Film-like sintered material with support sheet and method for manufacturing film-like sintered material with support sheet

The film-like fired material with a support sheet, characterized by specific roughness and a multi-step printing process, addresses the issues of wasted particles and irregular surfaces, ensuring secure separation and preventing water intrusion during the dicing process.

JP2024141676AInactive Publication Date: 2024-10-10LINTEC CORP

Patent Information

Application Number
JP2023053463
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing film-shaped fired materials result in wasted sinterable metal particles and irregular surfaces that cause floating and chip flying during separation, leading to water intrusion issues.

Method used

A film-like fired material with a support sheet comprising a base film and an adhesive layer, where the film-shaped fired material has an arithmetic mean roughness of 0.5 μm to 2.0 μm, is attached to a silicon wafer, peeled off, and then separated, using a method that includes screen printing and drying multiple times to achieve the desired surface roughness.

Benefits of technology

The solution minimizes floating and chip flying during separation, prevents water intrusion, and ensures effective dicing suitability by maintaining close contact between the film-like fired material and the support sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a film-like sintered material with a support sheet, which causes little floating between a film-like sintered material and a support sheet, causes little chip flying when a semiconductor wafer is diced together with the film-like sintered material on the support sheet, and has no risk of water intrusion during a water washing step.SOLUTION: A film-like sintered material 100 with a support sheet includes a support sheet 2 having a base film 3 and an adhesive layer 4 provided on the base film 3, and a film-like sintered material 1 containing sinterable metal particles 10 and a binder component 20 provided on the adhesive layer 4. The film-like sintered material 100 with the support sheet is attached to the mirror surface of a silicon mirror wafer by the film-like sintered material 1, and then the film-like sintered material 1 is peeled off from the support sheet 2. When the arithmetic mean roughness (Ra1) of the surface 1a of the film-like sintered material 1 on the side of the support sheet 2 is measured, the arithmetic mean roughness (Ra1) is 0.5 μm or more and less than 2.0 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film-shaped sintered material with a support sheet, and a method for producing the film-shaped sintered material with a support sheet. [Background technology]

[0002] In recent years, the demand for power semiconductor elements (power devices) has increased along with the trend toward higher voltages and currents in automobiles, air conditioners, personal computers, etc. Since power semiconductor elements are characterized by their use under high voltages and currents, heat generation from the semiconductor elements can easily become a problem. Conventionally, a heat sink is sometimes attached around a semiconductor element to dissipate heat generated from the semiconductor element, but if the thermal conductivity at the joint between the heat sink and the semiconductor element is not good, efficient heat dissipation is hindered.

[0003] As a bonding material with excellent thermal conductivity, for example, Patent Document 1 discloses a paste-like metal microparticle composition in which specific heat-sinterable metal particles, a specific polymer dispersant, and a specific volatile dispersion medium are mixed. When the composition is sintered, it is said to become a solid metal with excellent thermal conductivity.

[0004] Patent Document 2 and the like disclose a film-shaped sintered material containing sinterable metal particles and a binder component. The film-shaped sintered material described in Patent Document 2 has excellent thickness stability. In addition, by providing a support sheet on the film-shaped sintered material, the support sheet can be used as a dicing sheet to separate a semiconductor wafer into chips together with the film-shaped sintered material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-111800 A [Patent Document 2] JP 2019-052366 A Summary of the Invention [Problem to be solved by the invention]

[0006] The method for forming a film-shaped sintered material involves coating or printing a sintered material composition containing each component and a solvent for constituting the film-shaped sintered material, and then volatilizing the solvent as necessary to form a film-shaped sintered material in the desired location.

[0007] Patent Document 2 describes a method in which a sintered material composition is applied onto a flat release film, and then cut into a desired size and shape (e.g., a 153 mm circle). However, there is a problem in that the peripheral area containing expensive sinterable metal particles is wasted.

[0008] On the other hand, by screen printing the sintered material composition, it can be directly printed into a shape of the desired size. However, the surface of the film-shaped sintered material obtained by screen printing using a conventional sintered material composition has large irregularities. Therefore, when the film-shaped sintered material is laminated to the support sheet, a lift occurs between the film-shaped sintered material and the support sheet, and when the semiconductor wafer is singulated into chips together with the film-shaped sintered material on the support sheet, there is a risk of chips flying or water intrusion during the water washing process.

[0009] The present invention has been made to solve the problems described above, and aims to provide a film-like sintered material with a support sheet, which has little floating between the film-like sintered material and a support sheet, which has little chip flying when the semiconductor wafer is diced together with the film-like sintered material on the support sheet, and which has no risk of water intrusion during the water washing process, and a method for producing the film-like sintered material with a support sheet. [Means for solving the problem]

[0010] That is, the present invention has the following aspects. [1] A film-shaped sintered material with a support sheet, comprising: a support sheet having a base film and an adhesive layer provided on the base film; and a film-shaped sintered material containing sinterable metal particles and a binder component provided on the adhesive layer, The film-shaped sintered material with support sheet is attached to the mirror surface of a silicon mirror wafer using the film-shaped sintered material, and then the film-shaped sintered material is peeled off from the support sheet. When the arithmetic mean roughness (Ra1) of the surface of the film-shaped sintered material facing the support sheet is measured, the arithmetic mean roughness (Ra1) is 0.5 μm or more and less than 2.0 μm. [2] The film-shaped sintered material with a support sheet according to [1], wherein the pressure-sensitive adhesive layer is energy ray curable. [3] A step of forming a film-shaped sintered material, the step comprising screen-printing a sintered material composition containing sinterable metal particles, a binder component and a solvent on a release-treated surface of a release film and drying the sintered material composition; A step of preparing a support sheet having a base film and a pressure-sensitive adhesive layer provided on the base film; A method for producing a film-shaped sintered material with a support sheet according to [1] or [2], comprising a step of attaching the support sheet to the exposed surface of the film-shaped sintered material using the exposed surface of the adhesive layer. [4] A method for producing a film-shaped sintered material with a support sheet described in [3], wherein the step of forming the film-shaped sintered material includes screen-printing the sintered material composition on a release-treated surface of a release film, drying the sintered material composition, screen-printing the sintered material composition again on an exposed surface of the obtained film, and drying the sintered material composition. Effect of the Invention

[0011] According to the present invention, it is possible to provide a film-like sintered material with a support sheet, in which there is little floating between the film-like sintered material and the support sheet, there is little chip flying when the semiconductor wafer is singulated together with the film-like sintered material on the support sheet, and there is no risk of water intrusion during the water washing process. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing a film-shaped sintered material with a support sheet according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a state in which a film-shaped sintered material with a support sheet according to one embodiment of the present invention is attached to a ring frame. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <Film-shaped baking material with support sheet> The film-shaped sintered material with a support sheet of the present embodiment is a film-shaped sintered material with a support sheet, comprising a support sheet having a base film and an adhesive layer provided on the base film, and a film-shaped sintered material containing sinterable metal particles and a binder component provided on the adhesive layer, The film-shaped sintered material with support sheet is attached to the mirror surface of a silicon mirror wafer using the film-shaped sintered material, and then the film-shaped sintered material is peeled off from the support sheet. When the arithmetic mean roughness (Ra1) of the surface of the film-shaped sintered material on the support sheet side is measured, the arithmetic mean roughness (Ra1) is 0.5 μm or more and less than 2.0 μm.

