Magnetic metal particle and magnetic viscous fluid

Fe-based alloy magnetic metal particles with controlled shapes and coatings enhance corrosion resistance and excitation shear stress in magnetorheological fluids, addressing rust issues and maintaining stability and responsiveness.

JP2024142258APending Publication Date: 2024-10-10SEIKO EPSON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054377
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Magnetorheological fluids with high Fe content face issues of increased rust and decreased corrosion resistance, which affects the excitation shear stress and magnetic properties.

Method used

The use of Fe-based alloy magnetic metal particles with a flat shape and specific area ratios (S1/S0 ≥ 4) and controlled aspect ratios (1.5 ≤ d1/d2 ≤ 30) to enhance bonding and dispersion stability, combined with oxide films and surface modification to improve corrosion resistance and excitation shear stress.

Benefits of technology

The solution results in magnetorheological fluids with high corrosion resistance and excitation shear stress, maintaining stability and responsiveness to magnetic fields, suitable for various devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142258000001_ABST
    Figure 2024142258000001_ABST
Patent Text Reader

Abstract

To provide a magnetic metal particle with which magnetic viscous fluid with high corrosion resistance and high excitation shear stress can be manufactured, and magnetic viscous fluid having the magnetic metal particle.SOLUTION: A magnetic metal particle is used for magnetic viscous fluid, is formed of an Fe-based alloy material, and has a flat shape having two principal surfaces in a front-and-back relationship and side faces connecting the principal surfaces to each other. When the area of each principal surface is defined as S1 μm2, and the area of each side face when it is observed from a direction parallel to the principal surfaces and becomes maximum is defined as S0 μm2, an area ratio S1 / S0 is 4 or more.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to magnetic metal particles and magnetorheological fluids. [Background technology]

[0002] A magnetorheological fluid is, for example, a fluid in which magnetic metal particles are dispersed in a dispersion medium. When a magnetic field is applied to a magnetorheological fluid, the magnetic metal particles are magnetized and align in the direction of the magnetic field. This causes the formation of chain-like clusters, which changes the viscosity of the fluid. Therefore, the use of the change in viscosity in vibration control devices, braking devices, etc. is being considered.

[0003] In these devices, for example, the viscosity of the magnetorheological fluid is adjusted by repeatedly applying and removing a magnetic field, thereby achieving various functions such as vibration suppression and braking.

[0004] For example, Patent Document 1 discloses a magnetorheological fluid in which magnetic metal particles made of an alloy containing Fe and fumed silica particles are dispersed in a liquid containing poly-alpha-olefin. It also discloses that the magnetic metal particles are particles having a bimodal distribution. A bimodal distribution means that the diameter distribution has two different maxima. It discloses that the yield stress of the magnetorheological fluid can be widely controlled by controlling the fraction of small particles and large particles that constitute the bimodal distribution. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-032114 Summary of the Invention [Problem to be solved by the invention]

[0006] In alloys containing Fe, increasing the Fe ratio improves the magnetic properties, but it also makes the alloy more susceptible to rust and reduces corrosion resistance. Changing the alloy composition can improve corrosion resistance, but it also reduces the magnetic properties. When the magnetic properties decrease, the excitation shear stress of the magnetorheological fluid decreases.

[0007] Therefore, the realization of magnetic metal particles that can be used to produce a magnetorheological fluid that has high corrosion resistance and high excitation shear stress has become an issue. [Means for solving the problem]

[0008] The magnetic metal particles according to the application example of the present invention are A magnetic metal particle for use in a magnetorheological fluid, comprising: It is made of Fe-based alloy material. The substrate has a flat shape having two main surfaces that are reversed to each other and a side surface connecting the main surfaces, The area of ​​the main surface is S1 [μm 2 ], and the area of ​​the side surface when it is maximum when observed from a direction parallel to the main surface is defined as S0 [μm 2 ], the area ratio S1 / S0 is 4 or more.

[0009] The magnetorheological fluid according to the application example of the present invention is Magnetic metal particles according to an application example of the present invention; A dispersion medium for dispersing the magnetic metal particles; has. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic diagram showing a magnetorheological fluid according to an embodiment; [Diagram 2] FIG. 2 is a diagram showing a schematic diagram of a state when a magnetic field is applied to the magnetorheological fluid shown in FIG. [Diagram 3] FIG. 2 is a partially sectional perspective view showing a schematic view of the magnetic metal particle shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The magnetic metal particles and magnetorheological fluid of the present invention will be described in detail below with reference to the embodiments shown in the accompanying drawings.

[0012] 1. Magnetorheological fluid First, the magnetorheological fluid according to the embodiment will be described.

