Liquid crystal polyester

A liquid crystal polyester resin with specific structural units addresses thermal expansion anisotropy and high-temperature molding issues, ensuring low dielectric loss and improved dimensional accuracy for high-frequency applications.

JP2024141356AInactive Publication Date: 2024-10-10KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052953
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Liquid crystal polyester resins exhibit high thermal expansion anisotropy and require high-temperature molding, which complicates their use in high-frequency communication applications and affects dimensional accuracy in FPC boards.

Method used

A liquid crystal polyester resin composition with a specific structural unit content of 1.0 to 20.0 mol% and a combination of aromatic oxycarbonyl, dioxy, and dicarboxy units, along with an alkyl chain, achieving a low dielectric loss tangent and reduced thermal expansion anisotropy, is developed.

Benefits of technology

The resin achieves low dielectric loss tangent, low melting temperature, and small CTE anisotropy, enhancing dimensional accuracy and suitability for high-frequency communications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a liquid crystal polyester resin having excellent dielectric tangent in a high frequency region and excellent aeolotropy of thermal expansion.SOLUTION: A liquid crystal polyester resin includes: at least one kind of structural unit (A) selected from an aromatic oxycarbonyl unit, an aromatic dioxy unit, and an aromatic dicarboxy unit; and a specific amount of the following structural unit (B).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal polyester resin, a method for producing the liquid crystal polyester resin, a liquid crystal polyester resin composition using the liquid crystal polyester resin, a film formed from the liquid crystal polyester resin, and a metal-clad laminate and a printed circuit board each including the film. [Background technology]

[0002] Liquid crystal polymers are known to have excellent heat resistance, electrical insulation, chemical stability, and mechanical strength, and are used in various applications such as electrical and electronic fields, optical devices, automobiles, and medical fields. Among them, liquid crystal polyesters (LCPs) in particular have excellent dielectric properties and low moisture absorption, and are therefore attracting attention for use as electronic circuit board materials. For example, flexible copper-clad laminates (hereinafter also referred to as FCCLs), in which copper foil is laminated on at least one side of an LCP film as a circuit board material, and flexible printed circuit boards (hereinafter also referred to as FPCs), in which a circuit is further formed on an FCCL, are used in various electronic devices.

[0003] With the recent spread of high-frequency communications such as 5G and 6G, even faster and larger data volumes are expected. However, there are concerns about delays due to transmission losses of electrical signals as the electrical signals propagate through circuits at higher frequencies in association with high-speed signal transmission in electronic devices. To reduce this transmission loss, there is a demand for electronic circuit board materials with lower dielectric constants and lower dielectric loss tangents.

[0004] Liquid crystal polyester resins with low dielectric loss tangents are known as materials that meet these requirements. Generally, fully aromatic polyesters are used for such liquid crystal polyester resins, which have a rigid molecular structure, small dipole properties, and little movement even when an electric field is applied, so that they have excellent dielectric loss tangents even in high frequency environments of 10 GHz or more. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-175995 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in general, liquid crystal polyester resins have low water absorption and low dielectric tangent as film properties, but the molecular chains are highly oriented, so there is a drawback in that there is a large difference in the coefficient of thermal expansion (hereinafter also referred to as CTE) between the planar direction and the thickness direction of the film. Therefore, there was a concern that the dimensional accuracy would be significantly deteriorated during FPC board processing. As a solution to this problem, as described in Patent Document 1, it has been reported that the anisotropy of CTE can be eliminated by blending one or more thermoplastic resins with liquid crystal polyester, but there is a concern that the dielectric tangent will deteriorate, making it difficult to use for high-frequency communication applications. In addition, since liquid crystal polyesters are generally not soluble in general-purpose solvents, film formation by melt molding is mainstream, but liquid crystal polyesters composed only of rigid aromatic monomers have a problem that the molecular chains are densely oriented and must be molded under high-temperature conditions exceeding 300 ° C.

[0007] The present invention has been made in consideration of the above problems, and aims to provide a liquid crystal polyester resin having a low dielectric tangent in the high frequency range, a low melting temperature, and small CTE anisotropy, a method for producing the liquid crystal polyester resin, a liquid crystal polyester resin composition using the liquid crystal polyester resin, a film molded from the liquid crystal polyester resin, and a metal-clad laminate and a printed circuit board including the film. [Means for solving the problem]

[0008] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. That is, the present invention provides the following 1) to 11).

