Film laminate, and sputtering target
The film laminate with a Ta alloy layer and controlled thicknesses addresses adhesion and heat resistance issues, ensuring low transmission loss and efficient pattern formation for high-frequency signal transmission.
Patent Information
- Application Number
- JP2023052700
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing film laminates with fluororesin and metal layers face issues of reduced adhesion due to chemical stability and oxidation, leading to increased transmission loss and poor heat resistance, especially in high-frequency and high-temperature environments.
A film laminate with a Ta alloy layer containing Mg and Ge between the fluororesin film and metal copper layer, which enhances adhesion by activating the fluororesin surface and suppressing chemical reactions, and a thickness range of 10 nm to 100 nm for the Ta alloy layer and 2 μm to 20 μm for the copper layer to maintain low transmission loss and structural integrity.
The laminate achieves excellent adhesion and heat resistance, maintaining low transmission loss and enabling efficient pattern formation, suitable for high-frequency signal transmission even in harsh environments.
Smart Images

Figure 2024141192000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, and to a sputtering target used in producing the film laminate. [Background technology]
[0002] Generally, as wiring substrates for use in electronic and electric devices, film laminates in which a metallic copper layer is laminated as a conductive layer or a heat transfer layer on the surface of an insulating resin layer are used. Here, wiring boards for high-frequency signal transmission devices such as antennas and radars in the GHz band or above are required to have low transmission loss when used in the high-frequency range. In view of this, for example, film laminates using fluororesin films have been provided as shown in Patent Documents 1 and 2. Fluororesins have a low dielectric constant and low dielectric loss, and are therefore particularly suitable as resin films constituting wiring boards for high-frequency signal transmission.
[0003] Incidentally, since the surface of a fluororesin film is very chemically stable, the adhesive strength with other materials tends to be low. Therefore, in Patent Document 1, protrusions are formed on the surface of the fluororesin, the metal foil is roughened, and the conditions for pressure lamination are optimized to improve the adhesion between the copper film and the fluororesin through the anchor effect. In addition, in Patent Document 2, a thin metal film (nickel film or titanium film) is formed on the surface of the fluororesin by physical vapor deposition, and then a copper film is formed by copper plating on this thin metal film, thereby improving the adhesion between the copper film and the fluororesin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-019932 A [Patent Document 2] International Publication No. 2018 / 179904 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in Patent Document 1, the interface between the fluororesin and the metal foil becomes rough, which causes an increase in transmission loss. Furthermore, in Patent Document 2, when used in a high-temperature environment, the thin metal film formed on the surface of the fluororesin may oxidize, resulting in a decrease in adhesion, and the heat resistance was insufficient.
[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a film laminate that is particularly suitable for wiring boards for high-frequency signal transmission, having particularly excellent adhesion between a fluororesin film with low transmission loss in the high-frequency range and a metallic copper layer, and that does not significantly decrease in adhesion even when used in a high-temperature environment, and a sputtering target for use in producing this film laminate. [Means for solving the problem]
[0007] In order to solve the above problems, the film laminate of aspect 1 of the present invention is a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, and is characterized in that a Ta alloy layer is formed between the fluororesin film and the metallic copper layer, the Ta alloy layer containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % or more and 50.0 atomic % or less, with the remainder being Ta and unavoidable impurities.
[0008] According to the film laminate of the first aspect of the present invention, a Ta alloy layer is formed on the surface of the fluororesin film, the Ta alloy layer being composed of a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % to 50.0 atomic % with the remainder being Ta and unavoidable impurities, so that Mg and Ge can extract F from the C-F bonds on the outermost surface of the fluororesin to form dangling bonds, resulting in an active surface and realizing a strong bond with the Ta alloy of the parent phase. In addition, the Ta alloy layer and the metallic copper layer have good bonding properties, so that the adhesion between the fluororesin film and the metallic copper layer is particularly excellent. In addition, Ta is chemically stable and is less likely to react with free F (fluorine) or adsorbed O (oxygen) on the surface of the fluororesin, making it possible to prevent a decrease in adhesion even when used in a high-temperature environment.
