Composition
A composition with silver molybdate and diallylamine polymers prevents precipitation, maintaining antibacterial and antiviral efficacy in paints and coatings.
Patent Information
- Application Number
- JP2023054012
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Silver molybdate precipitates in paints and coating materials due to its high specific gravity, leading to insufficient antibacterial and antiviral properties.
A composition containing silver molybdate and diallylamine polymers or their derivatives, such as acetates and hydrochlorides, is used to suppress precipitation and maintain effective antibacterial and antiviral properties.
The composition effectively prevents silver molybdate precipitation, ensuring sufficient antibacterial and antiviral properties in paint and coating materials.
Smart Images

Figure 2024142047000001 
Figure 2024142047000002 
Figure 2024142047000003
Abstract
Description
[Technical field]
[0001] The present invention relates to compositions containing silver molybdate. [Background technology]
[0002] Silver molybdate is used as an antibacterial agent and an antiviral agent (for example, Patent Document 1).
[0003] Examples of uses of silver molybdate include paints and coating materials. When a paint or coating material containing silver molybdate is applied to an object such as a handrail or film, the object is also imparted with antibacterial and antiviral properties. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-190808 A Summary of the Invention [Problem to be solved by the invention]
[0005] When silver molybdate is added to the above-mentioned paint or coating material, molybdic acid may be added directly to the paint or coating material, or a slurry in which silver molybdate is mixed with water beforehand may be added.
[0006] Because silver molybdate has a large specific gravity, it may settle under slurries, paints, coating materials, etc. If silver molybdate settles, it will not be able to impart sufficient antibacterial or antiviral properties to the target object, so it must be handled with care.
[0007] An object of the present invention is to provide a composition capable of suppressing precipitation of silver molybdate under a slurry, paint, coating material, or the like. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. [1] A composition comprising silver molybdate and one or more compounds selected from the group consisting of a diallylamine polymer represented by general formula (I), its acetate, and its hydrochloride. TIFF2024142047000001.tif2939 (wherein A represents hydrogen or a methyl group, Q represents CH2 or CH2-SO2, and n is an integer of 3 to 10,000.) [2] The above composition, wherein the one or more compounds selected from the group consisting of a diallylamine polymer represented by the general formula (I), its acetate and its hydrochloride are one or more compounds selected from the group consisting of a diallylamine polymer, a diallylamine acetate-sulfur dioxide copolymer, a diallylamine hydrochloride-sulfur dioxide copolymer and a methyldiallylamine acetate polymer. [3] The above composition further comprising water. to provide. Effect of the Invention
[0009] According to the present invention, it is possible to provide a composition capable of suppressing the precipitation of silver molybdate under a slurry, paint, coating material, or the like, and it is possible to impart sufficient antibacterial and antiviral properties to an object. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, a composition containing silver molybdate according to the first embodiment of the present invention and one or more compounds selected from the group consisting of a diallylamine polymer represented by general formula (I), its acetate, and its hydrochloride will be exemplified. Applications of the composition include, for example, water-based paints and water-based coating materials.
[0011] The silver molybdate used in this embodiment can be obtained by reacting a silver salt such as silver nitrate, silver acetate, or silver sulfate with a molybdate such as sodium molybdate, potassium molybdate, lithium molybdate, or ammonium molybdate in water as a reaction solvent. The silver molybdate obtained by the reaction is then separated from the water by a method such as vacuum filtration or centrifugation, and dried using a dryer or the like.
[0012] In this embodiment, a diallylamine polymer represented by the general formula (I), an acetate salt thereof, or a hydrochloride salt thereof is used. TIFF2024142047000002.tif2939 (wherein A represents hydrogen or a methyl group, Q represents CH2 or CH2-SO2, and n is an integer of 3 to 10,000.) These may be used alone or in combination of two or more. Of these, it is preferable to use one or more compounds selected from the group consisting of diallylamine polymer, diallylamine acetate-sulfur dioxide copolymer, diallylamine hydrochloride-sulfur dioxide copolymer, and methyldiallylamine acetate polymer, and it is particularly preferable to use diallylamine acetate-sulfur dioxide copolymer. Furthermore, n is an integer of 3 to 10,000, preferably an integer in the range of 5 to 5,000, and more preferably an integer in the range of 10 to 1,000.