[0009] 1) A liquid crystal polyester resin comprising at least one structural unit (A) selected from an aromatic oxycarbonyl unit, an aromatic dioxy unit, and an aromatic dicarboxy unit, and a structural unit (B) having an alkyl chain, the content of the structural unit (B) being in the range of 1.0 to 20.0 mol % based on the total structural units constituting the liquid crystal polyester. (n is an integer of 2 to 18. R is an aromatic unit.)

[0010] [ka]

[0011] [ka] 2) The liquid crystal polyester resin according to 1), having a dielectric tangent value of 0.00300 or less at 28 GHz.

[0012] 3) The liquid crystal polyester resin according to 1) or 2), wherein the aromatic skeleton of the structural unit (A) contains a benzene skeleton in the range of 20 to 70 mol % and a naphthalene skeleton in the range of 20 to 80 mol %.

[0013] 4) The liquid crystal polyester resin according to any one of 1) to 3), wherein the monomer constituting the aromatic oxycarbonyl unit is 4-hydroxybenzoic acid and / or 6-hydroxy-2-naphthoic acid.

[0014] 5) The liquid crystal polyester resin according to any one of 1) to 4), wherein the monomer constituting the aromatic dicarboxy unit is terephthalic acid and / or 2,6-naphthalenedicarboxylic acid.

[0015] 6) The liquid crystal polyester resin according to any one of 1) to 5), wherein the monomer constituting the aromatic dioxy unit is hydroquinone and / or 2,6-dihydroxynaphthalene.

[0016] 7) A liquid crystal polyester resin composition comprising the liquid crystal polyester resin according to any one of 1) to 6) and an inorganic or organic filler.

[0017] 8) A film obtained by molding the liquid crystal polyester resin according to any one of 1) to 6) or the liquid crystal polyester resin composition according to 7).

[0018] 9). A metal-clad laminate having the film described in 8).

[0019] 10). A printed circuit board having the film described in 8).

[0020] 11) A method for producing a liquid crystal polyester resin according to any one of 1) to 6), comprising producing the liquid crystal polyester resin according to any one of 1) to 6) above by using an aliphatic monomer having an aromatic ester terminal represented by structural formula (C). (Ar is an aromatic unit, and n is an integer of 2 to 18.)

[0021] [ka] Effect of the Invention

[0022] According to the present invention, it is possible to provide a liquid crystal polyester resin having a low dielectric tangent in the high frequency range, a low melting temperature, and small CTE anisotropy, a method for producing the liquid crystal polyester resin, a liquid crystal polyester resin composition using the liquid crystal polyester resin, a film molded from the liquid crystal polyester resin, and a metal-clad laminate and a printed circuit board including the film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] [Liquid crystal polyester] The liquid crystal polyester resin of the present invention is composed of structural units (A) and (B) and is a polyester that exhibits liquid crystallinity, i.e., an anisotropic molten phase when heated. It is usually called a thermotropic liquid crystal polyester in the technical field, but is not particularly limited thereto. (Note that n is an integer of 2 to 18, and R is an aromatic unit.)

[0024] [ka]

[0025] [ka] R in the structural unit (A) is preferably an aromatic unit, more preferably benzene or naphthalene.

[0026] The aromatic oxycarbonyl unit, aromatic dioxy unit, and aromatic dicarboxy unit constituting the structural unit (A) may be of a plurality of different types in combination, but a composition containing at least an aromatic oxycarbonyl unit is preferred.

[0027] The aromatic oxycarbonyl unit of the structural unit (A) is composed of an aromatic hydroxycarboxylic acid. Specific examples of aromatic hydroxycarboxylic acid include 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 2-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 6-hydroxy-1-naphthoic acid, 7-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 7-hydroxy-1-naphthoic acid, 4'-hydroxyphenyl-4-benzoic acid, 3'-hydroxyphenyl-4-benzoic acid, 4'-hydroxyphenyl-3-benzoic acid, and their alkyl, alkoxy or halogen substitution products. Among these, 4-hydroxybenzoic acid or 6-hydroxy-2-naphthoic acid or a combination thereof can be more preferably used in terms of the heat resistance and dielectric properties of the obtained liquid crystal polyester, as well as the ease of adjusting the melting point. Ester derivatives of aromatic hydroxycarboxylic acids and ester-forming derivatives such as acid halides can also be suitably used in the same manner as aromatic hydroxycarboxylic acids.

