Spark plug insulator and spark plug
The spark plug insulator achieves improved bending strength and thermal shock resistance through controlled particle size and distribution, addressing the limitations of existing alumina-based sintered bodies.
Patent Information
- Application Number
- JP2023053309
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing spark plug insulators made of alumina-based sintered bodies face challenges in improving bending strength and thermal shock resistance.
The insulator is designed with specific particle size and distribution parameters, including an average particle area of 4.4 μm² to 8.0 μm² and a maximum particle area of 600 μm², with controlled numbers of large and small particles to enhance mechanical strength and thermal shock resistance.
The designed particle structure improves bending strength and thermal shock resistance by minimizing defects and ensuring appropriate particle distribution, leading to enhanced durability and performance.
Smart Images

Figure 2024141578000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a spark plug insulator and a spark plug. [Background technology]
[0002] Patent Document 1 discloses a prior art technique for a spark plug having an insulator made of an alumina-based sintered body, in which the average grain size of the insulator's crystal grains is set to 1.5 μm or less and the standard deviation of the grain size distribution of the crystal grains is set to 1.2 μm or less in order to increase the mechanical strength of the insulator. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-57559 A Summary of the Invention [Problem to be solved by the invention]
[0004] There is a need in the prior art to improve the flexural strength and thermal shock resistance of insulation.
[0005] The present invention has been made in response to this demand, and an object of the present invention is to provide a spark plug insulator and a spark plug which are capable of improving bending strength and thermal shock resistance. [Means for solving the problem]
[0006] In order to achieve this object, a first aspect of the present invention is a spark plug insulator made of an alumina-based sintered body having an axial hole extending along an axis, wherein when a bending force is applied to the spark plug insulator to cause it to break, the fracture surface formed by the break is divided into two by a plane perpendicular to the force direction and including the axis, and the range including the break origin is such that the average area of particles appearing in a planar image of the range is 4.4 μm 2 8.0μm or more 2The maximum particle area is 600 μm 2 The particle has an area of 60 μm or less. 2 More than 600μm 2 Large particles include particles having a density of 0.1 particles / mm2 or less per unit area of a flat image. 2 There are more than one.
[0007] In the second embodiment, the large particles are 6.2 particles / mm 2 per unit area of the planar image in the first embodiment. 2 The following exists.
[0008] In a third embodiment, in the first or second embodiment, the particles have an area of 20 μm 2 More than 59μm 2 The small particles include small particles having a density of 613 particles / mm2 or less per unit area of the planar image. 2 More than 2270 pieces / mm 2 The following exists.
[0009] A fourth aspect is a spark plug comprising the spark plug insulator according to any one of the first to third aspects. Effect of the Invention
[0010] The average particle area shown in the planar image of the spark plug insulator is 4.4μm 2 8.0μm or more 2 The maximum particle area is 600 μm 2 and the area is 60μm 2 More than 600μm 2 Large particles with a density of 0.1 particles / mm or less per unit area of a flat image 2 Since these elements are present, bending strength and thermal shock resistance can be improved. [Brief description of the drawings]
[0011] [Figure 1] 1 is a half-sectional view of a spark plug according to an embodiment; [Diagram 2] FIG. 2 is a schematic diagram of a fracture surface of an insulator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. Fig. 1 is a half-side cross-sectional view combining an outline view and a full cross-sectional view taken along the axis C of an axial hole 12 of a spark plug 10 in one embodiment. The lower side of the page in Fig. 1 is the leading end side of the spark plug 10, and the upper side is the rear end side of the spark plug 10. The spark plug 10 includes an insulator 11 (spark plug insulator). The insulator 11 is a cylindrical member provided with an axial hole 12 extending along the axis C, and is an alumina-based sintered body having excellent insulating properties and mechanical properties at high temperatures.
[0013] A rod-shaped metal center electrode 13 is disposed in an axial hole 12 of an insulator 11. The center electrode 13 has a core material with excellent thermal conductivity embedded in a base material. The base material is made of an alloy mainly containing Ni or a metal material made of Ni. The core material is made of copper or an alloy mainly containing copper. The core material can be omitted.