[0013] Fig. 1 is a schematic diagram showing a magnetorheological fluid 1 according to an embodiment. The magnetorheological fluid 1 shown in Fig. 1 has a dispersoid 5 and a dispersion medium 4. The dispersoid 5 contains magnetic metal particles 2 and an additive 3, and is dispersed in the liquid dispersion medium 4.

[0014] Such a magnetorheological fluid 1 behaves like a liquid when no magnetic field is applied, and behaves like a semi-solid when a magnetic field is applied. By utilizing this change in viscosity, it is possible to control the stress of the magnetorheological fluid 1. This allows the magnetorheological fluid 1 to be used in various devices that utilize the change in stress to perform various functions.

[0015] 1.1. Composition of magnetorheological fluid The magnetic metal particles 2 (magnetic metal particles according to the embodiment), additive 3 and dispersion medium 4 that constitute the magnetorheological fluid 1 will be described in order.

[0016] 1.1.1.Characteristics of magnetic metal particles First, various characteristics of the magnetic metal particles 2 will be described.

[0017] 1.1.1.1. Flatness The magnetic metal particle 2 has a flat shape. The flat shape refers to a plate shape having two main surfaces 212, 212 that are reversed to each other and a side surface 214 connecting the main surfaces 212, and refers to a shape in which the area of ​​the main surface 212 is sufficiently larger than the maximum area of ​​the side surface 214.

[0018] More specifically, the area of ​​the main surface 212 of the magnetic metal particle 2 when viewed in plan is defined as S1 [μm 2], and the area of ​​the side surface 214 at its maximum when the side surface 214 is observed from a direction parallel to the main surface 212 is S0 [μm 2 In this case, the magnetic metal particles 2 satisfy an area ratio S1 / S0 of 4 or more. By using magnetic metal particles 2 having a sufficiently large flatness in this way, it is possible to realize a magnetorheological fluid 1 having a high excitation shear stress. Such an effect is believed to be due to the following reasons.

[0019] FIG. 2 is a diagram showing a schematic state when a magnetic field B is applied to the magnetorheological fluid 1 shown in FIG.

[0020] When the flat magnetic metal particles 2 are magnetized by the application of a magnetic field B, as shown in FIG. 2, they are aligned in the direction of the magnetic field B to form a chain-like cluster CL. At this time, when the flat magnetic metal particles 2 are attracted to each other and come into contact with each other, a large contact area can be secured. FIG. 2 shows each magnetic metal particle 2 as viewed from a direction parallel to the main surface 212. When the contact area between the magnetic metal particles 2 is increased, the bonding force between the magnetic metal particles 2 in the cluster CL can be increased. As a result, the excitation shear stress of the magnetorheological fluid 1 can be increased. In addition, since buoyancy based on the shape of the magnetic metal particles 2 is obtained, it is possible to suppress the aggregation and sedimentation of the magnetic metal particles 2 when no magnetic field is applied. This can increase the dispersion stability of the magnetic metal particles 2.

[0021] The area ratio S1 / S0 of the magnetic metal particles 2 is set to 4 or more as described above, but is preferably set to 10 or more, and more preferably set to 30 or more. If the area ratio S1 / S0 is below the lower limit, the binding force between the magnetic metal particles 2 in the cluster CL cannot be sufficiently increased. Then, the excitation shear stress of the magnetorheological fluid 1 cannot be sufficiently increased. Also, the magnetic metal particles 2 tend to aggregate or be suppressed. On the other hand, the area ratio S1 / S0 of the magnetic metal particles 2 is preferably set to 1000 or less, more preferably set to 500 or less, and even more preferably set to 100 or less. If the area ratio S1 / S0 exceeds the upper limit, the magnetic metal particles 2 become too thin, and therefore, when a magnetic field is applied, the excitation shear stress cannot be sufficiently increased. Also, if the area ratio S1 / S0 exceeds the upper limit, the resistance to the movement of the magnetic metal particles 2 increases. Then, the excitation shear stress of the magnetorheological fluid 1 decreases, and the responsiveness to the change decreases.

[0022] The area ratio S1 / S0 is the average value of the area ratios S1 / S0 calculated from the areas S1 and S0 measured for 50 or more randomly selected magnetic metal particles 2. The areas S1 and S0 can be measured using, for example, an optical microscope, an electron microscope, an atomic force microscope, or the like.

