a viscosity of 10,000 Pa s under a pressure of 4 MPa, and it is preferable that the temperature difference (T1-T3) is 5°C or more. The temperature difference (T1-T2) is generally 25°C or less. Adhesive particles are prone to phase transition due to pressure, so the temperature difference (T 1 -T 2 ) is preferably 5°C or higher, and more preferably 10°C or higher. The upper limit of the temperature difference (T1-T3) is generally 25°C or less.

[0170] From the viewpoint of a temperature difference (T1-T3) of 5°C or more, the adhesive particles preferably have a temperature T3 at which they exhibit a viscosity of 10,000 Pa s under a pressure of 4 MPa of 90°C or less, more preferably 85°C or less, and even more preferably 80°C or less. The lower limit of the temperature T3 is preferably 60°C or more.

[0171] The temperature T1, the temperature T2, and the temperature T3 are calculated as follows. The adhesive particles are compressed to prepare a pellet-shaped sample. The pellet-shaped sample is set in a flow tester (Shimadzu Corporation, CFT-500), and the applied pressure is fixed at 1 MPa, and the viscosity at 1 MPa is measured against the temperature. From the obtained viscosity graph, it is found that the viscosity is 10 4 Determine the temperature T1 when the pressure becomes Pa·s. Determine the temperature T2 in the same manner as for temperature T1, except that the applied pressure of 1 MPa is changed to 10 MPa. Determine the temperature T3 in the same manner as for temperature T1, except that the applied pressure of 1 MPa is changed to 4 MPa. Calculate the temperature difference (T1-T2) from temperatures T1 and T2. Calculate the temperature difference (T1-T3) from temperatures T1 and T3.

[0172] [Method of manufacturing adhesive particles] The adhesive particles can be obtained by producing base particles and then externally adding an external additive to the base particles.

[0173] The base particles may be produced by any of a dry production method (e.g., a kneading and grinding method, etc.) and a wet production method (e.g., an aggregation and coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). There are no particular limitations on these production methods, and any known production method may be used. Among these, it is preferable to obtain the base particles by the aggregation and coalescence method.

[0174] Hereinafter, a method for producing base particles by the aggregation-coalescence method will be described as an example. When the base particles are produced by the aggregation and coalescence method, for example, A step of preparing a styrene-based resin particle dispersion liquid in which styrene-based resin particles containing a specific styrene-based resin are dispersed (a styrene-based resin particle dispersion liquid preparation step); a step of polymerizing a specific (meth)acrylic acid ester-based resin in a styrene-based resin particle dispersion to form composite resin particles containing the specific styrene-based resin and the specific (meth)acrylic acid ester-based resin (composite resin particle forming step); a step of aggregating the composite resin particles in the composite resin particle dispersion liquid in which the composite resin particles are dispersed to form aggregated particles (aggregated particle forming step); The aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated to fuse and coalesce the aggregated particles to form mother particles (fusion and coalescence step), and the mother particles are produced through this process.

[0175] The adhesive particles may be used as they are by coating, or may be used as an electrostatic image developer. The electrostatic image developer may be a one-component developer containing only adhesive particles, or may be a two-component developer containing a mixture of adhesive particles and a carrier.

[0176] The carrier is not particularly limited, and may be a known carrier. For example, the carrier may be a coated carrier in which the surface of a core material made of magnetic powder is coated with a resin; a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin; a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin; etc. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material, and the surface of the core material is coated with a resin.

[0177] Examples of magnetic powders include magnetic metals such as iron, nickel, and cobalt; magnetic oxides such as ferrite and magnetite; and the like.

[0178] Examples of the resin and matrix resin for coating include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin or its modified product containing organosiloxane bonds, fluororesin, polyester, polycarbonate, phenolic resin, epoxy resin, etc. The resin and matrix resin for coating may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, potassium titanate, etc.

