Method for producing silica particle, method for producing silica sol, method for producing polishing composition, polishing method, method for producing semiconductor wafer and method for producing semiconductor device
By producing silica particles with mixed sizes through controlled hydrolysis and condensation, the method addresses the issues of adhesion and scratches in conventional silica particles, resulting in improved polishing quality and surface flatness.
Patent Information
- Application Number
- JP2023053734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional silica particles used in polishing compositions have uniform particle sizes, leading to poor adhesion, high mechanical strength, and increased scratches during polishing, which affects the flatness and quality of polished surfaces.
Producing silica particles with a mixture of main particles (10 nm to 200 nm) and fine particles (1/2 or less of the main particles) through a controlled hydrolysis and condensation reaction, maintaining an alkali catalyst concentration of 0.75% by mass or less.
Improves the flatness of polished surfaces and reduces scratches by balancing the particle sizes, enhancing the polishing process's effectiveness and stability.
Smart Images

Figure 2024141877000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing silica particles, a method for producing a silica sol, a method for producing a polishing composition, a polishing method, a method for producing a semiconductor wafer, and a method for producing a semiconductor device. [Background technology]
[0002] Polishing methods using polishing liquids are known as methods for polishing the surfaces of materials such as metals and inorganic compounds. In particular, in the final polishing of prime silicon wafers and reclaimed silicon wafers for semiconductors, and in chemical mechanical polishing (CMP) for planarizing interlayer insulating films during semiconductor device manufacturing, forming metal plugs, forming buried wiring, and the like, the surface condition has a significant effect on the semiconductor characteristics, so the surfaces and end faces of these components are required to be polished with extremely high precision.
[0003] In such precision polishing, a polishing composition containing silica particles is adopted, and colloidal silica is widely used as the abrasive grains, which are the main component. Depending on the manufacturing method, colloidal silica is known to be produced by pyrolysis of silicon tetrachloride (fumed silica, etc.), by deionization of alkali silicate such as water glass, and by hydrolysis and condensation reaction of alkoxysilane (generally called the "sol-gel method").
[0004] Many studies have been conducted on methods for producing silica particles. For example, Patent Documents 1 and 2 disclose methods for producing silica particles by hydrolysis and condensation reactions of alkoxysilanes. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-060217 A [Patent Document 2] JP 2018-108924 A Summary of the Invention [Problem to be solved by the invention]
[0006] Conventionally, silica particles used in polishing compositions are mostly uniform in particle size, and many of the manufacturing methods only disclose the manufacture of silica particles with narrow particle size distribution by one hydrolysis reaction and condensation reaction.However, compared with the silica particles with small particle size and the silica particles with large particle size mixed, the silica particles with uniform particle size have poor adhesion to the polishing target, poor flatness processability, and when made into polishing composition, the average mechanical strength becomes too high, resulting in high scratching.
[0007] The method for producing silica particles disclosed in Patent Document 1 aims to obtain silica particles with a uniform particle size, and only silica particles with a narrow particle size distribution can be obtained. Moreover, the method for producing silica particles disclosed in Patent Document 2 does not describe the particle size distribution of the obtained silica particles, and does not describe a method for producing silica particles with different particle sizes by a single hydrolysis and condensation reaction.
[0008] As described above, conventional methods for producing silica particles can only produce silica particles with a uniform particle size, and conventional methods for producing silica particles having pores have not fully resolved problems such as poor adhesion to the object to be polished when used for polishing, poor flattening processability, and excessively high average mechanical strength when made into a polishing composition, resulting in high scratching.
[0009] The present invention has been made in consideration of such problems, and an object of the present invention is to provide a method for producing silica particles that contain a mixture of main particles having a particle diameter of 10 nm to 200 nm and fine particles having a particle diameter of 1 / 2 or less of the main particles. [Means for solving the problem]
[0010] As a result of extensive research, the inventors have discovered a method for directly producing silica particles comprising a mixture of main particles having a particle size of 10 nm to 200 nm and fine particles having a particle size of 1 / 2 or less of the main particles through a single hydrolysis reaction and condensation reaction, thereby completing the present invention.
[0011] That is, the gist of the present invention is as follows. [1] A method for producing silica particles having a mixture of main particles having a particle size of 10 nm to 200 nm and fine particles having a particle size of 1 / 2 or less of the main particles, by subjecting tetraalkoxysilane to a hydrolysis reaction and a condensation reaction, comprising: The method for producing silica particles further comprises adjusting the concentration of the alkali catalyst in the reaction solution at the completion of the hydrolysis reaction and the condensation reaction to 0.75 mass % or less. [2] The method for producing silica particles according to [1], comprising adding a solution (B) containing a tetraalkoxysilane and a solution (C) containing water to a solution (A) containing water, thereby carrying out a hydrolysis reaction and a condensation reaction of the tetraalkoxysilane. [3] The method for producing silica particles according to [1] or [2], wherein the reaction temperatures of the hydrolysis reaction and the condensation reaction are 20°C to 50°C. [4] The method for producing silica particles according to any one of [1] to [3], wherein the ratio of main particles to fine particles in the silica particles is 1:99 to 99:1 in terms of number ratio. [5] A method for producing silica particles according to any one of [1] to [4], comprising at least one of the following steps (1) and (2): Step (1): A step of concentrating the dispersion of silica particles obtained by the hydrolysis reaction and the condensation reaction. Step (2): A step of concentrating the dispersion of silica particles obtained by the hydrolysis reaction and the condensation reaction, and adding a dispersion medium. [6] A method for producing a silica sol, comprising the method for producing silica particles according to any one of [1] to [5]. [7] The method for producing a silica sol according to [6], wherein a concentration of silica particles in the silica sol is 3% by mass to 50% by mass. [8] A method for producing a polishing composition, comprising producing a polishing composition using the silica sol obtained by the method for producing a silica sol according to [6] or [7]. [9] A polishing method comprising a step of polishing with the polishing composition according to [8].
[10] A method for manufacturing a semiconductor wafer, comprising the polishing method described in [9].
[11] A method for manufacturing a semiconductor device, comprising the polishing method described in [9]. Effect of the Invention
[0012] According to the method for producing silica particles and the method for producing silica sol of the present invention, silica particles and silica sol containing a mixture of silica particles with small particle diameters and silica particles with large particle diameters can be directly produced by a hydrolysis reaction and a condensation reaction. Furthermore, by using a polishing composition containing such silica sol for polishing, it is possible to improve the flatness of the object to be polished and reduce scratches. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified and practiced in various ways within the scope of the gist. In addition, when the expression "~" is used in this specification, it is used as an expression including the numerical values or physical property values before and after it.