[0023] Aspect Ratio The length of the long axis of the main surface 212 of the magnetic metal particle 2 is d1, the length of the short axis of the main surface 212 is d2, and the ratio d1 / d2 of the long axis length d1 to the short axis length d2 is the aspect ratio of the main surface 212. The average aspect ratio d1 / d2 of the main surface 212 of the magnetic metal particle 2 is preferably 1.5 to 30.0, more preferably 2.0 to 20.0, and even more preferably 2.5 to 10.0. When the average aspect ratio of the main surface 212 is within the above range, the excitation shear stress of the magnetorheological fluid 1 can be particularly increased. In other words, when the average aspect ratio of the main surface 212 is within the above range, the chain-like clusters CL are formed along the long axis, and the contact area between the magnetic metal particles 2 becomes wider. As a result, the binding force between the magnetic metal particles 2 in the clusters CL can be further increased.

[0024] If the average aspect ratio of the main surface 212 is below the lower limit, the contact area between the magnetic metal particles 2 may not be sufficiently large when a magnetic field is applied. On the other hand, if the average aspect ratio of the main surface 212 exceeds the upper limit, the resistance to the movement of the magnetic metal particles 2 may increase. This may result in a decrease in the excitation shear stress of the magnetorheological fluid 1 or a decrease in responsiveness to changes.

[0025] The length d1 of the long axis is the maximum length of the main surface 212. The length d2 of the short axis is the maximum length in a direction perpendicular to the long axis of the main surface 212. The average aspect ratio of the main surface 212 is the average value of the aspect ratios d1 / d2 measured and calculated for 50 or more randomly selected magnetic metal particles 2. The length d1 of the long axis and the length d2 of the short axis can be measured using, for example, an optical microscope, an electron microscope, an atomic force microscope, or the like.

[0026] 1.1.1.3. Average particle size The average particle size of the magnetic metal particles 2 is preferably 1 μm or more and 450 μm or less, more preferably 3 μm or more and 250 μm or less, and even more preferably 5 μm or more and 100 μm or less. If the average particle size of the magnetic metal particles 2 is within the above range, the excitation shear stress of the magnetorheological fluid 1 can be further increased. In addition, the aggregation and sedimentation of the magnetic metal particles 2 in a state where a magnetic field is not applied can be suppressed. Furthermore, the magnetic field responsiveness of the magnetorheological fluid 1 can be suppressed from decreasing.

[0027] If the average particle size of the magnetic metal particles 2 falls below the lower limit, the excitation shear stress of the magnetorheological fluid 1 may decrease or the magnetic metal particles 2 may be more likely to aggregate, depending on the material of the magnetic metal particles 2. In addition, the viscosity change range may become smaller. On the other hand, if the average particle size of the magnetic metal particles 2 exceeds the upper limit, the magnetic metal particles 2 may settle and become unevenly distributed in the dispersion medium 4, depending on the material of the magnetic metal particles 2. In addition, the resistance to the movement of the magnetic metal particles 2 may increase, and the magnetic field responsiveness of the magnetorheological fluid 1 may become smaller.

[0028] The average particle size of the magnetic metal particles 2 can be determined by measuring the volumetric particle size distribution by a laser diffraction / dispersion method and then calculating from the cumulative distribution curve obtained from this particle size distribution. Specifically, the particle size (median diameter) at which the cumulative value from the small diameter side is 50% in the cumulative distribution curve is the average particle size D50 of the magnetic metal particles 2. An example of an apparatus for measuring particle size distribution by a laser diffraction / dispersion method is the MT3300 series manufactured by Microtrack Bell.

[0029] 1.1.1.4.Average thickness The average thickness of the flattened magnetic metal particles 2 is not particularly limited, but is preferably 0.1 μm to 200 μm, more preferably 0.5 μm to 150 μm, and even more preferably 1 μm to 100 μm. When the average thickness of the magnetic metal particles 2 is within the above range, the thickness of the magnetic metal particles 2 becomes sufficiently thin, so that sedimentation of the magnetic metal particles 2 is unlikely to occur even if the area ratio S1 / S0 of the magnetic metal particles 2 is within the above range.

[0030] Fig. 3 is a partial cross-sectional perspective view showing a schematic view of the magnetic metal particle 2 shown in Fig. 1. The average thickness of the magnetic metal particle 2 is an average value obtained by measuring the thickness t shown in Fig. 3 for 50 or more magnetic metal particles 2 and averaging them. For example, an optical microscope, an electron microscope, an atomic force microscope, etc. can be used to measure the thickness t.

[0031] 1.1.1.5.Saturation magnetization The saturation magnetization of the magnetic metal particles 2 is preferably 50 emu / g or more, and more preferably 100 emu / g or more. The saturation magnetization is the value of magnetization when the magnetization exhibited by a magnetic material is constant regardless of the magnetic field when a sufficiently large magnetic field is applied from the outside. The higher the saturation magnetization of the magnetic metal particles 2, the more fully the magnetic material can function. Specifically, the excitation shear stress of the magnetorheological fluid 1 can be further increased, and the range of viscosity change can be further expanded.