[0179] To coat the surface of the core material with a resin, a method of coating with a coating layer forming solution in which the coating resin and various additives (used as necessary) are dissolved in a suitable solvent can be mentioned. The solvent is not particularly limited and may be selected taking into consideration the type of resin used, suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer; a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material; a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air; and a kneader coater method in which the carrier core material and the solution for forming a coating layer are mixed in a kneader coater and then the solvent is removed.

[0180] The mixing ratio (mass ratio) of adhesive particles to carrier in the two-component developer is preferably particles:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100. EXAMPLES

[0181] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are based on mass.

[0182] <Preparation of Dispersion Containing Styrene-Based Resin Particles> [Preparation of styrene-based resin particle dispersion (St1)] Styrene: 390 parts n-Butyl acrylate: 100 parts Acrylic acid: 10 parts Dodecanethiol: 7.5 parts The above materials were mixed and dissolved to prepare a monomer solution. 8 parts of anionic surfactant (Dowfax2A1, manufactured by Dow Chemical Company) was dissolved in 205 parts of ion-exchanged water, and the monomer solution was added thereto and dispersed and emulsified to obtain an emulsion. 2.2 parts of anionic surfactant (Dowfax2A1, manufactured by The Dow Chemical Company) was dissolved in 462 parts of ion-exchanged water, and the solution was charged into a polymerization flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, and the mixture was heated to 73°C with stirring and maintained at that temperature. 3 parts of ammonium persulfate was dissolved in 21 parts of ion-exchanged water and added dropwise to the polymerization flask via a metering pump over 15 minutes, and then the emulsion was added dropwise to the solution via a metering pump over 160 minutes. The polymerization flask was then maintained at 75° C. for 3 hours with continued slow stirring, and then allowed to cool to room temperature (25° C.). This resulted in a styrene-based resin particle dispersion (St1) containing styrene-based resin particles, with a volume average particle size (D50v) of 174 nm, a weight average molecular weight of 49 k by GPC (UV detection), a glass transition temperature of 54°C, and a solid content of 42%.

[0183] The styrene-based resin particle dispersion (St1) was dried to extract the styrene-based resin particles, and the thermal behavior was analyzed in the temperature range of -100°C to 100°C using a differential scanning calorimeter (Shimadzu Corporation, DSC-60A). One glass transition temperature was observed, which was 54°C.

[0184] <Preparation of Dispersion Containing Composite Resin Particles> [Preparation of composite resin particle dispersion (M1)] Styrene-based resin particle dispersion (St1): 1,190 parts (solids: 500 parts) 2-Ethylhexyl acrylate: 250 parts -n-Butyl acrylate: 250 parts Ion-exchanged water: 982 parts The above materials were charged into a polymerization flask and stirred at 25°C for 1 hour, then heated to 70°C. 2.5 parts of ammonium persulfate was dissolved in 75 parts of ion-exchanged water, and the solution was added dropwise to the polymerization flask over 60 minutes via a metering pump. The polymerization flask was then kept at 70° C. for 3 hours with continued slow stirring, and then allowed to return to room temperature (RT). This resulted in a composite resin particle dispersion (M1) containing composite resin particles, with a volume average particle size (D50v) of the resin particles of 219 nm, a weight average molecular weight by GPC (UV detection) of 219 k, and a solid content of 32%.

[0185] The composite resin particle dispersion (M1) was dried to extract the composite resin particles, and the thermal behavior was analyzed in the temperature range of -150°C to 100°C using a differential scanning calorimeter (Shimadzu Corporation, DSC-60A). Two glass transition temperatures were observed. The two glass transition temperatures were -52°C and 54°C. The mass ratio of the styrene resin to the (meth)acrylic acid ester resin in the composite resin particles is 50:50.

