Honeycomb structure, electric heating type carrier, and exhaust gas cleaning apparatus

The honeycomb structure with varied heat capacity and electrode layers addresses non-uniform heat generation in EHC, improving temperature uniformity and preventing cracks.

JP2024142080AInactive Publication Date: 2024-10-10NGK INSULATORS LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054068
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing honeycomb structures in electrically heated catalysts (EHC) suffer from non-uniform heat generation, leading to localized high temperatures and potential cracking due to thermal stress from temperature differences.

Method used

A honeycomb structure design with specific regions of varying heat capacity, thermal conductivity, and electrical resistance, featuring band-shaped electrode layers and distinct peripheral and central regions, to enhance uniform heat distribution.

Benefits of technology

The design improves heat generation uniformity, reducing temperature differences and preventing cracks, thereby enhancing the durability and performance of the EHC.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a honeycomb structure improved in heat generation uniformity.SOLUTION: A honeycomb structure comprises: a columnar honeycomb structure part which has an outer peripheral wall, and a partition wall which is provided at inside of the outer peripheral wall, and partitions and forms a plurality of cells forming a channel from one end face to the other end face; a first electrode layer which is provided in a belt shape in a direction where the cells extend on an outer face of the outer peripheral wall; and a second electrode layer which is provided in a belt shape in a direction where the cells extend on the outer surface of the outer peripheral wall, the second electrode layer provided facing the first electrode layer across a center axis of the honeycomb structure part. In a cross section orthogonal to a direction where the cells extend, when a coordinate axis is arranged in a radial direction, a coordinate value of a centroid O is 0, and a coordinate value of the outer surface of the outer peripheral wall is 1.00 R, an average heat capacity at 25°C per unit volume of prescribed first and second outer peripheral regions is greater than an average heat capacity at 25°C per unit volume of the first center region in the honeycomb structure.SELECTED DRAWING: Figure 2A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a honeycomb structure, an electrically heated carrier having a honeycomb structure, and an exhaust gas purification device having an electrically heated carrier. [Background technology]

[0002] In recent years, an electrically heated catalyst (EHC) having a honeycomb structure has been proposed to improve the deterioration of exhaust gas purification performance immediately after starting the engine. An EHC generally comprises an outer peripheral wall, a conductive honeycomb structure part having partition walls arranged inside the outer peripheral wall and partitioning a plurality of cells that form a flow path from one end face to the other end face, and a pair of electrode layers arranged on the outer peripheral wall of the honeycomb structure part. When a voltage is applied by connecting terminals to the pair of electrode layers to apply electricity to the EHC, heat is generated by Joule heat caused by the electricity flowing through the honeycomb structure part, which is a conductive resistor. In an EHC, it is desired to uniformize the temperature distribution in the honeycomb structure part and prevent cracks from occurring due to thermal stress caused by the temperature difference between high temperature and low temperature parts.

[0003] Patent Document 1 (JP 2019-173662 A) describes that a honeycomb structure part is composed of end regions near a pair of electrode parts and a central region excluding the end regions, and that the average electrical resistivity A of the material constituting the end regions is lower than the average electrical resistivity B of the material constituting the central region. This configuration is said to improve the uniform heat generation of the honeycomb structure. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-173662 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the invention described in Patent Document 1, current is concentrated in the end regions near the pair of electrodes when electricity is applied, and the temperature tends to become high locally. Therefore, there is still room for improvement in terms of heat generation uniformity within the honeycomb structure.

[0006] The present invention has been created in view of the above circumstances, and an object of the present invention is to provide a honeycomb structure having improved heat generation uniformity in one embodiment. An object of the present invention is to provide an electrically heated carrier including such a honeycomb structure in another embodiment. An object of the present invention is to provide an exhaust gas purification device including such an electrically heated carrier in yet another embodiment. [Means for solving the problem]

[0007] The above problems can be solved by the present invention, which is exemplified below. [1] a cylindrical honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and partitioning a plurality of cells forming a flow path from one end face to the other end face; a first electrode layer provided in a strip shape in the extension direction of the cell on the outer surface of the outer peripheral wall; and a second electrode layer provided in a band shape in a cell extension direction on an outer surface of the outer peripheral wall, the second electrode layer being provided so as to face the first electrode layer across a central axis of the honeycomb structure section; Equipped with In a cross section perpendicular to the extension direction of the cells, when the coordinate axis is taken in the radial direction, the coordinate value of the center of gravity O is 0, and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average heat capacity at 25 ° C. per unit volume of the first outer peripheral region and the second outer peripheral region shown below is higher than the average heat capacity at 25 ° C. per unit volume of the first central region, Honeycomb structure: The first outer peripheral region is a region of coordinate values ​​0.90R to 1.00R, and indicates a portion of the honeycomb structure part adjacent to the first electrode layer, and extending from a point protruding by 5° from one end of the first electrode layer in the circumferential direction to a point protruding by 5° from the other end of the first electrode layer in the circumferential direction, expressed by a central angle based on the center of gravity O; The second outer peripheral region is a region of coordinate values ​​0.90R to 1.00R, and indicates a portion of the honeycomb structure portion adjacent to the second electrode layer, and extending from a point protruding by 5° from one end of the second electrode layer in the circumferential direction to a point protruding by 5° from the other end of the second electrode layer in the circumferential direction, expressed by a central angle based on the center of gravity O; The first central region indicates a portion of the honeycomb structure portion excluding the first outer peripheral region and the second outer peripheral region. [2] The honeycomb structure according to [1], wherein the average heat capacity per unit volume of the first peripheral region and the second peripheral region at 25°C is 1.2 to 1.5 times the average heat capacity per unit volume of the first central region at 25°C. [3] The coefficient of variation of the heat capacity at 25° C. per unit volume of the first outer peripheral region is H 1v The coefficient of variation of the heat capacity at 25° C. per unit volume of the second outer circumferential region is H 2v The coefficient of variation of the heat capacity at 25° C. per unit volume of the first central region is H 3v Then, H 1v ≦0.2, H 2v ≦0.2, and H 3v The honeycomb structure according to [1] or [2], wherein ≦0.3 is satisfied. [4] The honeycomb structure according to any one of [1] to [3], wherein the first peripheral region and the second peripheral region have an average electrical resistance at 25° C. lower than that of the first central region. [5] The honeycomb structure according to any one of [1] to [4], wherein the average thermal conductivity at 25° C. of the first peripheral region and the second peripheral region is higher than that of the first central region. [6] The honeycomb structure according to any one of [1] to [5], wherein the average thermal conductivity at 25° C. of the first outer peripheral region and the second outer peripheral region is 4 to 30 W / (m·K), respectively. [7] The honeycomb structure according to any one of [1] to [6], wherein the average true density of the first peripheral region and the average true density of the second peripheral region are each higher than that of the first central region. [8] The honeycomb structure according to any one of [1] to [7], wherein the average porosity of the first peripheral region and the average porosity of the second peripheral region are lower than that of the first central region. [9] The honeycomb structure according to any one of [1] to [8], wherein the average partition wall thicknesses of the first peripheral region and the second peripheral region are larger than that of the first central region.

[10] The honeycomb structure according to any one of [1] to [9], wherein the average cell density of the first peripheral region and the average cell density of the second peripheral region are higher than that of the first central region.

[11] The honeycomb structure according to any one of [1] to

[10] , wherein the average opening ratios of the first peripheral region and the second peripheral region are each lower than that of the first central region.

[12] In a cross section perpendicular to the extension direction of the cell, when the coordinate axis is taken in the radial direction, the coordinate value of the center of gravity O is 0, and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average heat capacity at 25 ° C. per unit volume of the third outer peripheral region and the fourth outer peripheral region shown below is higher than the average heat capacity at 25 ° C. per unit volume of the second central region, The honeycomb structure according to any one of [1] to

[11] : the third outer peripheral region indicates a portion of the honeycomb structure part that is adjacent to the first electrode layer and is expressed by a central angle based on the center of gravity O, from a point that protrudes by 12.5° from one end of the first electrode layer in the circumferential direction to a point that protrudes by 12.5° from the other end of the first electrode layer in the circumferential direction, within a region of coordinate values ​​0.80R to 1.00R; the fourth outer peripheral region is a region of coordinate values ​​0.80R to 1.00R, adjacent to the second electrode layer, and is represented by a central angle based on the center of gravity O, and indicates a portion of the honeycomb structure portion from a point protruding by 12.5° from one end of the second electrode layer in the circumferential direction to a point protruding by 12.5° from the other end of the second electrode layer in the circumferential direction, The second central region indicates a portion of the honeycomb structure portion excluding the third outer peripheral region and the fourth outer peripheral region.

[13] The honeycomb structure according to

[12] , wherein the average heat capacity per unit volume of the third peripheral region and the fourth peripheral region at 25°C is 1.05 to 1.4 times the average heat capacity per unit volume of the second central region at 25°C.

[14] The coefficient of variation of the heat capacity at 25°C per unit volume of the third outer peripheral region is H 4v The coefficient of variation of the heat capacity at 25° C. per unit volume of the fourth outer circumferential region is H 5v H is the coefficient of variation of the heat capacity at 25° C. per unit volume of the second central region. 6v Then, H 4v ≦0.3, H 5v ≦0.3, and H 6v The honeycomb structure according to

[12] or

[13] , wherein ≦0.3 is satisfied.