[0028] The aromatic dicarboxy unit of the structural unit (A) is composed of aromatic dicarboxylic acid. Specific examples of aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 4,4'-dicarboxybiphenyl, 3,4'-dicarboxybiphenyl, 4,4'-dicarboxydiphenyl ether, and 4,4'-dicarboxyterphenyl, and alkyl, alkoxy, or halogen-substituted derivatives thereof. Among these, terephthalic acid or 2,6-naphthalenedicarboxylic acid or a combination thereof can be preferably used.

[0029] Ester derivatives of aromatic dicarboxylic acids and ester-forming derivatives such as acid halides can also be suitably used in the same manner as aromatic dicarboxylic acids.

[0030] The aromatic dioxy unit of the structural unit (A) is composed of an aromatic diol. Specific examples of aromatic diols include hydroquinone, resorcin, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, and 2,2'-dihydroxybinaphthyl, their alkyl, alkoxy or halogen substitution products, and their acylated products and other ester-forming derivatives. Among these, hydroquinone or 2,6-dihydroxynaphthalene or a combination thereof can be preferably used.

[0031] In terms of melt moldability of the liquid crystal polyester, R, which is an aromatic unit in the structural unit (A), preferably contains 20 to 70 mol % of a benzene skeleton and 20 to 80 mol % of a naphthalene skeleton, and more preferably contains 30 to 65 mol % of a benzene skeleton and 25 to 75 mol % of a naphthalene skeleton.

[0032] [Introduction of structural unit (B) into liquid crystal polyester] [ka] In the structural unit (B), n is an integer of 2 to 18, preferably 4 to 12, more preferably 6 to 10, and particularly preferably 6 or 10.

[0033] To synthesize a liquid crystal polyester resin consisting of structural units (A) and (B), it is necessary to use a monomer whose end is modified with an aromatic hydroxycarboxylic acid ester, as represented by structural formula (C). In other words, if an alkanediol monomer is used, the liquid crystal polyester resin of the present invention cannot be produced. (Ar is an aromatic unit, and n is an integer of 2 to 18.)

[0034] [ka] When the total number of monomers constituting the structural unit (A) is A moles and the total number of monomers constituting the structural unit (B) is B moles, the content x of the structural unit (B) can be expressed by the following formula (1): The monomer constituting the structural unit (B) has a structure represented by structural formula (C), and in the main chain of the resulting liquid crystal polyester, this monomer becomes one unit of the structural unit (B) and two units of the structural unit (A), so the content x of the structural unit (B) in the liquid crystal polyester of the present invention can be calculated by formula (1).

[0035]

number

[0036] From the viewpoint of lowering the dielectric constant, Ar in the structural formula (C) is preferably a benzene skeleton or a naphthalene skeleton.

[0037] Specific examples of structural formula (C) include 1,2-dimethylenebis(4-hydroxybenzoate), 1,3-trimethylenebis(4-hydroxybenzoate), 1,4-tetramethylenebis(4-hydroxybenzoate), 1,5-pentamethylenebis(4-hydroxybenzoate), 1,6-hexamethylenebis(4-hydroxybenzoate), 1,7-heptamethylenebis(4-hydroxybenzoate), 1,8-octamethylenebis(4-hydroxybenzoate), 1,9-nonamethylenebis(4-hydroxybenzoate), 1,10-decamethylenebis(4-hydroxybenzoate), 1,11-undecamethylenebis(4-hydroxybenzoate), and 1,12-dodecamethylenebis(4-hydroxybenzoate).

