Laminate, method for producing the same and metal gasket

The laminate with a rubber layer containing cellulose nanofibers addresses stress relaxation issues in rubber-coated metal plates by using aqueous-soluble rubber, achieving high stress relaxation rates and environmental benefits.

JP2024142230APending Publication Date: 2024-10-10UCHIYAMA MFG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023054308
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for producing laminates with rubber-coated metal plates do not adequately consider stress relaxation rates, particularly when using certain types of rubber, and water-based coating agents fail to account for lamination with metal plates.

Method used

A laminate configuration involving a rubber layer laminated on a metal plate, where the rubber layer contains cellulose nanofibers, with a content of 5 to 50 parts by weight based on 100 parts by weight of rubber, and uses rubber dispersible in an aqueous solvent, eliminating the need for organic solvents.

Benefits of technology

The laminate achieves an excellent stress relaxation rate of 10% or less at 100°C and 20.6 MPa for 22 hours, contributing to environmental sustainability by reducing solvent use and enhancing stress relaxation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142230000001_ABST
    Figure 2024142230000001_ABST
Patent Text Reader

Abstract

To achieve a laminate with an improved stress relaxation rate.SOLUTION: A laminate according to one embodiment includes a metal plate, and a rubber layer laminated on the surface of the metal plate, where the rubber layer includes rubber and cellulose nanofibers.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, a manufacturing method thereof, and a metal gasket. [Background technology]

[0002] A laminate in which a rubber layer is laminated on the surface of a metal plate (hereinafter, also referred to as rubber-coated metal) is preferably used as a gasket for use in an automobile engine or the like. A method for producing such a laminate includes a process of immersing a metal plate in a rubber liquid, as described in Patent Document 1. Patent Document 2 describes a water-based coating agent that is effectively applied to the surface of a sealing material or a sliding member. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-166644 A [Patent Document 2] JP 2016-204509 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the stress relaxation rate of the resulting laminate is not taken into consideration in the above-mentioned Patent Documents 1 and 2. The inventors found that the manufacturing method of the laminate described in Patent Document 1 has room for improvement in the stress relaxation rate depending on the type of rubber used. In addition, the water-based coating agent described in Patent Document 2 does not take into consideration lamination with a metal plate.

[0005] One aspect of the present invention has been made in view of the above problems, and has an object to provide a laminate having an excellent stress relaxation rate. [Means for solving the problem]

[0006] In view of the above problems, the present inventors have found that the above problems can be solved by laminating a rubber layer containing cellulose nanofibers onto a metal plate. <1> A laminate comprising a metal plate and a rubber layer laminated on a surface of the metal plate, the rubber layer containing rubber and cellulose nanofibers. <2> In the rubber layer, the content of the cellulose nanofiber is 5 to 50 parts by weight based on 100 parts by weight of the rubber. <1> The laminate according to claim 1. <3> The rubber is a rubber dispersible in an aqueous solvent. <1> or <2> The laminate according to claim 1. <4> The rubber dispersible in the aqueous solvent is at least one selected from the group consisting of acrylic rubber, acrylonitrile-butadiene rubber, and styrene-butadiene rubber. <3> The laminate according to claim 1. <5> <1> ~ <4> A metal gasket comprising the laminate according to any one of claims 1 to 5. <6> A method for producing a laminate, comprising: laminating a rubber layer on a surface of a metal plate, the rubber layer comprising rubber and cellulose nanofibers. <7> The step of laminating the rubber layer includes a step of contacting a metal plate with latex having cellulose nanofibers dispersed therein. <6> A method for producing the laminate described in claim 1. <8> The rubber is at least one selected from the group consisting of acrylic rubber, acrylonitrile-butadiene rubber, and styrene-butadiene rubber. <6> or <7> A method for producing the laminate described in claim 1. Effect of the Invention

[0007] According to one aspect of the present invention, a laminate having an excellent stress relaxation rate can be realized. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic diagram showing a laminate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a schematic structure of a manufacturing apparatus for a rubber-coated metal in an embodiment. [Diagram 3] FIG. 2 is a schematic diagram showing a manufacturing process of a rubber-coated metal in an embodiment. [Figure 4] 1 is a graph showing the results of a stress relaxation rate test for laminates according to an example and a comparative example. [Diagram 5] 1 is a graph showing the results of a stress relaxation rate test for the laminates according to the examples, comparative examples, and reference examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] 1. Laminate Hereinafter, a laminate according to one embodiment of the present invention (hereinafter also referred to as this laminate) comprises a metal plate and a rubber layer laminated on the surface of the metal plate, and the rubber layer contains rubber and cellulose nanofibers.