[15] A honeycomb structure according to any one of [1] to

[14] , a metal terminal joined to an outer surface of each of the first electrode layer and the second electrode layer; An electrically heated carrier comprising:

[16]

[15] An electrically heated carrier according to the present invention; A cylindrical metal tube that accommodates the electrically heated carrier; An exhaust gas purification device comprising: Effect of the Invention

[0008] According to one embodiment of the present invention, a honeycomb structure with improved heat generation uniformity can be provided. As a result, it is possible to reduce the temperature difference in the honeycomb structure, and it is expected that the occurrence of cracks will be suppressed. By joining a metal terminal to this honeycomb structure, it can be used as an electrically heated carrier for EHC, for example. [Brief description of the drawings]

[0009] [Figure 1A] 1 is a schematic diagram of an electrically heated carrier according to one embodiment of the present invention, observed from one end face. [Figure 1B] FIG. 1 is a schematic perspective view of an electrically heated carrier according to an embodiment of the present invention. [Figure 2A] FIG. 2 is a schematic diagram for illustrating a first peripheral region, a second peripheral region, and a first central region in a cross section perpendicular to a cell extension direction of a honeycomb structure according to one embodiment of the present invention. [Figure 2B] FIG. 2 is a schematic diagram for illustrating a third peripheral region, a fourth peripheral region, and a second central region in a cross section perpendicular to a cell extension direction of a honeycomb structure according to one embodiment of the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing an exhaust gas purification device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0011] (1. Electrically heated carrier) Fig. 1A is a schematic diagram of an electrically heated carrier 100 according to one embodiment of the present invention when observed from one end face 116. Fig. 1B is a schematic perspective view of the electrically heated carrier 100 according to one embodiment of the present invention. The electrically heated carrier 100 includes a honeycomb structure 110 and metal terminals 130a and 130b. By supporting a catalyst on the electrically heated carrier 100, the electrically heated carrier 100 can be used as a catalyst body.

[0012] Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts and oxidation catalysts in which precious metals such as platinum (Pt), palladium (Pd), and rhodium (Rh) are supported on the surface of alumina pores and contain co-catalysts such as ceria and zirconia, and alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts). x Examples of the catalyst include selective catalytic reduction catalysts (SCR catalysts). Two or more catalysts selected from these catalysts may be used. There is no particular limitation on the method of supporting the catalyst, and any known method for supporting a catalyst on a honeycomb structure may be used.

[0013] (1-1. Honeycomb structure) The honeycomb structure 110 is a cylindrical honeycomb structure part having an outer peripheral wall 114 and partition walls 113 disposed inside the outer peripheral wall 114 and partitioning a plurality of cells 115 that form flow paths from one end face 116 to the other end face 118. a first electrode layer 112a provided in a strip shape on the outer surface of the outer peripheral wall 114 in the extension direction of the cells 115; and A second electrode layer 112b is provided in a strip shape on the outer surface of the outer peripheral wall 114 in the extending direction of the cells 115, the second electrode layer 112b being provided so as to face the first electrode layer 112a across the central axis of the honeycomb structure portion; Equipped with.

[0014] Referring to Figure 2A, in a cross section perpendicular to the extension direction of the cells 115, in one embodiment of a honeycomb structure 110, when the coordinate axis is taken in the radial direction, the coordinate value of the center of gravity O (corresponding to the central axis) is 0, and the coordinate value of the outer surface of the peripheral wall 114 is 1.00R, the average heat capacity at 25°C per unit volume of the first peripheral region 121 and the second peripheral region 122 shown below is each higher than the average heat capacity at 25°C per unit volume of the first central region 131.

[0015] The first outer peripheral region 121 is the region between coordinate values ​​0.90R and 1.00R, adjacent to the first electrode layer 112a, and indicates the portion of the honeycomb structure portion (the upper hatched portion in Figure 2A) that is adjacent to the first electrode layer 112a and extends from a point 5° protruding from one circumferential end 112a1 of the first electrode layer 112a to a point 5° protruding from the other circumferential end 112a2 of the first electrode layer 112a, expressed as a central angle based on the center of gravity O. The second outer peripheral region 122 is adjacent to the second electrode layer 112b within the region of coordinate values ​​0.90R to 1.00R, and indicates the portion of the honeycomb structure portion (the lower hatched portion in Figure 2A) that is adjacent to the second electrode layer 112b and extends from a point 5° protruding from one circumferential end 112b1 of the second electrode layer 112b to a point 5° protruding from the other circumferential end 112b2 of the second electrode layer 112b, expressed as a central angle based on the center of gravity O. The first central region 131 indicates a portion of the honeycomb structure portion excluding the first outer peripheral region 121 and the second outer peripheral region 122 (the dot pattern portion in FIG. 2A).

[0016] When the average heat capacity per unit volume of the first outer peripheral region 121 and the second outer peripheral region 122 at 25°C is the same as the average heat capacity per unit volume of the first central region 131 at 25°C, the temperatures near both ends in the circumferential direction of the first electrode layer 112a and the second electrode layer 112b tend to be high when the first electrode layer 112a and the second electrode layer 112b are energized by connecting terminals to the first electrode layer 112a and the second electrode layer 112b and applying a voltage. On the other hand, when the average heat capacity per unit volume of the first outer peripheral region 121 and the second outer peripheral region 122 at 25°C is higher than the average heat capacity per unit volume of the first central region 131 at 25°C, the heat generation of the first outer peripheral region 121 and the second outer peripheral region 122 is suppressed. This reduces the temperature difference with the first central region 131, improving the heat generation uniformity.

[0017] If the average heat capacity at 25°C per unit volume of the first outer peripheral region 121 is H1 (J / K), the average heat capacity at 25°C per unit volume of the second outer peripheral region 122 is H2 (J / K), and the average heat capacity at 25°C per unit volume of the first central region 131 is H3 (J / K), then it is preferable that 1.2≦H1 / H3≦1.5, more preferably 1.3≦H1 / H3≦1.5, and even more preferably 1.4≦H1 / H3≦1.5. It is also preferable that 1.2≦H2 / H3≦1.5, more preferably 1.3≦H2 / H3≦1.5, and even more preferably 1.4≦H2 / H3≦1.5. It is also preferable that 0.7≦H1 / H2≦1.4, more preferably 0.8≦H1 / H2≦1.3, and even more preferably 0.9≦H1 / H2≦1.1.

[0018] Referring to Figure 2B, in a cross section perpendicular to the extension direction of the cells 115, in a honeycomb structure 110 according to a preferred embodiment, when the coordinate axis is taken in the radial direction, the coordinate value of the center of gravity O (corresponding to the central axis) is 0, and the coordinate value of the outer surface of the peripheral wall 114 is 1.00R, the average heat capacity at 25°C per unit volume of the third peripheral region 123 and the fourth peripheral region 124 shown below is each higher than the average heat capacity at 25°C per unit volume of the second central region 132.

[0019] The third outer peripheral region 123 is adjacent to the first electrode layer 112a in the region of coordinate values ​​0.80R to 1.00R, and indicates a portion of the honeycomb structure portion from a point protruding by 12.5° from one end 112a1 of the first electrode layer 112a in the circumferential direction to a point protruding by 12.5° from the other end 112a2 of the first electrode layer 112a in the circumferential direction (the upper hatched portion in FIG. 2B ), expressed as a central angle based on the center of gravity O; The fourth outer peripheral region 124 is adjacent to the second electrode layer 112b in the region of coordinate values ​​0.80R to 1.00R, and indicates a portion of the honeycomb structure portion from a point protruding by 12.5° from one end 112b1 of the second electrode layer 112b in the circumferential direction to a point protruding by 12.5° from the other end 112b2 of the second electrode layer 112b in the circumferential direction, expressed as a central angle based on the center of gravity O (the lower hatched portion in FIG. 2B ); The second central region 132 indicates a portion of the honeycomb structure portion excluding the third outer peripheral region 123 and the fourth outer peripheral region (the dot pattern portion in FIG. 2B).

[0020] If the average heat capacity at 25°C per unit volume of the third outer peripheral region 123 is H4 (J / K), the average heat capacity at 25°C per unit volume of the fourth outer peripheral region 124 is H5 (J / K), and the average heat capacity at 25°C per unit volume of the second central region 132 is H6 (J / K), then it is preferable that 1.05≦H4 / H6≦1.4, more preferably 1.1≦H4 / H6≦1.4, and even more preferably 1.2≦H4 / H6≦1.4. It is also preferable that 1.05≦H5 / H6≦1.4, more preferably 1.1≦H5 / H6≦1.4, and even more preferably 1.2≦H5 / H6≦1.4. It is also preferable that 0.7≦H4 / H5≦1.4, more preferably 0.8≦H4 / H5≦1.3, and even more preferably 0.9≦H4 / H5≦1.1.

[0021] The unit volume (1 mm 3The average heat capacity at 25° C. per unit area is preferably 0.00018 to 0.00059 (J / K), more preferably 0.00019 to 0.00059 (J / K), and further more preferably 0.00022 to 0.00059 (J / K). The unit volume (1 mm 3 The average heat capacity at 25° C. per unit area is preferably 0.00018 to 0.00059 (J / K), more preferably 0.00019 to 0.00059 (J / K), and further more preferably 0.00022 to 0.00059 (J / K). The unit volume (1 mm 3 The average heat capacity at 25° C. per unit area is preferably 0.00016 to 0.00054 (J / K), more preferably 0.00016 to 0.00049 (J / K), and further more preferably 0.00016 to 0.00042 (J / K).

[0022] In this specification, the average heat capacity at 25°C per unit volume of the first peripheral region 121, the second peripheral region 122, the third peripheral region 123, and the fourth peripheral region 124 is determined by the following method. The honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) are cut out from each outer peripheral region at six locations without bias, so as not to include the outer peripheral wall. The mass (g) of each of these six test pieces at 25°C is measured. Next, these six test pieces are thoroughly ground into powder, and the specific heat (J / (g K)) at 25°C is measured using a differential scanning calorimeter. The mass and specific heat of each test piece are multiplied together, and then divided by the volume of the test piece to obtain the unit volume (1 mm) of each test piece at 25°C. 3) can be obtained. The average of the heat capacities of the six test pieces is taken as the average heat capacity of each outer peripheral region. When it is not possible to cut out cylindrical test pieces with a diameter of 3 mm and a length of 10 mm from each outer peripheral region due to a small diameter of the honeycomb structure, a test piece of a different shape with an equivalent volume is appropriately cut out and measured.

[0023] In this specification, the average heat capacity at 25°C per unit volume of the first central region 131 and the second central region 132 is determined by the following method. The honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) are cut out evenly from six central regions. The mass (g) of each of these six test pieces at 25°C is measured. Next, these six test pieces are thoroughly ground into powder and their specific heat (J / (g K)) at 25°C is measured using a differential scanning calorimeter. The mass and specific heat of each test piece are multiplied together and then divided by the volume of the test piece to obtain the unit volume (1 mm) of each test piece at 25°C. 3 ) can be obtained. The average of the heat capacities of the six test pieces is taken as the average heat capacity of each central region. If it is not possible to cut out test pieces with a diameter of 3 mm and a length of 10 mm from each central region due to a small diameter of the honeycomb structure, a test piece of a different shape with an equivalent volume is appropriately cut out and measured.