[0032] The upper limit of the saturation magnetization of the magnetic metal particles 2 is not particularly limited, but from the viewpoint of ease of material selection that balances performance and cost, it is preferably 250 emu / g or less, and more preferably 200 emu / g or less.

[0033] The saturation magnetization of the magnetic metal particles 2 can be measured by a vibrating sample magnetometer (VSM) etc. The maximum applied magnetic field when measuring the saturation magnetization is, for example, 1194 [kA / m] (15 [kOe]) or more.

[0034] Coercivity The coercive force of the magnetic metal particles 2 is preferably 1595 [A / m] or less (20 [Oe] or less), more preferably 1196 [A / m] or less (15 [Oe] or less), and even more preferably 797 [A / m] or less (10 [Oe] or less). The coercive force refers to the value of an external magnetic field in the opposite direction required to return a magnetized magnetic body to an unmagnetized state. In other words, the coercive force means the resistance to an external magnetic field. The magnetic metal particles 2 having a coercive force within the above range have small residual magnetization, so they are hardly magnetized when a magnetic field is not applied, but are magnetized when a magnetic field is applied, so that the magnetization has high follow-up ability to changes in the magnetic field. Therefore, the magnetorheological fluid 1 having the magnetic metal particles 2 with such low coercive force has excellent responsiveness to changes in the magnetic field. In addition, the magnetic metal particles 2 with such low coercive force are not easily aggregated when a magnetic field is not applied, so they can be uniformly dispersed even if they are contained in a high concentration in the dispersion medium 4. Therefore, such a magnetorheological fluid 1 has sufficient low viscosity recovery property.

[0035] Furthermore, if the low viscosity recovery is sufficient, it is possible to ensure a sufficient range of viscosity change between when a magnetic field is applied and when the magnetic field is removed. Furthermore, since the hysteresis of the viscosity change can be kept small, the range of viscosity change can be stabilized even when the magnetic field is repeatedly applied and removed. This makes it possible to realize a magnetorheological fluid 1 that exhibits good characteristics over a long period of time. As a result, it is possible to impart high performance and long-term reliability to various devices that use the magnetorheological fluid 1.

[0036] The lower limit of the coercivity of the magnetic metal particles 2 does not need to be specifically set, but is set to 8 [A / m] or more (0.1 [Oe] or more) from the viewpoint of sufficiently suppressing the variation in coercivity between production lots.

[0037] The coercive force of the magnetic metal particles 2 is measured, for example, using a vibrating sample magnetometer (VSM). An example of a vibrating sample magnetometer is TM-VSM1550HGC manufactured by Tamagawa Manufacturing Co., Ltd. The maximum applied magnetic field when measuring the coercive force is, for example, 1194 [kA / m] (15 [kOe]). When separating the magnetic metal particles 2 from the magnetorheological fluid 1, a method is used in which the dispersion medium 4 is removed using an organic solvent such as normal hexane or acetone.

[0038] 1.1.2. Magnetic metal particle content The content of the magnetic metal particles 2 is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more of the entire magnetorheological fluid 1. This allows the magnetorheological fluid 1 to have an appropriate viscosity when a magnetic field is applied and when the magnetic field is removed, and allows the excitation shear stress to be sufficiently high. On the other hand, when the handleability of the magnetorheological fluid 1 is taken into consideration, the content of the magnetic metal particles 2 is preferably 95% by mass or less.

[0039] 1.1.3. Composition of magnetic metal particles 3 has a particle body 21, an oxide film 22 provided on the surface of the particle body 21, and a surface modification film 23 provided on the surface of the particle body 21. The oxide film 22 and the surface modification film 23 may be provided as necessary, and either one or both may be omitted.

[0040] 1.1.3.1. Materials of the Particle Body The constituent material of the particle body 21 is an Fe-based alloy material, which is useful in terms of its large saturation magnetization.

[0041] The Fe-based alloy material is an alloy material whose main component is Fe. The term "main component" means that the Fe content in the Fe-based alloy material is 50% or more in terms of atomic ratio. Such an Fe-based alloy material has higher corrosion resistance than pure iron, and contributes to suppression of rusting in the magnetic metal particles 2. In addition, the saturation magnetization is larger than ferrite and the like, and the toughness and strength are also high. For this reason, the Fe-based alloy material is useful as a constituent material of the particle body 21.