[0013] In this embodiment, the blending ratio of silver molybdate to one or more compounds selected from the group consisting of the diallylamine polymer represented by general formula (I), its acetate and its hydrochloride is usually 0.001:1 to 1:1 by weight.
[0014] The composition of the present embodiment is usually blended during the production of a water-based paint or water-based coating material. For example, when blending a defoamer, a viscosity adjuster, a dispersant, a wetting agent, a preservative, a pigment, a dye, an ultraviolet absorber, an antioxidant, a foaming agent, an organic or inorganic filler, a flame retardant, an antistatic agent, an antirust agent, or the like to an emulsion in which a resin component is dispersed in a water medium, the composition of the present embodiment is also blended to process the emulsion into a water-based paint or water-based coating material having antibacterial or antiviral properties.
[0015] Hereinafter, a composition containing silver molybdate according to the second embodiment of the present invention, one or more compounds selected from the group consisting of a diallylamine polymer represented by general formula (I), its acetate and its hydrochloride, and water will be exemplified. Applications of the composition include, for example, water-based paints, water-based coating materials, and textile products.
[0016] The silver molybdate and the one or more compounds selected from the group consisting of the diallylamine polymer represented by the general formula (I), its acetate and its hydrochloride, which are used in the composition of the present embodiment, are as described above.
[0017] Examples of the water used in the composition of the present embodiment include ion-exchanged water, distilled water, industrial water, etc. In addition, water used as a solvent in the reaction of a silver salt with a molybdate may be used.
[0018] The composition of the present embodiment typically contains 10 to 70 wt % silver molybdate, 0.1 to 10 wt % of one or more compounds selected from the group consisting of a diallylamine polymer represented by general formula (I), an acetate thereof, or a hydrochloride thereof, and 20 to 89.9 wt % of water, based on the total weight of the composition.
[0019] The composition of the present embodiment can be produced by weighing various raw materials to the above ratio, and then adding one or more compounds selected from the group consisting of silver molybdate and the diallylamine polymer represented by the general formula (I), its acetate or its hydrochloride to water, and mixing them using a mixer. For the silver molybdate, for example, silver molybdate containing water as a reaction solvent when the silver salt and the molybdate are reacted may be used, or silver molybdate separated from water by a method such as leaving the reaction liquid after the reaction and removing the supernatant by vacuum filtration or centrifugation may be used, or silver molybdate dried using a dryer or the like may be used. Examples of the mixer used during mixing include a stirrer equipped with a stirring blade, a Henschel mixer, a bead mill, and a ball mill.
[0020] The composition of the present embodiment may contain viscosity modifiers (polysaccharides such as cellulose), discoloration inhibitors, UV absorbers, antioxidants, antibacterial agents, surfactants, etc., within the scope of the invention.
[0021] The composition of the present embodiment is mixed during the production of a paint or coating material to be processed into a paint or coating material having antibacterial or antiviral properties. Also, a textile product is processed into a textile product having antibacterial or antiviral properties by immersing the textile product in the composition of the present embodiment and drying it.
[0022] Examples of objects to which the paint or coating material containing the composition of the first or second embodiment of the present invention can be applied include building materials such as handrails, flooring, and wallpaper, electrical appliances such as toilet seats, housings that constitute portable electronic devices such as smartphones and tablets, housings and operation buttons that constitute office automation equipment such as copiers, films to be attached to image display units of tablets, and packaging films for various products.
[0023] In order to impart antibacterial or antiviral properties to the above-mentioned object, the amount of silver molybdate is 0.01 to 5 g / m2 relative to the surface area of the object. 2 It is preferable that the concentration is adjusted so that EXAMPLES
[0024] The present invention will be further described below with reference to examples, but the present invention is not limited to these.
[0025] (Preparation of Silver Molybdate) A solution of 6.5 g of sodium molybdate dihydrate (Kanto Chemical Co., Ltd.) dissolved in 100 ml of ion-exchanged water was added dropwise to a solution of 9.1 g of silver nitrate (Kanto Chemical Co., Ltd.) dissolved in 100 ml of ion-exchanged water over a period of 30 minutes while stirring. After the dropwise addition, the mixture was stirred for 1 hour, filtered, washed with ion-exchanged water, and dried at 100°C for 24 hours to obtain silver molybdate.