[0024] The coefficient of variation of the heat capacity at 25° C. per unit volume of the first outer peripheral region 121 is H 1v The coefficient of variation of the heat capacity at 25° C. per unit volume of the second outer peripheral region 122 is H 2v , the coefficient of variation of the heat capacity at 25° C. per unit volume of the first central region 131 is H 3v , the coefficient of variation of the heat capacity at 25° C. per unit volume of the third outer peripheral region 123 is H 4v The coefficient of variation of the heat capacity at 25° C. per unit volume of the fourth outer peripheral region 124 is H 5v, the coefficient of variation of the heat capacity at 25° C. per unit volume of the second central region 132 is H 6v Then, H 1v H 1v ≦0.2 is preferable, H 1v ≦0.1 is more preferable, and H 1v Even more preferably, H is ≦0.05. 2v H 2v ≦0.2 is preferable, H 2v ≦0.1 is more preferable, and H 2v Even more preferably, H is ≦0.05. 3v H 3v ≦0.3 is preferable, H 3v ≦0.15 is more preferable, and H 3v Even more preferably, H is ≦0.08. 4v H 4v ≦0.3 is preferable, H 4v ≦0.15 is more preferable, and H 4v Even more preferably, H is ≦0.08. 5v H 5v ≦0.3 is preferable, H 5v ≦0.15 is more preferable, and H 5v Even more preferably, H is ≦0.08. 6v H 6v ≦0.3 is preferable, H 6v ≦0.15 is more preferable, and H 6v Even more preferably, H is ≦0.08. 1v , H 2v , H 3v , H 4v , H 5v and H 6v There is no particular restriction on the lower limit of each of these, and they can be set to 0, but for example they may be 0.01 or more, 0.02 or more, or 0.03 or more.

[0025] In this specification, the coefficient of variation (=standard deviation / average value) of heat capacity per unit volume at 25°C for the first outer peripheral region 121, the second outer peripheral region 122, the third outer peripheral region 123, and the fourth outer peripheral region 124 is each calculated from the heat capacity value of each test piece when the average heat capacity is determined.

[0026] In this specification, the coefficient of variation (=standard deviation / average value) of heat capacity per unit volume at 25°C of the first central region 131 and the second central region 132 is calculated from the heat capacity value of each test piece when the average heat capacity is determined.

[0027] As a method for changing the average heat capacity per unit volume of the honeycomb structure portion between the peripheral region (first peripheral region 121, second peripheral region 122, third peripheral region 123, and fourth peripheral region 124) and the central region (first central region 131 and second central region 132), for example, there is a method of extruding a clay using raw materials having different true densities in the portion that will become the peripheral region after extrusion molding and the portion that will become the central region after extrusion molding.

[0028] In a preferred embodiment, the average electrical resistance at 25°C of the first outer peripheral region 121 and the second outer peripheral region 122 is preferably lower than that of the first central region 131. Although it is not intended that the present invention be limited by theory, this configuration suppresses heat generation in the first outer peripheral region 121 and the second outer peripheral region 122, while heat is less likely to stagnate near the boundary with the first central region, which has a high electrical resistance, because heat can be diffused in all directions. As a result, the uniformity of heat generation is improved.

[0029] If the average electrical resistance of the first outer peripheral region 121 at 25°C is E1 (Ω), the average electrical resistance of the second outer peripheral region 122 at 25°C is E2 (Ω), and the average electrical resistance of the first central region 131 at 25°C is E3 (Ω), then it is preferable that 0.1≦E1 / E3≦0.9, more preferably 0.2≦E1 / E3≦0.8, and even more preferably 0.3≦E1 / E3≦0.8. It is also preferable that 0.1≦E2 / E3≦0.9, more preferably 0.2≦E2 / E3≦0.8, and even more preferably 0.3≦E2 / E3≦0.8. It is also preferable that 0.8≦E1 / E2≦1.3, more preferably 0.9≦E1 / E2≦1.1, and even more preferably 0.95≦E1 / E2≦1.05.

[0030] The average electrical resistance of the first outer peripheral region 121 and the second outer peripheral region 122 at 25° C. is preferably 10 to 10,000 (Ω). The average electrical resistance of the first central region 131 at 25° C. is preferably 10 to 10,000 (Ω).

[0031] In this specification, the average electrical resistance at 25°C of the first peripheral region 121 and the second peripheral region 122 is determined by the following method. The honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) are cut out from each outer circumferential region at six locations without bias. The electrical resistance between both end faces of each of these six test pieces at 25°C is measured using a multimeter by the four-terminal method, and the average value is calculated.

[0032] In this specification, the average electrical resistance at 25°C of the first central region 131 is determined by the following method. A honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) are cut out from the first central region at six locations without bias. The electrical resistance between both end faces of these six test pieces at 25°C is measured by a four-terminal method using a multimeter, and the average value is calculated.

[0033] As a method for changing the average electrical resistance of the honeycomb structure part between the peripheral region (first peripheral region 121, second peripheral region 122) and the central region (first central region 131), for example, there is a method of extruding a clay using raw materials having different volume resistivities in the portion that will become the peripheral region after extrusion molding and the portion that will become the central region after extrusion molding. Another example is a method of changing the porosity and / or the opening ratio between the peripheral region and the central region.

[0034] In a preferred embodiment, the average thermal conductivity at 25° C. of the first outer peripheral region 121 and the second outer peripheral region 122 is higher than that of the first central region 131. Although it is not intended that the present invention be limited by theory, this configuration facilitates thermal diffusion in the first outer peripheral region 121 and the second outer peripheral region 122, making it possible to suppress heat generation near both circumferential ends of the first electrode layer 112a and the second electrode layer 112b, which tend to become hot.

[0035] If the average thermal conductivity of the first outer peripheral region 121 at 25°C is C1 (W / (m·K)), the average thermal conductivity of the second outer peripheral region 122 at 25°C is C2 (W / (m·K)), and the average thermal conductivity of the first central region 131 at 25°C is C3 (W / (m·K)), then it is preferable that 1.1≦C1 / C3≦6.0, more preferably 1.2≦C1 / C3≦5.0, and even more preferably 1.3≦C1 / C3≦4.0. It is also preferable that 1.1≦C2 / C3≦6.0, more preferably 1.2≦C2 / C3≦5.0, and even more preferably 1.3≦C2 / C3≦4.0. Moreover, it is preferable that 0.9≦C1 / C2≦1.1, it is more preferable that 0.95≦C1 / C2≦1.05, and it is even more preferable that 0.97≦C1 / C2≦1.03.

[0036] The average thermal conductivity of the first outer peripheral region 121 and the second outer peripheral region 122 at 25° C. is preferably 4 to 30 (W / (m·K)). The average thermal conductivity of the first central region 131 at 25° C. is preferably 3 to 25 (W / (m·K)).

[0037] In this specification, the average thermal conductivity at 25°C of the first outer peripheral region 121 and the second outer peripheral region 122 is determined by the following method. The honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3) are cut out from each outer peripheral region at six locations without bias. The non-porosity (1-porosity / 100) (%) and non-opening ratio (1-opening ratio / 100) (%) of these six test pieces are calculated, and the average value is calculated. Next, these test pieces are thoroughly ground into powder, and the material thermal conductivity at 25°C is measured by the laser flash method, and the average value is calculated. The average material thermal conductivity is calculated by multiplying the average material thermal conductivity by the non-porosity and non-opening ratio, and the average thermal conductivity at 25°C of the first outer peripheral region 121 and the second outer peripheral region 122. The size of the test pieces to be cut out may be changed as appropriate depending on the minimum sample amount for measuring the material thermal conductivity and the size of the honeycomb structure. The porosity of each test piece is measured by the following procedure. An SEM image of 200 times magnification is obtained from each test piece in a range of 1 mm length × 1 mm width for a cross section perpendicular to the extension direction of the cells. Next, the obtained SEM image is subjected to image analysis to binarize the solid parts of the partition walls and the void parts (pores) in the partition walls by the mode method. Then, the percentage of the ratio of the void parts in the partition walls to the total area of ​​the solid parts and void parts of the partition walls is calculated, and the obtained value is regarded as the porosity of each test piece. The opening ratio of each test specimen is a value obtained by dividing the total cell opening area of ​​each test specimen in a cross section perpendicular to the cell extension direction by the total of the partition wall area (excluding the outer peripheral wall) and the cell opening area of ​​each test specimen (total cell opening area / (total cell opening area+total partition wall area)), expressed as a percentage.

[0038] In this specification, the average thermal conductivity at 25°C of the first central region 131 is determined by the following method. A honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3) are cut out from six locations without bias from the first central region. The non-porosity (1-porosity / 100) (%) and non-opening ratio (1-opening ratio / 100) (%) of these six test pieces are calculated, and the average value is calculated. Next, these test pieces are thoroughly ground into powder, and the material thermal conductivity at 25°C is measured by the laser flash method, and the average value is calculated. The average material thermal conductivity is calculated by multiplying the average material thermal conductivity by the non-porosity and non-opening ratio. The size of the test pieces to be cut out may be changed as appropriate depending on the minimum sample amount for measuring the material thermal conductivity and the size of the honeycomb structure.

[0039] As a method for changing the average thermal conductivity of the honeycomb structure part between the peripheral region (first peripheral region 121, second peripheral region 122) and the central region (first central region 131), for example, there is a method of extruding a clay using raw materials having different thermal conductivities in the portion that will become the peripheral region after extrusion molding and the portion that will become the central region after extrusion molding. Another example is a method of changing the porosity and / or opening ratio between the peripheral region and the central region.

[0040] In a preferred embodiment, the average true density of the first outer peripheral region 121 and the second outer peripheral region 122 is higher than that of the first central region 131. Although it is not intended that the present invention be limited by theory, this configuration increases the heat capacity of the first outer peripheral region 121 and the second outer peripheral region 122, making it possible to suppress heat generation near both circumferential ends of the first electrode layer 112a and the second electrode layer 112b, which tend to become hot.