[0038] In the synthesis of the liquid crystal polyester resin of the present invention, when only aromatic hydroxycarboxylic acid and monomer represented by structural formula (C) are used, the amount of acetoxy groups in the polymer becomes excessive, and the polymerization stops before proceeding sufficiently, so that low dielectric tangent cannot be achieved. By using dicarboxylic acid monomer in combination, the difference between the amount of acetoxy groups and the amount of carboxyl groups decreases, so that the molecular weight increases and a liquid crystal polyester with a small dielectric tangent can be synthesized.

[0039] The amount of acetoxy groups contained in all monomers constituting the liquid crystal polyester of the present invention is preferably 1.0 times or more and less than 1.1 times the amount of carboxyl groups from the viewpoint of low dielectric tangent, and the closer to 1.0 times the amount, the more preferable.

[0040] The presence or absence of the structural unit (B) in the synthesized liquid crystal polyester resin is determined by 1 H-nuclear magnetic resonance spectrum ( 1 The composition was confirmed by H-NMR measurement. 1 The composition ratio of various monomers can be calculated from the H-NMR spectrum.

[0041] As the base used during solvolysis, for example, an inorganic compound exhibiting strong basicity such as potassium hydroxide, sodium hydroxide, barium hydroxide, etc. is preferably used.

[0042] As the solvent used in the solvolysis, for example, water or a lower alcohol such as methanol or ethanol is preferably used. [Method of manufacturing liquid crystal polyester] The liquid crystal polyester resin of the present invention is typically produced by polycondensing a monomer mixture containing an acylated product of a monomer having a phenolic hydroxyl group. The method of polycondensation is not particularly limited, and the liquid crystal polyester of the present invention can be obtained by, for example, a melt acidolysis method, a slurry polymerization method, or the like.

[0043] The melt acidolysis method is a preferred method for producing the liquid crystal polymer of the present invention in terms of cost and production time. In this method, the monomer is first heated to melt, and then the polycondensation reaction is continued to obtain a molten polymer. Note that a vacuum may be applied to facilitate removal of volatile by-products (e.g., acetic acid, water, etc.) produced at the final stage of condensation.

[0044] A slurry polymerization process is a process in which monomers are reacted in the presence of a heat exchange fluid and a solid product is obtained in suspension in the heat exchange medium.

[0045] The acylated product of a monomer having a phenolic hydroxyl group may be synthesized in the reaction system by adding an acylating agent such as acetic anhydride or acetic acid during the synthesis of the liquid crystal polyester, or may be synthesized by separate acylation.

[0046] When a monomer having a phenolic hydroxyl group is acylated in the reaction system, the acylating agent is preferably used in an amount of at least 1.1 times the total amount of phenolic hydroxyl groups on the monomer.

[0047] The polymerization reaction temperature is 200 to 400° C., preferably 250 to 350° C., and is preferably carried out under normal pressure and / or reduced pressure.

[0048] The polycondensation is preferably carried out in the presence of a catalyst, examples of which include metal compounds such as magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, and antimony trioxide, and nitrogen-containing heterocyclic compounds such as 1-methylimidazole.

[0049] The amount of the catalyst used is not particularly limited, but is preferably, for example, 0.1 part by mass or less per 100 parts by mass of the monomer mixture. The liquid crystal polyester resin of the present invention obtained by such a polycondensation reaction is usually discharged in a molten state from a reaction vessel, and then processed into a powder, pellet, or flake form.

[0050] The liquid crystal polyester resin in the form of pellets, flakes, or powder may be heated under reduced pressure, vacuum, or an inert gas atmosphere such as nitrogen or helium to cause a polymerization reaction in a solid phase and increase the molecular weight. By carrying out the heat treatment in the solid phase, improvement of heat resistance, etc. can be expected.

[0051] Whether the liquid crystal polyester resin obtained by the above method exhibits liquid crystallinity can be evaluated by confirming the presence or absence of optical anisotropy when melted by a conventional polarization inspection method using crossed polarizers.

[0052] [Other additives] The liquid crystal polyester composition may contain an inorganic filler as required. Examples of inorganic fillers include calcium carbonate, talc, clay, silica, magnesium carbonate, barium sulfate, titanium oxide, alumina, montmorillonite, gypsum, glass flakes, glass fibers, milled glass fibers, carbon fibers, alumina fibers, silica alumina fibers, aluminum borate whiskers, and potassium titanate fibers. The inorganic fillers may be used alone or in combination of two or more.