[0014] In the measurement of the arithmetic mean roughness (Ra1), the mirror surface of the silicon mirror wafer may be, for example, a mirror surface obtained by subjecting the surface of the silicon wafer to chemical mechanical polishing until the arithmetic mean roughness (Ra) becomes 0.02 μm or less. The exposed surface of the film-shaped sintered material is laminated to the mirror surface of the silicon mirror wafer, and then the film-shaped sintered material is peeled off from the support sheet to form a laminate of the film-shaped sintered material and the silicon mirror wafer. The arithmetic mean roughness (Ra1) of the exposed surface of the film-shaped sintered material in the laminate can then be measured, for example, using a commercially available surface roughness meter in accordance with JIS B0601:2013.

[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. In addition, the figures used in the following explanation may show key parts enlarged for convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0016] FIG. 1 is a cross-sectional view that illustrates a film-shaped sintered material with a support sheet according to the present embodiment. The film-shaped sintered material 100 with a support sheet is formed by temporarily attaching a film-shaped sintered material 1 to a support sheet 2 in a peelable manner. As shown in FIG. 1, the film-shaped sintered material 1 contains sinterable metal particles 10 and a binder component 20. The support sheet 2 is formed by providing an adhesive layer 4 on a base film 3, and the film-shaped sintered material 1 is provided on the adhesive layer 4. The film-shaped sintered material 1 is provided in direct contact with the adhesive layer 4. The film-shaped sintered material 100 with a support sheet of this embodiment has an arithmetic mean roughness (Ra1) of 0.5 μm or more and less than 2.0 μm, and there is little lift 50 between the film-shaped sintered material 1 and the support sheet 2. The arithmetic mean roughness (Ra1) is preferably 0.6 μm or more and 1.9 μm or less.

[0017] The film-shaped sintered material with support sheet of this embodiment can be used as a dicing sheet used when dividing a semiconductor wafer into chips. By dividing it together with the semiconductor wafer using a blade or the like, it can be processed into a film-shaped sintered material of the same shape as the chip, and a chip with the film-shaped sintered material can be manufactured.

[0018] Hereinafter, one embodiment of the film-shaped sintered material with a support sheet will be described. FIG. 2 shows a schematic cross-sectional view of the film-shaped sintered material with a support sheet of this embodiment. As shown in FIG. 2, the film-shaped sintered material with a support sheet of this embodiment 100a is formed by temporarily attaching a film-shaped sintered material 1 to the inner periphery of a support sheet 2 in a peelable manner. As shown in FIG. 2, the support sheet 2 is an adhesive sheet having an adhesive layer 4 on the upper surface of a base film 3, and the inner periphery surface of the adhesive layer 4 is covered with the film-shaped sintered material 1, and the adhesive portion is exposed on the outer periphery. In this configuration example, it is preferable that the film-shaped sintered material 1 having a smaller diameter than the support sheet 2 is peelably laminated concentrically on the adhesive layer 4 of the support sheet 2.

[0019] The film-shaped sintered material 1 is preferably formed on the inner periphery of the support sheet 2 in substantially the same shape as the workpiece (for example, a semiconductor wafer, an insulating wafer, etc.) to be attached thereto.

[0020] The semiconductor wafer may be a silicon wafer, and the insulating wafer may be a glass wafer or a sapphire wafer, but is not limited thereto.

[0021] The support sheet 2 has an adhesive portion on its outer periphery. In a preferred embodiment, a film-shaped sintered material 1 having a smaller diameter than the support sheet 2 is laminated concentrically on the circular support sheet 2. The adhesive portion on the outer periphery is used to fix a ring frame 5 as shown in the figure. The film-shaped sintered material 100a with support sheet having the above-mentioned configuration is attached to a ring frame 5 at the adhesive layer 4 exposed on the outer periphery of the support sheet 2.

[0022] In addition, a ring-shaped double-sided tape or adhesive layer may be provided separately on the margin for the ring frame (the adhesive layer exposed at the outer periphery of the adhesive sheet). The double-sided tape has a structure of adhesive layer / core material / adhesive layer, and the adhesive layer in the double-sided tape is not particularly limited, and adhesives such as rubber-based resin, acrylic resin, silicone resin, polyvinyl ether, etc. are used. The adhesive layer is attached to the ring frame at its outer periphery when manufacturing the chip-attached substrate described later. As the core material of the double-sided tape, for example, polyester film, polypropylene film, polycarbonate film, polyimide film, fluororesin film, liquid crystal polymer film, etc. are preferably used.

[0023] The thickness of the film-shaped sintered material with a support sheet is preferably 1 to 500 μm, more preferably 5 to 300 μm, and even more preferably 10 to 200 μm.

[0024] In this specification, the "thickness" is a value expressed as an average value of thicknesses measured at any five points, and can be obtained using a constant pressure thickness measuring device in accordance with JIS K7130.

[0025] (Film-shaped fired material) As shown in FIG. 1, the film-shaped sintered material 1 contains sinterable metal particles 10 and a binder component 20.

[0026] The film-shaped fired material may be made up of one layer (single layer), but is preferably made up of two or more layers. When a conventional sintered material composition is used to form a single-layered film-shaped sintered material of suitable thickness on a release film by screen printing once, it is necessary to use a screen mesh with wide openings, and the arithmetic mean roughness (Ra0) of the exposed surface of the film-shaped sintered material becomes rough. As a result, the arithmetic mean roughness (Ra1) of the surface of the film-shaped sintered material on the side of the support sheet after it is attached to the mirror surface of the silicon mirror wafer also becomes rough, and the arithmetic mean roughness (Ra1) of the surface cannot be adjusted to a suitable range. When the film-shaped sintered material is composed of multiple layers, by using a screen mesh with narrow mesh openings, the arithmetic mean roughness (Ra1) of the surface on the support sheet side of the film-shaped sintered material can be adjusted to a suitable range by performing screen printing multiple times, even when using a conventional sintered material composition for screen printing. Alternatively, by using a sintered material composition containing an acrylic resin with a glass transition temperature (Tg) of -20°C or lower as a binder component, even with a single screen printing process, the arithmetic mean roughness (Ra1) of the surface of the support sheet side of the film-shaped sintered material can be adjusted to a suitable range, and a single-layer film-shaped sintered material of a suitable thickness can be formed.

[0027] In this specification, not only in the case of a film-shaped fired material, "multiple layers may be the same or different" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different" means "at least one of the constituent materials, the composition ratio of the constituent materials, and the thickness of each layer is different".

[0028] The thickness of the film-shaped sintered material before sintering is not particularly limited, but is preferably 30 to 200 μm, more preferably 40 to 150 μm, and even more preferably 50 to 90 μm. Here, "thickness of the film-shaped sintered material" means the thickness of the entire film-shaped sintered material; for example, the thickness of a film-shaped sintered material consisting of multiple layers means the total thickness of all layers that make up the film-shaped sintered material.