[0042] In addition to Fe, the Fe-based alloy material may contain an element that exhibits ferromagnetism by itself, such as Ni or Co, and, depending on the target properties, may contain at least one element selected from the group consisting of Cu, Si, V, Cr, Mn, platinum group elements, Sc, Y, Au, Zn, Sn, Re, B, and C. The platinum group elements refer to at least one element of Ru, Rh, Pd, Os, Ir, and Pt.

[0043] In addition, the Fe-based alloy material may contain unavoidable impurities as long as the effects of the embodiment are not impaired. The unavoidable impurities are impurities that are unintentionally mixed in the raw materials or during production. Examples of the unavoidable impurities include O, N, S, Na, Mg, and K.

[0044] Such Fe-based alloy materials are not particularly limited, but examples thereof include Fe-Si-Al-based alloys such as Sendust, Fe-Ni-based, Fe-Co-based, Fe-Ni-Co-based, Fe-Si-B-based, Fe-Si-Cr-B-based, Fe-Si-BC-based, Fe-Si-B-Cr-C-based, Fe-Si-Cr-based, Fe-B-based, Fe-PC-based, Fe-Co-Si-B-based, Fe-Si-B-Nb-based, Fe-Si-B-Nb-Cu-based, Fe-Zr-B-based, Fe-Cr-based, and Fe-Cr-Al-based Fe-based alloy materials.

[0045] The material of the particle body 21 may be an amorphous alloy material, a crystalline alloy material, or a microcrystalline (nanocrystalline) alloy material. Among these, an amorphous alloy material or a microcrystalline alloy material is preferably used. The microcrystalline alloy material refers to an alloy material in which microcrystals (nanocrystals) having a crystal grain size of 100 nm or less are present. These materials contribute to sufficiently lowering the coercive force of the magnetic metal particles 2 and enhancing the redispersibility of the magnetic metal particles 2. In addition, these materials have higher toughness and strength than, for example, metal oxides, and therefore can effectively suppress wear and damage of the particle body 21. As a result, a magnetorheological fluid 1 with a particularly stable viscosity change range can be realized. Furthermore, since amorphous alloy materials and microcrystalline alloy materials do not have crystal grain boundaries or the crystal grain boundaries are very small, corrosion originating from the crystal grain boundaries is unlikely to occur. For this reason, by using these alloy materials, the corrosion resistance of the magnetic metal particles 2 can be particularly enhanced.

[0046] Examples of amorphous alloy materials include binary or multi-component Fe-based amorphous alloys such as Fe-Si-B, Fe-Si-Cr-B, Fe-Si-BC, Fe-Si-B-Cr-C, Fe-Si-Cr, Fe-B, Fe-BC, Fe-PC, Fe-Co-Si-B, Fe-Si-B-Nb, and Fe-Zr-B systems; Ni-based amorphous alloys such as Ni-Si-B and Ni-PB systems; and Co-based amorphous alloys such as Co-Si-B systems.

[0047] Examples of microcrystalline alloy materials include Fe-based nanocrystalline alloys such as Fe-Si-B-Nb-Cu, Fe-Zr-B, Fe-Hf-B, Fe-Nb-B, Fe-Zr-B-Co, Fe-Hf-B-Co, Fe-Nb-B-Co, and Fe-Si-BP-Cu.

[0048] Particularly preferred Fe-based alloy materials are alloy materials mainly composed of Fe and containing at least one selected from the group consisting of Si, Cr, B, C, Ni, Mn and Cu. Such Fe-based alloy materials have high saturation magnetization and high corrosion resistance. Therefore, by using such Fe-based alloy materials, magnetic metal particles 2 that can be used to produce a magnetorheological fluid 1 that has particularly high corrosion resistance and particularly high excitation shear stress can be obtained.

[0049] The content of Si (silicon) in the Fe-based alloy material is preferably 1.0 atomic % or more and 20.0 atomic % or less, more preferably 1.5 atomic % or more and 13.0 atomic % or less, and even more preferably 2.0 atomic % or more and 11.0 atomic % or less. Such alloys have high magnetic permeability and tend to have high saturation magnetization. This allows the magnetic metal particles 2 to be obtained that can produce a magnetorheological fluid 1 with particularly high excitation shear stress and magnetic field response.

[0050] The content of B (boron) in the Fe-based alloy material is preferably 5.0 atomic % or more and 16.0 atomic % or less, and more preferably 9.0 atomic % or more and 14.0 atomic % or less. B is an element that promotes amorphization, and contributes to the formation of a stable amorphous structure or microcrystalline structure in the magnetic metal particles 2.

[0051] The C (carbon) content in the Fe-based alloy material is preferably 0.5 atomic % or more and 5.0 atomic % or less, and more preferably 1.0 atomic % or more and 3.0 atomic % or less. C is an element that promotes amorphization, and contributes to the formation of a stable amorphous structure or microcrystalline structure in the magnetic metal particles 2.