[0053] The amount of these inorganic fillers used is appropriately determined according to the application of the liquid crystal polyester composition, within a range that does not impair the low dielectric properties of the liquid crystal polyester composition. For example, when forming a film using the liquid crystal polyester composition, the upper limit of the amount of inorganic fillers used is determined within a range that does not significantly impair the mechanical strength of the film.

[0054] The liquid crystal polyester composition may further contain various additives, such as an organic filler, an antioxidant, a heat stabilizer, a light stabilizer, a flame retardant, a lubricant, an antistatic agent, a colorant, a rust inhibitor, a crosslinking agent, a foaming agent, a fluorescent agent, a surface smoothing agent, a surface gloss improving agent, and a mold release improving agent, if necessary. These additives may be used alone or in combination of two or more kinds.

[0055] [Film molding] The liquid crystal polyester resin of the present invention can be processed into molded products, films, fibers, etc. by known molding methods such as press molding, extrusion molding, injection molding, compression molding, or blow molding, by heating at a temperature above the melting point.

[0056] The melting point of the liquid crystal polyester resin of the present invention is 300° C. or less, preferably 270° C. or less, more preferably 230° C. or less, and particularly preferably 200° C. or less. The melting point of the resin can be measured by the method described later in the Examples. The liquid crystal polyester resin of the present invention has a lower melting point than fully aromatic liquid crystal polyesters because the structural unit (B) is introduced into the main chain, and is therefore useful for applications requiring low-temperature processability.

[0057] The dielectric loss tangent at a frequency of 28 GHz of the film obtained by molding the liquid crystal polyester resin of the present invention is preferably 0.00300 or less, more preferably 0.00280 or less, even more preferably 0.00270 or less, and particularly preferably 0.00250 or less. The dielectric loss tangent of the resin film can be measured by the method described later in the examples.

[0058] The value of the thermal expansion coefficient in the planar direction (hereinafter also referred to as XY-CTE) of the film obtained by molding the liquid crystal polyester resin of the present invention is not particularly limited, but is preferably 100 ppm / K or less, more preferably 80 ppm / K or less, and particularly preferably 70 ppm / K or less. XY-CTE can be evaluated by the method described later in the examples. The value of the coefficient of thermal expansion in the thickness direction (hereinafter also referred to as Z-CTE) is not particularly limited, but is preferably 120 ppm / K or less, more preferably 100 ppm / K or less, and particularly preferably 90 ppm / K or less. The Z-CTE can be evaluated by the method described later in the examples.

[0059] The index of anisotropy of thermal expansion of the film obtained by molding the liquid crystal polyester resin of the present invention is 4.0 or less, preferably in the range of 0.2 to 3.0, more preferably in the range of 0.5 to 2.0, and particularly preferably closer to 1.0. The index of anisotropy of thermal expansion coefficient is a value obtained by dividing the value of Z-CTE by the value of XY-CTE. The anisotropy of thermal expansion can be evaluated by the method described later in the examples.

[0060] The liquid crystal polyester resin film of the present invention exhibits a low dielectric tangent and excellent low-temperature processability, and has a small anisotropy of thermal expansion, so that the dimensional accuracy is greatly improved during processing of FPC boards. Therefore, such a film is suitably used as a film constituting a metal-clad laminate or a printed circuit board. EXAMPLES

[0061] The present invention will be described in detail below with reference to examples, but the present invention is not limited to only these examples. [Monomer synthesis] The following was synthesized and used as the monomer of structural formula (3). HDP: 1,6-hexamethylenebis(4-hydroxybenzoate) DDP: 1,10-decamethylenebis(4-hydroxybenzoate) As an example of the synthesis of a monomer of structural formula (3), a method for synthesizing DDP is shown below, but the monomer that can be synthesized by this method is not limited to DDP.

