Film laminate

The film laminate with an amorphous oxide layer between fluororesin and copper layers addresses adhesion and heat resistance issues, ensuring low transmission loss and stability for high-frequency signal transmission.

JP2024141186AInactive Publication Date: 2024-10-10MITSUBISHI MATERIALS CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing film laminates with fluororesin and metal copper layers face issues of reduced adhesion due to interface roughness and oxidation, leading to increased transmission loss and insufficient heat resistance, especially in high-frequency and high-temperature environments.

Method used

A film laminate with an amorphous oxide layer formed between the fluororesin film and the metal copper layer, which enhances chemical bonding and acts as a barrier to prevent interdiffusion and oxidation, maintaining adhesion even in high-temperature conditions.

Benefits of technology

The laminate achieves excellent adhesion and low transmission loss in high-frequency ranges while maintaining stability in high-temperature environments, suitable for wiring boards in high-frequency signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141186000001_ABST
    Figure 2024141186000001_ABST
Patent Text Reader

Abstract

To provide a film laminate which is especially excellent in adhesiveness between a fluororesin film having a low transmission loss in a high frequency region and a metal copper layer, does not significantly lose the adhesiveness even when used under a high temperature environment, and is especially suitable for a wiring board for high frequency signal transmission.SOLUTION: There is provided a film laminate 10 in which a metal copper layer 12 is laminated on one surface or both surfaces of a fluororesin film 11, and an amorphous oxide layer 13 is formed between the fluororesin film 11 and the metal copper layer 12. The thickness of the amorphous oxide layer 13 preferably falls within the range of 10 nm or more and 100 nm or less. An oxide constituting the amorphous oxide layer 13 preferably includes one or two or more kinds selected from among Ge, Si, Al, Ti, Ta, Zr and Cr.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film. [Background technology]

[0002] Generally, a film laminate in which a metallic copper layer is laminated as a conductive layer or a heat transfer layer on the surface of an insulating resin layer is used as a wiring substrate for use in electronic and electric devices. Here, wiring boards for high-frequency signal transmission devices such as antennas and radars in the GHz band or above are required to have low transmission loss when used in the high-frequency range. In view of this, for example, film laminates using fluororesin films have been provided as shown in Patent Documents 1 and 2. Fluororesins have a low dielectric constant and low dielectric loss, and are therefore particularly suitable as resin films constituting wiring boards for high-frequency signal transmission.

[0003] Incidentally, since the surface of a fluororesin film is very chemically stable, the adhesive strength with other materials tends to be low. Therefore, in Patent Document 1, protrusions are formed on the surface of the fluororesin, the metal foil is roughened, and the conditions for pressure lamination are optimized to improve the adhesion between the copper film and the fluororesin through the anchor effect. In addition, in Patent Document 2, a thin metal film (nickel film or titanium film) is formed on the surface of the fluororesin by physical vapor deposition, and then a copper film is formed by copper plating on this thin metal film, thereby improving the adhesion between the copper film and the fluororesin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-019932 A [Patent Document 2] International Publication No. 2018 / 179904 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in Patent Document 1, the interface between the fluororesin and the metal foil becomes rough, which causes an increase in transmission loss. Furthermore, in Patent Document 2, when used in a high-temperature environment, the thin metal film formed on the surface of the fluororesin may oxidize, resulting in a decrease in adhesion, and the heat resistance was insufficient.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a film laminate that is particularly excellent in adhesion between a fluororesin film having low transmission loss in the high frequency range and a metallic copper layer, and that does not significantly decrease in adhesion even when used in a high-temperature environment, and is particularly suitable for wiring boards for high-frequency signal transmission. [Means for solving the problem]

[0007] In order to solve the above problems, the film laminate of aspect 1 of the present invention is a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, and is characterized in that an amorphous oxide layer is formed between the fluororesin film and the metallic copper layer.