[0009] The film laminate of the second aspect of the present invention is characterized in that in the film laminate of the first aspect, the thickness of the Ta alloy layer is within the range of 10 nm or more and 100 nm or less. According to the film laminate of the second aspect of the present invention, the thickness of the Ta alloy layer is 10 nm or more, so that it is possible to reliably improve the adhesion between the fluororesin film and the metallic copper layer, while the thickness of the Ta alloy layer is 100 nm or less, so that warping of the film due to membrane stress can be suppressed.
[0010] The film laminate of the third aspect of the present invention is characterized in that in the film laminate of the first or second aspect, the thickness of the metallic copper layer is within the range of 2 μm or more and 20 μm or less. According to the film laminate of the third aspect of the present invention, the thickness of the metallic copper layer is 2 μm or more, so that the influence of radiation loss can be suppressed and the transmission loss can be reliably kept low. Meanwhile, the thickness of the metallic copper layer is 20 μm or less, so that pattern formation by etching can be performed efficiently and accurately.
[0011] A film laminate according to a fourth aspect of the present invention is characterized in that in the film laminate according to any one of the first to third aspects, the electrical conductivity of the metallic copper layer is 80% IACS or more. According to the film laminate of the fourth aspect of the present invention, the electrical conductivity of the metallic copper layer is 80% IACS or more, and therefore the transmission characteristics are particularly excellent.
[0012] The sputtering target of the fifth aspect of the present invention is a sputtering target used for forming a Ta alloy layer formed between a fluororesin film and a metallic copper layer, and is characterized in that it is made of a Ta alloy having a composition containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % or more and 50.0 atomic % or less, with the remainder being Ta and unavoidable impurities.
[0013] According to the sputtering target of aspect 5 of the present invention, the target is composed of a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % or more and 50.0 atomic % or less, with the remainder being Ta and unavoidable impurities. Therefore, in a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, a Ta alloy layer can be formed as an intermediate layer between the fluororesin film and the metallic copper layer, and a film laminate having excellent adhesion and heat resistance between the fluororesin film and the metallic copper layer can be produced. Effect of the Invention
[0014] According to the present invention, it is possible to provide a film laminate that is particularly suitable for wiring boards for high-frequency signal transmission, having excellent adhesion between a fluororesin film with low transmission loss in the high-frequency range and a metallic copper layer, and in which the adhesion does not decrease significantly even when used in a high-temperature environment, and a sputtering target used in producing this film laminate. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram illustrating a film laminate according to an embodiment of the present invention. [Diagram 2]FIG. 2 is a flow diagram showing an example of a method for producing a film laminate according to the present embodiment. [Diagram 3] FIG. 2 is a schematic diagram of a peel test in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, a film laminate according to one embodiment of the present invention will be described. The film laminate according to one embodiment of the present invention is used as a wiring board for transmitting high-frequency signals.
[0017] As shown in FIG. 1, the film laminate 10 of this embodiment includes a fluororesin film 11 and a metallic copper layer 12 laminated on this fluororesin film 11, and has a structure in which a Ta alloy layer 13 is formed between the fluororesin film 11 and the metallic copper layer 12.
[0018] The fluororesin film 11 is made of a fluororesin such as PFA (perfluoroalkoxyalkane), PTFE (polytetrafluoroethylene), ETFE (ethylene-tetrafluoroethylene copolymer), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PCTFE (polychlorotrifluoroethylene), etc. Fluororesin has a low dielectric constant and low dielectric loss, and is therefore particularly suitable as a resin film constituting a wiring board for transmitting high-frequency signals. Here, the thickness t1 of the fluororesin film 11 is not particularly limited, but is preferably within the range of 5 μm to 200 μm.
[0019] The metallic copper layer 12 is made of copper or a copper alloy having excellent electrical and thermal conductivity, and functions as an electrically conductive layer or a heat transfer layer. Here, the electrical conductivity of the metallic copper layer 12 is preferably 80% IACS or more, and more preferably 85% IACS or more.