[0010] Conventionally, when forming a rubber layer of a laminate, rubber is generally dissolved in an organic solvent, but if a rubber dispersible in an aqueous solvent can be used, it is not necessary to use an organic solvent, which is preferable from the viewpoint of environmental load. The present inventors have considered using a rubber dispersible in an aqueous solvent for the rubber layer, and have independently found that there is a problem in that the stress relaxation rate of the laminate decreases in the process. The present inventors have also considered a method of adding a filler such as silica that is dispersible in an aqueous solvent as a method for increasing the stress relaxation rate, but a sufficient stress relaxation rate was not obtained. In this laminate, the rubber layer contains cellulose nanofibers, so that the stress relaxation rate can be prevented from decreasing even when any rubber is used. Furthermore, since a rubber dispersible in an aqueous solvent can be used as the rubber of this laminate, it is possible to manufacture the laminate without using an organic solvent, unlike conventional laminates.

[0011] In this specification, "excellent stress relaxation rate" means that the stress relaxation rate measured according to ASTM F1276 is 10% or less when subjected to, for example, 100° C. and a pressure of 20.6 MPa for 22 hours.

[0012] In addition, according to the above-mentioned configuration, since rubber dispersible in an aqueous solvent can be used as a material, the laminate can be manufactured without using organic solvents. This effect also contributes to the achievement of Goal 3 of the Sustainable Development Goals (SDGs) advocated by the United Nations, "Ensure good health and promote well-being for all."

[0013] The present laminate will be described with reference to Fig. 1. Fig. 1 is a schematic diagram showing an example of the cross-sectional structure of the present laminate. As shown in Fig. 1, the present laminate is formed by laminating a rubber layer 2 containing rubber and cellulose nanofibers on the surface of a metal plate 1. In the present laminate, an adhesive layer 10 may be present between the rubber layer 2 and the metal plate 1 as necessary. The presence of the adhesive layer 10 improves the adhesion between the rubber layer 2 and the metal plate 1.

[0014] <Rubber layer> The rubber layer provided in the laminate contains rubber and cellulose nanofibers. The rubber layer is provided on at least one surface of the metal plate, and is preferably provided on both surfaces of the metal plate.

[0015] From the viewpoint of ensuring a sufficient stress relaxation rate, the thickness of the rubber layer is preferably 0.1 mm or less on one side, and more preferably 0.05 mm or less on one side, while from the viewpoint of sealing performance, the thickness of the rubber layer may be preferably 0.025 mm or more, more preferably 0.05 mm or more, or may be 0.1 mm or more.

[0016] (Cellulose nanofiber) The rubber layer of the laminate contains cellulose nanofibers. In this specification, "cellulose nanofibers" refers to nano-sized cellulose fibers obtained by processing cellulose derived from plant biomass. Hereinafter, cellulose nanofibers are also referred to as CNFs.

[0017] In the rubber layer, the content of the CNF is preferably 5 to 50 parts by weight, more preferably 5 to 40 parts by weight, and further preferably 5 to 35 parts by weight, based on 100 parts by weight of the rubber. When the CNF content is 5 parts by weight or more, the stress relaxation rate of the obtained laminate is improved. When the CNF content is 50 parts by weight or less, the sealing performance is excellent. In another embodiment, the CNF content may be, for example, 25 parts by weight or more.

[0018] The fiber width or fiber diameter of the CNF is preferably 500 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less. The lower limit of the fiber width or fiber diameter may be, for example, 3 nm or more. The fiber length of the CNF is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 10 μm or less. The fiber length of the CNF may be, for example, 1 μm or more. The aspect ratio of the CNF may be preferably 10 or more, more preferably 50 or more, and even more preferably 100 or more. The upper limit of the aspect ratio may be, for example, 30,000 or less. The longer the fiber length of the CNF, the better the reinforcing property, and the shorter the fiber length of the CNF, the better the dispersibility.