[0186] <Preparation of adhesive particles> [Preparation of adhesive particles (1) and developer (1)] ·Composite resin particle dispersion (M1): 504 parts Ion-exchanged water: 710 parts Anionic surfactant (Dow Chemical Company, Dowfax2A1): 1 part

[0187] The above materials were placed in a reaction vessel equipped with a thermometer and a pH meter, and a 1.0% aqueous nitric acid solution was added at a temperature of 25°C to adjust the pH to 3.0. Then, 23 parts of a 2.0% aqueous aluminum sulfate solution was added while dispersing with a homogenizer (Ultra Turrax T50, manufactured by IKA) at a rotation speed of 5000 rpm. Next, a stirrer and a mantle heater were installed in the reaction vessel, and the temperature was increased at a rate of 0.2°C / min up to 40°C, and at a rate of 0.05°C / min after exceeding 40°C, and the particle size was measured every 10 minutes with a Multisizer II (aperture diameter 50 μm, manufactured by Beckman Coulter). When the volume average particle size reached 5.0 μm, the temperature was maintained, and 170 parts of a styrene-based resin particle dispersion (St1) was added over 5 minutes. After the addition was completed, the mixture was held at 50°C for 30 minutes, and then a 1.0% aqueous sodium hydroxide solution was added to adjust the pH of the slurry to 6.0. Next, the temperature was increased to 90°C at a rate of 1°C / min while adjusting the pH to 6.0 every 5°C, and then maintained at 90°C. When the particle shape and surface properties were observed using an optical microscope and a field emission scanning electron microscope (FE-SEM), coalescence of the particles was confirmed after 10 hours, so the container was cooled to 30°C over 5 minutes with cooling water.

[0188] The cooled slurry was passed through a nylon mesh with a mesh size of 15 μm to remove coarse particles, and the slurry that passed through the mesh was filtered under reduced pressure with an aspirator. The solids remaining on the filter paper were crushed as finely as possible by hand, and then added to ion-exchanged water (temperature 30°C) with 10 times the amount of solids, and stirred for 30 minutes. Next, the mixture was filtered under reduced pressure with an aspirator, and the solids remaining on the filter paper were crushed as finely as possible by hand, and then added to ion-exchanged water (temperature 30°C) with 10 times the amount of solids, and then stirred for 30 minutes, and then filtered under reduced pressure again with an aspirator, and the electrical conductivity of the filtrate was measured. This operation was repeated until the electrical conductivity of the filtrate was 10 μS / cm or less, and the solids were washed.

[0189] The washed solid content was crushed finely with a wet-dry type granulator (Comil) and vacuum-dried in an oven at 25° C. for 36 hours to obtain base particles (1). The base particles (1) had a volume average particle size of 8.0 μm.

[0190] 100 parts of the base particles (1) and 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) were mixed and mixed for 30 seconds at a rotation speed of 13,000 rpm using a sample mill. The mixture was sieved using a vibrating sieve with an opening of 45 μm to obtain adhesive particles (1).

[0191] When the thermal behavior of the adhesive particle (1) sample was analyzed in the temperature range of -150°C to 100°C using a differential scanning calorimeter (Shimadzu Corporation, DSC-60A), two glass transition temperatures were observed. The two glass transition temperatures were -52°C and 54°C.

[0192] When the temperatures T1, T2, and T3 of the adhesive particles (1) were determined using the measurement method described above, the adhesive particles (1) satisfied formula 1 "10°C≦T1-T2", the temperature T3 was 75°C, and the temperature difference (T1-T3) was 15°C.

[0193] When the cross section of the adhesive particle (1) was observed with a scanning electron microscope (SEM), a sea-island structure was observed. The adhesive particle (1) had a core portion in which an island phase existed and a shell layer in which no island phase existed. The sea phase contained a styrene-based resin, and the island phase contained a (meth)acrylic ester-based resin.

[0194] 10 parts of the adhesive particles (1) and 100 parts of the resin-coated carrier described below were placed in a V-type blender and stirred for 20 minutes, and then sieved through a vibrating sieve with 212 μm openings to obtain developer (1).