[0008] According to the film laminate of the first aspect of the present invention, since an amorphous oxide layer is formed on the surface of the fluororesin film, a chemical bond is formed via O (oxygen) on the outermost surface of the fluororesin, and a strong bond between the fluororesin film and the amorphous oxide layer can be realized. In addition, since the amorphous oxide layer and the metallic copper layer have good bonding properties, the adhesion between the fluororesin film and the metallic copper layer is particularly excellent. In addition, because the amorphous oxide layer is chemically stable, the reaction between the free F (fluorine) present on the surface of the fluororesin and the adsorbed O (oxygen) and the amorphous oxide layer are suppressed, and the decrease in adhesion can be suppressed even when used in a high-temperature environment. Furthermore, because it is an amorphous oxide layer, there are no grain boundaries and it has excellent barrier properties, so that even when used in a high-temperature environment, it is possible to suppress interdiffusion between the fluororesin and the metallic copper layer, and the decrease in adhesion due to fluorination and oxidation of copper can be suppressed.

[0009] The film laminate of the second aspect of the present invention is characterized in that in the film laminate of the first aspect, the amorphous oxide layer has a thickness in the range of 10 nm or more and 100 nm or less. According to the film laminate of the second aspect of the present invention, the thickness of the amorphous oxide layer is 10 nm or more, so that the barrier properties can be ensured and the interdiffusion between the fluororesin and the metallic copper layer can be appropriately suppressed. Meanwhile, the thickness of the amorphous oxide layer is 100 nm or less, so that the warping of the film due to the membrane stress can be suppressed.

[0010] The film laminate of the third aspect of the present invention is characterized in that, in the film laminate of the first or second aspect, the oxide constituting the amorphous oxide layer contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr. According to the film laminate of the third aspect of the present invention, the oxide constituting the amorphous oxide layer contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr, so that the amorphous oxide layer is more chemically stable and it is possible to further suppress the reaction between the amorphous oxide layer and the free F (fluorine) or the adsorbed O (oxygen) present on the surface of the fluororesin. In addition, it is possible to sufficiently secure the barrier property, suppress the interdiffusion between the fluororesin and the metallic copper layer, and appropriately suppress the decrease in adhesion due to the fluorination and oxidation of copper.

[0011] The film laminate of the fourth aspect of the present invention is characterized in that in the film laminate of the first or second aspect, the oxide constituting the amorphous oxide layer contains In and Zn. According to the film laminate of the fourth aspect of the present invention, the oxide constituting the amorphous oxide layer contains In and Zn, so that the amorphous oxide layer is more chemically stable, and it is possible to further suppress the reaction between the amorphous oxide layer and the free F (fluorine) present on the surface of the fluororesin or the adsorbed O (oxygen). In addition, it is possible to sufficiently ensure the barrier properties, suppress the interdiffusion between the fluororesin and the metallic copper layer, and appropriately suppress the decrease in adhesion due to the fluorination and oxidation of copper.

[0012] The film laminate of a fifth aspect of the present invention is characterized in that in the film laminate of any one of the first to fourth aspects, the thickness of the metallic copper layer is within the range of 2 μm or more and 20 μm or less. According to the film laminate of the fifth aspect of the present invention, the thickness of the metallic copper layer is 2 μm or more, so that the influence of radiation loss can be suppressed and the transmission loss can be reliably kept low. Meanwhile, the thickness of the metallic copper layer is 20 μm or less, so that pattern formation by etching can be performed efficiently and accurately.

[0013] A film laminate according to a sixth aspect of the present invention is characterized in that in the film laminate according to any one of the first to fifth aspects, the electrical conductivity of the metallic copper layer is 80% IACS or more. According to the film laminate of embodiment 6 of the present invention, the electrical conductivity of the metallic copper layer is 80% IACS or more, and therefore the transmission characteristics are particularly excellent. Effect of the Invention

[0014] According to the present invention, it is possible to provide a film laminate which has particularly excellent adhesion between a fluororesin film having low transmission loss in the high frequency range and a metallic copper layer, and which does not significantly decrease in adhesion even when used in a high-temperature environment, and is particularly suitable for wiring boards for high-frequency signal transmission. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic diagram illustrating a film laminate according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flow diagram showing an example of a method for producing a film laminate according to the present embodiment. [Diagram 3] FIG. 2 is a diagram showing an example of an XRD measurement result in an example. [Figure 4] FIG. 2 is a schematic diagram of a peel test in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a film laminate according to one embodiment of the present invention will be described. The film laminate according to one embodiment of the present invention is used as a wiring board for transmitting high-frequency signals.