[0019] (Rubber) The rubber layer of the laminate contains rubber. The type of rubber contained in the rubber layer is not particularly limited, and any rubber can be used. The rubber layer may contain only one type of rubber, or multiple types of rubber may be used in appropriate combination.

[0020] The rubber is preferably a rubber that can be made into a rubber liquid. A rubber liquid means a liquid in which the rubber is dispersed in a solvent. When the rubber can be made into a rubber liquid, a rubber layer can be easily laminated on the surface of the metal plate. In particular, among rubber liquids, a rubber liquid in which the solvent is an aqueous solvent is also referred to as "latex" in this specification.

[0021] The rubber is preferably a rubber that can be dispersed in an aqueous solvent (hereinafter, also referred to as water-dispersible rubber). In other words, water-dispersible rubber can be said to be a rubber that can form latex. When the rubber is water-dispersible rubber, latex can be formed by dispersing the rubber using an aqueous solvent. This eliminates the need to use an organic solvent in the manufacturing process of the rubber liquid, thereby improving safety and reducing the environmental load.

[0022] The water-dispersible rubber preferably has one or more functional groups selected from a carbonyl group, an isocyanate group, and a vinyl group. When the water-dispersible rubber has the functional group, the water-dispersible rubber is easily dispersed in an aqueous solvent.

[0023] The water-dispersible rubber may preferably contain one or more bonds selected from a urethane bond, a carbon-carbon double bond, and a hydrogen bond in the molecule. When the water-dispersible rubber contains the above bonds, it becomes easy to form a crosslinked structure by radical or dehydration condensation.

[0024] Examples of the water-dispersible rubber include acrylic rubber, acrylonitrile-butadiene rubber, styrene-butadiene rubber, natural rubber, butyl rubber, etc. Among these, from the viewpoint of excellent strength and adhesiveness, preferred are acrylic rubber, acrylonitrile-butadiene rubber, and styrene-butadiene rubber, and more preferred are acrylic rubber.

[0025] Examples of the acrylic rubber monomer include one or a mixture of two or more selected from ethyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-methylpentyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, n-decyl acrylate, n-dodecyl acrylate, n-octadecyl acrylate, cyanomethyl acrylate, 1-cyanoethyl acrylate, 2-cyanoethyl acrylate, 1-cyanopropyl acrylate, and 2-cyanopropyl acrylate.

[0026] (Other Ingredients) The rubber layer may contain components other than the above-mentioned cellulose nanofibers and rubber, as long as the effects of the present invention are not impaired. Examples of such components include fillers, adhesives, vulcanizing agents, vulcanization aids, acid acceptors, colorants, plasticizers, processing aids, and antioxidants. These components can be added to the rubber liquid to be contained in the rubber layer. The content of the other components in the rubber layer may be, for example, 0 to 30 parts by weight.

[0027] <Metal plate> There is no limitation on the metal plate that can be used for the laminate, and any metal plate can be used. Examples of the metal plate include metal plates made of copper, iron, steel, silver, gold, nickel, chromium, titanium, stainless steel, aluminum, etc., or alloy plates of these metal plates. Among these, from the viewpoint of excellent strength, it is preferable that the raw material of the metal plate is steel, stainless steel, or aluminum.

[0028] The thickness of the metal plate is preferably 0.05 mm or more, more preferably 0.1 mm or more, and even more preferably 0.2 mm or more. If the thickness of the metal plate is 0.05 mm or more, the metal plate is less likely to deform, and when the rubber liquid layer is formed as described below, unevenness in the thickness of the rubber liquid layer is less likely to occur. In addition, if the thickness of the metal plate is 0.2 mm or more, this is also preferable from the viewpoint of the shape retention of the obtained laminate. The thickness of the metal plate is preferably 3 mm or less, and more preferably 2 mm or less. If the thickness of the metal plate is 3 mm or less, the metal plate is less likely to warp, and when the rubber liquid layer is formed, unevenness in the thickness of the rubber liquid layer is less likely to occur.

[0029] The shape of the metal plate is not particularly limited, and may be, for example, rectangular, annular, etc. When the laminate is to be used as a metal gasket as described below, it is preferable to shape the metal plate in advance to a shape close to that of the metal gasket. This makes it possible to reduce the amount of rubber layer discarded during press molding, etc.