[0041] The average true density of the first outer peripheral region 121 is D1 (g / cm 3 ), the average true density of the second outer peripheral region 122 is D2 (g / cm 3 ), the average true density of the first central region 131 is D3 (g / cm 3), it is preferable that 1.04≦D1 / D3≦1.10, and more preferably that 1.045≦D1 / D3≦1.100. It is also preferable that 1.04≦D2 / D3≦1.10, and more preferably that 1.045≦D2 / D3≦1.100. It is also preferable that 0.95≦D1 / D2≦1.05, and more preferably that 0.96≦D1 / D2≦1.04, and even more preferably that 0.97≦D1 / D2≦1.03.

[0042] The average true density of the first outer peripheral region 121 and the second outer peripheral region 122 is 2.89 to 3.13 (g / cm 3 ), preferably 2.91 to 3.13 (g / cm 3 ) is more preferable, and 2.94 to 3.13 (g / cm 3 ) is even more preferred. The average true density of the first central region 131 is 2.86 to 3.10 (g / cm 3 ), and 2.86 to 3.08 (g / cm 3 ) is more preferable, and 2.86 to 3.05 (g / cm 3 ) is even more preferred.

[0043] In this specification, the average true density of the first outer peripheral region 121 and the second outer peripheral region 122 is determined by the following method. The honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) having a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) are cut out from each outer peripheral region at six locations without bias. The six cut out test pieces are thoroughly ground into powder, and the true density of each is measured by the pycnometer method, and the average value is calculated. The size of the test pieces to be cut out may be changed as appropriate depending on the minimum sample amount for the pycnometer method and the size of the honeycomb structure.

[0044] In this specification, the average true density of the first central region 131 is determined by the following method. A honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) is cut out from the first central region at six locations without bias. The six cut out test pieces are thoroughly ground into powder, and the true density of each is measured by the pycnometer method, and the average value is calculated. The size of the test pieces to be cut out may be changed as appropriate depending on the amount of sample required for the pycnometer method and the size of the honeycomb structure.

[0045] As a method for changing the average true density of the honeycomb structure portion between the peripheral region (first peripheral region 121, second peripheral region 122) and the central region (first central region 131), for example, there is a method of extruding a clay using raw materials having different true densities for the portion that will become the peripheral region after extrusion molding and the portion that will become the central region after extrusion molding.

[0046] In a preferred embodiment, the average porosity of the first outer peripheral region 121 and the second outer peripheral region 122 is lower than that of the first central region 131. Although it is not intended that the present invention be limited by theory, this configuration makes it possible to increase the heat capacity of the first outer peripheral region 121 and the second outer peripheral region 122 and to facilitate thermal diffusion, thereby suppressing heat generation near both circumferential ends of the first electrode layer 112a and the second electrode layer 112b, which are prone to high temperatures.

[0047] If the average porosity of the first outer peripheral region 121 is P1 (%), the average porosity of the second outer peripheral region 122 is P2 (%), and the average porosity of the first central region 131 is P3 (%), then it is preferable that 0.5≦P1 / P3≦0.91, more preferably 0.56≦P1 / P3≦0.87, and even more preferably 0.67≦P1 / P3≦0.87. It is also preferable that 0.5≦P2 / P3≦0.91, more preferably 0.56≦P2 / P3≦0.87, and even more preferably 0.67≦P2 / P3≦0.87. It is also preferable that 0.9≦P1 / P2≦1.1, more preferably 0.95≦P1 / P2≦1.05, and even more preferably 0.97≦P1 / P2≦1.03.

[0048] The average porosity of the first outer peripheral region 121 and the second outer peripheral region 122 is preferably 30 to 54% and more preferably 30 to 50% in order to balance the strength and the prevention of deformation during firing. The average porosity of the first central region 131 is preferably 33 to 60% and more preferably 36 to 60% in order to balance between ensuring strength and preventing deformation during firing.

[0049] In this specification, the average porosity of the first peripheral region 121 and the second peripheral region 122 is determined by the following method. The honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) are cut out from each outer peripheral region at six locations without bias. From each test piece, an SEM image is obtained at a magnification of 200 times within a range of 1 mm vertical x 1 mm horizontal for a cross section perpendicular to the extension direction of the cells. Next, the obtained SEM image is subjected to image analysis to binarize the solid parts of the partition walls and the void parts (pores) in the partition walls by the mode method. Then, the percentage of the ratio of the void parts in the partition walls to the total area of ​​the solid parts and void parts of the partition walls is calculated, and the obtained value is regarded as the porosity of each test piece. The average value of the porosities of the six test pieces is regarded as the average porosity of each outer peripheral region.

[0050] In this specification, the average porosity of the first central region 131 is determined by the following method. A honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) with a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) are cut out from the first central region at six locations without bias. From each test piece, an SEM image of 200 times magnification is obtained in an area of ​​1 mm length × 1 mm width for a cross section perpendicular to the extension direction of the cells. Next, the obtained SEM image is subjected to image analysis to binarize the solid parts of the partition walls and the void parts (pores) in the partition walls by the mode method. Then, the percentage of the ratio of the void parts in the partition walls to the total area of ​​the solid parts and void parts of the partition walls is calculated, and the obtained value is regarded as the porosity of each test piece. The average value of the porosities of the six test pieces is regarded as the average porosity of the first central region.

[0051] As a method for changing the average porosity of the honeycomb structure between the peripheral region (first peripheral region 121, second peripheral region 122) and the central region (first central region 131), for example, there is a method of extruding a clay using raw materials having different mixing ratios of pore-forming material in the part that will become the peripheral region after extrusion molding and the part that will become the central region after extrusion molding.

[0052] In a preferred embodiment, the average partition wall thickness of the first outer peripheral region 121 and the second outer peripheral region 122 is greater than that of the first central region 131. Although it is not intended that the present invention be limited by theory, this configuration increases the heat capacity of the first outer peripheral region 121 and the second outer peripheral region 122, making it possible to suppress heat generation near both circumferential ends of the first electrode layer 112a and the second electrode layer 112b, which are prone to high temperatures.

[0053] If the average partition wall thickness of the first outer peripheral region 121 is T1 (mm), the average partition wall thickness of the second outer peripheral region 122 is T2 (mm), and the average partition wall thickness of the first central region 131 is T3 (mm), then it is preferable that 1.1≦T1 / T3≦2.5, more preferably 1.1≦T1 / T3≦2.0, and even more preferably 1.1≦T1 / T3≦1.5. It is also preferable that 1.1≦T2 / T3≦2.5, more preferably 1.1≦T2 / T3≦2.0, and even more preferably 1.1≦T2 / T3≦1.5. It is also preferable that 0.9≦T1 / T2≦1.1, more preferably 0.95≦T1 / T2≦1.05, and even more preferably 0.97≦T1 / T2≦1.03.

[0054] The average partition wall thickness of the first outer peripheral region 121 and the second outer peripheral region 122 is preferably 0.12 to 0.25 (mm) in view of the balance between the strength of the honeycomb structure and the pressure loss when exhaust gas is allowed to flow. The average partition wall thickness of the first central region 131 is preferably 0.10 to 0.23 (mm), more preferably 0.10 to 0.21 (mm), and even more preferably 0.10 to 0.19 (mm), in view of the balance between the strength of the honeycomb structure and the pressure loss when exhaust gas is passed through it.

[0055] In this specification, the average partition wall thicknesses of the first peripheral region 121 and the second peripheral region 122 are determined by the following method. A honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) having a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3) are cut out from each outer peripheral region at six locations without bias. From each test piece, an SEM image of 100 times magnification within an area of ​​2 mm length × 2 mm width is obtained for a cross section perpendicular to the extension direction of the cells, and the thickness of the partition walls included in the SEM image is determined at six arbitrary locations, and the average value is defined as the thickness of the partition walls in each test piece. Then, the average value of the thicknesses of the partition walls of the six test pieces is defined as the average thickness of the partition walls in each outer peripheral region. The thickness of the partition walls 113 is defined as the length of the part that passes through the partition walls 113 among the line segments connecting the centers of gravity of adjacent cells 115 in a cross section perpendicular to the extension direction of the cells 115.

[0056] In this specification, the average partition wall thickness of the first central region 131 is determined by the following method. A honeycomb structure is divided into two at the center in the cell extension direction, and a cross section perpendicular to the cell extension direction is exposed. For one of the two honeycomb structures, a cylindrical test piece (70.7 mm long) having a diameter of 3 mm and a length of 10 mm (in the cell extension direction) including the cross section is cut. 3 ) is cut out from the first central region at six locations without bias. From each test piece, an SEM image at a magnification of 100 times is obtained in an area of ​​2 mm length × 2 mm width for a cross section perpendicular to the extension direction of the cells, and the thickness of the partition walls included in the SEM image is determined at any six locations, and the average value is regarded as the partition wall thickness of each test piece. Then, the average value of the partition wall thicknesses of the six test pieces is regarded as the average partition wall thickness of the first central region.

[0057] As a method for changing the average partition wall thickness of the honeycomb structure between the peripheral region (first peripheral region 121, second peripheral region 122) and the central region (first central region 131), for example, in the process of producing the honeycomb molded body by extrusion molding described below, a die having a structure in which the average partition wall thickness changes between the peripheral region and the central region can be used.

[0058] In a preferred embodiment, the average cell density of the first outer peripheral region 121 and the second outer peripheral region 122 is higher than that of the first central region 131, respectively. Although the present invention is not intended to be limited by theory, this configuration increases the heat capacity of the first outer peripheral region 121 and the second outer peripheral region 122 and facilitates heat diffusion, and it is possible to suppress heat generation in the vicinity of both circumferential ends of the first electrode layer 112a and the second electrode layer 112b, which tend to become hot.

[0059] Let the average cell density of the first outer peripheral region 121 be G1 (cells / cm 2 ), the average cell density of the second outer peripheral region 122 be G2 (cells / cm 2 ), and the average cell density of the first central region 131 be G3 (cells / cm 2 ). Then, it is preferable that 1 < G1 / G3 ≤ 2, more preferably 1 < G1 / G3 ≤ 1.7, and even more preferably 1 < G1 / G3 ≤ 1.5. Also, it is preferable that 1 < G2 / G3 ≤ 2, more preferably 1 < G2 / G3 ≤ 1.7, and even more preferably 1 < G2 / G3 ≤ 1.5. Further, it is preferable that 0.9 ≤ G1 / G2 ≤ 1.1, more preferably 0.95 ≤ G1 / G2 ≤ 1.05, and even more preferably 0.97 ≤ G1 / G2 ≤ 1.03.