[0029] (Release film) The film-shaped sintered material can be formed with a release film laminated thereon. When in use, the release film is peeled off and the film-shaped sintered material is placed on the object to be sintered and bonded. The release film also functions as a protective film to prevent damage to the film-shaped sintered material and adhesion of dirt. The release film needs to be provided on at least one side of the film-shaped sintered material, and may be provided on both sides of the film-shaped sintered material. When provided on both sides, one of the films functions as a support sheet.

[0030] Examples of the release film include transparent films such as polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate copolymer films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these films are also used. Furthermore, laminated films of these films may be used. Furthermore, colored films and opaque films of these films may be used. Examples of the release agent include silicone-based, fluorine-based, olefin-based, alkyd-based, and long-chain alkyl group-containing carbamates. In this specification, the term "(meth)acrylic" is used to mean both acrylic and methacrylic.

[0031] The thickness of the release film is usually about 10 to 500 μm, preferably about 15 to 300 μm, and particularly preferably about 20 to 250 μm.

[0032] <Sinterable metal particles> Sinterable metal particles are metal particles that can be fused and bonded together to form a sintered body by heat treatment at a temperature equal to or higher than the melting point of the metal particles as the sintering of the film-shaped sintered material. By forming a sintered body, it is possible to sinter-bond the film-shaped sintered material and an article that is sintered in contact with it. Specifically, it is possible to sinter-bond a chip and a substrate via the film-shaped sintered material.

[0033] The constituent materials of the sinterable metal particles include simple metals, barium titanate, oxides and alloys of the simple metals. The simple metals include silver, gold, copper, iron, nickel, aluminum, silicon, palladium, platinum, titanium, etc. The constituent materials of the sinterable metal particles are preferably silver and silver oxide. The sinterable metal particles may be mixed in one type or in a combination of two or more types.

[0034] The sinterable metal particles are preferably silver nanoparticles, which are nano-sized silver particles.

[0035] The particle size of the sinterable metal particles contained in the film-shaped sintered material is not particularly limited as long as it can exhibit the above sinterability, but may be 100 nm or less, 50 nm or less, or 30 nm or less. The particle size of the metal particles contained in the film-shaped sintered material is the diameter of the projected area circle equivalent of the particle size of the metal particles observed with an electron microscope. Metal particles falling within the above particle size range are preferable because they have excellent sinterability. The particle size of the sinterable metal particles contained in the film-shaped sintered material may be 0.1 to 95 nm, 0.3 to 50 nm, or 0.5 to 30 nm, as determined by observing the particle size of the metal particles with a projected area circle equivalent diameter of 100 nm or less under an electron microscope. The number of metal particles to be measured is 100 or more randomly selected per film-shaped sintered material.

[0036] Before mixing with the binder component and other additive components, the sinterable metal particles may be dispersed in a high-boiling point solvent such as isobornylcyclohexanol or decyl alcohol in advance to make the particles free of agglomerates. The boiling point of the high-boiling point solvent may be, for example, 200 to 350°C. In this case, if a high-boiling point solvent is used, the sinterable metal particles are prevented from becoming concentrated because the solvent hardly volatilizes at room temperature, improving workability and preventing re-agglomeration of the sinterable metal particles, resulting in good quality. Examples of dispersion methods include a kneader, a triple roll mill, a bead mill, and ultrasonic waves.

[0037] In addition to metal particles (sinterable metal particles) having a particle diameter of 100 nm or less, the film-shaped fired material may further contain non-sinterable metal particles having a particle diameter exceeding 100 nm that do not fall under the above. The particle diameter of the non-sinterable metal particles having a particle diameter exceeding 100 nm may be a number average particle diameter of more than 150 nm and not more than 50,000 nm, 150 to 10,000 nm, or 180 to 5,000 nm, calculated by measuring the particle diameter of the metal particles observed by an electron microscope and the projected area circle equivalent diameter of the particles exceeding 100 nm.

[0038] The content of metal particles having a particle diameter (diameter equivalent to a circle having a projected area) of more than 300 nm relative to the total mass (100% by mass) of all metal particles is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. The upper limit of the content may be, for example, 90% by mass or less, 85% by mass or less, or 80% by mass or less. As an example of the numerical range of the above numerical value, the content ratio of metal particles having the above particle diameter (diameter equivalent to a circle having a projected area) of more than 300 nm relative to the total mass (100 mass%) of all metal particles may be 10 to 90 mass%, 15 to 85 mass%, or 20 to 80 mass%.

[0039] Examples of the metal species of the non-sinterable metal particles having a particle size of more than 100 nm include the same metal species as those exemplified above for the sinterable metal particles, and silver, copper, and oxides thereof are preferred. The metal particles having a particle size of 100 nm or less and the non-sintered metal particles having a particle size of more than 100 nm may be the same metal type or different metal types. For example, the metal particles having a particle size of 100 nm or less may be silver particles, and the non-sintered metal particles having a particle size of more than 100 nm may be silver or silver oxide particles. For example, the metal particles having a particle size of 100 nm or less may be silver or silver oxide particles, and the non-sintered metal particles having a particle size of more than 100 nm may be copper or copper oxide particles.

[0040] In the film-shaped sintered material, the content of sinterable metal particles relative to the total mass (100 mass%) of all metal particles may be 10 mass% or more, may be 10 to 90 mass%, or may be 20 to 85 mass%.

[0041] The surfaces of the sinterable metal particles and / or the non-sinterable metal particles may be coated with an organic material. By having an organic coating, the compatibility with the binder component is improved, the aggregation of the particles can be prevented, and the particles can be dispersed uniformly. When the surfaces of the sinterable metal particles and / or non-sinterable metal particles are coated with an organic substance, the mass and particle size of the sinterable metal particles and non-sinterable metal particles include the coating.

[0042] <Binder components> By adding the binder component, the fired material can be formed into a film shape and the film-shaped fired material before firing can be given adhesiveness. The binder component may be pyrolytic, which is pyrolyzed by heat treatment in firing the film-shaped fired material. The binder component is not particularly limited, but a suitable example of the binder component is a resin. Examples of the resin include acrylic resin, polycarbonate, polylactic acid, and polymers of cellulose derivatives, and acrylic resin is preferred. The acrylic resin includes a homopolymer of a (meth)acrylate compound, a copolymer of two or more kinds of (meth)acrylate compounds, and a copolymer of a (meth)acrylate compound and another copolymerizable monomer.

[0043] In this specification, the term "derivative" refers to a compound in which one or more hydrogen atoms of the original compound have been replaced with a group (substituent) other than a hydrogen atom.

[0044] In the resin constituting the binder component, the content of the structural unit derived from the (meth)acrylate compound is preferably 50 to 100 mass%, more preferably 80 to 100 mass%, and further preferably 90 to 100 mass%, relative to the total mass (100 mass%) of the structural units. "Derived from" in this context means that the monomer has undergone the structural changes necessary to be polymerized.