[0014] (Method of producing silica particles) The method for producing silica particles of the present invention is a method for producing silica particles having a mixture of primary particles (hereinafter sometimes simply referred to as "primary particles") having a particle diameter of 10 nm to 200 nm and fine particles (hereinafter sometimes simply referred to as "fine particles") having a particle diameter of 1 / 2 or less of the primary particles by subjecting tetraalkoxysilane to a hydrolysis reaction and a condensation reaction, and is characterized in that the concentration of the alkali catalyst in the reaction solution at the end of the hydrolysis reaction and the condensation reaction is 0.75 mass% or less. The specific method for producing silica particles of the present invention is not particularly limited, but because of excellent controllability of the hydrolysis reaction and condensation reaction, it is preferable to carry out the hydrolysis reaction and condensation reaction of the tetraalkoxysilane of the present invention by adding a solution (B) containing a tetraalkoxysilane and a solution (C) containing water to a solution (A) containing water.
[0015] <Main particles and fine particles> The silica particles produced by the hydrolysis reaction and condensation reaction of tetraalkoxysilane in the present invention (hereinafter, sometimes referred to as "silica particles of the present invention") are silica particles that contain a mixture of main particles with a particle diameter of 10 nm to 200 nm and fine particles with a particle diameter of 1 / 2 or less of the main particles. Here, the particle diameter of the main particle and the particle diameter of the fine particle are Heywood diameters measured by the method described in the Examples section below, and when a number distribution diagram of Heywood diameters is produced, the peak at the position of the largest particle diameter among peaks in the range of 10 nm to 200 nm is taken as the particle diameter of the main particle. The peak at the position of the largest particle diameter within a range of 1 / 2 or less of the particle diameter of the main particle is defined as the particle diameter of the fine particles.
[0016] In addition, the silica particles of the present invention preferably have a ratio of such main particles to fine particles in terms of number ratio within the range of 1:99 to 99:1, more preferably 5:95 to 95:5, and further preferably 10:90 to 90:10. By achieving such a well-balanced ratio of the main particles to the fine particles, it is possible to more effectively obtain the effects of improving flatness during polishing and reducing scratches, which are achieved by including both the main particles and the fine particles. Here, the abundance ratio of the main particles and the fine particles is determined by determining the midpoint between the peak representing the particle diameter of the main particles and the peak representing the particle diameter of the fine particles in a Heywood diameter number distribution diagram prepared in the measurement of the Heywood diameter described in the Examples section below, and the number of main particles present in the range of particle diameters larger than that is regarded as the number of fine particles present, and the ratio of these numbers present is regarded as the abundance ratio.
[0017] Below, the method for producing silica particles of the present invention will be described according to a preferred embodiment of the method for producing silica particles of the present invention, in which a solution (B) containing a tetraalkoxysilane and a solution (C) containing water are added to a solution (A) containing water, and a hydrolysis reaction and condensation reaction of the tetraalkoxysilane are carried out. However, the method for producing silica particles of the present invention may be any method that can produce silica particles of the present invention in which main particles and fine particles are mixed through a hydrolysis reaction and condensation reaction of the tetraalkoxysilane, and the method for producing silica particles of the present invention is in no way limited to the method described below.
[0018] <Solution (A)> The solution (A) contains water, and the inclusion of water in the solution (A) allows the hydrolysis reaction and condensation reaction of the tetraalkoxysilane to proceed. It is preferable that the solution (A) contains water and an alkali catalyst, since this can increase the reaction rates of the hydrolysis reaction and condensation reaction of the tetraalkoxysilane.
[0019] Examples of the alkali catalyst in the solution (A) include ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. These alkali catalysts may be used alone or in combination of two or more. Among these alkali catalysts, ammonia is preferred because it has excellent catalytic action, is easy to control the particle shape, can suppress the inclusion of metal impurities, is highly volatile, and is easy to remove after the hydrolysis reaction and the condensation reaction.
[0020] The solution (A) preferably contains water, since this allows the hydrolysis reaction and condensation reaction of the tetraalkoxysilane to proceed.
[0021] It is preferable that the solution (A) contains a solvent other than water, since this provides excellent dispersibility of the tetraalkoxysilane in the reaction liquid. Examples of the solvent other than water in the solution (A) include alcohols such as methanol, ethanol, propanol, isopropanol, and ethylene glycol, ketones such as acetone and methyl ethyl ketone, and esters such as ethyl acetate. These solvents may be used alone or in combination of two or more. Among these solvents, alcohols are preferred, more preferably methanol and ethanol, and even more preferably methanol, because they are easy to dissolve tetraalkoxysilane, the by-products are the same as those used in the hydrolysis reaction and the condensation reaction, and they are convenient to manufacture.
[0022] The concentration of the alkali catalyst in solution (A) is preferably 0.5% by mass to 2.0% by mass, more preferably 0.6% by mass to 1.5% by mass, based on 100% by mass of solution (A). When the concentration of the alkali catalyst in solution (A) is equal to or higher than the lower limit, aggregation of silica particles is suppressed, and the dispersion stability of the silica particles in the resulting dispersion is excellent. When the concentration of the alkali catalyst in solution (A) is equal to or lower than the upper limit, the reaction does not proceed excessively fast, and the reaction controllability is excellent.
[0023] The concentration of water in solution (A) is preferably 3% by mass to 90% by mass, more preferably 5% by mass to 50% by mass, based on 100% by mass of solution (A). When the concentration of water in solution (A) is equal to or higher than the lower limit, the dispersibility of silicic acid produced by hydrolysis in the reaction liquid is excellent. When the concentration of water in solution (A) is equal to or lower than the upper limit, the dispersibility of tetraalkoxysilane in the reaction liquid is excellent.
[0024] The concentration of the solvent other than water in the solution (A) is preferably the balance of the alkali catalyst and water.
[0025] <Solution (B)> The solution (B) contains a tetraalkoxysilane. Examples of the tetraalkoxysilane in solution (B) include tetraalkoxysilanes having an alkoxy group with 1 to 12 carbon atoms, such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetraisopropoxysilane. These tetraalkoxysilanes may be used alone or in combination of two or more. Among these tetraalkoxysilanes, tetramethoxysilane and tetraethoxysilane are preferred, and tetramethoxysilane is more preferred, since they undergo a fast hydrolysis reaction, are less likely to leave unreacted substances, are highly productive, and can easily produce a stable silica sol.