[0030] The metal sheet may be subjected to a surface treatment such as plating. Specific examples of the metal sheet include SECC as specified by JIS (G3313), SUS301 as specified by JIS (G4305), SPCC as specified by JIS (G3141), and TE-91 (trade name) manufactured by Toyo Kohan Co., Ltd.

[0031] The adhesive layer may be formed by applying an adhesive to the surface of the metal plate. The adhesive layer improves the adhesion between the metal plate and the rubber layer. The adhesive contained in the adhesive layer is not particularly limited, but examples thereof include water-based adhesives, phenol-based adhesives, epoxy-based adhesives, silane coupling agents, etc. Among these, water-based adhesives are preferred from the viewpoints of safety and environmental load. The water-based adhesive refers to an adhesive in which an adhesive component such as an epoxy resin is dissolved or dispersed in water and the solvent is water.

[0032] <Metal gasket> A metal gasket according to an embodiment of the present invention preferably includes the above-mentioned present laminate. The present laminate can be processed into a desired shape by pressing or the like to form a metal gasket. In one embodiment, the present laminate itself may be used as a metal gasket.

[0033] The metal gasket has an excellent stress relaxation rate, and is therefore preferably used in products that require stress relaxation resistance, such as automobile engine parts, automobile electrical components, and other parts that require standard gaskets.

[0034] 2. Manufacturing method of laminate The method for producing the laminate includes a step of laminating a rubber layer on a surface of a metal plate, the rubber layer including rubber and cellulose nanofibers. The laminate, the metal plate, and the rubber layer may be appropriately described in the above [1. Laminate].

[0035] The step of laminating the rubber layer preferably includes a step of contacting the metal plate with latex in which CNF is dispersed. The latex is, in other words, an aqueous dispersion containing rubber and CNF. The solid content concentration of the rubber liquid (latex) is usually 10 to 50% by weight. The viscosity of the rubber liquid is preferably 50 to 30,000 mPa·s. The method of contacting the latex with the metal plate is not particularly limited, but examples include immersion, transfer, and coating. Immersion is preferred because it is easy to laminate on the surface of the metal plate. In particular, it is preferred to use the device and method described in JP 2016-166644 A.

[0036] Specifically, a method in which the upper part of the metal plate is clamped with a clamp and the clamp is lowered into a rubber liquid tank containing rubber liquid is simple and preferable. The speed at which the clamp is lowered is not particularly limited, but is usually 10 to 100 mm / sec. It is also preferable to bring two rods provided above the rubber liquid tank close to each other and set the distance between the rods to a predetermined distance that is wider than the thickness of the metal plate. It is preferable that the distance between the two rods (W (mm)) and the thickness of the metal plate (t (mm)) satisfy the following formula (1). In the following formula (1), (Wt) is preferably 0.3 mm or more, and more preferably 0.6 mm or less. 0.1<(Wt)<1 (1) It is preferable to obtain a rubber-coated metal having a layer of rubber liquid formed on both sides of a metal plate by smoothing the surface of the rubber liquid layer with the rods while pulling up the metal plate immersed in the rubber liquid through the gap between the two rods. The speed at which the metal plate is pulled up is not particularly limited, but is usually 10 to 100 mm / sec.

[0037] The form of CNF used is not particularly limited, but from the viewpoint of facilitating production, it is preferable to use a dispersion in which CNF is dispersed in a solvent. The dispersion of CNF has high dispersibility in latex, which is also a liquid, so that the time required for dispersion can be shortened compared to solids such as silica, and productivity can be increased. The solvent of the CNF dispersion is not particularly limited, but from the viewpoints of dispersibility when mixed with latex, as well as safety and environmental load, it is preferably an aqueous solvent.

[0038] The aqueous solvent may be, for example, water or a mixture of water and a water-soluble solvent. Examples of such solvents include lower alcohols such as ethanol, methanol, and isopropanol, and polyhydric alcohols such as propylene glycol and polyethylene glycol. Among these, the aqueous solvent is preferably water from the viewpoints of availability, safety, and environmental load.