[0052] The Cr (chromium) content in the Fe-based alloy material is preferably 1.0 atomic % or more and 20.0 atomic % or less, and more preferably 1.5 atomic % or more and 5.0 atomic % or less. By keeping the Cr content within this range, the corrosion resistance of the magnetic metal particles 2 can be improved.

[0053] The total content of impurities is preferably 1.0 atomic % or less, so that the effect of the magnetic metal particles 2 is not impaired even if impurities are contained.

[0054] The constituent elements and composition of the particle body 21 can be identified by ICP emission spectrometry as specified in JIS G 1258:2014, spark emission spectrometry as specified in JIS G 1253:2002, or the like. If the particle body 21 is covered with a coating film or the like, it can be removed by a chemical or physical method and then measured by the above method. The magnetic metal particle 2 may be cut and the core part of the particle body 21 may be analyzed by an analyzer such as an EPMA (Electron Probe Micro Analyzer) or EDX (Energy Dispersive X-ray spectroscopy).

[0055] 1.1.3.2. Method for manufacturing the particle body The particle body 21 may be a particle manufactured by any method. An example of the manufacturing method is a method having a step of manufacturing spherical particles and a step of flattening the spherical particles.

[0056] In the process of producing spherical particles, various powder production methods are used. Examples of the powder production methods include various atomization methods such as water atomization, gas atomization, and rotary water flow atomization, as well as pulverization. Among these, the atomization method can produce particles with a uniform particle size.

[0057] In the process of flattening spherical particles, various mechanochemical methods are used. Examples of mechanochemical methods include methods of subjecting spherical particles to flattening using a mechanochemical apparatus such as a planetary mill, a planetary ball mill, a jet mill, a Jacobson mill, a vibration mill, a vibro mill, an acoustic resonance mixer, etc. Note that this step may be carried out wet or dry. By adjusting the time for carrying out this step, the flatness, aspect ratio, and average particle size of the above-described magnetic metal particles 2 can be controlled. For example, when the time for carrying out this step becomes longer, the flatness, aspect ratio, and average particle size tend to increase.

[0058] 1.1.3.3. Oxide film The oxide film 22 is a film provided on the surface of the particle body 21. The oxide film 22 is interposed between the particle body 21 and a surface modification film 23 described later, and enhances the adhesion of the surface modification film 23 to the particle body 21. Further, the oxide film 22 can protect the particle body 21 and suppress aggregation, and can enhance the moisture absorption resistance and rust prevention property of the particle body 21. Note that the oxide film 22 preferably covers the entire surface of the particle body 21, but may be provided only on a part of the surface.

[0059] Examples of the constituent material of the oxide film 22 include silicon oxide, aluminum oxide, titanium oxide, vanadium oxide, niobium oxide, chromium oxide, manganese oxide, tin oxide, zinc oxide, etc., and one or more mixtures or composites thereof, etc. are included.

[0060] Among these, silicon oxide is preferably used. Silicon oxide is an oxide represented by the compositional formula SiO x (0 < x ≦ 2), but is preferably SiO2.

[0061] The average thickness of the oxide film 22 is preferably 1 nm or more and 500 nm or less, more preferably 3 nm or more and 300 nm or less, and even more preferably 20 nm or more and 100 nm or less. If the average thickness of the oxide film 22 is within the above range, the oxide film 22 can be prevented from becoming thicker than necessary while ensuring the above-mentioned functions of the oxide film 22. This makes it possible to suppress the aggregation and deterioration of the magnetic metal particles 2, while suppressing the deterioration of the magnetic properties of the magnetic metal particles 2 that occurs when the ratio of the oxide film 22 becomes too high.

[0062] The average thickness of the oxide film 22 is determined by observing the cross section of the magnetic metal particle 2 with an electron microscope and averaging the thicknesses of the oxide film 22 at 10 or more points.

[0063] The method for forming the oxide film 22 is not particularly limited, but examples thereof include wet film formation methods such as sol-gel methods including the Stober method, and vapor phase film formation methods such as ALD (Atomic Layer Deposition), CVD (Chemical Vapor Deposition), and ion plating. Among these, the sol-gel method, particularly the Stober method, is useful because it allows the oxide film 22 to be formed evenly at low cost.

[0064] The Stöber method is a method for forming an oxide film 22 by hydrolysis of silicon alkoxide. As the silicon alkoxide, for example, TEOS (tetraethoxysilane, Si(OC2H5)4) is preferably used.