[0014] The terminal fitting 14 is a rod-shaped member to which an ignition device (not shown) is connected, and is made of a conductive metal material (such as low carbon steel). The tip side of the terminal fitting 14 is disposed in the axial hole 12 of the insulator 11, and the rear end side of the terminal fitting 14 protrudes from the insulator 11. The terminal fitting 14 is electrically connected to the center electrode 13 in the axial hole 12.
[0015] The metal shell 15 is a substantially cylindrical member made of a conductive metal material (such as low carbon steel, etc.). The metal shell 15 is disposed on the outer periphery of the insulator 11. A male thread 16 is provided on the tip side of the metal shell 15.
[0016] The ground electrode 17 is a rod-shaped metal (eg, nickel-based alloy) member connected to the metallic shell 15. A spark gap is formed between the ground electrode 17 and the center electrode 13.
[0017] The spark plug 10 is manufactured, for example, by the following method. After inserting the center electrode 13 into the axial hole 12 of the insulator 11, the axial hole 12 is filled with conductive powder containing a glass component. After inserting the terminal fitting 14 from the rear end side of the axial hole 12, the terminal fitting 14 is pressed into the axial hole 12 while heating the powder to a temperature higher than the softening point of the glass component contained therein, for example, so that the terminal fitting 14 applies an axial load to the powder. The powder is compressed and sintered, and the center electrode 13 and the terminal fitting 14 are electrically connected in the axial hole 12. Next, the metallic shell 15 to which the ground electrode 17 is connected is assembled to the outer periphery of the insulator 11, and the ground electrode 17 is bent to set a spark gap between the ground electrode 17 and the center electrode 13, thereby obtaining the spark plug 10.
[0018] An example of a method for manufacturing the insulator 11 will be described. The insulator 11 is manufactured through the steps of slurry preparation, degassing, granulation, molding, grinding, and firing. Each step will be described below in order.
[0019] The slurry preparation process is a process of preparing a slurry by mixing a raw material powder, a binder, and a solvent. The raw material powder mainly contains a powder of a compound that is converted to alumina by firing (hereinafter referred to as "Al compound powder"). As the Al compound powder, for example, alumina powder is used.
[0020] In the slurry preparation process, a pulverization process is carried out for the purpose of mixing and pulverizing the raw material powder. The pulverization process is carried out using a wet pulverizer using a ball mill or the like. The diameter of the balls used in the wet pulverizer is not particularly limited as long as it does not impair the object of the present invention, but is preferably 2 mm to 20 mm, more preferably 2 mm to 10 mm, and even more preferably 2 mm to 6 mm. Two or more types of balls having different diameters may be combined. By such a pulverization process, the raw material powder has a small variation in particle size (particle size) and a sharp particle size distribution. By using such a raw material powder, the particle size can be controlled and the sintering density can be increased in the alumina-based sintered body obtained after sintering.
[0021] The particle size (particle size after pulverization) of the Al compound powder (alumina powder, etc.) is not particularly limited as long as it does not impair the object of the present invention, but is preferably 1.5 μm or more, more preferably 1.7 μm or more, more preferably 2.5 μm or less, and more preferably 2.0 μm or less. When the particle size of the Al compound powder is in this range, the number of defects in the insulator is suppressed and an appropriate sintering density is obtained. The particle size is the volume-based median diameter (D50) measured by a laser diffraction method (Microtrack particle size distribution measuring device, product name "MT-3000", manufactured by Nikkiso Co., Ltd.).
[0022] The Al compound powder is preferably prepared so that it is 90% by mass or more in terms of oxide when the mass (oxide equivalent) of the alumina-based sintered body after firing is taken as 100% by mass. More preferably, it is 90% by mass or more and 98% by mass or less, and even more preferably, it is 90% by mass or more and 97% by mass or less. As long as it does not impair the object of the present invention, the raw material powder may contain powder other than the Al compound powder.