[0039] The method for producing the laminate of the present invention may further include a step of drying the layer of rubber liquid laminated on the surface of the metal plate, and a step of shaping the obtained metal plate by hot pressing or the like.

[0040] The method for drying the rubber liquid layer is not particularly limited, but a method of drying the rubber liquid layer while clamping it and hanging it is preferable. The drying temperature is usually 15 to 80°C. Wind or hot air can also be blown onto the rubber liquid layer. In addition, the rubber liquid layer can be dried by natural drying by leaving it at room temperature for a predetermined time.

[0041] The method of hot pressing is not particularly limited, but may be a method of sandwiching the dried rubber-coated metal between heated plates. Here, the thickness of the resulting laminate can be adjusted by placing spacers around the rubber-coated metal.

[0042] After the hot pressing, the resulting laminate may be further heated, if necessary, to volatilize the remaining curing agent.

[0043] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0044] An embodiment of the present invention will now be described.

[0045] 〔material〕 The following materials were used for the laminate: Metal plate: Product name TE-91, manufactured by Toyo Kohan Co., Ltd. (Zn+Co+Mo alloy-plated steel, length 150 mm x width 120 mm x thickness 0.2 mm, rectangular flat plate shape) Rubber dispersion A: Product name LX874, made by Zeon Corporation (acrylic rubber) Rubber dispersion B: Product name XA-5032A, manufactured by Tohpe (acrylic rubber containing urethane bonds) CNF dispersion: Product name ELLEX-S, manufactured by Daio Paper Corporation Adhesive: Product name: Toasuisei 21 Primer, made by Tohpe Silica: Product name ULTRASIL360, manufactured by Eponic Degussa Japan [Stress relaxation rate measurement test] The stress relaxation rate of the laminate was measured by a method in accordance with ASTM F 1276. The laminate of the example is a gasket defined as 9FMF6E11G11H1 in ASTM F868 and as 701111 in ASTM F104.

[0046] 〔Device〕 A layer of rubber liquid was formed on the surface of a metal plate 1 using a rubber-coated metal manufacturing apparatus 101 shown in FIG. 2. The metal plate 1 can be hung on a fastener 112 at the tip of an arm 113. 50 L of rubber liquid is placed in a rubber liquid tank 111. The two rods 114 are round rods made of polytetrafluoroethylene (PTFE) with a diameter of 50 mm. The protective film 117 wound around a delivery roller 115 is a polyethylene film with a thickness of 50 μm. The protective film 117 can be wound around a winding roller 116.

[0047] Example 1 A laminate in which rubber layers were laminated on both sides of a metal plate was obtained according to the following procedure. 1. A rubber liquid was prepared by mixing rubber dispersion A and CNF dispersion B so that the ratio of each component in the rubber liquid was 100 parts by weight of rubber and 6 parts by weight of CNF. 2. The metal plate was degreased using acetone. 3. Adhesive was applied to both sides of a degreased metal plate and dried at 80°C for 10 minutes. 4. A layer of rubber liquid was formed on both sides of the dried metal plate. The procedure is explained below with reference to Figure 3. (1) Metal plate 1 was hung on fastener 112 (not shown in FIG. 3), and fastener 112 was lowered at a speed of 50 mm / sec to immerse metal plate 1 in the rubber liquid in rubber liquid tank 111 (step 1001 in FIG. 3). (2) The two rods 114 provided above the rubber liquid tank 111 were brought close to each other (step 1002 in FIG. 3). At this time, the distance between the rods 114 was 0.6 mm. (3) One second after the metal plate 1 was immersed in the rubber liquid, the arm 113 (not shown in FIG. 3) was moved to raise the fastener 112 at a speed of 50 mm / sec. In this way, the metal plate 1 was raised between the two rods 114, while the protective film 117 covering the rods 114 was used to level the surface of the rubber liquid layer (step 1003 in FIG. 3). (4) The winding roller 116 was rotated to wind up the protective film 117 with the rubber liquid attached thereto (step 1004 in FIG. 3). 5. Thereafter, the metal plate 1 was dried at 80° C. for 10 minutes while still hung on the fastener 112, and then the metal plate 1 was removed from the fastener 112 to obtain a rubber-coated metal in which a rubber layer was formed on both sides of the metal plate 1. 6. In order to harden the rubber layer on the surface, the rubber-coated metal was placed in an oven and heated at 130° C. for 10 minutes. In this way, a laminate was obtained.