[0065] 1.1.3.4.Surface modified membrane The surface modification film 23 covers the surface of the particle body 21 via the oxide film 22. This can improve the dispersibility of the magnetic metal particles 2 in the dispersion medium 4. Note that the surface modification film 23 preferably covers the entire surface of the oxide film 22 or the particle body 21, but may be provided only on a portion of the surface.

[0066] The constituent materials of the surface modification film 23 include a coupling agent, a surfactant, or an organic compound derived from a polymerized film. Among these, the coupling agent is a compound having a functional group and a hydrolyzable group. By using a coupling agent, a functional group can be introduced to the surface of the oxide film 22 (the surface of the magnetic metal particles 2). This can suppress the aggregation of the magnetic metal particles 2 and further increase the dispersibility in the dispersion medium 4. This can realize magnetic metal particles 2 that are excellent in following the change in the magnetic field and can be uniformly dispersed in the dispersion medium 4 even at high concentrations.

[0067] The surface modification film 23 also contributes to improving the moisture resistance, rust prevention, etc. of the magnetic metal particles 2. By improving the moisture resistance and rust prevention, deterioration of the magnetic metal particles 2 due to moisture absorption and rust generation can be suppressed.

[0068] Examples of the functional group possessed by the coupling agent include those containing an aliphatic hydrocarbon group, a cyclic structure-containing group, a fluoroalkyl group, a fluoroaryl group, a nitro group, an acyl group, a cyano group, etc., and in particular, an aliphatic hydrocarbon group or a cyclic structure-containing group is preferably used.

[0069] The aliphatic hydrocarbon group may be a branched or unbranched alkyl group. The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 12, more preferably 1 to 6. This allows the magnetic metal particles 2 to be dispersed particularly well in the oil-based dispersion medium 4.

[0070] The cyclic structure-containing group is a functional group having a cyclic structure. Examples of the cyclic structure-containing group include an aromatic hydrocarbon group, an alicyclic hydrocarbon group, and a cyclic ether group.

[0071] The aromatic hydrocarbon group is a residue obtained by removing a hydrogen atom from an aromatic hydrocarbon, and preferably has 6 to 20 carbon atoms. Examples of the aromatic hydrocarbon group include an aryl group, an alkylaryl group, an aminoaryl group, and a halogenated aryl group. Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and an indenyl group. Examples of the alkylaryl group include a benzyl group, a methylbenzyl group, a phenethyl group, a methylphenethyl group, and a phenylbenzyl group.

[0072] The alicyclic hydrocarbon group is a residue obtained by removing a hydrogen atom from an alicyclic hydrocarbon, and preferably has 3 to 20 carbon atoms. Examples of the alicyclic hydrocarbon group include a cycloalkyl group and a cycloalkylalkyl group. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. Examples of the cycloalkylalkyl group include a cyclopentylmethyl group and a cyclohexylmethyl group.

[0073] Examples of the cyclic ether group include an epoxy group, a 3,4-epoxycyclohexyl group, and an oxetanyl group.

[0074] The fluoroalkyl group is an alkyl group having from 1 to 16 carbon atoms, which is substituted with one or more fluorine atoms, or a cycloalkyl group having from 3 to 16 carbon atoms. In particular, the fluoroalkyl group is preferably a perfluoroalkyl group.

[0075] The fluoroaryl group is an aryl group substituted with one or more fluorine atoms and having from 6 to 20 carbon atoms. In particular, the fluoroaryl group is preferably a perfluoroaryl group.

[0076] Examples of the hydrolyzable group contained in the coupling agent include an alkoxy group, an acyloxy group, an aryloxy group, an aminoxy group, an amide group, a ketoxime group, an isocyanate group, and a halogen atom.

[0077] Examples of the coupling agent include a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, and a zirconium coupling agent, with the silane coupling agent being particularly preferred.

[0078] The amount of the coupling agent added is preferably 0.01 part by mass to 1.0 part by mass, and more preferably 0.02 part by mass to 0.10 part by mass, when the amount of the particle body 21 is taken as 1 part by mass.

[0079] Additives Examples of additives 3 include settling inhibitors, detergents, dispersants, antioxidants, antiwear agents, extreme pressure agents, friction modifiers, surfactants, thixotropy-imparting agents (thickeners), viscosity reducers, etc., and one or a mixture of two or more of these is used.

[0080] Examples of the sedimentation inhibitor include solid particles composed of non-magnetic materials such as fumed silica, clay powders such as bentonite and hectorite, and one or a mixture of two or more of these is used. Such solid particles are particles of a non-magnetic material whose constituent material is different from that of the magnetic metal particles 2, and suppress the sedimentation of the magnetic metal particles 2. This makes it possible to suppress a decrease in the viscosity change range even if a long period of time continues in which a magnetic field is not applied.