[0045] Specific examples of the (meth)acrylate compound include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, and octyl (meth)acrylate, alkyl (meth)acrylates such as isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-hydroxybutyl (meth)acrylate; phenoxyalkyl (meth)acrylates such as phenoxyethyl (meth)acrylate and 2-hydroxy-3-phenoxypropyl (meth)acrylate; Alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, and 2-methoxybutyl (meth)acrylate; Polyalkylene glycol (meth)acrylates such as polyethylene glycol mono(meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, polypropylene glycol mono(meth)acrylate, methoxypolypropylene glycol (meth)acrylate, ethoxypolypropylene glycol (meth)acrylate, and nonylphenoxypolypropylene glycol (meth)acrylate; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, 4-butylcyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, bornyl (meth)acrylate, isobornyl (meth)acrylate, and tricyclodecanyl (meth)acrylate; Examples of the (meth)acrylate compound include benzyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, etc. Alkyl (meth)acrylate or alkoxyalkyl (meth)acrylate is preferred, and particularly preferred (meth)acrylate compounds include butyl (meth)acrylate, ethylhexyl (meth)acrylate, lauryl (meth)acrylate, isodecyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, and 2-ethoxyethyl (meth)acrylate. In this specification, the term "(meth)acrylate" is a concept that encompasses both "acrylate" and "methacrylate".

[0046] The acrylic resin is preferably a methacrylate. When the binder component contains a structural unit derived from a methacrylate, the binder can be fired at a relatively low temperature, and the condition for obtaining sufficient adhesive strength after sintering can be easily satisfied.

[0047] In the resin constituting the binder component, the content of the methacrylate-derived structural unit relative to the total mass (100 mass%) of the structural units is preferably 50 to 100 mass%, more preferably 80 to 100 mass%, and even more preferably 90 to 100 mass%.

[0048] The other copolymerizable monomer is not particularly limited as long as it is a compound copolymerizable with the above-mentioned (meth)acrylate compound, and examples thereof include unsaturated carboxylic acids such as (meth)acrylic acid, vinyl benzoic acid, maleic acid, and vinyl phthalic acid; and vinyl group-containing radical polymerizable compounds such as vinyl benzyl methyl ether, vinyl glycidyl ether, styrene, α-methylstyrene, butadiene, and isoprene.

[0049] The mass average molecular weight (Mw) of the resin constituting the binder component is preferably 1,000 to 1,000,000, and more preferably 10,000 to 800,000. When the mass average molecular weight of the resin is within the above range, the film exhibits sufficient film strength and can easily be imparted with flexibility. In this specification, unless otherwise specified, the "mass average molecular weight" is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0050] The glass transition temperature (Tg) of the resin constituting the binder component can be calculated using the Fox formula shown below, and is preferably -60 to 50°C, more preferably -55 to 10°C, and even more preferably -50°C or more and less than 0°C. When the Tg of the resin calculated from the Fox formula is equal to or less than the upper limit, the adhesive strength between the film-shaped sintered material and the adherend (e.g., chip, substrate, etc.) before sintering is improved. In addition, the flexibility of the film-shaped sintered material is increased. On the other hand, when the Tg of the resin calculated from the Fox formula is equal to or more than the lower limit, the film shape can be maintained, and the film-shaped sintered material can be more easily separated from the support sheet, etc.

[0051] 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+...+(Wm / Tgm) (wherein Tg is the glass transition temperature of the resin constituting the binder component, Tg1, Tg2,...Tgm are the glass transition temperatures of the homopolymers of the monomers that are the raw materials of the resin constituting the binder component, and W1, W2,...Wm are the mass fractions of the monomers. However, W1+W2+...+Wm=1.) As the glass transition temperature of the homopolymer of each monomer in the Fox formula, the value described in the Polymer Data Handbook or the Adhesive Handbook can be used.

[0052] Even when screen printing is performed using a conventional fired material composition, the arithmetic mean roughness (Ra1) of the surface of the film-shaped fired material on the support sheet side can be adjusted to a suitable range by performing screen printing multiple times. On the other hand, by using an acrylic resin with a glass transition temperature (Tg) of -20°C or lower, the arithmetic mean roughness (Ra1) of the surface on the support sheet side of the film-shaped fired material can be adjusted to a suitable range even with a single screen printing.

[0053] Examples of acrylic resins having a glass transition temperature (Tg) of -20°C or lower include homopolymers of (meth)acrylate compounds, copolymers of two or more types of (meth)acrylate compounds, and copolymers of (meth)acrylate compounds and other copolymerizable monomers.

[0054] For example, when the resin constituting the binder component is a homopolymer of an alkyl (meth)acrylate compound, the longer the alkyl group of the alkyl (meth)acrylate, the lower the glass transition temperature (Tg). In addition, when the length of the alkyl group is the same, the glass transition temperature (Tg) of the homopolymer of the alkyl acrylate compound tends to be lower than the glass transition temperature (Tg) of the homopolymer of the alkyl methacrylate compound. The glass transition temperature (Tg) of a copolymer of two or more types of (meth)acrylate compounds can be appropriately adjusted by adjusting the content ratio of each of the structural units derived from the (meth)acrylate compound in the copolymer.

[0055] The binder component may be pyrolytic, that is, pyrolyzed by heat treatment as firing of the film-shaped fired material. The pyrolysis of the binder component can be confirmed by the mass reduction of the binder component by firing. The components blended as the binder component may be almost pyrolyzed by firing, but the total mass of the components blended as the binder component may not be pyrolyzed by firing. The binder component may be one whose mass after firing is 10% by mass or less, 5% by mass or less, or 3% by mass or less, relative to the total mass (100% by mass) of the binder components before firing.

[0056] A copolymer or homopolymer containing a large amount of structural units derived from an alkyl methacrylate compound has better thermal decomposition properties when formed into a film-shaped fired material than a copolymer or homopolymer containing a large amount of structural units derived from an alkyl acrylate compound. Therefore, the content of structural units derived from an alkyl methacrylate compound is preferably 70 to 100% by mass, more preferably 80 to 100% by mass, and even more preferably 90 to 100% by mass, based on the total mass (100% by mass) of the structural units.

[0057] In addition to the above-mentioned sinterable metal particles, non-sinterable metal particles, and binder components, the film-shaped sintered material may contain other additives that do not fall under the category of sinterable metal particles, non-sinterable metal particles, and binder components, within a range that does not impair the effects of the present invention.

[0058] Other additives that may be contained in the film-shaped sintered material include solvents, dispersants, plasticizers, tackifiers, storage stabilizers, antifoamers, thermal decomposition promoters, and antioxidants. Only one type of additive may be contained, or two or more types may be contained. These additives are not particularly limited, and can be appropriately selected from those commonly used in this field.