[0026] It is preferable that the solution (B) contains a solvent, since this provides excellent dispersibility of the tetraalkoxysilane in the reaction liquid. Examples of the solvent in the solution (B) include alcohols such as methanol, ethanol, propanol, isopropanol, and ethylene glycol, ketones such as acetone and methyl ethyl ketone, and esters such as ethyl acetate. These solvents may be used alone or in combination of two or more. Among these solvents, alcohols are preferred, more preferably methanol and ethanol, and even more preferably methanol, because the solvents used in the hydrolysis reaction and the by-products are the same and are convenient to manufacture.
[0027] The concentration of tetraalkoxysilane in solution (B) is preferably 60% by mass to 95% by mass, more preferably 70% by mass to 90% by mass, based on 100% by mass of solution (B). When the concentration of tetraalkoxysilane in solution (B) is equal to or higher than the lower limit, the amount of solvent used can be reduced, and the productivity of silica particles is excellent. When the concentration of tetraalkoxysilane in solution (B) is equal to or lower than the upper limit, the dispersibility of tetraalkoxysilane in the reaction liquid is excellent.
[0028] The concentration of the solvent in solution (B) is preferably 5% by mass to 40% by mass, more preferably 10% by mass to 30% by mass, in 100% by mass of solution (B). When the concentration of the solvent in solution (B) is equal to or higher than the lower limit, the dispersibility of the tetraalkoxysilane in the reaction liquid is excellent. When the concentration of the solvent in solution (B) is equal to or lower than the upper limit, the amount of the solvent used can be reduced, and the productivity of the silica particles is excellent. In addition, the concentration of the solvent in solution (B) is usually preferably the remainder of the tetraalkoxysilane in solution (B).
[0029] <Solution (C)> The solution (C) contains water. When solution (C) contains water, the composition fluctuation of the reaction liquid can be reduced.
[0030] It is preferable that solution (C) contains an alkali catalyst in addition to water, since this can increase the reaction rates of the hydrolysis and condensation reactions of the tetraalkoxysilane. Examples of the alkali catalyst in solution (C) include ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. These alkali catalysts may be used alone or in combination of two or more. The alkali catalyst in solution (C) is preferably the same type as the alkali catalyst in solution (A). As in solution (A), among these alkali catalysts, ammonia is preferred because it has excellent catalytic action, is easy to control the particle shape, can suppress the inclusion of metal impurities, is highly volatile, and is easily removable after hydrolysis and condensation reactions.
[0031] Solution (C) may contain a solvent other than water, and examples of the solvent other than water include alcohols such as methanol, ethanol, propanol, isopropanol, and ethylene glycol. These solvents may be used alone or in combination of two or more. Among these solvents, alcohol is preferred because the by-products and the solvents used in the hydrolysis reaction and condensation reaction are the same, and are therefore convenient to manufacture. However, solution (C) preferably contains only water as a solvent because it can promote the hydrolysis reaction of tetraalkoxysilane.
[0032] The concentration of the alkali catalyst in solution (C) is preferably 0.5% by mass to 10% by mass, more preferably 1% by mass to 6% by mass, based on 100% by mass of solution (C). When the concentration of the alkali catalyst in solution (C) is equal to or higher than the lower limit, aggregation of silica particles is suppressed, and the dispersion stability of the silica particles in the resulting dispersion is excellent. When the concentration of the alkali catalyst in solution (C) is equal to or lower than the upper limit, the reaction does not proceed excessively fast, and the reaction controllability is excellent.
[0033] The concentration of water in solution (C) is preferably 90% by mass to 99.5% by mass, more preferably 94% by mass to 95% by mass, based on 100% by mass of solution (C). When the concentration of water in solution (C) is equal to or higher than the lower limit, the dispersibility of silicic acid produced by hydrolysis in the reaction liquid is excellent. When the concentration of water in solution (C) is equal to or lower than the upper limit, the dispersibility of tetraalkoxysilane in the reaction liquid is excellent.
[0034] <Addition of solution (B) and solution (C) to solution (A)> The amounts of solution (B) and solution (C) added to solution (A) vary depending on the alkali catalyst concentration and tetraalkoxysilane concentration of each solution, but it is preferable to add 40% by mass to 60% by mass of solution (B) and 5% by mass to 25% by mass of solution (C) to 25% by mass to 45% by mass of solution (A) so that the total amount of 100% by mass is achieved, so that the water concentration of the reaction solution and the alkali catalyst concentration of the reaction solution at the end of the hydrolysis reaction and the condensation reaction are concentrations described below, from the viewpoint of excellent dispersibility of tetraalkoxysilane and silicic acid, which is an intermediate product, in the reaction solution and from the viewpoint of efficiently producing the silica particles of the present invention in which main particles and fine particles are mixed, and it is more preferable to add 45% by mass to 55% by mass of solution (B) and 10% by mass to 20% by mass of solution (C) to 30% by mass to 40% by mass of solution (A) so that the total amount of 100% by mass is achieved.
[0035] There is no particular limitation on the rate at which solutions (B) and (C) are added to solution (A). However, it is preferable to add solutions (B) and (C) to solution (A) simultaneously at a constant rate over a period of about 100 to 200 minutes.
[0036] <Reaction conditions> The reaction temperature (temperature of the reaction solution) of the hydrolysis reaction and condensation reaction of tetraalkoxysilane, which are carried out by adding solution (B) and solution (C) to solution (A), is preferably 20° C. to 50° C., more preferably 25° C. to 45° C. When the reaction temperature is equal to or higher than the lower limit, the reaction does not proceed too slowly, and controllability is excellent. On the other hand, when the reaction temperature is equal to or lower than the upper limit, a good balance between the hydrolysis reaction rate and the condensation reaction rate is obtained.
[0037] It is preferable that the concentration of water in the reaction system of the hydrolysis reaction and the condensation reaction does not change significantly during the reaction. This is because if the concentration of water changes through step (1), the dispersibility of the intermediate product silicic acid in the reaction liquid changes, and the particle size controllability of the silica particles is impaired. The rate of change of the concentration of water is preferably 75% or less, more preferably 50% or less. Here, the reaction liquid in the reaction system corresponds to a mixture of solution (A), solution (B) and solution (C).