[0195] Mn-Mg-Sr ferrite particles (average particle size 40 μm): 100 parts Toluene: 14 parts Polymethylmethacrylate: 2 parts Carbon black (VXC72: manufactured by Cabot): 0.12 parts The above materials except for the ferrite particles were mixed with glass beads (diameter 1 mm, same amount as toluene) and stirred for 30 minutes at a rotation speed of 1200 rpm using a sand mill manufactured by Kansai Paint Co., Ltd. to obtain a dispersion liquid. The dispersion liquid and the ferrite particles were placed in a vacuum degassing kneader, and dried under reduced pressure while stirring to obtain a resin-coated carrier.

[0196] <Examples 1 to 22 and Comparative Examples 1 to 2: Preparation of Perfect-bound Booklets> A developer (1) containing adhesive particles (1) was placed in a developing device of an electrophotographic image forming apparatus ("PC1120" manufactured by Fujifilm Business Innovation Co., Ltd.). As the paper, A4 size paper having the basis weight shown in Table 1 was prepared.

[0197] The image forming apparatus applies a particle amount of 0.72 g / m2 to the edge of the short side of the paper, in an area 3 mm from the edge (i.e., the adhesive layer forming area). 2 A diagonal line pattern was formed using adhesive particles, and the adhesive particles were passed through a belt roll type fixing machine to fix (i.e., fix). The adhesive particle fixing conditions (i.e., fixing conditions) were a heating temperature of 200°C. Then, the line width of the diagonal line pattern was changed to obtain multiple papers with different amounts of adhesive per unit area. The obtained papers were cut to 5 cm length x 9 cm width so that the adhesive layer was at the top, to obtain paper for booklets. In this case, the area of ​​the adhesive layer was 3 mm length x 9 cm width.

[0198] Next, a plurality of sheets of paper were collated under the following conditions shown in Table 1 so that the sheets were overlapped with an adhesive layer between them to obtain a paper group. Unit area (mm 2 ) the amount of adhesive on the first and second surface sides per unit area (referred to as "adhesive amount on the first and second surface sides" in Table 1) The ratio of the amount of adhesive in the adhesive layer between the sheets at the center in the thickness direction of the paper group (i.e., the booklet) to the amount of adhesive in the adhesive layer between the sheets on the first surface side and the second surface side of the paper group (i.e., the booklet) (in Table 1, this is indicated as "the ratio of the amount of adhesive in the center in the thickness direction to the first and second surface sides"). The amount of change in the amount of adhesive in the adhesive layer from the first surface side and second surface side of the paper group (i.e., the booklet) toward the center in the thickness direction of the paper group (i.e., the booklet) per five sheets of paper (represented as "change in adhesive amount" in Table 1) - Number of sheets to be collated (referred to as "Number of sheets of paper group" in Table 1)

[0199] Next, the papers (their adhesive layers) were sealed for 2 seconds using Fuji Impulse's "Thick Gusset Sealer T130" under the pressure and temperature conditions shown in Table 1 to produce a booklet.

[0200] In Example 22, a circular dot pattern was formed by adhesive particles instead of the oblique line pattern, the diameter of the circular dot pattern was changed, and multiple sheets of paper were obtained with different amounts of adhesive per unit area. Then, booklets were made using the multiple sheets of paper obtained.

[0201] <Evaluation> The following evaluations were carried out for each example booklet.

[0202] (Paper adhesive strength) The paper is rolled from the first surface of the booklet to the surface of the paper located in the center of the thickness direction. Next, the edge of the paper located at the center in the thickness direction (the edge on the side where the adhesive layer was not provided) was lifted up until the entire booklet was floating in the air, and the adhesive strength of the paper was evaluated according to the following criteria. A: No peeling even after shaking 5 times after 5 seconds B: Adhesion is maintained for 5 seconds C: Adhesion is maintained for 2 seconds D: When the edge of the paper is lifted, it peels off and falls.