[0060] From the viewpoint of increasing the catalyst-supported area and improving the purification performance while reducing the pressure loss, the average cell density of the first outer peripheral region 121 and the second outer peripheral region 122 is preferably 55 to 124 (cells / cm 2 ), more preferably 62 to 124 (cells / cm 2 ), and even more preferably 70 to 124 (cells / cm 2 ). From the viewpoint of improving the purification performance by the catalyst while reducing the pressure loss, the average cell density of the first central region 131 is preferably 47 to 116 (cells / cm 2 ), more preferably 47 to 109 (cells / cm 2 ), and even more preferably 47 to 101 (cells / cm 2 ).

[0061] In this specification, the average cell densities of the first peripheral region 121 and the second peripheral region 122 are respectively the values ​​obtained by dividing the number of cells at least partially contained within each peripheral region in a cross section perpendicular to the direction in which the cells extend, by the area of ​​each peripheral region excluding the peripheral wall.

[0062] In this specification, the average cell density of the first central region 131 is the value obtained by dividing the number of cells at least partially contained within the first central region in a cross section perpendicular to the cell extension direction by the area of ​​the first central region excluding the outer peripheral wall.

[0063] As a method for changing the average cell density of the honeycomb structure between the peripheral region (first peripheral region 121, second peripheral region 122) and the central region (first central region 131), for example, in the process of producing the honeycomb molded body by extrusion molding described below, a die having a structure in which the average cell density changes between the peripheral region and the central region can be used.

[0064] In a preferred embodiment, the average opening ratio of the first outer peripheral region 121 and the second outer peripheral region 122 is lower than that of the first central region 131. Although it is not intended that the present invention be limited by theory, this configuration makes it possible for the first outer peripheral region 121 and the second outer peripheral region 122 to have a large heat capacity and to easily diffuse heat, thereby suppressing heat generation near both circumferential ends of the first electrode layer 112a and the second electrode layer 112b, which are prone to high temperatures.

[0065] If the average aperture ratio of the first outer peripheral region 121 is F1 (%), the average aperture ratio of the second outer peripheral region 122 is F2 (%), and the average aperture ratio of the first central region 131 is F3 (%), then it is preferable that 0.75≦F1 / F3≦0.98, more preferably 0.85≦F1 / F3≦0.98, and even more preferably 0.90≦F1 / F3≦0.98. It is also preferable that 0.75≦F2 / F3≦0.98, more preferably 0.85≦F2 / F3≦0.98, and even more preferably 0.90≦F2 / F3≦0.98. It is also preferable that 0.9≦F1 / F2≦1.1, more preferably 0.95≦F1 / F2≦1.05, and even more preferably 0.97≦F1 / F2≦1.03.

[0066] The average opening ratio of the first outer peripheral region 121 and the second outer peripheral region 122 is preferably 60 to 78(%), more preferably 60 to 76(%), and even more preferably 60 to 74(%). The average opening ratio of the first central region 131 is preferably from 62 to 80(%), more preferably from 64 to 80(%), and further more preferably from 66 to 80(%).

[0067] In this specification, the average opening ratios of the first peripheral region 121 and the second peripheral region 122 are respectively a value obtained by dividing the total cell opening area in each peripheral region in a cross section perpendicular to the cell extension direction by the total of the partition wall area (excluding the peripheral wall) and the cell opening area in each peripheral region (total cell opening area / (total cell opening area+total partition wall area)), expressed as a percentage.

[0068] In this specification, the average opening ratio of the first central region 131 is the value obtained by dividing the total cell opening area in the first central region in a cross section perpendicular to the extension direction of the cells by the total of the partition wall area (excluding the outer peripheral wall) and the cell opening area in the first central region (total cell opening area / (total cell opening area+total partition wall area)), expressed as a percentage.

[0069] As a method for changing the average opening ratio of the honeycomb structure between the peripheral region (first peripheral region 121, second peripheral region 122) and the central region (first central region 131), for example, in the process of producing the honeycomb molded body by extrusion molding described below, a die having a structure in which the average opening ratio changes between the peripheral region and the central region can be used.

[0070] The illustrated honeycomb structure 110 has a circular end face shape and is cylindrical overall. There is no particular limit to the height of the honeycomb structure 110 (the length from one end face to the other end face) and it may be set appropriately depending on the application and required performance. There is no particular limit to the relationship between the height of the honeycomb structure and the diameter of each end face. Therefore, the height of the honeycomb structure may be longer than the diameter of each end face, or the height of the honeycomb structure may be shorter than the diameter of each end face.

[0071] The size of the honeycomb structure 110 is set to 3,000 to 20,000 mm2 in terms of the area of ​​one end face in order to increase heat resistance (suppress cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm. 2 It is more preferable that:

[0072] The outer peripheral wall 114 and the partition walls 113 have a higher volume resistivity than the electrode layers 112a and 112b, but are conductive. The volume resistivity of the outer peripheral wall 114 and the partition walls 113 is not particularly limited as long as they can generate heat by Joule heat when current is applied, but is preferably 0.1 to 200 Ωcm, more preferably 1 to 200 Ωcm, and even more preferably 10 to 100 Ωcm, when measured at 25°C by a four-terminal method.

[0073] Providing the outer peripheral wall 114 in the honeycomb structure 110 is useful in terms of ensuring the structural strength of the honeycomb structure 110 and suppressing leakage of the fluid flowing through the cells 115 from the outer peripheral wall 114. In this respect, the thickness of the outer peripheral wall 114 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the outer peripheral wall 114 is made too thick, it becomes too strong, and the strength balance with the partition walls 113 is lost, resulting in a decrease in thermal shock resistance. Therefore, the thickness of the outer peripheral wall 114 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Here, the thickness of the outer peripheral wall 114 is defined as the thickness in the normal direction to the tangent of the outer surface of the outer peripheral wall 114 at the measurement point when the portion of the outer peripheral wall 114 to be measured for thickness is observed in a cross section perpendicular to the extension direction of the cells 115.

[0074] There is no limitation on the opening shape of the cells in a cross section perpendicular to the extension direction of the cells 115, and the cell may be, for example, a polygonal shape, preferably a square, a hexagon, an octagon, or a combination of these. Among these, square and hexagonal shapes are preferable. By making the cell shape like this, the pressure loss when exhaust gas flows through the honeycomb structure 110 is reduced, and the purification performance of the catalyst is improved. Even if these cells have arc-shaped corners, they are considered to be polygonal cells.

[0075] The cells 115 may penetrate from one end face 116 to the other end face 118. In addition, the cells 115 may be arranged so that first cells each having one end face 116 plugged and the other end face 118 having an opening and second cells each having one end face 116 opening and the other end face 118 plugged are alternately adjacent to each other with the partition wall 113 in between.

[0076] The material of the outer peripheral wall 114 and the partition wall 113 is not particularly limited as long as it can generate heat by Joule heat when electricity is applied, and ceramics (particularly conductive ceramics) can be used alone or in combination. The material of the outer peripheral wall 114 and the partition wall 113 is not limited, and one or more of oxide ceramics such as alumina, mullite, zirconia, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride can be used. In addition, silicon carbide-metal silicon composite material, silicon carbide / graphite composite material, and the like can also be used. Among these, from the viewpoint of achieving both heat resistance and conductivity, the material of the outer peripheral wall 114 and the partition wall 113 is preferably a silicon-silicon carbide composite material or a material mainly composed of silicon carbide, and more preferably a silicon-silicon carbide composite material or silicon carbide. When the material of the outer peripheral wall 114 and the partition wall 113 is said to be mainly composed of silicon-silicon carbide composite, it means that the outer peripheral wall 114 and the partition wall 113 each contain 90 mass% or more of the silicon-silicon carbide composite (total mass). Here, the silicon-silicon carbide composite contains silicon carbide particles as aggregates and silicon as a binder for binding the silicon carbide particles, and it is preferable that a plurality of silicon carbide particles are bound by silicon so as to form pores between the silicon carbide particles. When the material of the outer peripheral wall 114 and the partition wall 113 is said to be mainly composed of silicon carbide, it means that the outer peripheral wall 114 and the partition wall 113 each contain 90 mass% or more of the silicon carbide (total mass).

[0077] When the outer peripheral wall 114 and the partition walls 113 contain a silicon-silicon carbide composite material, the ratio of the "mass of silicon as a binder" contained in the outer peripheral wall 114 and the partition walls 113 to the sum of the "mass of silicon carbide particles as aggregate" contained in the outer peripheral wall 114 and the partition walls 113 and the "mass of silicon as a binder" contained in the outer peripheral wall 114 and the partition walls 113 is preferably 10 to 40 mass%, and more preferably 15 to 35 mass%. When it is 10 mass% or more, the strength of the outer peripheral wall 114 and the partition walls 113 is sufficiently maintained. When it is 40 mass% or less, the shape is easily maintained during firing.

[0078] (1-2. Electrode layer) The electrode layers 112a and 112b will be described with reference to Figs. 1A and 1B. On the surface of the outer peripheral wall 114, the first electrode layer 112a is provided in a strip shape in the extension direction of the cells 115. On the surface of the outer peripheral wall 114, the second electrode layer 112b is provided in a strip shape in the extension direction of the cells 115 so as to face the first electrode layer 112a across the central axis of the honeycomb structure 110. In general, the first electrode layer 112a and the second electrode layer 112b have a lower volume resistivity than the outer peripheral wall 114. Therefore, by disposing the pair of electrode layers 112a and 112b on the surface of the outer peripheral wall 114, the current is easily spread in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115, so that the uniform heat generation of the honeycomb structure 110 can be improved. Specifically, in a cross section perpendicular to the extension direction of the cell 115, the angle θ (0°≦θ≦180°) formed by two line segments extending from the circumferential center of each of the pair of electrode layers 112a, 112b to the central axis of the honeycomb structure 110 is preferably 150°≦θ≦180°, more preferably 160°≦θ≦180°, even more preferably 170°≦θ≦180°, and most preferably 180°.