[0059] Since the binder component is preferably thermally decomposed by heat treatment in the firing of the film-shaped fired material, the content of thermosetting resin such as epoxy resin is preferably 10 mass% or less, more preferably 5 mass% or less, relative to 100 mass% of the binder component, and even more preferably contains substantially no thermosetting resin. From a similar viewpoint, in the resin constituting the binder component, the content of acrylate-derived structural units, out of "acrylate" and "methacrylate", relative to the total mass (100 mass%) of the structural units is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably it does not substantially contain any acrylate-derived structural units.

[0060] <Composition> The film-shaped sintered material may be composed of sinterable metal particles, a binder component, and other additives, and the sum of their contents (mass%) may be 100 mass%. When the film-shaped sintered material contains non-sinterable metal particles, the film-shaped sintered material may be composed of sinterable metal particles, non-sinterable metal particles, a binder component, and other additives, and the sum of their contents (mass%) may be 100 mass%.

[0061] In the film-shaped fired material, the content of the sinterable metal particles relative to the total mass (100 mass%) of all components other than the solvent (hereinafter referred to as "solid content") is preferably 15 to 88 mass%, more preferably 15 to 85 mass%, and even more preferably 20 to 80 mass%. By having the content of the sinterable metal particles be equal to or less than the above upper limit, the content of the binder component can be sufficiently ensured, making it easy to maintain the film shape. On the other hand, by having the content of the sinterable metal particles be equal to or more than the above lower limit, the sinterable metal particles are fused to each other or to the non-sinterable metal particles during firing, and the effect of expressing high bonding adhesive strength (shear adhesive strength) after firing can be obtained.

[0062] When the film-shaped sintered material contains non-sinterable metal particles, the total content of the sinterable metal particles and non-sinterable metal particles relative to the total mass (100 mass%) of the solid contents in the film-shaped sintered material is preferably 50 to 98 mass%, more preferably 70 to 95 mass%, and even more preferably 80 to 95 mass%.

[0063] The content of the binder component relative to the total mass (100 mass%) of the solid content in the film-shaped sintered material is preferably 2 to 50 mass%, more preferably 5 to 30 mass%, and even more preferably 5 to 20 mass%. By making the content of the binder component equal to or less than the upper limit, the content of the sinterable metal particles can be sufficiently ensured, and the bonding adhesive strength between the film-shaped sintered material and the adherend is further improved. On the other hand, by making the content of the binder component equal to or more than the lower limit, the film shape can be easily maintained.

[0064] In the film-shaped sintered material, the mass ratio of the sinterable metal particles to the binder component (sinterable metal particles:binder component) is preferably 50:1 to 1:5, more preferably 20:1 to 1:2, and even more preferably 10:1 to 1:1. When the film-shaped sintered material contains non-sinterable metal particles, the mass ratio of the sinterable metal particles and non-sinterable metal particles to the binder component ((sinterable metal particles + non-sinterable metal particles):binder component) is preferably 50:1 to 1:1, more preferably 20:1 to 2:1, and even more preferably 9:1 to 4:1.

[0065] The film-shaped sintered material may contain a high-boiling point solvent used when mixing the sinterable metal particles, non-sinterable metal particles, binder components, and other additive components. The content of the high-boiling point solvent relative to the total mass (100 mass%) of the film-shaped sintered material is preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less.

[0066] [Manufacturing method of film-shaped fired material] The film-shaped fired material can be formed using a fired material composition containing the constituent materials. For example, a sintered material composition containing the components and a solvent for constituting the film-shaped sintered material can be coated or printed on the surface on which the film-shaped sintered material is to be formed, and the solvent can be volatilized as necessary to form a film-shaped sintered material in the desired location. The surface on which the film-shaped fired material is formed can be the surface of a release film.

[0067] When applying the fired material composition, the solvent preferably has a boiling point of less than 200° C., such as n-hexane (boiling point: 68° C.), ethyl acetate (boiling point: 77° C.), 2-butanone (boiling point: 80° C.), n-heptane (boiling point: 98° C.), methylcyclohexane (boiling point: 101° C.), toluene (boiling point: 111° C.), acetylacetone (boiling point: 138° C.), n-xylene (boiling point: 139° C.), and dimethylformamide (boiling point: 153° C.). These may be used alone or in combination.

[0068] The firing material composition may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a Comma Coater (registered trademark), a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0069] When printing the sintered material composition, the solvent may be one that can be evaporated and dried after printing, and preferably has a boiling point of 65 to 350° C. Examples of such solvents include the above-mentioned solvents with a boiling point of less than 200° C., as well as isophorone (boiling point: 215° C.), butyl carbitol (boiling point: 230° C.), 1-decanol (boiling point: 233° C.), butyl carbitol acetate (boiling point: 247° C.), and isobornyl cyclohexanol (boiling point: 318° C.). If the boiling point exceeds 350°C, the solvent will not volatilize easily during drying after printing, making it difficult to obtain the desired shape, or the solvent may remain in the film during baking, causing deterioration of bonding and adhesion. If the boiling point is below 65°C, the solvent will volatilize during printing, which may cause the thickness stability to be impaired. If a solvent with a boiling point of 200 to 350°C is used, the viscosity increase due to the evaporation of the solvent during printing can be suppressed, and printing suitability can be obtained.

[0070] The firing material composition can be printed by a known printing method, but is preferably printed by a screen printing method such as silk screen printing or rotary screen printing.

[0071] The shape of the film-shaped sintered material may be appropriately set according to the shape of the object to be sintered, and is preferably circular or rectangular. A circular shape corresponds to the shape of a semiconductor wafer. A rectangular shape corresponds to the shape of a chip. The corresponding shape may be the same or approximately the same as the shape of the object to be sintered. When the film-shaped sintered material is circular, the area of ​​the circle is 3.5 to 1,600 cm 2 may be 85 to 1,400 cm 2 When the film-shaped fired material is rectangular, the area of ​​the rectangle may be 0.01 to 25 cm 2 0.25 to 9 cm 2 It may be. In particular, by printing the sintered material composition, a film-like sintered material having a desired shape can be easily formed.

[0072] The drying conditions for the sintered material composition are not particularly limited. When the sintered material composition contains a solvent, it is preferable to dry it by heating. In this case, it is preferable to dry it under conditions of, for example, 70 to 250°C, e.g., 80 to 180°C, for 10 seconds to 10 minutes.

[0073] (Base film) The base film 3 is not particularly limited, and examples of films that can be used include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ethylene-propylene copolymer, polypropylene, polybutene, polybutadiene, polymethylpentene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-methyl (meth)acrylate copolymer, ethylene-ethyl (meth)acrylate copolymer, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, polyurethane film, and ionomer. Furthermore, when higher heat resistance is required for the support sheet, examples of the base film 3 include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, and polyolefin films such as polypropylene and polymethylpentene. Crosslinked films of these films and films modified by radiation, discharge, etc. can also be used. The base film may be a laminate of the above films.

[0074] These films may be laminated or combined. Furthermore, these films may be colored or printed. The film may be a sheet made by extrusion molding of a thermoplastic resin, or may be a stretched film, or a sheet made by thinning and curing a curable resin by a predetermined means may be used.