[0023] The binder is added to the slurry for the purpose of improving the moldability of the raw material powder. Examples of such binders include hydrophilic binders such as polyvinyl alcohol, aqueous acrylic resin, gum arabic, and dextrin. These may be used alone or in combination of two or more. The amount of the binder is not particularly limited as long as it does not impair the object of the present invention, but for example, it is mixed in a ratio of 1 to 10 parts by mass, preferably 3 to 7 parts by mass, per 100 parts by mass of the raw material powder.
[0024] The solvent is used for the purpose of dispersing the raw material powder, etc. Examples of the solvent include water, alcohol, etc. These may be used alone or in combination of two or more. The amount of the solvent is not particularly limited as long as it does not impair the object of the present invention, but for example, it is mixed in a ratio of 23-40 parts by mass, preferably 25-35 parts by mass, per 100 parts by mass of the raw material powder. The slurry may contain other components other than the raw material powder, binder, and solvent as necessary. A known stirring / mixing device or the like can be used to mix the slurry.
[0025] The prepared slurry may be degassed as necessary. In the degassing step, for example, a container containing the mixed (kneaded) slurry is placed in a vacuum degassing device, and the pressure is reduced to place it in a low-pressure environment, thereby removing the bubbles contained in the slurry. The amount of bubbles in the slurry can be determined by comparing the density of the slurry before and after degassing.
[0026] The granulation process is a process of producing spherical granulated powder from a slurry containing raw material powders and the like. The method of producing granulated powder from a slurry is not particularly limited as long as it does not impair the object of the present invention, and for example, a spray drying method can be mentioned. In the spray drying method, a granulated powder having a predetermined particle size is obtained by spray drying the slurry using a predetermined spray dryer device. The particle size of the granulated powder is not particularly limited as long as it does not impair the object of the present invention, and for example, 212 μm pass ≧ 95% or less is preferable, and 180 μm pass ≧ 95% or less is more preferable.
[0027] The molding process is a process in which the granulated powder is molded into a predetermined shape using a mold to obtain a molded body. The molding process is carried out by rubber press molding, die press molding, or the like. In the case of this embodiment, the pressure (press pressure rise rate) applied to the mold (e.g., the inner rubber mold and the outer rubber mold of a rubber press molding machine) from the outer periphery is adjusted so as to increase in stages. In addition, it is preferable to adjust the pressure range to a higher pressure range than before (e.g., 100 MPa or more). The upper limit of the pressure is not particularly limited as long as it does not impair the object of the present invention, but may be adjusted to, for example, 200 MPa or less.
[0028] The grinding process is a process for removing the machining allowance of the molded body obtained after the molding process and polishing the surface of the molded body. In the grinding process, the machining allowance is removed and the surface of the molded body is polished by grinding with a resinoid grinding wheel or the like. By such a grinding process, the shape of the molded body is adjusted.
[0029] The firing step is a step of firing the molded body, the shape of which has been adjusted by the grinding step, to obtain an insulator. In the firing step, for example, firing is performed in an air atmosphere at 1450°C to 1650°C for 1 to 8 hours. After firing, the molded body is cooled to obtain the insulator 11 made of an alumina-based sintered body.
[0030] The insulator 11 is a brittle material and is vulnerable to tensile stress, and when a bending force is applied to the insulator 11, cracks develop from pores and defects present in the insulator 11. By observing the structure of the fracture surface created by breaking the insulator 11, it is possible to clarify defects and the like present in the insulator 11. The insulator 11 can be broken by applying a tensile force to the insulator 11 using various means, such as a three-point bending test or a four-point bending test specified in JIS R1601:2008, or an insulator bending strength test specified in JIS B8031:2006, and the like, and a fracture surface can be created in the insulator 11.