[0079] Although there is no particular restriction on the formation region of the electrode layers 112a and 112b, from the viewpoint of improving the uniform heat generation of the honeycomb structure 110, it is preferable that the electrode layers 112a and 112b are each provided in a strip shape extending on the outer surface of the outer peripheral wall 114 in the circumferential direction of the honeycomb structure 110 and in the extending direction of the cells 115. Specifically, in a cross section perpendicular to the extending direction of the cells 115, the central angle α formed by two line segments connecting both ends in the circumferential direction of each electrode layer 112a and 112b and the central axis is preferably 30° or more, more preferably 40° or more, and even more preferably 60° or more, from the viewpoint of spreading the current in the circumferential direction and improving the uniform heat generation. However, if the central angle α is too large, the current passing through the inside of the honeycomb structure 110 decreases, and the current passing through the vicinity of the outer peripheral wall 114 increases. Therefore, from the viewpoint of uniform heat generation of the honeycomb structure 110, the central angle α is preferably 140° or less, more preferably 130° or less, and even more preferably 120° or less. Moreover, it is desirable that each of the electrode layers 112a and 112b extends over 80% or more of the length between both end faces of the honeycomb structure 110, preferably over 90% or more, and more preferably over the entire length. The electrode layers 112a and 112b may be composed of a single layer, or may have a laminated structure in which multiple layers are laminated.

[0080] The thickness of the electrode layers 112a, 112b is preferably 0.01 to 5 mm, and more preferably 0.01 to 3 mm. By setting the thickness in this range, the uniform heat generation can be improved. When the thickness of the electrode layers 112a, 112b is 0.01 mm or more, the electrical resistance is appropriately controlled, and the heat can be generated more uniformly. When the thickness is 5 mm or less, the risk of breakage during canning is reduced. The thickness of the electrode layers 112a, 112b is defined as the thickness in the normal direction to the tangent of the outer surface of the electrode layers 112a, 112b at the measurement point when the part of the electrode layers 112a, 112b to be measured for thickness is observed in a cross section perpendicular to the extension direction of the cell 115.

[0081] By making the volume resistivity of the electrode layers 112a, 112b lower than that of the partition walls 113 and the outer peripheral wall 114, electricity flows preferentially through the electrode layers 112a, 112b, and electricity spreads easily in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115 when electricity is applied. The volume resistivity of the electrode layers 112a, 112b is preferably 1 / 10 or less of the volume resistivity of the partition walls 113 and the outer peripheral wall 114, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less. However, if the difference in volume resistivity between the two becomes too large, current concentrates between the ends of the opposing electrode layers 112a, 112b, causing uneven heat generation in the honeycomb structure 110, and therefore the volume resistivity of the electrode layers 112a, 112b is preferably 1 / 200 or more, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more of the volume resistivity of the partition walls 113 and the outer peripheral wall 114. In this specification, the volume resistivities of the electrode layers, partition walls, and outer peripheral wall are values ​​measured at 25°C by a four-terminal method.

[0082] The material of the electrode layers 112a and 112b is not limited, but a composite material (cermet) of metal and ceramic (particularly conductive ceramic) can be used. Examples of metals include, for example, a single metal such as Cr, Fe, Co, Ni, Si, or Ti, or an alloy containing at least one metal selected from these metals. Examples of ceramics include, but are not limited to, silicon carbide (SiC), as well as metal compounds such as metal silicides such as tantalum silicide (TaSi2) and chromium silicide (CrSi2). Specific examples of composite materials (cermets) of metal and ceramics include composite materials of metal silicon and silicon carbide, composite materials of metal silicides such as tantalum silicide and chromium silicide, and composite materials in which one or more insulating ceramics such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride are added to one or more of the above metals from the viewpoint of reducing thermal expansion. Of the various metals and ceramics mentioned above, the electrode layers 112a and 112b are preferably made of a composite material of silicon metal and silicon carbide, because this can be fired simultaneously with the partition walls and the outer peripheral wall, which contributes to simplifying the manufacturing process.

[0083] (1-3. Metal terminal) 1A and 1B, the electrically heated carrier 100 may be provided with at least one first metal terminal 130a electrically connected to the first electrode layer 112a and at least one second metal terminal 130b electrically connected to the second electrode layer 112b. The first electrode layer 112a and the first metal terminal 130a may be directly bonded to each other, or one or more underlayers (not shown) may be provided between them in order to improve the bonding reliability by reducing the thermal expansion difference. Similarly, the second electrode layer 112b and the second metal terminal 130b may be directly bonded to each other, or one or more underlayers may be provided between them in order to improve the bonding reliability by reducing the thermal expansion difference.

[0084] When a voltage is applied to the honeycomb structure 110 via the metal terminals 130a and 130b, electricity is passed and Joule heat is generated in the honeycomb structure 110. Therefore, the honeycomb structure 110 can be suitably used as a heater. This makes it possible to improve the uniform heat generation property of the honeycomb structure 110. The voltage to be applied is preferably 12 to 900 V, more preferably 48 to 600 V, but the voltage to be applied can be changed as appropriate.

[0085] The method for joining the metal terminals 130a, 130b and the electrode layers 112a, 112b (or the underlayer if provided) is not particularly limited, but examples include welding, thermal spraying, and brazing. Among these, welding and thermal spraying are preferred because they cause little deterioration of the joint even when heated to 800° C. or higher.

[0086] The material of the metal terminals 130a, 130b is not particularly limited as long as it is a metal, and an elemental metal or an alloy, etc. can be adopted. From the viewpoints of corrosion resistance, volume resistivity, and linear expansion coefficient, for example, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, and Ti is preferable, and stainless steel and an Fe-Ni alloy are more preferable.

[0087] (2. Exhaust gas purification device) The electrically heated carrier according to one embodiment of the present invention can be used in an exhaust gas purification device. Referring to Fig. 3, an exhaust gas purification device 200 has an electrically heated carrier 100 and a cylindrical metal tube 220 that houses the electrically heated carrier 100. An electric wire 240 for supplying electricity can be connected to the metal terminals 130a and 130b of the electrically heated carrier 100. The material of the metal tube 220 is not limited to, but may be, for example, stainless steel.

[0088] In the exhaust gas purification device 200, the electrically heated carrier 100 can be installed in the middle of a flow path of a fluid such as automobile exhaust gas. The electrically heated carrier 100 can be fixed in the metal tube 220 by, for example, push-in canning, which pushes the electrically heated carrier 100 into the metal tube 220 and fits it in a positional relationship in which the extension direction of the cell and the extension direction of the metal tube 220 coincide. A cushioning material 260 may be placed between the metal tube 220 and the electrically heated carrier 100. The material of the cushioning material 260 is not limited, but ceramic fibers such as alumina fibers and mullite fibers are preferable for the reasons of suppressing the positional deviation of the electrically heated carrier and maintaining the surface pressure between the metal tube and the gas heated carrier.

[0089] (3. Manufacturing method) Next, a method for manufacturing an electrically heated carrier according to one embodiment of the present invention will be described by way of example. The electrically heated carrier can be manufactured by a manufacturing method including step 1 of obtaining a honeycomb molded body, step 2 of obtaining an unfired honeycomb structure with an electrode layer forming paste, step 3 of firing the unfired honeycomb structure with an electrode layer forming paste to obtain a honeycomb structure, and step 4 of joining a metal terminal to the electrode layer.

[0090] (Process 1) Step 1 is a step of preparing a honeycomb molded body, which is a precursor of a honeycomb structure. The honeycomb molded body can be prepared according to a method for preparing a honeycomb molded body in a known method for manufacturing a honeycomb structure. For example, first, a forming raw material is prepared by adding metal silicon powder (metal silicon), a binder, a surfactant, a pore former, water, and the like to silicon carbide powder (silicon carbide). The mass of the metal silicon powder is preferably 10 to 40 mass% with respect to the total mass of the silicon carbide powder and the metal silicon powder. The average particle diameter of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 μm, more preferably 3 to 40 μm. The average particle diameter of the metal silicon particles in the metal silicon powder is preferably 2 to 35 μm. The average particle diameter of the silicon carbide particles and the metal silicon particles refers to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size is measured by a laser diffraction method. The silicon carbide particles are fine particles of silicon carbide that constitute the silicon carbide powder, and the metallic silicon particles are fine particles of metallic silicon that constitute the metallic silicon powder. Note that this is the blending of the forming raw materials when the material of the honeycomb structure is a silicon-silicon carbide composite material, and when the material of the honeycomb structure is silicon carbide, metallic silicon is not added.

[0091] Examples of the binder include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.

[0092] The surfactant may be ethylene glycol, dextrin, fatty acid soap, polyalcohol, etc. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.

[0093] The pore-forming material is not particularly limited as long as it becomes pores after firing, and examples thereof include graphite, starch, foamed resin, water-absorbent resin, silica gel, etc. The content of the pore-forming material is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass. The average particle diameter of the pore-forming material is preferably 10 to 30 μm. The average particle diameter of the pore-forming material refers to the arithmetic mean diameter based on volume when the frequency distribution of particle size is measured by a laser diffraction method. When the pore-forming material is a water-absorbent resin, the average particle diameter of the pore-forming material refers to the average particle diameter after water absorption.

[0094] The content of water is preferably 20 to 60 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is taken as 100 parts by mass.

[0095] Next, the obtained forming raw material is kneaded to form a columnar clay. It is also possible to change the amount of pore former added between the part of the clay that will form the outer peripheral region after extrusion molding and the part that will form the central region after extrusion molding, or to change the compounding ratio of silicon carbide powder and metal silicon powder to change the true density. Then, the clay is extrusion molded to prepare a columnar honeycomb molded body having an outer peripheral wall and partition walls. This makes it possible to provide the honeycomb structure as an integrally molded product. In extrusion molding, a die having a desired overall shape, cell shape, partition wall thickness, cell density, opening rate, etc. can be used. The die structure can be changed depending on the location of the honeycomb structure part, and for example, it is also possible to change it between the outer peripheral region (first outer peripheral region 121, second outer peripheral region 122, third outer peripheral region 123, and fourth outer peripheral region 124) and the central region (first central region 131 and second central region 132). Next, it is preferable to dry the obtained honeycomb molded body. When the length of the honeycomb formed body in the central axial direction is not the desired length, both ends of the honeycomb formed body can be cut to obtain the desired length. The honeycomb formed body after drying is called a dried honeycomb body.