[0020] The thickness t2 of the metallic copper layer 12 is preferably within the range of 2 μm to 20 μm. If the thickness t2 of the metallic copper layer 12 is 2 μm or more, the effect of radiation loss can be ignored without being equivalent to the skin effect. On the other hand, if the thickness t2 of the metallic copper layer 12 is 20 μm or less, when a circuit pattern is formed on the metallic copper layer 12 by etching, the etching can be performed efficiently and accurately. The lower limit of the thickness t2 of the metallic copper layer 12 is more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the thickness t2 of the metallic copper layer 12 is more preferably 18 μm or less, and even more preferably 15 μm or less.
[0021] Between the fluororesin film 11 and the metallic copper layer 12, there is formed a Ta alloy layer 13 made of a Ta alloy having a composition containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % or more and 50.0 atomic % or less, with the remainder being Ta and unavoidable impurities. The Mg and Ge contained in this Ta alloy layer 13 extract F from the C-F bonds on the outermost surface of the fluororesin film 11 to form dangling bonds, activate the surface, and achieve strong bonds with the Ta parent phase, significantly improving the adhesion between the fluororesin film 11 and the Ta alloy layer 13. Furthermore, since Ta is chemically stable, even when the film is used in a high-temperature environment, the reaction between the Ta alloy layer 13 and the free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin film 11 is suppressed, thereby improving the heat resistance.
[0022] If the total content of at least one or two of Mg and Ge in the Ta alloy layer 13 is less than 0.5 atomic %, the surface of the fluororesin film may not be sufficiently activated. On the other hand, if the total content of at least one or two of Mg and Ge in the Ta alloy layer 13 exceeds 50.0 atomic %, the Ta content may be insufficient, and the heat resistance may not be sufficiently improved. The lower limit of the total content of at least one or two of Mg and Ge in the Ta alloy layer 13 is preferably 1.0 atomic % or more, and more preferably 2.0 atomic % or more. On the other hand, the upper limit of the total content of at least one or two of Mg and Ge in the Ta alloy layer 13 is preferably 40.0 atomic % or less, and more preferably 20.0 atomic % or less.
[0023] Moreover, the thickness t3 of the Ta alloy layer 13 is preferably within the range of 10 nm to 100 nm. When the thickness t3 of the Ta alloy layer 13 is 10 nm or more, it is possible to sufficiently improve the adhesion between the fluororesin film 11 and the metallic copper layer 12. On the other hand, when the thickness t3 of the Ta alloy layer 13 is 100 nm or less, it is possible to suppress the warping of the film due to the membrane stress. The lower limit of the thickness t3 of the Ta alloy layer 13 is more preferably 15 nm or more, and even more preferably 20 nm or more. The upper limit of the thickness t3 of the Ta alloy layer 13 is more preferably 80 nm or less, and even more preferably 50 nm or less.
[0024] Next, a method for producing the film laminate 10 according to this embodiment will be described with reference to the flow chart of FIG.
[0025] (Fluororesin film preparation process S01) First, prepare the fluororesin film 11. For the purpose of introducing functional groups into the surface of the fluororesin film 11, a surface treatment such as a plasma treatment may be performed.
[0026] (Ta alloy layer formation step S02) Next, a Ta alloy layer 13 is formed to a predetermined thickness on the surface of the fluororesin film 11 by sputtering. Here, in the Ta alloy layer forming step S02, the sputtering target of this embodiment is used to form the Ta alloy layer 13. The sputtering target of this embodiment is configured to be a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % to 50.0 atomic % with the remainder being Ta and unavoidable impurities.
[0027] (Seed layer formation process S03) Next, a copper layer is formed by sputtering as a seed layer for plating on the Ta alloy layer 13. The thickness of the seed layer (sputtered copper layer) is preferably within a range of 10 nm to 1000 nm. The seed layer is preferably formed successively after the above-mentioned Ta alloy layer 13 is formed, without being exposed to the atmosphere.
[0028] (Copper plating layer formation process S04) Next, after forming a seed layer, a copper plating layer of a predetermined thickness is formed by electrolytic plating. The seed layer and the copper plating layer constitute the metallic copper layer 12.
[0029] The film laminate 10 of this embodiment is manufactured by the above-mentioned steps. When forming the metallic copper layers 12 on both sides of the fluororesin film 11, the Ta alloy layer forming step S02 and the seed layer forming step S03 may be performed on one side of the fluororesin film 11, and then the Ta alloy layer forming step S02 and the seed layer forming step S03 may be performed on the opposite side, followed by the copper plating layer forming step S04.