[0048] Example 2 A laminate was obtained in the same manner as in Example 1, except that the rubber liquid was prepared so that the ratio of each component in the rubber liquid was 100 parts by weight of rubber and 33 parts by weight of CNF.

[0049] Comparative Example 1 A laminate was obtained in the same manner as in Example 1, except that CNF was not added to the rubber liquid.

[0050] [Result 1] A stress relaxation rate measurement test was carried out on the laminates of Examples 1 and 2, and Comparative Example 1. The results are shown in FIG.

[0051] 4, the laminates of Examples 1 and 2 using CNF showed superior stress relaxation rates compared to Comparative Example 1 not using CNF. Therefore, it was shown that the stress relaxation rate of the laminate can be increased by using CNF, even if a rubber that reduces the stress relaxation rate is used in the rubber layer.

[0052] Example 3 A laminate was obtained in the same manner as in Example 2, except that the rubber dispersion B was used instead of the rubber dispersion A.

[0053] Comparative Example 2 A laminate was obtained in the same manner as in Example 3, except that 33 parts by weight of silica was added instead of CNF per 100 parts by weight of rubber.

[0054] [Reference example 1] A rubber-coated metal produced based on the description in paragraphs

[0044] to

[0055] of Japanese Patent No. 7125105 was used as Reference Example 1.

[0055] [Result 2] A stress relaxation rate measurement test was carried out on the laminates of Example 3, Comparative Example 2, and Reference Example 1. The results are shown in FIG.

[0056] From FIG. 5, Example 3 had a superior stress relaxation rate compared to Comparative Example 2, which used general silica. Also, compared to Reference Example 1, which is a commercially available rubber-coated metal produced using an organic solvent, it had a similar stress relaxation rate. Also, the CNF dispersion used in the production of the rubber liquid of Example 3 was liquid and had good dispersibility in latex. As a result, the CNF dispersion was easily dispersed and the rubber liquid could be produced in a short time, so it was judged to have excellent productivity. On the other hand, the silica used in the production of the rubber liquid of Comparative Example 2 was solid, so it had poor dispersibility in latex and it took a long time to disperse when producing the rubber liquid, so it was judged to have poor productivity. [Industrial Applicability]

[0057] The present invention can be suitably used for metal gaskets and the like. [Explanation of symbols]

[0058] 1 metal plate 2. Rubber layer containing rubber and cellulose nanofibers 10 Adhesive layer

Claims

1. A metal plate and a rubber layer laminated on a surface of the metal plate, The rubber layer comprises rubber and cellulose nanofibers.

2. The laminate according to claim 1, wherein the rubber layer has a content of the cellulose nanofibers of 5 to 50 parts by weight per 100 parts by weight of the rubber.

3. 2. The laminate according to claim 1, wherein the rubber is a rubber that is dispersible in an aqueous solvent.

4. 4. The laminate according to claim 3, wherein the rubber dispersible in the aqueous solvent is at least one selected from the group consisting of acrylic rubber, acrylonitrile-butadiene rubber, and styrene-butadiene rubber.

5. A metal gasket comprising the laminate according to any one of claims 1 to 4.

6. A step of laminating a rubber layer on a surface of a metal plate, The method for producing a laminate, wherein the rubber layer contains rubber and cellulose nanofibers.

7. 7. The method for producing a laminate according to claim 6, wherein the step of laminating the rubber layer includes a step of contacting a metal plate with latex having cellulose nanofibers dispersed therein.

8. The method for producing a laminate according to claim 6 or 7, wherein the rubber is at least one selected from the group consisting of acrylic rubber, acrylonitrile-butadiene rubber, and styrene-butadiene rubber.

Citation Information

Patent Citations

  • Material for use in gasket, and manufacturing method thereof

    JP2009084453A

  • Fluororubber composition, formed article, and fuel hose

    JP2024095578A

  • Crosslinkable nitrile rubber composition and crosslinked rubber material

    WO2016031848A1

  • Manufacturing method of gasket and manufacturing device of rubber coat metal

    JP2016166644A

  • Aqueous coating agent

    JP2016204509A