[0017] As shown in FIG. 1, the film laminate 10 of this embodiment includes a fluororesin film 11 and a metallic copper layer 12 laminated on this fluororesin film 11, and has a structure in which an amorphous oxide layer 13 is formed between the fluororesin film 11 and the metallic copper layer 12.

[0018] The fluororesin film 11 is made of a fluororesin such as PFA (perfluoroalkoxyalkane), PTFE (polytetrafluoroethylene), ETFE (ethylene-tetrafluoroethylene copolymer), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PCTFE (polychlorotrifluoroethylene), etc. Fluororesin has a low dielectric constant and low dielectric loss, and is therefore particularly suitable as a resin film constituting a wiring board for transmitting high-frequency signals. Here, the thickness t1 of the fluororesin film 11 is not particularly limited, but is preferably within the range of 5 μm to 200 μm.

[0019] The metallic copper layer 12 is made of copper or a copper alloy having excellent electrical and thermal conductivity, and functions as an electrically conductive layer or a heat transfer layer. Here, the electrical conductivity of the metallic copper layer 12 is preferably 80% IACS or more, and more preferably 85% IACS or more.

[0020] The thickness t2 of the metallic copper layer 12 is preferably within the range of 2 μm to 20 μm. If the thickness t2 of the metallic copper layer 12 is 2 μm or more, the effect of radiation loss can be ignored without being equivalent to the skin effect. On the other hand, if the thickness t2 of the metallic copper layer 12 is 20 μm or less, when a circuit pattern is formed on the metallic copper layer 12 by etching, the etching can be performed efficiently and accurately. The lower limit of the thickness t2 of the metallic copper layer 12 is more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the thickness t2 of the metallic copper layer 12 is more preferably 18 μm or less, and even more preferably 15 μm or less.

[0021] Between the fluororesin film 11 and the metallic copper layer 12, an amorphous oxide layer 13 made of an amorphous oxide is formed. This amorphous oxide layer 13 firmly bonds the fluororesin film 11 and the amorphous oxide layer 13 by chemical bonds COM (M is a component element contained in the amorphous oxide layer 13) via O (oxygen). Furthermore, the amorphous oxide layer 13 is chemically stable, and reaction between the amorphous oxide layer 13 and free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin film 11 is suppressed. Furthermore, since the amorphous oxide layer 13 has no grain boundaries and has excellent barrier properties, it can suppress interdiffusion between the fluororesin film 11 and the metallic copper layer 12, and can suppress a decrease in adhesion due to fluorination and oxidation of copper.

[0022] Here, the oxide constituting the amorphous oxide layer 13 preferably contains one or more elements selected from the group consisting of Ge, Si, Al, Ti, Ta, Zr, and Cr. When the oxides of these metals are formed into a film by sputtering or the like, an amorphous oxide film is formed, making it possible to ensure sufficient barrier properties.

[0023] Alternatively, the oxide constituting the amorphous oxide layer 13 preferably contains In and Zn. When the oxides of these metals are formed into a film by sputtering or the like, an amorphous oxide film is formed, making it possible to ensure sufficient barrier properties.

[0024] Moreover, the thickness t3 of the amorphous oxide layer 13 is preferably within the range of 10 nm to 100 nm. If the thickness t3 of the amorphous oxide layer 13 is 10 nm or more, the barrier property can be sufficiently ensured. On the other hand, if the thickness t3 of the amorphous oxide layer 13 is 100 nm or less, the occurrence of warping of the film due to membrane stress can be suppressed. The lower limit of the thickness t3 of the amorphous oxide layer 13 is more preferably 15 nm or more, and even more preferably 20 nm or more. The upper limit of the thickness t3 of the amorphous oxide layer 13 is more preferably 80 nm or less, and even more preferably 50 nm or less.