[0031] The bending strength test for insulators specified in JIS B8031:2006 will be explained with reference to Figure 1. After the male thread 16 of the spark plug 10 is tightened to an iron jig 18 with the specified maximum torque and the spark plug 10 is fixed to the jig 18, a force F perpendicular to the axis C is applied to a position within 5 mm from the rear end of the insulator 11. Without applying any impact to the insulator 11, the force F pushes the insulator 11 at a speed of 10 mm / min or less, destroying the insulator 11 and creating a fracture surface.
[0032] 2 is a schematic diagram of a fracture surface of the insulator 11. Of the areas 21 and 22 obtained by dividing the fracture surface (the ring around the axial hole 12) into two by a plane 20 that is perpendicular to the direction of the force F (see FIG. 1) applied to the insulator 11 and includes the axis C, the area 21 including the fracture origin is a surface formed mainly by the application of a tensile force. The area 22 is a surface formed by the progression of a crack that has occurred in the area 21. Particles that have grown abnormally during firing are one of the defects inherent to the insulator 11. Using a scanning electron microscope (SEM), the structure of the area 21 including the fracture origin (in this embodiment, the surface including the side where the force F was applied) is observed, and the size and distribution of the particles in the area 21 are examined.
[0033] Since the size of the particles cannot be confirmed even if the entire area 21 is captured in a single SEM image, the entire area 21 is divided into multiple parts, and an SEM image (planar image) is obtained for each part. An example of an SEM image is one in which the area 21 is divided into rectangular parts measuring 985 μm in length and 1231 μm in width, and enlarged at a low magnification (for example, 100 times). Since the area 21 has the shape of a ring cut in half, some SEM images show the shaft hole 12 inside the area 21 and the space outside the area 21 in part of the rectangular image, but an SEM image of the entire area 21 is obtained, including images in which there is blank space other than the area 21 in part of the image.
[0034] After acquiring a low-magnification SEM image of the entire area 21, image analysis is performed using known image analysis software (e.g., WinROOF (registered trademark), manufactured by Mitani Shoji Co., Ltd.). In the image analysis, the size of each SEM image is calibrated based on the scale bar attached to the SEM image, and then the SEM image is binarized to extract the edges of the image. In the binarization, the luminance (brightness) of each pixel of the SEM image is converted to two levels using a predetermined threshold (e.g., threshold 0-25). By converting the pixels to two levels and eliminating intermediate gradations, a binarized image in which grain boundaries are emphasized is obtained.
[0035] The area of the particles is calculated by a known image analysis method using the binary image of the range 21, and among all the particles included in the range 21, the area of the particles with an area of 60 μm 2 More than 600μm 2 The number of particles that are larger than or equal to 100 mm (hereinafter referred to as "large particles") is counted. Particles that have grown abnormally during firing are one of the defects that have a high possibility of becoming the starting point of destruction. In the insulator 11, the points where defects are concentrated become the starting point of destruction, so if there are particles that have grown abnormally during firing, they will appear in the range 21.
[0036] In order to reduce defects caused by abnormally grown grains and ensure the bending strength of the insulator 11, the grains present in the planar image of the range 21 have a maximum area of 600 μm 2 The particles in the planar image in range 21 have a maximum area of 60 μm 2This is desirable in order to ensure the toughness of the insulator 11 and to ensure thermal shock resistance.
[0037] The insulator 11 has a density of 0.1 particles / mm2 per unit area on the planar image of the range 21. 2 The presence of large particles ensures the toughness of the insulator 11. The presence of large particles is evident in the planar image of the area 21, with a particle count of 6.2 particles / mm2 per unit area. 2 This is to ensure the bending strength of the insulator 11.
[0038] In addition to the low-magnification SEM images used to check the number of large particles, ten high-magnification SEM images are randomly acquired by enlarging a rectangular portion of range 21 measuring 100 μm in length and 163 μm in width. The position at which the image is acquired is set so that the entire high-magnification SEM image shows range 21, and there is no blank space other than range 21 in any part of the image. After the high-magnification SEM image is acquired, image analysis is performed in the same manner as the processing used to create the low-magnification SEM image, and a binary image in which the grain boundaries are emphasized is obtained.