[0038] In the method for producing silica particles of the present invention, the concentration of the alkali catalyst in the reaction system of hydrolysis and condensation reactions is 0.75 mass% or less in 100 mass% of reaction solution as the concentration of the alkali catalyst in the reaction solution at the end of hydrolysis and condensation reactions. If the alkali catalyst concentration exceeds 0.75 mass%, it is not possible to produce silica particles having a mixture of main particles with a particle diameter of 10nm to 200nm and fine particles with a particle diameter of 1 / 2 or less of the main particles. From the viewpoint of more efficiently producing silica particles having a mixture of main particles with a particle diameter of 10nm to 200nm and fine particles with a particle diameter of 1 / 2 or less of the main particles, the alkali catalyst concentration of the reaction solution at the end of hydrolysis and condensation reactions is preferably 0.75 mass% or less, more preferably 0.70 mass% or less. On the other hand, if the alkali catalyst concentration in the reaction solution is excessively low, this may cause aggregation of the silica particles and a decrease in the dispersion stability of the silica particles in the resulting silica particle dispersion solution. Therefore, the alkali catalyst concentration in the reaction solution at the end of the hydrolysis reaction and the condensation reaction is preferably 0.10 mass% or more, more preferably 0.30 mass% or more, and even more preferably 0.50 mass% or more. In the present invention, by setting the alkali catalyst concentration in the reaction solution at the end of the hydrolysis reaction and condensation reaction to 0.75 mass% or less, it is possible to produce silica particles having a mixture of main particles with a particle size of 10 nm to 200 nm and fine particles with a particle size of 1 / 2 or less of the main particles. Although the details of the mechanism are not clear, it is believed that the alkali catalyst concentration is 0.75 mass% or less, which is lower than usual, and therefore prevents the silica fine particles from dissolving, resulting in excellent long-term stability of the fine particles.
[0039] <Process (1) / Process (2)> Since the method for producing silica particles of the present invention can remove unnecessary components and add necessary components, it is preferable that the method further includes the following step (1) or step (2) after the above-mentioned tetraalkoxysilane hydrolysis reaction and condensation reaction steps. Step (1): A step of concentrating a dispersion of silica particles obtained by a hydrolysis reaction and a condensation reaction of tetraalkoxysilane. Step (2): A step of concentrating the dispersion of silica particles obtained by the hydrolysis reaction and condensation reaction of tetraalkoxysilane and adding a dispersion medium.
[0040] In the step (2), either the concentration of the dispersion of silica particles or the addition of the dispersion medium may be carried out first.
[0041] The method for concentrating the dispersion of silica particles is not particularly limited, and examples thereof include a heat concentration method and a membrane concentration method. In order to concentrate the dispersion of silica particles by the heat concentration method, the dispersion may be heated and concentrated under normal pressure or reduced pressure. To concentrate a dispersion of silica particles by the membrane concentration method, membrane separation by ultrafiltration is preferred. The molecular cutoff of the ultrafiltration membrane used here is selected according to the particle size of the silica particles in the dispersion so that the silica particles can be filtered and separated to be concentrated. Examples of the material of the ultrafiltration membrane include polysulfone, polyacrylonitrile, sintered metal, ceramic, carbon, etc. Examples of the form of the ultrafiltration membrane include a spiral type, a tubular type, a hollow fiber type, etc.
[0042] In addition, the dispersion medium to be added to the dispersion liquid of silica particles may be, for example, water, methanol, ethanol, propanol, isopropanol, alcohol such as ethylene glycol, etc. These dispersion media may be used alone or in combination of two or more. Among these dispersion media, water and alcohol are preferred, and water is more preferred, because they have excellent affinity with silica particles.
[0043] In the present invention, it is preferable to obtain a dispersion of silica particles having a silica particle concentration of 3% by mass to 50% by mass, particularly an aqueous dispersion of silica particles having a silica particle concentration of 4% by mass to 40% by mass, by carrying out the above-mentioned step (1) or step (2) as necessary, using the method for producing silica particles of the present invention.
[0044] (Physical properties of silica particles) The average primary particle diameter of the silica particles of the present invention produced by the method for producing silica particles of the present invention is preferably 5 nm to 100 nm, more preferably 10 nm to 60 nm. When the average primary particle diameter of the silica particles is 5 nm or more, the storage stability of the silica sol is excellent. In addition, when the average primary particle diameter of the silica particles is 100 nm or less, the surface roughness and scratches of the polished object, typified by a silicon wafer, can be reduced, and the sedimentation of the silica particles can be suppressed.
[0045] The average primary particle size of the silica particles is measured by the BET method. Specifically, the specific surface area of the silica particles is measured using an automatic specific surface area measuring device, and the average primary particle size is calculated using the following formula (1). Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 )) ... (1)
[0046] The average primary particle size of the silica particles can be set within a desired range by known conditions and methods.
[0047] The average secondary particle diameter of the silica particles of the present invention is preferably 10 nm to 200 nm, more preferably 20 nm to 100 nm. When the average secondary particle diameter of the silica particles is 10 nm or more, the removability of particles and the like during cleaning after polishing is excellent, and the storage stability of the silica sol is excellent. When the average secondary particle diameter of the silica particles is 200 nm or less, the surface roughness and scratches of the polished object, typically a silicon wafer, during polishing can be reduced, the removability of particles and the like during cleaning after polishing can be excellent, and sedimentation of the silica particles can be suppressed.
[0048] The average secondary particle size of the silica particles is measured by a DLS method (dynamic light scattering method), specifically, using a dynamic light scattering particle size measuring device.
[0049] The average secondary particle size of the silica particles can be set within a desired range by known conditions and methods.
[0050] The cv value of the silica particles of the present invention is preferably 10 to 50, more preferably 15 to 40, and even more preferably 20 to 35. When the cv value of the silica particles is equal to or greater than the lower limit, the polishing rate for a polished object, such as a silicon wafer, is excellent, and the productivity is excellent. When the cv value of the silica particles is equal to or less than the upper limit, the surface roughness and scratches of a polished object, such as a silicon wafer, during polishing can be reduced, and the removability of particles and the like during cleaning after polishing is excellent.
[0051] The cv value of the silica particles is calculated using the following formula (2) by measuring the average secondary particle size of the silica particles using a dynamic light scattering particle size measuring device. cv value = (standard deviation (nm) / average secondary particle size (nm)) × 100 (2)
[0052] The association ratio of the silica particles of the present invention is preferably 1.0 to 4.0, more preferably 1.1 to 3.0. When the association ratio of the silica particles is equal to or greater than the lower limit, the polishing rate for the object to be polished, such as a silicon wafer, is excellent, and the productivity is excellent. When the association ratio of the silica particles is equal to or less than the upper limit, the surface roughness and scratches of the object to be polished, such as a silicon wafer, during polishing can be reduced, and the aggregation of the silica particles can be suppressed.