[0062] [Synthesis of DDP] 38.8g (0.15 mol) of 1,10-diacetoxydecane (hereinafter also referred to as 1,10-DAD), 45.6g (0.33 mol) of 4-hydroxybenzoic acid, 20mL of toluene, and 5 drops of concentrated sulfuric acid were added with a dropper to a reaction vessel equipped with a nitrogen gas inlet tube, a water content measuring tube, and a reflux condenser. After thoroughly replacing the atmosphere in the reaction vessel with nitrogen gas, the vessel was heated to 150°C under a nitrogen gas flow and refluxed for 5 hours while maintaining the temperature. After confirming that no water was distilled into the water content measuring tube, the vessel was allowed to cool to room temperature. Then, 50mL of methanol was added while cooling on ice, and the precipitated solid was collected. The mixture was then recrystallized from methanol and purified.

[0063] [Polymer synthesis] In the examples, the following abbreviations represent the following compounds. PHB: 4-hydroxybenzoic acid HNA: 6-hydroxy-2-naphthoic acid HDBA: 1,6-bis(4-carboxyphenoxy)hexane TPA: Terephthalic acid HQ: Hydroquinone

[0064] [Examples 1 to 6, Comparative Examples 1 to 3, Reference Example 1] The compounds listed in Tables 1 and 2 were charged in a reaction vessel equipped with a torque meter-equipped stirrer, a distillation tube, and a reflux condenser in the ratios listed, and 1.1 times the moles of acetic anhydride and a catalytic amount of 1-methylimidazole were added to the hydroxyl group amount (mol) of all the compounds charged. The inside of the reaction vessel was thoroughly replaced with nitrogen gas, and the mixture was heated to 145°C while stirring and held at the same temperature for 30 minutes. The temperature was then quickly raised to 185°C and held at the same temperature for 30 minutes. The temperature was then raised to 260°C over 20 minutes while distilling off the by-product acetic acid, and held for 2 hours and 30 minutes. The pressure inside the reaction vessel was then reduced to 7.5 torr over 10 minutes, and the reaction was held for 1 hour. The temperature was then quickly raised to 265°C while maintaining the vacuum, and held for 30 minutes. The temperature was then quickly raised to 270°C while maintaining the vacuum, and the reaction was deemed to be complete when the torque reached a predetermined value, and the contents were removed. The solid matter obtained was allowed to cool to room temperature, then crushed in a grinder, washed with methanol and dried. It was then held at 300°C for 2 hours in a nitrogen gas atmosphere to allow the polymerization reaction to proceed in the solid phase, and the resulting solid was crushed again in a grinder to obtain a liquid crystal polyester powder.

[0065] [Comparative Examples 4 and 5, Reference Example 2] The compounds shown in Table 2 were charged in the reaction vessel equipped with a torque meter-equipped stirrer, a distillation tube and a reflux condenser in the ratios shown, and 1.1 times the moles of acetic anhydride and a catalytic amount of 1-methylimidazole were added to the hydroxyl group amount (mol) of all the compounds charged. The inside of the reaction vessel was thoroughly replaced with nitrogen gas, and the mixture was heated to 145°C while stirring and held at the same temperature for 30 minutes. The temperature was then quickly raised to 185°C and held at the same temperature for 30 minutes. The temperature was then raised to 260°C over 30 minutes while distilling off the by-product acetic acid, and held for 2 hours and 30 minutes. The pressure inside the reaction vessel was then reduced to 7.5 torr over 10 minutes, and the reaction vessel was held for 1 hour. The temperature was then quickly raised to 265°C while maintaining the vacuum, and held for 30 minutes. The temperature was then quickly raised to 270°C while maintaining the vacuum, and held for 30 minutes. The temperature was then quickly raised to 275°C while maintaining the vacuum, and held for 30 minutes. After that, the temperature was raised to 280°C quickly while maintaining the vacuum, and the reaction was deemed to be completed when the torque reached a predetermined value, and the contents were removed. The obtained solid was allowed to cool to room temperature, pulverized in a grinder, washed with methanol, and dried. After that, it was held at 300°C for 2 hours under a nitrogen gas atmosphere to proceed with the polymerization reaction in the solid phase, and the obtained solid was pulverized again in a grinder to obtain a liquid crystal polyester powder. The glass transition temperature, melting point, dielectric loss tangent, thermal expansion coefficient in the planar direction and thermal expansion coefficient in the thickness direction, and anisotropy of thermal expansion of the examples were evaluated by the methods described below. The obtained values ​​are summarized in Tables 3 and 4.