[0025] Next, a method for producing the film laminate 10 according to this embodiment will be described with reference to the flow chart of FIG.

[0026] (Fluororesin film preparation process S01) First, prepare the fluororesin film 11. For the purpose of introducing functional groups into the surface of the fluororesin film 11, a surface treatment such as a plasma treatment may be performed.

[0027] (Amorphous oxide layer forming step S02) Next, an amorphous oxide layer 13 is formed to a predetermined thickness on the surface of the fluororesin film 11 by sputtering. As the sputtering target, an oxide target of a predetermined composition may be used, or a metal target may be used to introduce oxygen for film formation.

[0028] (Seed layer formation process S03) Next, a copper layer is formed by sputtering as a seed layer for plating on the amorphous oxide layer 13. The thickness of the seed layer (sputtered copper layer) is preferably within a range of 10 nm to 1000 nm. It is preferable that the seed layer is formed continuously after the amorphous oxide layer 13 is formed, without exposing the layer to the atmosphere.

[0029] (Copper plating layer formation process S04) Next, after forming a seed layer, a copper plating layer of a predetermined thickness is formed by electrolytic plating. The seed layer and the copper plating layer constitute the metallic copper layer 12.

[0030] The film laminate 10 of this embodiment is manufactured by the above-mentioned steps. When forming the metallic copper layers 12 on both sides of the fluororesin film 11, the amorphous oxide layer forming step S02 and the seed layer forming step S03 may be performed on one side of the fluororesin film 11, and then the amorphous oxide layer forming step S02 and the seed layer forming step S03 may be performed on the opposite side, followed by the copper plating layer forming step S04.

[0031] According to the film laminate 10 of this embodiment configured as described above, the amorphous oxide layer 13 is formed on the surface of the fluororesin film 11, and therefore a chemical bond is formed via O (oxygen) on the outermost surface of the fluororesin film 11, and the fluororesin film 11 and the amorphous oxide layer 13 can be firmly bonded together. Furthermore, since the amorphous oxide layer 13 and the metallic copper layer 12 have good bonding properties, the adhesion between the fluororesin film 11 and the metallic copper layer 12 is particularly excellent. In addition, the amorphous oxide layer 13 is chemically stable, and the reaction between the amorphous oxide layer 13 and the free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin film 11 is suppressed, so that the decrease in adhesion can be suppressed even when the film is used in a high-temperature environment. Furthermore, the amorphous oxide layer 13 having no grain boundaries acts as a barrier layer, which can suppress interdiffusion between the fluororesin film 11 and the metallic copper layer 13 even when used in a high-temperature environment, and can suppress a decrease in adhesion due to fluorination and oxidation of copper.

[0032] In the film laminate 10 of this embodiment, when the thickness t3 of the amorphous oxide layer 13 is within the range of 10 nm or more and 100 nm or less, the barrier properties can be ensured, and the interdiffusion between the fluororesin and the metallic copper layer can be appropriately suppressed, and warping of the film due to membrane stress can be suppressed.

[0033] In the film laminate 10 of this embodiment, when the oxide constituting the amorphous oxide layer 13 contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr, the amorphous oxide layer 13 is even more chemically stable, and it is possible to further suppress the reaction between the amorphous oxide layer 13 and the free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin. Moreover, an amorphous oxide film can be formed by sputtering, and the barrier properties of the amorphous oxide layer 13 can be sufficiently ensured.

[0034] In the film laminate 10 of this embodiment, when In and Zn are contained, the amorphous oxide layer 13 is even more chemically stable, and it is possible to further suppress the reaction between the amorphous oxide layer 13 and the free F (fluorine) and adsorbed O (oxygen) present on the surface of the fluororesin. Moreover, an amorphous oxide film can be formed by sputtering, and the barrier properties of the amorphous oxide layer 13 can be sufficiently ensured.