[0053] The association ratio of silica particles is calculated using the following formula (3) from the average primary particle diameter measured by the above-mentioned measuring method and the average secondary particle diameter measured by the above-mentioned measuring method. Association ratio = average secondary particle diameter / average primary particle diameter (3)
[0054] The surface silanol group density of the silica particles of the present invention is 0.1 / nm 2 ~10 pieces / nm 2 is preferable, and 0.5 particles / nm 2 ~7.5 pieces / nm 2 More preferably, 2.0 particles / nm 2 ~7.0 pieces / nm 2 More preferably, the surface silanol group density of the silica particles is 0.1 / nm 2When the surface silanol group density of the silica particles is 10 / nm or more, the silica particles have a suitable surface repulsion, and the dispersion stability of the silica sol is excellent. 2 When the amount is equal to or less than this, the silica particles have an appropriate surface repulsion, and aggregation of the silica particles can be suppressed.
[0055] The surface silanol group density of the silica particles is measured by the Sears method, specifically, under the following conditions.
[0056] Take a silica sol equivalent to 1.5 g of silica particles, add pure water to make the liquid volume 90 mL, add 0.1 mol / L hydrochloric acid aqueous solution until the pH becomes 3.6 in an environment of 25°C, add 30 g of sodium chloride, gradually add pure water to completely dissolve the sodium chloride, and finally add pure water until the total volume of the test liquid is 150 mL to obtain the test liquid. The obtained test liquid is placed in an automatic titrator, and 0.1 mol / L aqueous sodium hydroxide solution is added dropwise to measure the titer A (mL) of 0.1 mol / L aqueous sodium hydroxide solution required to change the pH from 4.0 to 9.0. The amount of 0.1 mol / L sodium hydroxide solution consumed per 1.5 g of silica particles, V (mL), required to change the pH from 4.0 to 9.0 was calculated using the following formula (4), and the surface silanol group density ρ (particles / nm 2 ) is calculated. V=(A×f×100×1.5) / (W×C) ··· (4) A: The amount (mL) of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles f: Potency of the 0.1 mol / L sodium hydroxide solution used C: Concentration of silica particles in silica sol (mass%) W: Amount of silica sol collected (g) ρ = (B × N A ) / (10 18 ×M×S BET ) ··· (5) B: The amount of sodium hydroxide (mol) required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles calculated from V N A : Avogadro's number (pieces / mol) M: Silica particle amount (1.5g) S BET : The specific surface area (m2) of silica particles measured when calculating the average primary particle size 2 / g)
[0057] The method for measuring and calculating the surface silanol group density of the silica particles was based on "GW Ears, Jr., Analytical Chemistry, Vol. 28, No. 12, pp. 1981-1983 (1956)," "Haba Shinichi, Development of Abrasives for Semiconductor Integrated Circuit Processing, Doctoral Dissertation, Kochi University of Technology, pp. 39-45, March 2004," "Patent No. 5967118," and "Patent No. 6047395."
[0058] The surface silanol group density of the silica particles can be set within a desired range by adjusting the conditions for the hydrolysis reaction and condensation reaction of the alkoxysilane.
[0059] The content of metal impurities in the silica particles of the present invention is preferably 5 ppm or less, more preferably 2 ppm or less.
[0060] When polishing silicon wafers for semiconductor devices, metallic impurities adhere to and contaminate the surface of the workpiece to be polished, adversely affecting the characteristics of the wafer and diffusing into the interior of the wafer, degrading its quality, resulting in a significant decrease in the performance of semiconductor devices manufactured from such wafers. In addition, when metal impurities are present on silica particles, coordination interactions occur between the acidic surface silanol groups and the metal impurities, changing the chemical properties (acidity, etc.) of the surface silanol groups and the three-dimensional environment of the silica particle surface (e.g. the ease of aggregation of silica particles), thereby affecting the polishing rate.
[0061] The metal impurity content of silica particles is measured by inductively coupled plasma mass spectrometry (ICP-MS). Specifically, a silica sol containing 0.4 g of silica particles is accurately weighed, sulfuric acid and hydrofluoric acid are added, and the mixture is heated, dissolved, and evaporated. Pure water is added to the remaining sulfuric acid droplets so that the total amount is exactly 10 g to create a test solution, which is then measured using an inductively coupled plasma mass spectrometry device. The target metals are sodium, potassium, iron, aluminum, calcium, magnesium, zinc, cobalt, chromium, copper, manganese, lead, titanium, silver, and nickel, and the sum of the contents of these metals is the metal impurity content.
[0062] The metal impurity content of the silica particles can be reduced to 5 ppm or less by obtaining the silica particles through hydrolysis and condensation reactions using alkoxysilane as the main raw material. In the method of deionizing alkali silicate such as water glass, sodium and other impurities derived from the raw material remain, making it extremely difficult to reduce the metal impurity content of silica particles to 5 ppm or less.
[0063] Examples of the shape of silica particles include spherical, chain-like, cocoon-like (also called lump-like or peanut-like), irregular shapes (for example, wart-like, bent, branched, etc.) etc. Among these silica particle shapes, when it is desired to reduce the surface roughness or scratches of a polished object, such as a silicon wafer, during polishing, a spherical shape is preferred, and when it is desired to increase the polishing rate of a polished object, such as a silicon wafer, an irregular shape is preferred.
[0064] The silica particles of the present invention preferably have no pores, since they have excellent mechanical strength and storage stability. The presence or absence of pores in the silica particles is confirmed by multipoint BET analysis using adsorption isotherms with nitrogen as the adsorption gas.
[0065] The Heywood diameter of the main particles in the silica particles of the present invention is preferably in the range of 10 nm to 150 nm, more preferably 20 nm to 100 nm, and even more preferably 25 nm to 90 nm. When the Heywood diameter of the main particles is 10 nm or more, the aggregation of silica particles in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent. In addition, when the Heywood diameter of the main particles is 150 nm or less, the polishing rate for the polished object represented by silicon wafer is excellent.