[0030] According to the film laminate 10 of the present embodiment configured as described above, the Ta alloy layer 13 made of a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % to 50.0 atomic % and the remainder being Ta and unavoidable impurities is formed on the surface of the fluororesin film 11, so that Mg and Ge can extract F from the C-F bonds on the outermost surface of the fluororesin film 11 to form dangling bonds, activating the surface of the fluororesin film 11 and realizing a strong bond with the Ta alloy of the parent phase. In addition, since the Ta alloy layer 13 and the metallic copper layer 12 have good bondability, the adhesion between the fluororesin film 11 and the metallic copper layer 12 is particularly excellent. In addition, since Ta is chemically stable, it is suppressed from reacting with free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin film 11, and therefore it is possible to suppress a decrease in adhesion even when the film is used in a high-temperature environment.
[0031] In the film laminate 10 of this embodiment, when the thickness t3 of the Ta alloy layer 13 is within the range of 10 nm or more and 100 nm or less, the adhesion between the fluororesin film 11 and the metallic copper layer 12 can be reliably improved, and warping of the film due to membrane stress can be suppressed.
[0032] In the film laminate 10 of this embodiment, when the thickness t2 of the metal copper layer 12 is within the range of 2 μm or more and 20 μm or less, the effect of radiation loss can be suppressed, the transmission loss can be reliably kept low, and pattern formation by etching can be performed efficiently and accurately. Furthermore, in the film laminate 10 of this embodiment, when the electrical conductivity of the metallic copper layer 13 is 80% IACS or more, the transmission characteristics are particularly excellent.
[0033] According to the sputtering target of this embodiment, a Ta alloy layer 13 made of a Ta alloy containing at least one or two of Mg and Ge in a total amount ranging from 0.5 atomic % to 50.0 atomic % and the remainder being Ta and unavoidable impurities can be formed as an intermediate layer between the fluororesin film 11 and the metallic copper layer 12, and a film laminate 10 having excellent adhesion between the fluororesin film 11 and the metallic copper layer 12 and excellent heat resistance can be produced.
[0034] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES
[0035] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.
[0036] A PFA film (thickness: 50 μm) manufactured by AGC was prepared as the fluororesin film. On the surface of this fluororesin film, a Ta alloy layer having the composition shown in Table 1 was formed as an intermediate layer by sputtering. The film formation conditions are shown below. The atomic percentage of Mg / Ge was set to be the same as the mixture ratio of the target material.
[0037] Target material: Ta-Ge alloy, Ta-Mg alloy, Ta-Ge-Mg alloy Deposition start vacuum degree: 1.0×10 -4 Pa or less Sputtering gas: High purity argon Sputtering gas pressure in chamber: 0.2 Pa DC power density: 7.5W / cm 2
[0038] Next, a copper layer was formed to a thickness of 100 nm as a seed layer for plating by sputtering under the following sputtering conditions: The seed layer was formed continuously after the intermediate layer was formed without exposure to the atmosphere. (Seed layer deposition conditions) Target material: Cu (purity 99.99 mass% or more) Deposition start vacuum degree: 1.0×10 -4 Pa or less Sputtering gas: High purity argon Sputtering gas pressure in chamber: 0.2 Pa DC power density: 7.5W / cm 2
[0039] Next, a copper plating layer was formed on the seed layer by electrolytic plating under the following conditions: The thickness of the metallic copper layer shown in Table 1 is the total thickness of the seed layer and the copper plating layer. (Electrolytic plating conditions) Pretreatment: Sulfuric acid washing Liquid temperature: 25℃ Anode: phosphorus-containing copper Stirring conditions: Air 12.5L / min Plating conditions: 4A, 45min Plating solution: CuSO4·5H2O 200g / L H2SO4 54g / L 1mol HCl 1.37mL / L
[0040] The film laminate produced as described above was evaluated for the thickness of the intermediate layer (Ta alloy layer), the thickness of the metallic copper layer, the electrical conductivity of the metallic copper layer, the adhesive strength, and the heat resistance as described below. The evaluation results are shown in Table 1.