[0203] (Paper does not peel properly) The edge of the first sheet of paper (the edge on the side without the adhesive layer) was held from the first surface of the booklet, and the paper was peeled off at a speed of 500 mm / min. After peeling, the adhesive area was checked to see if the paper was damaged, and it was evaluated according to the following criteria. A: The peeled paper is not only torn but also frayed. B: There are no tears in the peeled paper. C: Slight tears are observed on the peeled paper surface. D: Tears or damage is observed on the peeled paper surface.

[0204] [Table 1]

[0205] From the above results, it can be seen that the booklet of this example has higher adhesion between the sheets than the booklet of the comparative example, and is less susceptible to peeling defects (tears or breakage) when the sheets are peeled off.

[0206] The present embodiment includes the following aspects. (((1))) A paper stack having a plurality of papers stacked thereon; a plurality of adhesive layers provided at the end of each sheet of the paper stack and interposed between each sheet of the paper stack, the adhesive layers including a thermoplastic adhesive, for releasably adhering the sheets of paper to each other; having A perfect bound booklet in which the amount of the thermoplastic adhesive in the plurality of adhesive layers varies from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet. (((2))) A perfect bound booklet as described in (((1))), wherein, among multiple adhesive layers interposed between each sheet of paper, the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets at the center of the thickness of the booklet is 1.2 to 4.0 times the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets on the first surface side and the second surface side of the booklet. (((3))) The amount of the thermoplastic adhesive in the adhesive layer changes from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, and the difference in the amount of adhesive on one sheet of paper out of five sheets of paper is 0.18 g / m 2 The above-mentioned perfect bound booklet is described in (((1))) or (((2))). (((4))) The adhesive layer is composed of the thermoplastic adhesive in a linear pattern, a dot pattern, or a combination of the linear pattern and the dot pattern. (((5))) A perfect bound booklet as described in (((4))), wherein the amount of the thermoplastic adhesive in the multiple adhesive layers changes from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet due to a change in at least one of the line width of the linear pattern and the diameter of the dot pattern of the thermoplastic adhesive. (((6))) The thermoplastic adhesive comprises at least two types of resins having different glass transition temperatures, and is a pressure phase transition adhesive in which the difference between the lowest glass transition temperature and the highest glass transition temperature of the at least two types of resins is 30°C or more. (((7))) The perfect bound booklet according to any one of ((1))) to (((6))), wherein the paper set is a paper set in which 10 to 100 sheets are stacked as the plurality of sheets. (((8))) 2. The perfect bound booklet according to any one of ((1))) to (((7))), wherein the paper has a basis weight of 200 gsm or less. (((9))) applying particles of the thermoplastic adhesive to the edges of the plurality of sheets; fixing the particles of thermoplastic adhesive to the paper; a bonding process in which the plurality of sheets of paper having an adhesive layer containing the thermoplastic adhesive are stacked together so that the adhesive layer is interposed between each of the sheets of paper to obtain a paper group, and then pressure and heat are applied to the adhesive layer to bond each of the sheets of paper together with the adhesive layer; The method for producing a perfect bound booklet according to any one of ((1))) to (((8))) above. (((10))) The method for producing a perfect bound booklet described in (((9))), wherein the applying step is a step of applying particles of the thermoplastic adhesive to the ends of the plurality of sheets of paper by an electrophotographic method. (((11))) The method for manufacturing a perfect bound booklet described in (((9))) or (((10))) is a process in which a pressure of 0.01 MPa to 1 MPa and heat of 90°C to 220°C are applied to the adhesive layer from the first surface side and the second surface side of the paper group, thereby bonding each of the papers with the adhesive layer.