[0075] The thickness of the base film is not particularly limited, and is preferably 30 to 300 μm, more preferably 50 to 200 μm. By setting the thickness of the base film within the above range, the base film is less likely to break even when cut by dicing. In addition, since the film-shaped sintered material with support sheet is given sufficient flexibility, it shows good attachment to the workpiece (e.g., semiconductor wafer, insulating wafer, etc.).

[0076] The substrate film can also be obtained by applying a release agent to the surface and carrying out a release treatment. Examples of the release agent used in the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents, and the alkyd-based, silicone-based, and fluorine-based release agents are particularly preferred because of their heat resistance.

[0077] In order to perform a release treatment on the surface of a base film using the above-mentioned release agent, the release agent may be applied as is without a solvent or after dilution with a solvent or emulsification using a gravure coater, a Mayer bar coater, an air knife coater, a roll coater or the like, and the base film to which the release agent has been applied may be subjected to curing at room temperature or under heating, or may be cured with an electron beam, or a laminate may be formed by wet lamination, dry lamination, hot melt lamination, melt extrusion lamination, coextrusion processing or the like.

[0078] (Adhesive layer) The pressure-sensitive adhesive layer 4 is in the form of a sheet or film, and can contain a pressure-sensitive adhesive. The support sheet 2 may be an ordinary adhesive sheet having an adhesive layer 4 on the entire upper surface of the base film 3 as shown in Fig. 2, or may be configured such that the inner peripheral surface of the adhesive layer 4 is covered with a film-like sintered material and the adhesive portion is exposed on the outer peripheral portion. In this case, the outer peripheral portion of the adhesive layer 4 is used to fix the above-mentioned ring frame 5, and the film-like sintered material is peelably laminated on the inner peripheral portion. The adhesive layer 4 may be a weakly adhesive one or an energy ray curable adhesive.

[0079] In this specification, the term "energy ray" refers to electromagnetic waves or charged particle beams that have an energy quantum, and examples of such beams include ultraviolet rays, radioactive rays, and electron beams. The ultraviolet light can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light, an LED lamp, etc. as an ultraviolet light source. The electron beam can be generated by an electron beam accelerator or the like. In this specification, "energy ray curable" means a property that is cured by irradiation with energy rays, and "non-energy ray curable" means a property that is not cured even when irradiated with energy rays.

[0080] As the weak adhesive, acrylic resin and silicone resin are preferably used. In addition, in consideration of the peelability of the film-like baked material, the adhesive strength of the adhesive layer 4 to the SUS plate at 23°C is preferably 30 to 120 mN / 25 mm, more preferably 50 to 1000 mN / 25 mm, and even more preferably 60 to 1000 mN / 25 mm. If this adhesive strength is too low, the ring frame may fall off. If the adhesive strength is too high, it becomes difficult to peel off from the ring frame, making it difficult to reuse the ring frame.

[0081] In the support sheet having the configuration of FIG. 2, when an energy ray-curable re-peelable adhesive layer is used, the area where the film-like sintered material is laminated may be irradiated with energy rays in advance to reduce the adhesiveness. In this case, the other areas may not be irradiated with energy rays, and the adhesive strength may be maintained high, for example, for the purpose of adhesion to the ring frame 5. In order to avoid irradiating only the other areas with energy rays, for example, an energy ray shielding layer may be provided by printing or the like in the area corresponding to the other areas of the base film, and energy rays may be irradiated from the base film side. In addition, in the support sheet having the configuration of FIG. 2, in order to strengthen the adhesion between the base film 3 and the adhesive layer 4, the surface of the base film 3 on which the adhesive layer 4 is provided may be subjected to a roughening treatment such as sandblasting or solvent treatment, or an oxidation treatment such as corona discharge treatment, electron beam irradiation, plasma treatment, ozone / ultraviolet irradiation treatment, flame treatment, chromate treatment, and hot air treatment, if desired. A primer treatment may also be applied.

[0082] The thickness of the pressure-sensitive adhesive layer 4 is not particularly limited, but is preferably 1 to 100 μm, more preferably 2 to 80 μm, and particularly preferably 3 to 50 μm.

[0083] The pressure-sensitive adhesive layer may be one layer (single layer) or two or more layers. When the pressure-sensitive adhesive layer is made up of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0084] <Adhesive composition> The adhesive layer can be formed using a known adhesive composition containing an adhesive. For example, the adhesive composition is applied to the surface on which the adhesive layer is to be formed, and dried as necessary to form the adhesive layer at the desired location. A more specific method for forming the adhesive layer will be described in detail later, together with the method for forming other layers. The ratio of the contents of the components that do not vaporize at room temperature in the adhesive composition is usually the same as the ratio of the contents of the components in the adhesive layer.

[0085] [Manufacturing method of film-shaped sintered material with support sheet] The manufacturing method of the film-shaped sintered material with a support sheet of this embodiment is a method for manufacturing the film-shaped sintered material with a support sheet of the above embodiment, A step of forming a film-like sintered material, the step comprising screen-printing a sintered material composition containing sinterable metal particles, a binder component, and a solvent on a release-treated surface of a release film, and drying the sintered material composition; A step of preparing a support sheet having a base film and a pressure-sensitive adhesive layer provided on the base film; and bonding the support sheet to the exposed surface of the film-shaped fired material using the exposed surface of the pressure-sensitive adhesive layer.

[0086] In the manufacturing method of the film-shaped sintered material with support sheet of this embodiment, the sintered material composition is screen printed on the release-treated surface of the release film, so that the sintered material composition can be directly printed in a shape of the desired size onto the release film, and expensive sinterable metal particles can be used effectively without wasting them.

[0087] The film-shaped sintered material with support sheet obtained by the manufacturing method of this embodiment has an arithmetic mean roughness (Ra1) of the surface of the film-shaped sintered material on the support sheet side after the film-shaped sintered material with support sheet is formed and attached to the mirror surface of a silicon mirror wafer, and is therefore excellent in dicing suitability, with little floating between the film-shaped sintered material and the support sheet, little chip flying when the semiconductor wafer is diced together with the film-shaped sintered material on the support sheet, and there is no risk of water intrusion during the water washing process.

[0088] For example, the arithmetic mean roughness (Ra0) of the exposed surface of the film-shaped fired material formed by screen printing on the release-treated surface of the release film can be adjusted by appropriately selecting the screen mesh. For example, when a screen mesh with a wide mesh size is used, the arithmetic mean roughness (Ra0) tends to be large, and when a screen mesh with a narrow mesh size is used, the arithmetic mean roughness (Ra0) tends to be small. When a screen mesh with a narrow mesh size is used, the film-shaped fired material may be thinner than the desired thickness, but in that case, a multi-layer film-shaped fired material of the desired thickness can be formed by screen printing multiple times.

[0089] For example, the arithmetic mean roughness (Ra1) can be adjusted by appropriately selecting a screen mesh when the sintered material composition is screen-printed on the release-treated surface of the release film. When a normal sintered material composition is used, the arithmetic mean roughness (Ra1) is adjusted to 0.5 μm or more and less than 2.0 μm, so the arithmetic mean roughness (Ra0) is also adjusted to 0.5 μm or more and less than 2.0 μm. However, for example, if a resin constituting the binder component of the film-shaped sintered material is selected that has a glass transition temperature (Tg) of -20°C or less, it is possible to adjust the arithmetic mean roughness (Ra1) to 0.5 μm or more and less than 2.0 μm even when the arithmetic mean roughness (Ra0) is 2.0 μm or more.