[0041] (Thickness of middle layer) The thickness of the intermediate layer is the target value based on the deposition rate. The deposition rate was calculated by measuring the film thickness after deposition on a dummy substrate for a certain period of time using a step measurement device (Dektak-XT by Bruker) and dividing the film thickness by the deposition time. Furthermore, the thickness of the intermediate layer was confirmed by observing the cross section of the film laminate with a TEM (transmission electron microscope), and was found to be equivalent to the target value based on the film formation rate.
[0042] (Thickness of metallic copper layer) The thickness of the metallic copper layer (seed layer and copper plating layer) was confirmed by an eddy current method.
[0043] (Conductivity of the metallic copper layer) Conductivity of the metallic copper layer σ A The resistivity (S / m) was measured by the four-probe method using a low resistivity meter (Loresta GP, manufactured by Mitsubishi Chemical Corporation), and was converted to %IACS using the following formula. σ(%IACS)=σ A / (5.8×10 7 )
[0044] (Adhesion strength) As shown in Figure 3, the intermediate layer and metallic copper layer formed on the fluororesin film were cut into 5 mm widths and evaluated using an A&D Tensilon universal testing machine (RTF-1310) at a peel angle of 90 degrees and a peel speed of 50 mm / min.
[0045] (Heat resistance test) As a heat resistance test, the film laminate was stored in a clean oven under the conditions of 150°C x 240h. After storage, the adhesion strength of the film laminate was measured as described above. Then, the rate of change in adhesion strength before and after the heat resistance test was calculated. (Change rate) = (Adhesion strength after test - Adhesion strength before test) / Adhesion strength before test × 100 (%)
[0046] [Table 1]
[0047] In Comparative Examples 1 and 3, a Ta alloy layer with a total content of Ge and Mg of 0.1 atomic % was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the initial adhesion strength was relatively low. This is presumably because the surface of the fluororesin film could not be sufficiently activated. In Comparative Examples 2 and 4, a Ta alloy layer with a total content of Ge and Mg of 60.0 atomic % was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the adhesion strength was significantly reduced after the heat resistance test. This is presumably because the Ta content was low and the reaction between the Ta alloy layer and fluorine and oxygen could not be sufficiently suppressed.
[0048] In contrast, in Examples 1 to 23 of the present invention, an intermediate layer was formed between the fluororesin film and the metallic copper layer, which was a Ta alloy layer composed of a Ta alloy containing at least one or both of Mg and Ge in a total amount ranging from 0.5 atomic % to 50.0 atomic %, with the remainder being Ta and unavoidable impurities. This had excellent initial adhesion, and even after the heat resistance test, the adhesion strength did not decrease significantly, indicating excellent heat resistance.
[0049] From the above, it was confirmed that the present invention can provide a film laminate that is particularly suitable for wiring boards for high-frequency signal transmission, which has excellent adhesion between a fluororesin film with low transmission loss in the high-frequency range and a metallic copper layer, and which does not significantly decrease in adhesion even when used in a high-temperature environment, as well as a sputtering target used in producing this film laminate.
Claims
1. A film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, A film laminate characterized in that a Ta alloy layer is formed between the fluororesin film and the metallic copper layer, the Ta alloy layer comprising a Ta alloy having a composition containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % or more and 50.0 atomic % or less, with the remainder being Ta and unavoidable impurities.
2. 2. The film laminate according to claim 1, wherein the Ta alloy layer has a thickness in the range of 10 nm to 100 nm.
3. 2. The film laminate according to claim 1, wherein the thickness of the metallic copper layer is within a range of 2 μm or more and 20 μm or less.
4. 2. The film laminate according to claim 1, wherein the electrical conductivity of the metallic copper layer is 80% IACS or more.
5. A sputtering target used in forming a Ta alloy layer formed between a fluororesin film and a metallic copper layer, comprising: A sputtering target comprising a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % or more and 50.0 atomic % or less, with the remainder being Ta and unavoidable impurities.
Citation Information
Patent Citations
Ag ALLOY FILM AND METHOD OF MANUFACTURING THE SAME
JP2014019932A
Metalized film and production method therefor
WO2018179904A1