[0039] Using the binarized images of range 21, the areas of all particles appearing in the 10 images are calculated using known image analysis techniques, and the area (average) of each particle is calculated. Even if a large particle is included in the 10 images, the large particle is counted as one particle and added to the area. If a particle is cut off at the edge of the image, the part that appears in the image is counted as one particle and added to the area. The average particle area of insulator 11 is 4.4 μm 2 8.0μm or more 2 The reason is as follows. This is to improve the bending strength and thermal shock resistance of the insulator 11.
[0040] The average particle area is 4.4 μm 2 If the average particle area is less than 8.0 μm, the toughness of the insulator 11 decreases and the thermal shock resistance tends to decrease. 2 If the porosity exceeds this value, the pores between the particles tend to become larger, resulting in a decrease in bending strength. In order to ensure bending strength, the porosity of the insulator 11 is preferably 5% or less.
[0041] Using a known image analysis method, it was determined that the particles contained in the 10 images had an area of 20 μm 2 More than 59μm 2 The number of particles that are smaller than 613 particles / mm2 per unit area of 10 images (hereinafter referred to as "small particles") is counted. 2 More than 2270 pieces / mm 2 The presence of the following small particles is preferred because the presence of the small particles improves the thermal shock resistance and bending strength of the insulator 11. EXAMPLES
[0042] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0043] (Making an insulator) Two insulators each having the same basic configuration as the insulator 11 of the spark plug 10 exemplified in the embodiment were produced in the same manner as the embodiment, for samples No. 1 to No. 12. For the insulator of sample No. 4, 50% by mass of 2 mm diameter pebbles and 50% by mass of 6 mm diameter pebbles were mixed and used when the raw material powder was pulverized by a wet pulverizer in the slurry production process. The insulators of samples No. 3 and 5-8 were produced in the same manner as sample No. 4, except that the ratio of the pebbles used when pulverizing the raw material powder in the slurry production process was appropriately changed.
[0044] For the insulator sample No. 1, 8 mm diameter pebbles and 12 mm diameter pebbles were mixed in a ratio of 50% by mass and 50% by mass, respectively, when the raw powder was pulverized in a wet pulverizer in the slurry preparation process. The insulators of samples No. 2 and 9-12 were prepared in the same manner as sample No. 1, except that the ratio of the pebbles used when pulverizing the raw powder in the slurry preparation process was appropriately changed.
[0045] (Insulator bending strength test) Using each of the two insulators of Samples No. 1-12, samples of the spark plug 10 described in the embodiment were produced one by one. The samples were produced in accordance with the insulator bending strength test specified in JIS B8031:2006. After the spark plug 10 was fastened to the jig 18 with a specified maximum torque, a force F perpendicular to the axis C was applied to a position within 5 mm from the rear end of the insulator 11, and the insulator 11 was pressed at a speed of 10 mm / min or less without applying any impact to the insulator 11 until the insulator 11 broke. Samples in which the magnitude of the force F (bending strength) at which the insulator 11 broke was 7.5 kN or more were judged to be A, and samples in which the bending strength was less than 7.5 kN were judged to be C.
[0046] [Table 1]
[0047] (Observation of fracture surface of insulator) The fracture surface of the insulator 11 that had broken in the insulator bending strength test was divided into two areas 21 and 22 by a plane 20 that was perpendicular to the direction of the force F applied to the insulator 11 and included the axis C. The structure of area 21, which included the starting point of the fracture, among areas 21 and 22, was then observed using a SEM (JEM-IT300LA, manufactured by JEOL Ltd.).
[0048] The entire area 21 was divided into several parts, and several SEM images were obtained by enlarging a rectangular area of 985 μm in length and 1231 μm in width at a low magnification (100 times). After processing with the image processing software WinROOF2013 (WinROOF is a registered trademark) to obtain a binary image, the area of the largest particle and the area of the largest particle with an area of 60 μm were determined by image analysis. 2 More than 600μm 2 The number of large particles per unit area was determined (rounded to one decimal place). The area of the largest particle is shown in the "Maximum" column of Table 1, and the number of large particles per unit area is shown in the "Number of large particles" column of Table 1.