[0090] In the manufacturing method of the film-shaped sintered material with support sheet of this embodiment, the step of forming the film-shaped sintered material preferably includes screen printing the sintered material composition on the release-treated surface of a release film, drying the sintered material composition, screen printing the sintered material composition again on the exposed surface of the obtained film, and drying the sintered material composition. By performing screen printing multiple times, it becomes easy to adjust the arithmetic mean roughness (Ra1) to 0.5 μm or more and less than 2.0 μm while ensuring an appropriate thickness of the film-shaped sintered material.

[0091] The film-shaped sintered material with a support sheet may be stored with a release film attached to the outermost surface of the film-shaped sintered material on the side opposite to the support sheet. The release film may be removed as necessary after the film-shaped sintered material with a support sheet is formed. EXAMPLES

[0092] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples.

[0093] [Example 1] <<Production of film-shaped fired material with support sheet>> <Production of fired material composition> The components used in the preparation of the sintered material composition are shown below. Here, metal particles with a particle size of 100 nm or less are referred to as "sinterable metal particles."

[0094] (Sinterable metal particle-containing paste material) - Paste material containing sinterable metal particles: Alko Nano Silver Paste ANP-8 (organic coated composite silver nano paste, manufactured by Applied Nanoparticles Research Institute: alcohol derivative coated silver particles, metal content 90% or more by mass, silver particles with an average particle size of 100 nm or less (sinterable metal particles) 25% or more by mass)

[0095] (Binder component) Acrylic polymer 1 (2-ethylhexyl methacrylate polymer, mass average molecular weight 260,000, Tg: -10°C) The Tg of the acrylic polymer 1 is a calculated value using the Fox formula.

[0096] A mixture of 88.0 parts by mass of sinterable metal particle-containing paste material and 12.0 parts by mass of binder component (acrylic polymer 1) was mixed, and the solid content was adjusted to 80.0% using butyl carbitol acetate as a solvent to obtain a sintered material composition. The sinterable metal particle-containing paste material is sold containing a high-boiling point solvent, and this remains in the film-shaped sintered material after coating or drying, so the components of the sinterable metal particle-containing paste material are listed including these. Considering that the solvent in the binder component evaporates during drying, the solid content is expressed as the mass part excluding the solvent component.

[0097] <Production of film-shaped fired material> The sintered material composition obtained above was screen-printed on one side of a 230 mm wide release film (thickness 38 μm, SP-PET381031, manufactured by Lintec Corporation) using a Sonocom screen (3D #165 mesh) so as to form a circle with a coating diameter of 155 mm, and dried at 150 ° C for 5 minutes to form a film on the release film. Furthermore, the film was screen-printed again using the same Sonocom screen (3D #165 mesh) so as to overlap the film, and dried at 150 ° C for 5 minutes to obtain a sintered material film with a thickness of 60 μm. The arithmetic mean roughness (Ra0) of the exposed surface of the film-shaped fired material was measured using a surface roughness meter (SV-3000, manufactured by Mitutoyo Corporation) in accordance with JIS B0601:2013, and was found to be 1.5 μm.

[0098] <Support sheet> A dicing sheet (Adwill D-458J, manufactured by Lintec Corporation) was used as a support sheet having a UV-curable adhesive layer laminated on a base film.

[0099] <Production of film-shaped fired material with support sheet> The exposed surface of the film-like sintered material printed in a circle with a diameter of 155 mm was attached to the exposed surface of the adhesive layer of the above support sheet using a laminator (MCL-650, manufactured by MCK Corporation) at room temperature under conditions of a speed of 0.3 m / min and a pressure of 0.3 MPa, and the support sheet was cut concentrically from the base film side into circles with a diameter of 207 mm, obtaining the film-like sintered material with support sheet of Example 1, in which the circular film-like sintered material and release film were laminated on top of the support sheet having the adhesive layer on the base film.

[0100] [Example 2] In producing the film-shaped sintered material, the film-shaped sintered material with support sheet of Example 2 was obtained in the same manner as in Example 1 above, except that the first, second, and third screen printings were performed three times using the same Sonocom screen (HS230 / N55 mesh).

[0101] [Example 3] In producing the film-shaped sintered material, a Sonocom screen (3D #120 mesh) was used for the first screen printing, and a Sonocom screen (HS230 / N55 mesh) was used for the second screen printing. Except for this, the film-shaped sintered material with support sheet of Example 3 was obtained in the same manner as in Example 1 above.

[0102] [Comparative Example 1] A film-like sintered material with a support sheet of Comparative Example 1 was obtained in the same manner as in Example 1 above, except that a film-like sintered material was formed on the release film by screen printing only once using a Sonocom screen (3D #80 mesh).

[0103] [Comparative Example 2] In the production of the film-shaped sintered material, the sintered material composition obtained above was applied to one side of a 230 mm wide release film (thickness 38 μm, SP-PET381031, manufactured by Lintec Corporation) using a knife coater so that the thickness after drying would be 60 μm, and then dried at 150 ° C. for 5 minutes. Then, it was cut into a circle with a diameter of 155 mm. Thereafter, a film-shaped sintered material with a support sheet of Comparative Example 2 was obtained in the same manner as in Example 1. The arithmetic mean roughness (Ra1) of the exposed surface of the film-shaped sintered material after peeling off the support sheet was measured as in the Example, and was 0.3 μm. When applied using a knife coater, it is necessary to cut into a circle with a diameter of 155 mm after drying, and the peripheral part containing expensive sinterable metal particles is wasted.

[0104] [Example 4] <Production of film-shaped fired material with support sheet> In the production of the film-like sintered material and the production of the film-like sintered material with a support sheet, the film-like sintered material with a support sheet of Example 4 was obtained in the same manner as in Comparative Example 1 above, except that the following acrylic polymer 2 was used as the binder component.

[0105] (Binder component) Acrylic polymer 2 (isodecyl methacrylate polymer, mass average molecular weight 230,000, Tg: -40°C) The Tg of the acrylic polymer 2 is a calculated value using the Fox formula.

[0106] [Example 5] <Production of film-shaped fired material with support sheet> In the production of the film-like sintered material and the film-like sintered material with a support sheet, the film-like sintered material with a support sheet of Example 5 was obtained in the same manner as in Comparative Example 1 above, except that the following acrylic polymer 3 was used as the binder component.

[0107] (Binder component) Acrylic polymer 3 (2-ethylhexyl methacrylate / isodecyl methacrylate polymer, copolymer mass ratio 20 / 80, mass average molecular weight 230,000, Tg: -30℃) The Tg of the acrylic polymer 3 is a calculated value using the Fox formula.