[0066] [Creating resin film] The resin film was made using a tabletop mini press (MP-2F, manufactured by Toyo Seiki Seisakusho Co., Ltd.). The resin was placed in a brass spacer with a thickness of 300 μm, and the spacer was heated and pressed to form a film.

[0067] [Measurement of glass transition temperature and melting point] The glass transition temperature and melting point of the resin were measured using a differential scanning calorimeter (Q1000, manufactured by TA Instruments). 5 to 8 mg of the resin was placed in an aluminum sample pan, covered, and heated from room temperature to 350 to 400°C at a rate of 10°C / min under a nitrogen gas flow until the resin was completely melted. The temperature was then lowered to 0°C at 20°C / min, and then further increased at 10°C / min. The intersection of the tangent line at the baseline and the inflection point (the point where the upward convex curve changes to a downward convex curve) in the chart obtained was determined as the glass transition temperature, and the apex of the endothermic peak was determined as the melting point.

[0068] [Dissipation factor] The dielectric loss tangent was measured using a network analyzer (KEYSIGHT N5222B) and a split cylinder resonator (EM Labs CR-728). A sample measuring 3.5 cm x 5.0 cm was cut out from the film, and the dielectric loss tangent was measured after 24 hours of humidity conditioning in a 23°C / 50% RH environment. The measurement was performed at 28 GHz.

[0069] [In-plane thermal expansion coefficient (XY-CTE)] The thermal expansion coefficient in the planar direction was measured by the tensile load method using a thermomechanical analyzer (TMA4000SA manufactured by NESZSCH). A sample with a size of 5 mm x 10 mm was cut out from the film, and heated to 80 to 150 °C at a heating rate of 10 °C / min under a nitrogen gas flow, then cooled to 30 °C at a cooling rate of 20 °C / min, and further heated at 10 °C / min. In the chart obtained by heating, the sample length at 25 °C (T1) was L1, the sample length at the glass transition temperature T2 (value obtained by a differential scanning calorimeter) was L2, and the reference length was L0. The value α expressed by formula (2) was obtained. XY is the thermal expansion coefficient in the planar direction.

[0070]

number

[0071] [Z-CTE (coefficient of thermal expansion through thickness)] The thermal expansion coefficient in the thickness direction was measured by the compression load method using a thermomechanical analyzer (TMA8310 manufactured by Rigaku). A sample of 5 mm x 5 mm and 1 mm thick was cut out, heated to 80-150°C at a rate of 10°C / min under a nitrogen gas flow, cooled to 25°C at a rate of 8°C / min, and then heated at a rate of 10°C / min. The chart obtained when the sample length at 25°C (T1) was L1, the sample length at the glass transition temperature T2 (value obtained by a differential scanning calorimeter) was L2, and the reference length was L0 was calculated by the value α expressed by formula (3). Z is the thermal expansion coefficient in the thickness direction.

[0072]

number

[0073] [Anisotropy of thermal expansion] The thermal expansion coefficients of each sample in the planar and thickness directions (α XY , α Z ) was used, and the value r expressed by equation (4) was taken as a value indicating the magnitude of the anisotropy of thermal expansion.

[0074]

number

[0075] [How to check liquid crystal properties] The liquid crystallinity was confirmed using a polarizing microscope (Olympus BX-51-33P-OC). The obtained liquid crystal oligomer sample was sandwiched between two slide glasses and melted on the heating stage of the microscope to confirm the presence or absence of optical anisotropy when melted. The objective lens was set to 10x or 50x for observation. Samples that showed optical anisotropy when melted were judged to show liquid crystallinity.

[0076] [Composition analysis of liquid crystal polyester] Composition analysis of liquid crystal polyester 1 H-nuclear magnetic resonance spectrum ( 1The measurement was carried out by H-NMR. 0.7 mL of a 30 wt% potassium hydroxide deuterium oxide solution was added to 10 mg of sample, and heated at 150°C for 3 hours. A portion of the resulting decomposition solution was diluted with deuterium oxide containing sodium trimethylsilylpropionate-d4, and NMR was performed at a temperature of 20°C and an observation frequency of 700 MHz using an NMR device (AVANCE NEO 700 manufactured by Bruker). 1 H-NMR measurement was performed. The composition ratio was calculated from the peak area ratio due to each structural unit observed around 1 to 4 ppm and 6.5 to 8.5 ppm on the obtained spectrum. Analysis was performed on the resins of Example 4 and Reference Example 2, and the obtained results are summarized in Table 5.