[0066] In addition, the Heywood diameter of the fine particles in the silica particles of the present invention is preferably in the range of 0.1 nm to 75 nm, more preferably 1 nm to 50 nm, and even more preferably 5 nm to 45 nm. When the Heywood diameter of the fine particles is 0.1 nm or more, the aggregation of silica particles in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent. When the Heywood diameter of the fine particles is 75 nm or less, the polishing rate for the polished object represented by silicon wafer is excellent.
[0067] (Method of producing silica sol) The method for producing a silica sol of the present invention includes the method for producing silica particles of the present invention.
[0068] The silica sol may be produced by using the dispersion liquid of silica particles obtained by the method for producing silica particles of the present invention as it is, or by removing unnecessary components from the obtained dispersion liquid of silica particles and adding necessary components.
[0069] The silica sol preferably contains silica particles and a dispersion medium. The dispersion medium in silica sol can be, for example, water, methanol, ethanol, propanol, isopropanol, ethylene glycol, and other alcohols.These dispersion mediums in silica sol can be used alone or in combination of two or more.Among these dispersion mediums in silica sol, water and alcohol are preferred, and water is more preferred, because they have excellent affinity with silica particles.
[0070] The content of silica particles in the silica sol is preferably 3% by mass to 50% by mass, more preferably 4% by mass to 40% by mass, and even more preferably 5% by mass to 30% by mass, based on the total amount of the silica sol (100% by mass). When the content of silica particles in the silica sol is 3% by mass or more, the polishing rate for a polished object such as a silicon wafer is excellent. When the content of silica particles in the silica sol is 50% by mass or less, the aggregation of silica particles in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent.
[0071] The content of the dispersion medium in the silica sol is preferably 50% by mass to 97% by mass, more preferably 60% by mass to 96% by mass, and even more preferably 70% by mass to 95% by mass, based on the total amount of the silica sol (100% by mass). When the content of the dispersion medium in the silica sol is 50% by mass or more, the aggregation of silica particles in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent. In addition, when the content of the dispersion medium in the silica sol is 97% by mass or less, the polishing rate for the polished object, typically a silicon wafer, is excellent.
[0072] The content of silica particles and dispersion medium in the silica sol can be set within a desired range by removing unnecessary components from the components in the obtained dispersion of silica particles and adding necessary components.
[0073] In addition to the silica particles and the dispersion medium, the silica sol may contain other components such as an oxidizing agent, a preservative, an antifungal agent, a pH adjuster, a pH buffer, a surfactant, a chelating agent, and an antibacterial and biocide, as necessary, within the range that does not impair the performance of the silica sol. In particular, it is preferable to include an antibacterial biocide in the silica sol, since this provides excellent storage stability of the silica sol.
[0074] Examples of antibacterial biocides include hydrogen peroxide, ammonia, quaternary ammonium hydroxide, quaternary ammonium salt, ethylenediamine, glutaraldehyde, methyl p-hydroxybenzoate, sodium chlorite, etc. These antibacterial biocides may be used alone or in combination of two or more. Among these antibacterial biocides, hydrogen peroxide is preferred because it has excellent affinity with silica sol. Antimicrobial biocides also include those commonly referred to as germicides.
[0075] The content of the antibacterial biocide in the silica sol is preferably 0.0001% by mass to 10% by mass, more preferably 0.001% by mass to 1% by mass, based on the total amount of the silica sol (100% by mass). When the content of the antibacterial biocide in the silica sol is 0.0001% by mass or more, the storage stability of the silica sol is excellent. When the content of the antibacterial biocide in the silica sol is 10% by mass or less, the inherent performance of the silica sol is not impaired.
[0076] The pH of the silica sol is preferably 6.0 to 8.0, more preferably 6.5 to 7.8. When the pH of the silica sol is 6.0 or more, the dispersion stability is excellent and the aggregation of the silica particles can be suppressed. Also, when the pH of the silica sol is 8.0 or less, dissolution of the silica particles is prevented, and the long-term storage stability is excellent. The pH of the silica sol can be adjusted to a desired range by adding a pH adjuster.
[0077] (Method of manufacturing the polishing composition) The silica particles obtained by the method for producing silica particles of the present invention and the silica sol obtained by the method for producing silica sol of the present invention can be suitably used as a polishing composition. The method for producing a polishing composition of the present invention is a method for producing a polishing composition (hereinafter sometimes referred to as "the polishing composition of the present invention") using the silica sol produced by the method for producing a silica sol of the present invention. The polishing composition of the present invention preferably contains the above-mentioned silica sol and a water-soluble polymer.
[0078] The water-soluble polymer enhances the wettability of the polishing composition to the object to be polished, such as a silicon wafer. The water-soluble polymer is preferably a polymer having a functional group with high water affinity, and the functional group with high water affinity has a high affinity with the surface silanol group of the silica particles, so that the silica particles and the water-soluble polymer are stably dispersed in the polishing composition in a closer vicinity. Therefore, when polishing the object to be polished, such as a silicon wafer, the effects of the silica particles and the water-soluble polymer function synergistically.
[0079] Examples of the water-soluble polymer include cellulose derivatives, polyvinyl alcohol, polyvinylpyrrolidone, copolymers having a polyvinylpyrrolidone skeleton, and polymers having a polyoxyalkylene structure.
[0080] Examples of cellulose derivatives include hydroxyethyl cellulose, hydrolyzed hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and carboxymethyl cellulose. An example of the copolymer having a polyvinylpyrrolidone skeleton is a graft copolymer of polyvinyl alcohol and polyvinylpyrrolidone. Examples of polymers having a polyoxyalkylene structure include polyoxyethylene, polyoxypropylene, and copolymers of ethylene oxide and propylene oxide.
[0081] These water-soluble polymers may be used alone or in combination of two or more. Among these water-soluble polymers, cellulose derivatives are preferred, and hydroxyethyl cellulose is more preferred, because they have high affinity with the surface silanol groups of silica particles and act synergistically to impart good hydrophilicity to the surface of the polished object.
[0082] The mass average molecular weight of the water-soluble polymer is preferably 1,000 to 3,000,000, more preferably 5,000 to 2,000,000, and even more preferably 10,000 to 1,000,000. When the mass average molecular weight of the water-soluble polymer is 1,000 or more, the hydrophilicity of the polishing composition is improved. When the mass average molecular weight of the water-soluble polymer is 3,000,000 or less, the affinity with silica sol is excellent, and the polishing rate for the object to be polished, typified by a silicon wafer, is excellent.