[0108] <Measurement and Evaluation> (Silicon wafer) A silicon wafer (manufactured by Science and Technology Research Institute, diameter: 150 mm, thickness: 350 μm) whose surface had been chemically and mechanically polished until the arithmetic mean roughness (Ra) was 0.02 μm or less was prepared as an adherend to which the film-like fired material was to be adhered.

[0109] (Measurement of arithmetic mean roughness (Ra0)) As in Example 1 above, the arithmetic mean roughness (Ra0) of the exposed surfaces of the film-shaped fired materials used in Examples 2 and 3 and Comparative Example 1 was measured.

[0110] (Measurement of arithmetic mean roughness (Ra1)) The release film was peeled off from the film-shaped sintered materials with support sheet obtained in Examples 1 to 3 and Comparative Example 1 above. The exposed surface of the film-shaped sintered material with support sheet was attached to the treated surface of the silicon wafer described above using a laminator (MCK Corporation, MCL-650) under conditions of temperature: 90°C, speed: 0.3 m / min, and pressure: 0.3 MPa. Then, ultraviolet light (high pressure mercury lamp, illuminance 230 mW / cm) was applied to the adhesive layer from the base film side of the support sheet. 2 , light intensity 190mJ / cm 2 ) to cure the adhesive layer, and then the support sheet was removed. The arithmetic mean roughness (Ra1) of the exposed surface of the film-shaped fired material was measured using a surface roughness meter (Mitutoyo Corporation, SV-3000) in accordance with JIS B0601:2013.

[0111] (Evaluation of lift between film-shaped fired material and support sheet) The release film was peeled off from the film-like sintered material with support sheet obtained in Examples 1 to 3 and Comparative Example 1 above, and the exposed surface of the film-like sintered material of the film-like sintered material with support sheet was attached to the treated surface of the silicon wafer described above, in the same manner as described above (measurement of arithmetic average roughness (Ra1)). Then, the adhesion surface between the film-like sintered material and the adhesive layer was observed from the base film side of the support sheet using a digital microscope (VHX-7000, manufactured by Keyence Corporation), and the lift between the film-like sintered material and the support sheet was evaluated using the following evaluation criteria.

[0112] ·Float evaluation criteria A: 90% or more of the area of ​​application is in contact with the skin B: The area of ​​the patch that is in close contact is 60% or more but less than 90% C: Less than 60% of the applied area is in contact with the skin

[0113] (Evaluation of water intrusion and chip scattering during dicing) The release film was peeled off from the film-like sintered material with support sheet obtained in Examples 1 to 3 and Comparative Example 1 above, and the exposed surface of the film-like sintered material of the film-like sintered material with support sheet was attached to the treated surface of the silicon wafer described above, in the same manner as described above (measurement of arithmetic average roughness (Ra1)). The obtained laminate test piece was then attached to a SUS ring frame (manufactured by Disco Corporation) for dicing, and diced using a dicing device (DFD6362, manufactured by Disco Corporation) under the following conditions to obtain 100 chips measuring 2 mm square.

[0114] <Dicing conditions> Dicing blade: NBC-ZH2050-SE27HECC, manufactured by Disco Blade thickness: 25μm width Blade rotation speed: 40,000 rpm ·Cutting speed: 40mm / s ·Cutting water amount: 1.5L / min ·Cutting water temperature: 24℃

[0115] After dicing, the number of chips that were skipped was counted for 100 chips, and the chip skipping during dicing was evaluated according to the following criteria.

[0116] ·Evaluation criteria for chip flying A: Less than 5 B: 5 or more but less than 10 C: 10 or more

[0117] After dicing, the attachment surface was observed from the support sheet side with a digital microscope (VHX-7000 (manufactured by Keyence Corporation)), and water penetration between the film-like sintered material and the support sheet was evaluated according to the following criteria.

[0118] Evaluation criteria for water infiltration during dicing: A: No water infiltration over the entire application area B: A small amount of water was seen in the application area. C: Water infiltration was observed in many areas of the application area.

[0119] The above evaluation results are shown in Tables 1 and 2 below.

[0120] [Table 1]

[0121] [Table 2]

[0122] In Examples 1 to 5, in which the arithmetic mean roughness (Ra1) is 0.5 μm or more and less than 2.0 μm, there is little lifting between the film-shaped sintered material and the support sheet, there is little chip flying when the semiconductor wafer is diced together with the film-shaped sintered material on the support sheet, there is no risk of water intrusion during the water washing process, and it is clear that the dicing suitability is excellent.

[0123] On the other hand, in Comparative Example 1, in which the arithmetic mean roughness (Ra1) was 2.0 μm or more, there was floating between the film-shaped sintered material and the support sheet, and when the semiconductor wafer was diced together with the film-shaped sintered material on the support sheet, chips flew off and water intrusion occurred during the water washing process, resulting in poor dicing suitability. [Explanation of symbols]

[0124] Reference Signs List 1...film-like sintered material, 2...support sheet, 3...base film, 4...adhesive layer, 5...ring frame, 10...sinterable metal particles, 20...binder component, 50...float, 100...film-like sintered material with support sheet, 100a...film-like sintered material with support sheet

Claims

1. A film-shaped sintered material with a support sheet, comprising: a support sheet having a base film and a pressure-sensitive adhesive layer provided on the base film; and a film-shaped sintered material containing sinterable metal particles and a binder component provided on the pressure-sensitive adhesive layer, The film-shaped sintered material with support sheet is attached to the mirror surface of a silicon mirror wafer using the film-shaped sintered material, and then the film-shaped sintered material is peeled off from the support sheet. When the arithmetic mean roughness (Ra1) of the surface of the film-shaped sintered material facing the support sheet is measured, the arithmetic mean roughness (Ra1) is 0.5 μm or more and less than 2.0 μm.

2. The film-shaped sintered material with a support sheet according to claim 1 , wherein the pressure-sensitive adhesive layer is energy ray curable.

3. A step of forming a film-like sintered material, the step comprising screen-printing a sintered material composition containing sinterable metal particles, a binder component, and a solvent on a release-treated surface of a release film, and drying the sintered material composition; A step of preparing a support sheet having a base film and a pressure-sensitive adhesive layer provided on the base film; The method for producing a film-shaped sintered material with a support sheet according to claim 1 or 2, further comprising a step of bonding the support sheet to the exposed surface of the film-shaped sintered material by means of the exposed surface of the pressure-sensitive adhesive layer.

4. The method for producing a film-shaped sintered material with a support sheet according to claim 3, wherein the step of forming the film-shaped sintered material comprises screen-printing the sintered material composition on a release-treated surface of a release film, drying the sintered material composition, screen-printing the sintered material composition again on an exposed surface of the obtained film, and drying the sintered material composition.

Citation Information

Patent Citations

  • Pasty metal particulate composition, method for manufacturing solid metal or solid metal alloy, method for joining metallic members, method for manufacturing print wire board, and method for manufacturing bump for connecting electric circuits

    JP2014111800A

  • Film-formed firing material and film-formed firing material with a support sheet

    JP2019052366A

Cited By

  • Production method of flexible film back line pressure sensor

    CN119147139A