[0207] The advantages of the above aspect are as follows. According to the invention pertaining to (((1))), (((4))), or (((5))), there is provided a perfect bound booklet having a paper group in which a plurality of papers are stacked, and a plurality of adhesive layers that are provided at the ends of each paper of the paper group and interposed between each paper and that removably adhere each paper, the plurality of adhesive layers including a thermoplastic adhesive, wherein the amount of thermoplastic adhesive in the plurality of adhesive layers is the same from each of the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, and the perfect bound booklet has higher adhesion between the papers and is less likely to have peeling problems (tears or breakage) when the papers are peeled off, compared to a case in which the amount of thermoplastic adhesive in the plurality of adhesive layers is the same from each of the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet.

[0208] According to the invention related to (((2))), a perfect bound booklet is provided in which the adhesion between the sheets is higher and peeling problems (tears or breakage) are less likely to occur when the sheets are peeled off, compared to when the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets on the first and second surface sides of the booklet, among the multiple adhesive layers interposed between the sheets, is less than 1.2 times or more than 4.0 times the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets at the thickness center of the booklet. According to the invention related to (((3))), the amount of thermoplastic adhesive in the adhesive layer changes from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, respectively, and the difference in the amount of adhesive on one sheet of paper out of five sheets is 0.18 g / m 2 This provides a perfect bound booklet in which the adhesion between the sheets is high and peeling failure (tearing or damage) is unlikely to occur when the sheets are peeled off, as compared with a case in which the adhesion is less than 100%.

[0209] According to the invention related to (((6))), a perfect bound booklet is provided which has higher adhesion between the sheets of paper than an adhesive containing one type of resin, and is less susceptible to peeling defects (tears or breakage) when the sheets are peeled away. According to the invention related to (((7))), a perfect bound booklet is provided in which the adhesion between the sheets of paper is high and peeling failure (tearing or damage) is less likely to occur when the sheets are peeled off, compared to a paper group in which more than 100 sheets are stacked as multiple sheets of paper. According to the invention of (((8))), a perfect bound booklet is provided in which the adhesion between the sheets is higher and peeling failure (tears or breakage) is less likely to occur when the sheets are peeled off, compared to when the basis weight of the sheets exceeds 200 gsm.

[0210] According to the invention pertaining to (((9))), (((10))) or (((11))), there is provided a method for producing a perfect bound booklet, the method comprising: an application step of applying a pre-thermoplastic adhesive to ends of a plurality of sheets of paper to form an adhesive layer containing a thermoplastic adhesive; and a fixing step of stacking the plurality of sheets of paper on which the adhesive layer containing the thermoplastic adhesive has been formed so that the adhesive layer is interposed between each sheet of paper to obtain a group of sheets of paper, and then applying pressure and heat to the adhesive layer to bond each sheet of paper with the adhesive layer, wherein, among a plurality of adhesive layers interposed between each sheet of paper, the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets of paper on the first surface side and the second surface side of the booklet is less than 1.2 times or more than 4.0 times the amount of thermoplastic adhesive in the adhesive layers interposed between the sheets of paper at the center in the thickness direction of the booklet, respectively, and the method for producing a perfect bound booklet is provided in which the adhesion between the sheets of paper is higher and peeling defects (tears or breakage) are less likely to occur when the sheets are peeled off. [Explanation of symbols]

[0211] 10 Perfect bound booklet 10A Perfect bound booklet, front page 10B Second surface of perfect bound booklet 10C Perfect bound booklet thickness center 12 Paper Group 12A paper 14 Adhesive layer 14A Thermoplastic Adhesive Pattern

[0212] 150 Placement means 516 Adhesive particles 516A Adhesive Particle Area 518 Particle Applicator 518A Supply Roll 564 Fixation device 564A Heating Roll 564B Pressure Roll 200 Crimping means 220 Paper group forming device 230 Pressurizing device 231, 232 Pressure roll P paper P1 Post-grant form P2 paper group P3 booklet