[0049] Ten locations were randomly selected from the range 21, and ten high-magnification SEM images were taken of a rectangular area measuring 100 μm in length and 163 μm in width. The images were then processed to obtain binary images, after which the area per particle (average rounded to the nearest tenth) and the area per particle of 20 μm2 were determined by image analysis. 2 More than 59μm 2 The number of small particles per unit area was determined (rounded to the nearest tenth). The area (average) per particle is shown in the "Average" column of Table 1, and the number of small particles per unit area is shown in the "Number of small particles" column of Table 1.
[0050] (Thermal shock test) The insulators 11 of Samples No. 1-12 were each stored in a thermostatic chamber maintained at a predetermined temperature for 30 minutes, and then immediately immersed in water at 20°C to rapidly cool. The orientation of the insulators 11 when immersed in water was set so that the axis C of the insulators 11 was parallel to the water surface. The presence or absence of cracks in the insulators 11 taken out of the water was visually confirmed by applying a penetrant inspection liquid. The temperature of the thermostatic chamber in which the insulators 11 were stored was increased in 10°C increments from 150°C until cracks were found in the insulators 11. The samples with a temperature difference (critical temperature difference) between the thermostatic chamber temperature and the water temperature (20°C) at the time when cracks were found in the insulators 11 were judged to be 240°C or more in thermal shock resistance were judged to be A, samples with a temperature difference of 230°C or more but less than 240°C were judged to be B, and samples with a temperature difference of less than 220°C were judged to be C.
[0051] As shown in Table 1, the average particle area is 4.4 μm 2 8.0μm or more 2 The maximum area is 600 μm 2 The number of large particles is 0.1 / mm or less. 2 The bending strength of sample No. 3-8 was rated as A, and the thermal shock resistance was rated as A or B.
[0052] On the other hand, the average particle area is 4.4 μm 2 8.0μm or more 2 The maximum area is 600 μm 2 Even if the number of large particles is less than 0.1 / mm 2Sample No. 2, which has a bending strength of less than 100%, was rated an A for bending strength, but was rated a C for thermal shock resistance. It was confirmed that the presence of a moderate number of large particles is effective in ensuring thermal shock resistance. It is presumed that the presence of a moderate number of large particles improves the toughness of the insulator.
[0053] Sample No. 2 has a maximum particle area of 60 μm 2 Therefore, the number of large particles was 0 / mm 2 Sample No. 2 had a maximum particle area of 60 μm 2 It is possible that the thermal shock resistance was rated C because the maximum area was less than 60 μm 2 The above is presumably effective in improving the toughness of the insulator.
[0054] The maximum particle area is 600 μm 2 The number of large particles is 0.1 / mm or less. 2 Even if the average area is 4.4μm 2 Sample No. 1, which is less than 4.4 μm, was rated A for bending strength, but C for thermal shock resistance. 2 It was confirmed that if the thickness is less than this, the thermal shock resistance is reduced.
[0055] The average particle area is 4.4 μm 2 8.0μm or more 2 The number of large particles is 0.1 / mm or less. 2 Even if the maximum area is 600 μm 2 Samples No. 9 and 10, which exceeded the maximum area of 600 μm, were rated as A for thermal shock resistance, but were rated as C for bending strength. 2 It was confirmed that when the bending strength exceeds this value, there is a tendency for the bending strength to decrease.
[0056] The maximum particle area is 600 μm 2 The number of large particles is 0.1 / mm or less. 2 Even if the average area is 8.0μm or more 2Samples No. 11 and No. 12, which exceeded the average area of 8.0 μm, were rated A for thermal shock resistance, but C for bending strength. 2 It was confirmed that when the bending strength exceeds this value, there is a tendency for the bending strength to decrease.