[0035] In the film laminate 10 of this embodiment, when the thickness t2 of the metal copper layer 12 is within the range of 2 μm or more and 20 μm or less, the effect of radiation loss can be suppressed, the transmission loss can be reliably kept low, and pattern formation by etching can be performed efficiently and accurately. Furthermore, in the film laminate 10 of this embodiment, when the electrical conductivity of the metallic copper layer 13 is 80% IACS or more, the transmission characteristics are particularly excellent.

[0036] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES

[0037] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.

[0038] A PFA film (thickness: 50 μm) manufactured by AGC was prepared as the fluororesin film. An oxide layer shown in Table 1 was formed on the surface of this fluororesin film by sputtering. The oxide layer was formed under the following conditions. In Comparative Example 3, a metal Ti film was formed as the intermediate layer using a Ti target.

[0039] (Oxide layer deposition conditions) Target material: Si, Al, Ti, Ta, Zr, Cr, Ge, Zn, In, Sn, IZO (85at%In-15at%Zn composite oxide) (purity 99.9mass% or more) Deposition start vacuum degree: 1.0×10 -4 Pa or less Sputtering gas: A mixture of high-purity argon and high-purity oxygen Sputtering gas pressure in the chamber: 0.2 Pa DC power density: 7.5W / cm 2 (Si,Al,Ti,Ta,Zr,Cr,Zn,In,Sn,IZO) AC power density: 10.0W / cm 2 (Ge)

[0040] Next, a copper layer was formed to a thickness of 100 nm as a seed layer for plating by sputtering under the following sputtering conditions: The seed layer was formed continuously after the intermediate layer was formed without exposure to the atmosphere. (Seed layer deposition conditions) Target material: Cu (purity 99.99 mass% or more) Deposition start vacuum degree: 1.0×10 -4 Pa or less Sputtering gas: High purity argon Sputtering gas pressure in the chamber: 0.2 Pa DC power density: 7.5W / cm 2

[0041] Next, a copper plating layer was formed on the seed layer by electrolytic plating under the following conditions: The thickness of the metallic copper layer shown in Table 1 is the total thickness of the seed layer and the copper plating layer. (Electrolytic plating conditions) Pretreatment: Sulfuric acid washing Liquid temperature: 25℃ Anode: phosphorus-containing copper Stirring conditions: Air 12.5L / min Plating conditions: 4A, 45min (time for film thickness 15μm) Plating solution: CuSO4·5H2O 200g / L H2SO4 54g / L 1mol HCl 1.37mL / L

[0042] The film laminate produced as described above was evaluated for the crystallinity of the intermediate layer (oxide layer), the thickness of the intermediate layer, the thickness of the metallic copper layer, the electrical conductivity of the metallic copper layer, the adhesive strength, and the heat resistance as described below. The evaluation results are shown in Table 1.

[0043] (Crystallization of the intermediate layer) A single oxide film of 50 nm was formed on a fluororesin film, and the presence or absence of crystallinity of the intermediate layer (oxide layer) was determined by measuring it using the GI-XRD method (Rigaku SmartLab). The incident X-ray was Cu Kα radiation, and the measurement was performed with an X-ray incidence angle of ω = 0.5° and a detection range of 2θ = 10 to 110°. An example of the XRD measurement result is shown in Figure 3. As shown in Fig. 3, in Example 6, the pattern is similar to that of the fluororesin film (reference data), and no peak indicating crystallinity is observed. On the other hand, in Comparative Example 1, a peak indicating crystallinity (see the arrow in Fig. 3) is observed.

[0044] (Thickness of middle layer) The thickness of the intermediate layer is the target value based on the deposition rate. The deposition rate was calculated by measuring the film thickness after deposition on a dummy substrate for a certain period of time using a step measurement device (Dektak-XT by Bruker) and dividing the film thickness by the deposition time. The thickness of the intermediate layer was confirmed by observing the cross section of the film laminate with a TEM (transmission electron microscope: JEM-2010F manufactured by JEOL Ltd.), and was found to be equivalent to the target value based on the film formation rate.