[0026] Example 1 A 200 mL container with an inner diameter of 5 cm was charged with 40 g of the above silver molybdate, 4 g of a 20% aqueous solution of diallylamine acetate-sulfur dioxide copolymer (Nittobo Medical Co., Ltd., PAS-92A), and 56 g of water to obtain a composition of the present invention.
[0027] Example 2 A 200 mL container with an inner diameter of 5 cm was charged with 40 g of the above silver molybdate, 4 g of a 20% aqueous solution of diallylamine hydrochloride-sulfur dioxide copolymer (Nittobo Medical Co., Ltd., PAS-92), and 56 g of water to obtain a composition of the present invention.
[0028] Example 3 A 200 mL container with an inner diameter of 5 cm was charged with 40 g of the above silver molybdate, 4 g of a 20% aqueous solution of methyldiallylamine acetate polymer (Nittobo Medical Co., Ltd., PAS-M-1A), and 56 g of water to obtain a composition of the present invention.
[0029] Example 4 A 200 mL container with an inner diameter of 5 cm was charged with 40 g of the above silver molybdate, 4 g of a 15% aqueous solution of diallylamine polymer (PAS-21, manufactured by Nittobo Medical Co., Ltd.), and 56 g of water to obtain a composition of the present invention.
[0030] [Reference example 1] A composition was obtained by putting 40 g of the silver molybdate and 60 g of water into a container having a capacity of 200 mL and an inner diameter of 5 cm.
[0031] [Reference example 2] A composition was obtained by putting 40 g of silver powder (manufactured by Nilaco Corporation, AG-404055) and 60 g of water into a 200 mL container having an inner diameter of 5 cm.
[0032] [Reference example 3] A composition was obtained by putting 40 g of silver powder (AG-404055, manufactured by Nilaco Corporation), 4 g of a 20% aqueous solution of diallylamine acetate-sulfur dioxide copolymer (PAS-92A, manufactured by Nittobo Medical Co., Ltd.) into a 200 mL container with an inner diameter of 5 cm.
[0033] 160 g of zirconia balls YTZ-0.3 (manufactured by Nikkato Corporation) were added to each of the containers containing the various compositions, and stirring was performed for 8 hours at a rotation speed of 1000 rpm using a Φ3 cm dispenser, after which the zirconia balls were collected. The settling properties of the compositions of Examples 1 to 4 and Reference Examples 1 to 3 after stirring were examined using a LUMiSizer. The evaluation was performed using 6112-88 12channels (manufactured by MS Scientific). For the evaluation, 0.4 mL of a diluted solution 25 times diluted with distilled water was placed in a sample cell (LUM 2 mm, PA, Rect, Synthetic Cell 110-134XY), and the time until the transmittance in the region 107 mm to 128 mm from the center of the rotation axis exceeded 70% was measured under the conditions of light source intensity 1, light wavelength 870 nm, 20°C, 500 rpm, and measurement interval 10 seconds, and was classified as follows: ◎: 3000 seconds or more, ○: 1000 to 3000 seconds, △: 500 to 1000 seconds, ×: 0 to 500 seconds. The results are shown in the following table.
[0034] 〔table〕 Table Evaluation results TIFF2024142047000003.tif4539
Claims
1. A composition comprising silver molybdate and one or more compounds selected from the group consisting of a diallylamine polymer represented by formula (I), its acetate salt and its hydrochloride salt. (In the formula, A represents hydrogen or a methyl group, and Q represents CH 2 or CH 2 -S.O. 2 where n is an integer from 3 to 10,000.
2. The composition according to claim 1, wherein the one or more compounds selected from the group consisting of the diallylamine polymer represented by the general formula (I), its acetate and its hydrochloride are one or more compounds selected from the group consisting of diallylamine polymer, diallylamine acetate-sulfur dioxide copolymer, diallylamine hydrochloride-sulfur dioxide copolymer and methyldiallylamine acetate polymer.
3. The composition according to claim 1 or 2, further comprising water.