[0057] Sample No. 12 had a large particle count of 7.8 particles / mm 2 Because there were many large particles, the average area of the particles including the large particles was 10.1 μm 2 The average particle area was 4.4 μm 2 8.0μm or more 2 In order to achieve the range below, the number of large particles is set to 6.2 particles / mm for sample No. 8. 2 The following was preferred:
[0058] The average particle area is 4.4 μm 2 8.0μm or more 2 The maximum area is 600 μm 2 The number of large particles is 0.1 / mm or less. 2 or more, and the number of small particles is 613 / mm 2 More than 2270 pieces / mm 2 The following sample No. 4-8 was rated A for both bending strength and thermal shock resistance. The presence of small particles was 613 pieces / mm 2 More than 2270 pieces / mm 2 It has been found that the following is effective in improving thermal shock resistance.
[0059] Although the present invention has been described above based on the embodiment, the present invention is not limited to the above embodiment, and it can be easily assumed that various improvements and modifications are possible without departing from the spirit of the present invention. For example, the shape of the insulator 11 is one example and can be set appropriately.
[0060] In the embodiment, the case where the insulator 11 is broken to create a fracture surface in accordance with the insulator bending strength test for spark plugs specified in JIS B8031:2006 has been described, but the present invention is not necessarily limited to this. It is of course possible for the insulator 11 before it is assembled into a spark plug by assembling the center electrode 13, the metal shell 15, etc., to break to create a fracture surface in accordance with a three-point bending test or a four-point bending test specified in JIS R1601:2008.
[0061] In the three-point bending test and four-point bending test specified in JIS R1601:2008, a force is applied between two supports of an insulator 11, causing the insulator 11 to break. The side where the supports are in contact becomes the range 21 including the starting point of the breakage.
[0062] In the embodiment, the spark plug 10 in which the ground electrode 17 is exposed in the combustion chamber when the spark plug 10 is attached to an engine (not shown) has been described, but the present invention is not necessarily limited to this. It is of course possible to apply the configuration of the embodiment to a spark plug in which the ground electrode 17 is covered with a cap having a through hole (a spark plug in which a sub-chamber is provided in the combustion chamber).
[0063] In the embodiment, the spark plug 10 in which spark discharge occurs between the center electrode 13 and the ground electrode 17 has been described, but the present invention is not necessarily limited to this. It is of course possible to apply the configuration of the embodiment to a spark plug that utilizes non-equilibrium plasma generated around the center electrode 13. [Explanation of symbols]
[0064] 10 Spark plug 11 Insulators (spark plug insulators) 12 Shaft hole 20 planes 21 Range C axis
Claims
1. A spark plug insulator made of an alumina-based sintered body having an axial hole extending along an axis, When the spark plug insulator is broken by applying a bending force to the spark plug insulator, The range including the origin of the fracture among the range obtained by dividing the fracture surface by a plane perpendicular to the direction of the force and including the axis is as follows: The average area of the particles appearing in the planar image of the above range is 4.4 μm 2 8.0 μm or more 2 The maximum area of the particles is 600 μm or less. 2 is as follows: The particles have an area of 60 μm 2 600 μm or more 2 including large particles that are: The large particles are 0.1 particles / mm2 per unit area of the planar image. 2 There are more than 100 spark plug insulators available.
2. The large particles are 6.2 particles / mm2 per unit area of the planar image. 2 2. The spark plug insulator of claim 1, wherein:
3. The particles have an area of 20 μm 2 More than 59 μm 2 Small particles that are: The small particles are 613 particles / mm2 per unit area of the planar image. 2 More than 2270 pieces / mm 2 3. A spark plug insulator according to claim 1 or 2, wherein:
4. A spark plug comprising the spark plug insulator according to claim 1 or 2.
Citation Information
Patent Citations
Insulating material for spark plug and spark plug
JP2001335360A
Alumina-based sintered body for spark plug, method for manufacturing the same, spark plug and method for manufacturing the same
JP2010135311A