[0083] The mass average molecular weight of the water-soluble polymer is measured by size exclusion chromatography using a 0.1 mol / L NaCl solution as the mobile phase, in terms of polyethylene oxide.
[0084] The content of the water-soluble polymer in the polishing composition is preferably 0.02% by mass to 10% by mass, more preferably 0.05% by mass to 5% by mass, based on the total amount of the polishing composition (100% by mass). When the content of the water-soluble polymer in the polishing composition is 0.02% by mass or more, the hydrophilicity of the polishing composition is improved. Furthermore, when the content of the water-soluble polymer in the polishing composition is 10% by mass or less, the aggregation of silica particles during preparation of the polishing composition can be suppressed.
[0085] In addition to the silica sol and the water-soluble polymer, the polishing composition may contain other components, such as a basic compound, a polishing accelerator, a surfactant, a hydrophilic compound, a preservative, an antifungal agent, a pH adjuster, a pH buffer, a surfactant, a chelating agent, and an antibacterial and biocide, as necessary, within the range that does not impair the performance of the polishing composition. In particular, it is preferable to include a basic compound in the polishing composition, since it is possible to perform chemical polishing (chemical etching) by applying a chemical action to the surface of an object to be polished, such as a silicon wafer, and because a synergistic effect with the surface silanol groups of the silica particles can improve the polishing speed of an object to be polished, such as a silicon wafer.
[0086] Examples of the basic compound include organic basic compounds, alkali metal hydroxides, alkali metal hydrogen carbonates, alkali metal carbonates, and ammonia. These basic compounds may be used alone or in combination of two or more. Among these basic compounds, ammonia, tetramethylammonium hydroxide, tetraethylammonium hydroxide, ammonium hydrogen carbonate, and ammonium carbonate are preferred because they are highly soluble in water and have excellent affinity with silica particles and water-soluble polymers, and ammonia, tetramethylammonium hydroxide, and tetraethylammonium hydroxide are more preferred, with ammonia being even more preferred.
[0087] The content of the basic compound in the polishing composition is preferably 0.001% by mass to 5% by mass, more preferably 0.01% by mass to 3% by mass, based on the total amount of the polishing composition (100% by mass). When the content of the basic compound in the polishing composition is 0.001% by mass or more, the polishing speed of the object to be polished, such as a silicon wafer, can be improved. In addition, when the content of the basic compound in the polishing composition is 5% by mass or less, the stability of the polishing composition is excellent.
[0088] The pH of the polishing composition is preferably 8.0 to 12.0, more preferably 9.0 to 11.0. When the pH of the polishing composition is 8.0 or more, the aggregation of silica particles in the polishing composition can be suppressed, and the dispersion stability of the polishing composition is excellent. When the pH of the polishing composition is 12.0 or less, the dissolution of silica particles can be suppressed, and the stability of the polishing composition is excellent. The pH of the polishing composition can be adjusted to a desired range by adding a pH adjuster.
[0089] The polishing composition can be obtained by mixing the silica sol obtained by the silica sol manufacturing method of the present invention, a water-soluble polymer, and, as necessary, other components. However, taking into consideration storage and transportation, the composition may be prepared at a high concentration and then diluted with water or the like immediately before polishing.
[0090] (polishing method) The polishing method of the present invention is a method of polishing using the polishing composition of the present invention, which contains the silica sol obtained by the method for producing a silica sol of the present invention. A specific example of the polishing method is a method in which the surface of a silicon wafer is pressed against a polishing pad, the polishing composition of the present invention is dropped onto the polishing pad, and the surface of the silicon wafer is polished.
[0091] (Method of manufacturing semiconductor wafers) The method for producing a semiconductor wafer of the present invention includes the polishing method of the present invention, and the specific polishing method is as described above. Examples of semiconductor wafers include silicon wafers and compound semiconductor wafers.
[0092] (Method of manufacturing semiconductor devices) The method for producing a semiconductor device of the present invention includes the polishing method of the present invention, and the specific polishing method is as described above.
[0093] (Application) The silica particles obtained by the method for producing silica particles of the present invention, the silica sol obtained by the method for producing a silica sol of the present invention, and the polishing composition obtained by the method for producing a polishing composition of the present invention can be suitably used for polishing purposes. For example, it can be used for polishing semiconductor materials such as silicon wafers, polishing electronic materials such as hard disk substrates, polishing in the planarization process in manufacturing integrated circuits (chemical mechanical polishing), polishing synthetic quartz glass substrates used in photomasks and liquid crystals, polishing magnetic disk substrates, polishing metals such as Si, Cu, W, Ti, Cr, Co, Zr, Hf, Mo, Ta, Ru, Au, Pt, and Ag, and metal compounds such as oxides, nitrides, and silicides of the above metals, etc. Among these, it can be particularly suitably used for polishing silicon wafers and chemical mechanical polishing. EXAMPLES
[0094] The present invention will be described in more detail below using examples. However, the present invention is not limited to the description of the following examples as long as it does not deviate from the gist of the present invention.
[0095] (Measurement of average primary particle size) The silica sol obtained in the examples and comparative examples was dried at 150°C, and the specific surface area of the silica particles was measured using an automatic specific surface area measuring device "BELSORP-MR1" (model name, Microtrack BEL Co., Ltd.). From the specific surface area thus obtained, the average primary particle size was calculated using the following formula (1). Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 )) (1)
[0096] (Measurement of average secondary particle size and cv value) The average secondary particle size of the silica particles in the silica sol obtained in the examples and comparative examples was measured using a dynamic light scattering particle size measurement device "Zetersizer Nano ZS" (model name, manufactured by Malvern Instruments), and the cv value was calculated using the following formula (2). cv value = (standard deviation (nm) / average secondary particle size (nm)) × 100 (2)
[0097] (Calculation of association ratio) The association ratio was calculated from the measured average primary particle size and average secondary particle size using the following formula (3). Association ratio = average secondary particle size / average primary particle size...(3)
[0098] (Heywood diameter and abundance ratio of main particles and fine particles) The silica particles in the silica sol obtained in the examples and comparative examples were photographed using a field emission scanning electron microscope "S-5200" (model name, manufactured by Hitachi High-Tech Corporation), and then the Heywood diameters of the main particles and fine particles were measured using image analysis type particle size distribution measurement software "Mac-View" (software name, manufactured by Mountec Co., Ltd.), and the abundance ratio was calculated based on the number distribution.