[0096] The honeycomb formed body may be fired once as a modified example of step 1. That is, in this modified example, the honeycomb formed body is fired to prepare a honeycomb fired body, and step 2 is then carried out on the honeycomb fired body.

[0097] (Process 2) Step 2 is a step of applying an electrode layer forming paste to the side surface of the honeycomb molded body to obtain an unfired honeycomb structure with an electrode layer forming paste. The electrode layer forming paste can be formed by appropriately adding various additives to raw material powders (metal powders, ceramic powders, pore formers, etc.) that are mixed according to the required characteristics of the electrode layer, and kneading the mixture. The average particle diameter of the raw material powders is not limited, but is preferably, for example, 5 to 50 μm, and more preferably 10 to 30 μm. The average particle diameter of the raw material powders refers to the arithmetic mean diameter based on volume when the frequency distribution of particle sizes is measured by a laser diffraction method.

[0098] Next, the obtained electrode layer forming paste is applied to required locations on the side surface of a honeycomb formed body (typically a dried honeycomb body) to obtain an unfired honeycomb structure with the electrode layer forming paste. The method of preparing the electrode layer forming paste and the method of applying the electrode layer forming paste to the honeycomb formed body can be performed in accordance with a known method of manufacturing a honeycomb structure, but in order to give the electrode layer a lower volume resistivity than the outer peripheral wall and the partition walls, the metal content can be made higher than that of the outer peripheral wall and the partition walls, or the particle size of the metal particles in the raw material powder can be made smaller.

[0099] (Step 3) Step 3 is a step of obtaining a honeycomb structure by firing the unfired honeycomb structure with the electrode layer forming paste. Before firing, the unfired honeycomb structure with the electrode layer forming paste may be dried. Also, before firing, degreasing may be performed to remove binders and the like. The method of degreasing and firing is not particularly limited, and firing can be performed using an electric furnace, a gas furnace, or the like. The firing conditions vary depending on the material of the honeycomb structure, but are preferably heated at 1400 to 1500°C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon.

[0100] (Step 4) Step 4 is a step of joining a metal terminal to the electrode layer. The joining method is not particularly limited, but examples thereof include thermal spraying, welding, and brazing. In order to improve the joining property between the electrode layer and the metal terminal, a base layer may be formed by a method such as thermal spraying. EXAMPLES

[0101] The following examples are provided to better understand the present invention and its advantages, but the present invention is not limited to these examples.

[0102] [1. Manufacturing of a cylindrical honeycomb structure in which the central angle α of each electrode layer is 100°] <Test Example 1-1> (1. Making cylindrical clay pots) A ceramic raw material was prepared by mixing silicon carbide (SiC) powder and metal silicon (Si) powder in a mass ratio of 80:20. Hydroxypropyl methylcellulose as a binder, a water-absorbent resin as a pore former, and water were added to the ceramic raw material to prepare a molding raw material. The molding raw material was kneaded by a vacuum kneader to prepare a cylindrical clay. The binder content was 7 parts by mass when the total of silicon carbide (SiC) powder and metal silicon (Si) powder was 100 parts by mass. The pore former content was 3 parts by mass when the total of silicon carbide (SiC) powder and metal silicon (Si) powder was 100 parts by mass. The water content was 42 parts by mass when the total of silicon carbide (SiC) powder and metal silicon (Si) powder was 100 parts by mass. In this case, in any cross section perpendicular to the height direction of the cylindrical clay, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer wall is 1.00R, within the region of coordinate values ​​0.90R to 1.00R, expressed as a central angle based on the center of gravity O, the portion of the clay (annular sector portion) from a point protruding 30° from one circumferential end of each electrode layer to be formed later to a point protruding 30° from the other circumferential end of each electrode layer was replaced with a clay having a different compounding ratio of silicon carbide (SiC) powder and metallic silicon (Si) powder (i.e., a different true density) and a different amount of added pore-forming material. The average particle size of the silicon carbide powder was 20 μm, and the average particle size of the metal silicon powder was 6 μm. The average particle size of the pore-forming material was 20 μm. The average particle sizes of the silicon carbide powder, metal silicon powder, and pore-forming material refer to the arithmetic mean diameter based on volume when the frequency distribution of particle size is measured by a laser diffraction method.

[0103] (2. Preparation of dried honeycomb body) The obtained cylindrical clay was molded using an extrusion molding machine having a checkerboard die structure to obtain a cylindrical honeycomb molded body in which each cell had a hexagonal shape in a cross section perpendicular to the extension direction of the cells. In this case, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average partition wall thickness, average cell density, and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from a point protruding 30° from one end in the circumferential direction of each electrode layer to a point protruding 30° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R, is switched from the other part of the honeycomb structure part. Note that the average electrical resistance and the average thermal conductivity were not changed independently, but were changed by changing the above parameters. This honeycomb molded body was dried by high-frequency dielectric heating, and then dried at 120° C. for 2 hours using a hot air dryer, and both end faces were cut off by a predetermined amount to prepare a dried honeycomb body.

[0104] (3. Preparation of electrode layer forming paste) Metallic silicon (Si) powder, silicon carbide (SiC) powder, methyl cellulose, glycerin, and water were mixed with a centrifugal mixer to prepare an electrode layer forming paste. The Si powder and the SiC powder were mixed so that the volume ratio was Si powder:SiC powder=40:60. In addition, when the total of the Si powder and the SiC powder was 100 parts by mass, the amount of methyl cellulose was 0.5 parts by mass, the amount of glycerin was 10 parts by mass, and the amount of water was 38 parts by mass. The average particle diameter of the metallic silicon powder was 6 μm. The average particle diameter of the silicon carbide powder was 35 μm. These average particle diameters refer to the arithmetic mean diameter based on the volume when the frequency distribution of particle size was measured by a laser diffraction method.

[0105] (4. Application of electrode layer forming paste) The electrode layer forming paste was applied to two locations on the outer surface of the outer peripheral wall of the honeycomb dried body by a curved surface printer so as to face each other across the central axis. Each applied portion was formed in a band shape over the entire length between both end faces of the honeycomb dried body (angle θ=180°, central angle α=100°).

[0106] (5. Firing) The honeycomb structure with the electrode layer forming paste was dried at 120°C, and then degreased at 550°C in an air atmosphere for 3 hours. Next, the degreased honeycomb structure with the electrode layer forming paste was fired and then oxidized to obtain a cylindrical honeycomb structure with a height of 60 mm and a diameter of 103 mm (excluding the electrode layer). The firing was performed in an argon atmosphere at 1450°C for 2 hours.

[0107] <Test Example 1-2> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 20° from one end in the circumferential direction of each electrode layer to the point protruding by 20° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0108] <Test Example 1-3> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 10° from one end in the circumferential direction of each electrode layer to the point protruding by 10° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0109] <Test Example 1-4> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0110] <Test Example 1-5> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from one end to the other end in the circumferential direction of each electrode layer to be formed later is switched from that of the other parts of the honeycomb structure part, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R. Other production conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0111] <Test Example 1-6> When the cylindrical honeycomb formed body was produced, the heat capacity of the honeycomb structure part was not changed.Other production conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0112] <Test Example 1-7> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.95R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0113] <Test Example 1-8> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.83R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0114] <Test Example 1-9> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O, in the region of coordinate values ​​0.76R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0115] [2. Manufacturing of a cylindrical honeycomb structure in which the central angle α of each electrode layer is 60°] <Test Example 2-1> The central angle α of each electrode layer was changed to 60°. In addition, when producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the part of the honeycomb structure part from the part protruding 20° from one end of the circumferential direction of each electrode layer to the part protruding 20° from the other end of the circumferential direction of each electrode layer to be formed later is switched from the other part of the honeycomb structure part, expressed by the central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R. Other manufacturing conditions were the same as those of Test Example 1-1, and a cylindrical honeycomb structure was obtained.

[0116] <Test Example 2-2> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 15° from one end in the circumferential direction of each electrode layer to the point protruding by 15° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained.

[0117] <Test Example 2-3> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 10° from one end in the circumferential direction of each electrode layer to the point protruding by 10° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained.

[0118] <Test Example 2-4> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.90R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained.

[0119] <Test Example 2-5> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, the coordinate value of the center of gravity O is 0, and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, and in the region of coordinate values ​​0.90R to 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density, and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from one end to the other end in the circumferential direction of each electrode layer to be formed later is switched from that of the other parts of the honeycomb structure part, expressed as a central angle based on the center of gravity O. The other production conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained.

[0120] <Test Example 2-6> When the cylindrical honeycomb formed body was produced, the heat capacity of the honeycomb structure part was not changed.Other production conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained. <Test Example 2-7> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.95R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained.

[0121] <Test Example 2-8> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O in the region of coordinate values ​​0.83R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained.

[0122] <Test Example 2-9> In producing a cylindrical honeycomb molded body, in any cross section perpendicular to the cell extension direction, when the coordinate value of the center of gravity O is 0 and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average electrical resistance, average thermal conductivity, average true density, average porosity, average partition wall thickness, average cell density and average opening ratio were changed so that the heat capacity per unit volume of the honeycomb structure part from the point protruding by 5° from one end in the circumferential direction of each electrode layer to the point protruding by 5° from the other end in the circumferential direction of each electrode layer, expressed as a central angle based on the center of gravity O, in the region of coordinate values ​​0.76R to 1.00R, is switched from the other parts of the honeycomb structure part. Other manufacturing conditions were the same as those of Test Example 2-1, and a cylindrical honeycomb structure was obtained.

[0123] [3. Manufacturing of cylindrical honeycomb structures with electrode layers having different electrical resistances] <Test Example 3-1> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-2, and a cylindrical honeycomb structure was obtained.

[0124] <Test Example 3-2> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-3, and a cylindrical honeycomb structure was obtained.

[0125] <Test Example 3-3> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-4, and a cylindrical honeycomb structure was obtained.

[0126] <Test Example 3-4> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-5, and a cylindrical honeycomb structure was obtained.

[0127] <Test Example 3-5> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-6, and a cylindrical honeycomb structure was obtained. <Test Example 3-6> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-7, and a cylindrical honeycomb structure was obtained.

[0128] <Test Example 3-7> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-8, and a cylindrical honeycomb structure was obtained.