[0045] (Thickness of metallic copper layer) The thickness of the metallic copper layer (seed layer and copper plating layer) was confirmed by an eddy current method.

[0046] (Conductivity of the metallic copper layer) Conductivity of the metallic copper layer σ A The resistivity (S / m) was measured by the four-probe method using a low resistivity meter (Loresta GP, manufactured by Mitsubishi Chemical Corporation), and was converted to %IACS using the following formula. σ(%IACS)=σ A / (5.8×10 7 )

[0047] (Adhesion strength) As shown in Figure 4, the intermediate layer and metallic copper layer formed on the fluororesin film were cut into 5 mm widths and evaluated using an A&D Corporation Tensilon universal testing machine (RTF-1310) at a peel angle of 90 degrees and a peel speed of 50 mm / min.

[0048] (Heat resistance test) As a heat resistance test, the film laminate was stored in a clean oven under the conditions of 150°C x 240h. After storage, the adhesion strength of the film laminate was measured as described above. Then, the rate of change in adhesion strength before and after the heat resistance test was calculated. (Change rate) = (Adhesion strength after test - Adhesion strength before test) / Adhesion strength before test × 100 (%)

[0049] [Table 1]

[0050] In Comparative Example 1, a crystalline Zn oxide layer was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the adhesion strength significantly decreased after the heat resistance test. This is presumably because interdiffusion occurred between the fluororesin sheet and the metallic copper layer, causing the copper to be fluorinated and oxidized. In Comparative Example 2, a crystalline In-Sn oxide layer (ITO layer) was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the adhesion strength significantly decreased after the heat resistance test. This is presumably because interdiffusion occurred between the fluororesin sheet and the metallic copper layer, causing the copper to be fluorinated and oxidized.

[0051] In Comparative Example 3, a metallic Ti layer was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the adhesion strength was significantly reduced after the heat resistance test. This is presumably because the metallic Ti layer, which was the intermediate layer, was fluorinated and oxidized. In Comparative Example 4, a metallic copper layer was formed directly on a fluororesin film without forming an intermediate layer, but the initial adhesive strength was low and the adhesive strength was significantly reduced after the heat resistance test.

[0052] In contrast, in Examples 1 to 22, an amorphous oxide layer was formed as an intermediate layer between the fluororesin film and the metallic copper layer, and the initial adhesion was excellent. The adhesion strength did not decrease significantly even after the heat resistance test, and the heat resistance was excellent.

[0053] From the above, it was confirmed that the examples can provide a film laminate that is particularly suitable for wiring boards for high-frequency signal transmission, since the adhesion between the fluororesin film, which has low transmission loss in the high-frequency range, and the metallic copper layer is particularly excellent and the adhesion does not decrease significantly even when used in a high-temperature environment.

Claims

1. A film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, A film laminate, comprising an amorphous oxide layer formed between the fluororesin film and the metallic copper layer.

2. 2. The film laminate according to claim 1, wherein the amorphous oxide layer has a thickness in the range of 10 nm to 100 nm.

3. 3. The film laminate according to claim 1, wherein the oxide constituting the amorphous oxide layer contains one or more elements selected from the group consisting of Ge, Si, Al, Ti, Ta, Zr, and Cr.

4. 3. The film laminate according to claim 1, wherein the oxide constituting the amorphous oxide layer contains In and Zn.

5. 3. The film laminate according to claim 1, wherein the thickness of the metallic copper layer is within a range of 2 μm or more and 20 μm or less.

6. 3. The film laminate according to claim 1, wherein the electrical conductivity of the metallic copper layer is 80% IACS or more.

Citation Information

Patent Citations

  • Ag ALLOY FILM AND METHOD OF MANUFACTURING THE SAME

    JP2014019932A

  • Metalized film and production method therefor

    WO2018179904A1