[0077] In Reference Example 1 in Table 4, the acetoxy group was in large excess in the polymer, and the molecular weight did not increase and the polymerization was terminated. As a result, the film strength was weak and the thermal expansion coefficient could not be measured. In Table 5, one molecule of DDP is hydrolyzed and decomposed into two molecules of PHB and one molecule of 1,10-DAD, so it was included in the calculation of the composition ratio with PHB and 1,10-DAD. While 1,10-DAD was not detected in the liquid crystal polyester of Reference Example 2, which used 1,10-DAD as the raw material, 1,10-DAD was detected when DDP was used as the raw material, so it is necessary to use DDP to introduce the structural unit (B) into the main chain of the liquid crystal polyester.

[0078] In the liquid crystal polyester of Comparative Example 3, the aliphatic chain and aromatic unit in the structure are bonded by ester bonds, and the molecular chain is extended. This liquid crystal polyester has a larger anisotropy of thermal expansion of the film than the liquid crystal polyester of the present invention having the same monomer charge ratio, so there is a concern that the dimensional accuracy will decrease during processing of the FPC board. The liquid crystal polyester resins of the present invention shown in the examples of Tables 1 to 4 have a low melting temperature while maintaining a low dielectric tangent in the high frequency range, and have improved thermal expansion anisotropy, and are therefore suitable for use as materials for FPC boards used in high frequency communications.

[0079] [Table 1]

[0080]

Table 2

[0081]

Table 3

[0082]

Table 4

[0083]

Table 5

Claims

1. A liquid crystal polyester resin comprising at least one structural unit (A) selected from an aromatic oxycarbonyl unit, an aromatic dioxy unit, and an aromatic dicarboxy unit, and a structural unit (B) having an alkyl chain, the content of the structural unit (B) being in the range of 1.0 to 20.0 mol % based on all structural units constituting the liquid crystal polyester (n is an integer of 2 to 18, and R is an aromatic unit). 【Chemistry 1】 【Chemistry 2】

2. 2. The liquid crystal polyester resin according to claim 1, wherein the dielectric tangent value at 28 GHz is 0.00300 or less.

3. 2. The liquid crystal polyester resin according to claim 1, wherein the aromatic skeleton of the structural unit (A) contains 20 to 70 mol % of a benzene skeleton and 20 to 80 mol % of a naphthalene skeleton.

4. 2. The liquid crystal polyester resin according to claim 1, wherein the monomer constituting the aromatic oxycarbonyl unit is 4-hydroxybenzoic acid and / or 6-hydroxy-2-naphthoic acid.

5. 2. The liquid crystal polyester resin according to claim 1, wherein the monomer constituting the aromatic dicarboxy unit is terephthalic acid and / or 2,6-naphthalenedicarboxylic acid.

6. 2. The liquid crystal polyester resin according to claim 1, wherein the monomer constituting the aromatic dioxy unit is hydroquinone and / or 2,6-dihydroxynaphthalene.

7. A liquid crystal polyester resin composition comprising the liquid crystal polyester resin according to any one of claims 1 to 6 and an inorganic or organic filler.

8. A film obtained by molding the liquid crystal polyester resin according to any one of claims 1 to 6.

9. A film obtained by molding the liquid crystal polyester resin composition according to claim 7.

10. A metal-clad laminate comprising the film of claim 8.

11. A metal-clad laminate comprising the film of claim 9.

12. A printed circuit board comprising the film according to claim 8.

13. A printed circuit board comprising the film according to claim 9.

14. A method for producing a liquid crystal polyester resin, comprising producing the liquid crystal polyester resin according to any one of claims 1 to 6, using an aliphatic monomer having an aromatic ester terminal represented by structural formula (C). (Ar is an aromatic unit. n is an integer from 2 to 18.) 【Chemistry 3】

Citation Information

Patent Citations

  • Liquid crystal polymer blend film

    JP2004175995A