[0213] 100 Placement means 101 Photoreceptor 102 Charging roll (an example of a charging means) 103 Exposure device (an example of an electrostatic image forming means) 104 Developing device (an example of developing means) 105 Transfer roll (an example of a transfer means) 106 Photoconductor cleaning device (an example of a cleaning means) 107 Fixing device (an example of a fixing part) 200 Crimping means 220 Paper group forming device 230 Pressurizing device 231, 232 Pressure roll P paper P1 Post-grant form P2 paper group P3 booklet

Claims

1. A paper stack having a plurality of papers stacked thereon; a plurality of adhesive layers provided at the end of each sheet of the paper stack and interposed between each sheet of the paper stack, the adhesive layers including a thermoplastic adhesive, for releasably adhering the sheets of paper to each other; having A perfect bound booklet in which the amount of the thermoplastic adhesive in the plurality of adhesive layers varies from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet.

2. 2. A perfect bound booklet as described in claim 1, wherein, among a plurality of adhesive layers interposed between each sheet of paper, the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets at the center of the thickness direction of the booklet is 1.2 to 4.0 times the amount of thermoplastic adhesive in the adhesive layer interposed between the sheets on the first surface side and the second surface side of the booklet.

3. The amount of the thermoplastic adhesive in the adhesive layer changes from the first surface side and the second surface side of the booklet toward the center in the thickness direction of the booklet, and the difference in the amount of adhesive on one sheet of paper out of five sheets of paper is 0.18 g / m 2 The perfect bound booklet according to claim 1.

4. The perfect bound booklet according to claim 1 , wherein the adhesive layer is configured with a linear pattern, a dotted pattern, or a combination of the linear pattern and the dotted pattern of the thermoplastic adhesive.

5. A perfect bound booklet as described in claim 4, wherein the amount of the thermoplastic adhesive in the multiple adhesive layers changes from the first surface side and the second surface side of the booklet toward the center of the booklet in the thickness direction due to a change in at least one of the line width of the linear pattern and the diameter of the dot pattern of the thermoplastic adhesive.

6. 2. The perfect bound booklet according to claim 1, wherein the thermoplastic adhesive comprises at least two types of resins having different glass transition temperatures, and the difference between the lowest glass transition temperature and the highest glass transition temperature of the at least two types of resins is a pressure phase transition adhesive of 30° C. or more.

7. The perfect bound booklet according to claim 1 , wherein the paper group is a paper group in which 10 to 100 sheets are stacked as the plurality of sheets.

8. 2. The perfect bound booklet according to claim 1, wherein the paper has a basis weight of 200 gsm or less.

9. applying particles of the thermoplastic adhesive to the edges of the plurality of sheets; fixing the particles of thermoplastic adhesive to the paper; a bonding process in which the plurality of sheets of paper having an adhesive layer containing the thermoplastic adhesive are stacked together so that the adhesive layer is interposed between each of the sheets of paper to obtain a paper group, and then pressure and heat are applied to the adhesive layer to bond each of the sheets of paper together with the adhesive layer; The method for producing a perfect bound booklet according to any one of claims 1 to 8, comprising the steps of:

10. The method for producing a perfect bound booklet according to claim 9 , wherein the applying step applies particles of the thermoplastic adhesive to the ends of the plurality of sheets of paper by an electrophotographic method.

11. The method for manufacturing a perfect bound booklet according to claim 9, wherein the bonding process is a process of applying a pressure of 0.01 MPa to 1 MPa and heat of 90°C to 220°C to the adhesive layer from the first surface side and the second surface side of the paper group to bond each of the papers with the adhesive layer.

Citation Information

Patent Citations

  • Staple device and image formation apparatus

    JP2013043751A

  • Paper sheet processing apparatus, image forming apparatus, and program

    JP2013126910A

  • Image forming system

    JP2015028592A

  • Method for manufacturing printed matter and system for manufacturing printed matter

    JP2021147454A

  • Measurement and calibration using colorimetric sensors

    JP2018503817A