[0129] <Test Example 3-8> When preparing the electrode layer forming paste, the thickness of the electrode layer was made thin so that the electrical resistance of the electrode layer would increase. The other manufacturing conditions were the same as those of Test Example 1-9, and a cylindrical honeycomb structure was obtained.

[0130] [4. Characterization] <1. Average heat capacity> For the cylindrical honeycomb structures according to the test examples obtained above, the average heat capacity per unit volume at 25°C of the first peripheral region, the second peripheral region, the first central region, the third peripheral region, the fourth peripheral region, and the second central region was measured according to the measurement method described above. The coefficient of variation of the heat capacity of each region was also calculated. The results are shown in Tables 1, 2, and 3.

[0131] <2. Average electrical resistance> For each of the cylindrical honeycomb structures according to the test examples obtained above, the average electrical resistances of the first peripheral region, the second peripheral region, and the first central region at 25° C. were measured according to the measurement method described above. The results are shown in Tables 1, 2, and 3.

[0132] <3. Average thermal conductivity> For each of the cylindrical honeycomb structures according to the test examples obtained above, the average thermal conductivity at 25° C. of the first peripheral region, the second peripheral region, and the first central region was measured according to the measurement method described above. The results are shown in Tables 1, 2, and 3.

[0133] <4. Average true density> For each of the cylindrical honeycomb structures according to the test examples obtained above, the average true density of the first peripheral region, the second peripheral region, and the first central region was measured according to the measurement method described above. The results are shown in Tables 1, 2, and 3.

[0134] <5. Average porosity> For each of the cylindrical honeycomb structures according to the test examples obtained above, the average porosity of the first peripheral region, the second peripheral region, and the first central region was measured according to the measurement method described above. The results are shown in Tables 1, 2, and 3.

[0135] <6. Average partition wall thickness> For each of the cylindrical honeycomb structures according to the test examples obtained above, the average partition wall thicknesses of the first peripheral region, the second peripheral region, and the first central region were measured according to the measurement method described above. The results are shown in Tables 1, 2, and 3.

[0136] 7. Average cell density For each of the cylindrical honeycomb structures according to the test examples obtained above, the average cell densities of the first peripheral region, the second peripheral region, and the first central region were measured according to the measurement method described above. The results are shown in Tables 1, 2, and 3.

[0137] <8.Average opening ratio> For each of the cylindrical honeycomb structures according to the test examples obtained above, the average opening ratios of the first peripheral region, the second peripheral region, and the first central region were measured according to the measurement method described above. The results are shown in Tables 1, 2, and 3.

[0138] [Table 1]

[0139] [Table 2]

[0140] [Table 3]

[0141] [5. Simulation of temperature distribution] For the honeycomb structure obtained under the above manufacturing conditions, a voltage was applied for 1 second to the center of the surface of each of the pair of electrode layers, resulting in a power consumption of 8 kW per 240 g mass of the honeycomb structure. The temperature distribution in the center of the honeycomb structure in the cell extension direction, which is a cross section perpendicular to the cell extension direction, was simulated using commercially available finite element method CAE analysis software. The simulation conditions were as follows: Solver type: Time history response analysis Honeycomb structure initial temperature: 25℃ The maximum and minimum temperatures obtained in the simulation, as well as the difference between the two, are shown in Tables 4, 5, and 6.

[0142] [Table 4]

[0143] [Table 5]

[0144] [Table 6]

[0145] [6. Discussion] As can be seen from the results of Tables 4, 5 and 6, by using the honeycomb structure (electrically heated support) according to the embodiment of the present invention, it is possible to improve the heat generation uniformity. [Explanation of symbols]

[0146] 100: Electrically heated carrier 110: Honeycomb structure 112a: First electrode layer 112a1: One end of the first electrode layer 112a2: the other end of the first electrode layer 112b: Second electrode layer 112b1: One end of the second electrode layer 112b2: the other end of the second electrode layer 113: Bulkhead 114:Outer wall 115: Cell 116: End face 118: End face 121: First outer peripheral area 122: Second outer peripheral area 123: Third outer peripheral area 124: Fourth outer peripheral area 130a: First metal terminal 130b:Second metal terminal 131:First central area 132:Second central area 200: Exhaust gas purification device 220:Metal tube 240: Electric wire 260: Cushioning material

Claims

1. a cylindrical honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and partitioning a plurality of cells forming a flow path from one end face to the other end face; a first electrode layer provided in a strip shape in the extension direction of the cell on the outer surface of the outer peripheral wall; and a second electrode layer provided in a band shape in a cell extension direction on an outer surface of the outer peripheral wall, the second electrode layer being provided so as to face the first electrode layer across a central axis of the honeycomb structure section; Equipped with In a cross section perpendicular to the extension direction of the cell, when the coordinate axis is taken in the radial direction, the coordinate value of the center of gravity O is 0, and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average heat capacity at 25 ° C. per unit volume of the first outer peripheral region and the second outer peripheral region shown below is higher than the average heat capacity at 25 ° C. per unit volume of the first central region, Honeycomb structure: the first outer peripheral region indicates a portion of the honeycomb structure part that is adjacent to the first electrode layer and is expressed by a central angle based on a center of gravity O, from a point that protrudes by 5° from one end of the first electrode layer in the circumferential direction to a point that protrudes by 5° from the other end of the first electrode layer in the circumferential direction, within a region of coordinate values ​​0.90R to 1.00R; the second outer peripheral region is a region of coordinate values ​​0.90R to 1.00R, and indicates a portion of the honeycomb structure part adjacent to the second electrode layer, and extending from a point protruding by 5° from one end of the second electrode layer in the circumferential direction to a point protruding by 5° from the other end of the second electrode layer in the circumferential direction, expressed by a central angle based on the center of gravity O; The first central region indicates a portion of the honeycomb structure portion excluding the first outer peripheral region and the second outer peripheral region.

2. The honeycomb structure according to claim 1, wherein the average heat capacity per unit volume of the first peripheral region and the second peripheral region at 25°C is 1.2 to 1.5 times the average heat capacity per unit volume of the first central region at 25°C.

3. The coefficient of variation of the heat capacity per unit volume of the first outer peripheral region at 25° C. is H 1v The coefficient of variation of the heat capacity at 25° C. per unit volume of the second outer peripheral region is H 2v The coefficient of variation of the heat capacity at 25° C. per unit volume of the first central region is H 3v Then, H 1v ≦0.2, H 2v ≦0.2, and H 3v 3. The honeycomb structure according to claim 1, wherein the relationship ≦0.3 is satisfied.

4. 3. The honeycomb structure according to claim 1, wherein the first peripheral region and the second peripheral region have an average electrical resistance at 25° C. lower than that of the first central region.

5. The honeycomb structure according to claim 1 or 2, wherein the first peripheral region and the second peripheral region have an average thermal conductivity at 25° C. higher than that of the first central region.

6. The honeycomb structure according to claim 5, wherein the average thermal conductivity at 25° C. of the first outer peripheral region and the second outer peripheral region is 4 to 30 W / (m·K).

7. The honeycomb structure according to claim 1 or 2, wherein an average true density of the first peripheral region and an average true density of the second peripheral region are higher than an average true density of the first central region.

8. The honeycomb structure according to claim 1 or 2, wherein the first peripheral region and the second peripheral region each have an average porosity lower than that of the first central region.

9. The honeycomb structure according to claim 1 or 2, wherein an average partition wall thickness of the first peripheral region and the second peripheral region is greater than an average partition wall thickness of the first central region.

10. The honeycomb structure according to claim 1 or 2, wherein an average cell density of the first peripheral region and an average cell density of the second peripheral region are higher than an average cell density of the first central region.

11. The honeycomb structure according to claim 1 or 2, wherein an average opening ratio of the first peripheral region and an average opening ratio of the second peripheral region are each lower than an average opening ratio of the first central region.

12. In a cross section perpendicular to the extension direction of the cell, when the coordinate axis is taken in the radial direction, the coordinate value of the center of gravity O is 0, and the coordinate value of the outer surface of the outer peripheral wall is 1.00R, the average heat capacity at 25 ° C. per unit volume of the third outer peripheral region and the fourth outer peripheral region shown below is higher than the average heat capacity at 25 ° C. per unit volume of the second central region, The honeycomb structure according to claim 1 or 2: the third outer circumferential region indicates a portion of the honeycomb structure portion that is adjacent to the first electrode layer and is expressed by a central angle based on a center of gravity O, from a point that protrudes by 12.5° from one end of the first electrode layer in the circumferential direction to a point that protrudes by 12.5° from the other end of the first electrode layer in the circumferential direction, within a region of coordinate values ​​0.80R to 1.00R; the fourth outer peripheral region indicates a portion of the honeycomb structure part that is adjacent to the second electrode layer and is expressed by a central angle based on the center of gravity O, from a point that protrudes by 12.5° from one end of the second electrode layer in the circumferential direction to a point that protrudes by 12.5° from the other end of the second electrode layer in the circumferential direction, within a region of coordinate values ​​0.80R to 1.00R; The second central region indicates a portion of the honeycomb structure portion excluding the third outer peripheral region and the fourth outer peripheral region.

13. The honeycomb structure according to claim 12, wherein the average heat capacity at 25°C per unit volume of the third peripheral region and the fourth peripheral region is 1.05 to 1.4 times the average heat capacity at 25°C per unit volume of the second central region.

14. The coefficient of variation of the heat capacity per unit volume of the third outer peripheral region at 25° C. is H 4v The coefficient of variation of the heat capacity at 25° C. per unit volume of the fourth outer peripheral region is H 5v The coefficient of variation of the heat capacity at 25° C. per unit volume of the second central region is H 6v Then, H 4v ≦0.3, H 5v ≦0.3, and H 6v The honeycomb structure according to claim 13, wherein the relationship ≦0.3 is satisfied.

15. The honeycomb structure according to claim 1 or 2, a metal terminal joined to an outer surface of each of the first electrode layer and the second electrode layer; An electrically heated carrier comprising:

16. An electrically heated carrier according to claim 15; A cylindrical metal tube that accommodates the electrically heated carrier; An exhaust gas purification device comprising:

Citation Information

Patent Citations

  • Honeycomb structure body

    JP2019173662A