[0099] [Example 1] A solution (B) of a mixture of 75 mass % tetramethoxysilane and 25 mass % methanol, and a solution (C) of a 1.7 mass % aqueous ammonia solution were prepared. A reaction vessel equipped with a thermometer, a stirrer, a supply pipe, and a distillation line was charged with a solution (A) prepared by mixing methanol, pure water, and ammonia in advance. The concentration of methanol in the solution (A) was 84 mass%, the concentration of water in the solution (A) was 15 mass%, and the concentration of ammonia in the solution (A) was 1.0 mass%.
[0100] While maintaining the temperature of the reaction solution at 35°C, 51% by mass of solution (B) and 13% by mass of solution (C) were added to 36% by mass of solution (A) at equal rates over 150 minutes to obtain a dispersion of silica particles with a silica particle content of about 15% by mass. At this time, it was confirmed that the ammonia concentration of the reaction solution (dispersion of silica particles) at the end of the reaction was 0.59% by mass. Thereafter, the reaction solution was concentrated by increasing the temperature, and water was added to replace the methanol with water. This was filtered to obtain an aqueous dispersion of silica particles with a silica concentration of about 20% by mass.
[0101] [Example 2] Similarly to Example 1, solutions (B), (C) and (A) were prepared. While maintaining the temperature of the reaction solution at 35°C, 51% by mass of solution (B) and 13% by mass of solution (C) were added to 36% by mass of solution (A) at equal rates over 120 minutes to obtain a dispersion of silica particles with a silica particle content of about 15% by mass. At this time, it was confirmed that the ammonia concentration of the reaction solution (dispersion of silica particles) at the end of the reaction was 0.59% by mass. Thereafter, the reaction solution was concentrated by increasing the temperature, and water was added to replace the methanol with water. This was filtered to obtain an aqueous dispersion of silica particles with a silica concentration of about 20% by mass.
[0102] [Example 3] In the same manner as in Example 1, solutions (B) and (A) were prepared. Also, a 1.4 mass % aqueous ammonia solution (C) was prepared. While maintaining the temperature of the reaction solution at 39°C, 51% by mass of solution (B) and 13% by mass of solution (C) were added to 36% by mass of solution (A) at equal rates over 150 minutes to obtain a dispersion of silica particles with a silica particle content of about 15% by mass. At this time, it was confirmed that the ammonia concentration of the reaction solution (dispersion of silica particles) at the end of the reaction was 0.59% by mass. Thereafter, the reaction solution was concentrated by increasing the temperature, and water was added to replace the methanol with water. This was filtered to obtain an aqueous dispersion of silica particles with a silica concentration of about 20% by mass.
[0103] [Comparative Example 1] In the same manner as in Example 1, solutions (B) and (A) were prepared. Also, a solution (C) of 3.1 mass % ammonia aqueous solution was prepared. While maintaining the temperature of the reaction solution at 37°C, 51% by mass of solution (B) and 14% by mass of solution (C) were added to 35% by mass of solution (A) at equal rates over 150 minutes to obtain a dispersion of silica particles with a silica particle content of about 15% by mass. At this time, it was confirmed that the ammonia concentration of the reaction solution (dispersion of silica particles) at the end of the reaction was 0.78% by mass. Thereafter, the reaction solution was concentrated by increasing the temperature, and water was added to replace the methanol with water. This was filtered to obtain an aqueous dispersion of silica particles with a silica concentration of about 15% by mass.
[0104] The evaluation results of the obtained aqueous dispersion of silica particles are shown in Table 1.
[0105] [Table 1]
[0106] As is clear from Table 1, in Examples 1 to 3, the ammonia concentration in the reaction solution at the end of the reaction was 0.75 mass% or less, and one hydrolysis reaction and condensation reaction were able to produce silica particles having a mixture of main particles with a particle size of 10 nm to 200 nm and fine particles with a particle size of 1 / 2 or less of the main particles. On the other hand, in Comparative Example 1, the ammonia concentration in the reaction liquid at the end of the reaction exceeded 0.75 mass %, so the produced silica particles were silica particles consisting of only main particles.
Claims
1. A method for producing silica particles having a mixture of main particles having a particle size of 10 nm to 200 nm and fine particles having a particle size of 1 / 2 or less of the main particles, by subjecting tetraalkoxysilane to a hydrolysis reaction and a condensation reaction, comprising the steps of: The method for producing silica particles further comprises adjusting the concentration of the alkali catalyst in the reaction solution at the completion of the hydrolysis reaction and the condensation reaction to 0.75 mass % or less.
2. The method for producing silica particles according to claim 1, wherein a solution (B) containing a tetraalkoxysilane and a solution (C) containing water are added to a solution (A) containing water, and a hydrolysis reaction and a condensation reaction of the tetraalkoxysilane are carried out.
3. The method for producing silica particles according to claim 1, wherein the reaction temperature of the hydrolysis reaction and the condensation reaction is 20°C to 50°C.
4. 2. The method for producing silica particles according to claim 1, wherein the ratio of main particles to fine particles in the silica particles is 1:99 to 99:1 in terms of number ratio.
5. The method for producing silica particles according to claim 1, comprising at least one of the following steps (1) and (2): Step (1): A step of concentrating the dispersion of silica particles obtained by the hydrolysis reaction and the condensation reaction. Step (2): A step of concentrating the dispersion of silica particles obtained by the hydrolysis reaction and the condensation reaction, and adding a dispersion medium.
6. A method for producing a silica sol, comprising the method for producing silica particles according to claim 1.
7. The method for producing a silica sol according to claim 6, wherein a concentration of silica particles in the silica sol is 3% by mass to 50% by mass.
8. A method for producing a polishing composition, comprising producing a polishing composition by using the silica sol obtained by the method for producing a silica sol according to claim 6 or 7.
9. A polishing method comprising a step of polishing with the polishing composition according to claim 8.
10. A method for producing a semiconductor wafer, comprising the polishing method according to claim 9.
11. A method for manufacturing a semiconductor device, comprising the polishing method according to claim 9.
Citation Information
Patent Citations
Silica sol and manufacturing method therefor
JP2005060217A
Silica sol and manufacturing method thereof
JP2009161371A
Modified colloidal silica, method for producing the same and abrasive using the same
JP2020073445A
Method for producing silica particle, method for producing silica sol, polishing process, method for producing semiconductor wafer, and method for producing semiconductor device
JP2021147267A
Method for producing silica sol, polishing method, method for producing semiconductor wafer and method for producing semiconductor device
JP2023043023A