[0081] The content of solid particles is preferably 5.0% by mass or less of the entire magnetorheological fluid 1, and more preferably 0.5% by mass or more and 3.0% by mass or less. This makes it possible to suppress the settling of the magnetic metal particles 2 without affecting the range of viscosity change, and to stabilize the range of viscosity change over a long period of time. Therefore, by adding an appropriate additive 3, the aforementioned rate of change can be optimized.

[0082] Dispersants include, for example, oleates, naphthenates, sulfonates, phosphates, stearic acid, stearates, glycerol monooleate, sorbitan sesquioleate, lauric acid, fatty acids, and fatty alcohols.

[0083] Examples of the anti-wear agent include organic molybdenum compounds such as molybdenum dialkyldithiocarbamate and molybdenum dialkyldithiophosphate, and organic zinc compounds such as zinc dialkyldithiocarbamate and zinc dialkyldithiophosphate.

[0084] The total content of the additives 3 is preferably 10 mass % or less, more preferably 8 mass % or less, and even more preferably 6 mass % or less of the entire magnetorheological fluid 1. This makes it possible to prevent the additives 3 from impairing the function of the magnetic metal particles 2.

[0085] The additive 3 may be added as necessary and may be omitted. The magnetorheological fluid 1 may also contain magnetic particles other than the magnetic metal particles 2, such as non-flat (close to spherical) magnetic particles and non-metallic magnetic particles such as ferrite particles.

[0086] 1.1.5.Dispersion medium The dispersion medium 4 is not particularly limited as long as it is a liquid capable of dispersing the magnetic metal particles 2 and the additive 3. Examples of the dispersion medium 4 include oils such as silicone oil, poly-α-olefin base oil, aromatic synthetic oil, paraffin oil, alkylated phenyl ether oil, ether oil, ester oil, polybutene oil, polyalkylene glycols, mineral oil, vegetable oil, and animal oil, organic solvents such as toluene, xylene, and hexane, and ionic liquids (room-temperature molten salts) such as ethylmethylimidazolium salt, 1-butyl-3-methylimidazolium salt, and 1-methylpyrazolium salt. The dispersion medium 4 may be a mixture containing two or more of these, or a mixture containing one or more of these and a liquid other than the above.

[0087] Among these, examples of the ester oil include a diester produced from a monohydric alcohol and a dicarboxylic acid, a polyol ester produced from a polyol and a monocarboxylic acid, and a complex ester produced from a polyol, a monocarboxylic acid, and a polycarboxylic acid.

[0088] Examples of the diester include esters of dibasic acids such as adipic acid, azelaic acid, sebacic acid, and dodecanedioic acid. The dibasic acid is preferably an aliphatic dibasic acid having 4 to 36 carbon atoms. The alcohol residue constituting the ester portion of the ester of the dibasic acid is preferably a monohydric alcohol residue having 4 to 26 carbon atoms. Examples of such diester include dioctyl adipate, dioctyl sebacate, diisodecyl adipate, and dioctyl azelate.

[0089] As the polyol used in the polyol ester and the complex ester, specifically, a hindered alcohol having no β-hydrogen such as trimethylolpropane, pentaerythritol, neopentyl glycol, etc. is preferably used. As the monocarboxylic acid used in the polyol ester and the complex ester, a linear saturated fatty acid such as coconut oil fatty acid and stearic acid, a linear unsaturated fatty acid such as oleic acid, a branched fatty acid such as isostearic acid, etc. are listed.

[0090] As the polycarboxylic acid, straight-chain saturated polycarboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid are preferably used.

[0091] Examples of the alkylated phenyl ether oil include alkylated diphenyl ethers and (alkylated) polyphenyl ethers.

[0092] Examples of polyalkylene glycols include polyethylene glycol, polypropylene glycol, polybutylene glycol, ethylene oxide-propylene oxide copolymer, propylene oxide-butylene oxide copolymer, and derivatives thereof.

[0093] 1.2. Properties of magnetorheological fluids The magnetorheological fluid 1 preferably has a shear stress of 20,000 Pa or more, and more preferably 25,000 Pa or more, measured at a shear rate of 333 [ / s] with a magnetic field of 0.8 T applied. When the magnetorheological fluid 1 having such an excitation shear stress is used in various devices that perform various functions by utilizing changes in stress, it contributes to improving the performance of the various devices.

[0094] For example, a rheometer MCR102 manufactured by Anton Paar is used to measure the shear stress. In addition, for example, a magnetic field application attachment MRD70 manufactured by Anton Paar is used as a device for applying a magnetic field during measurement.

[0095] The shear stress is measured by taking a 200μL sample of the magnetorheological fluid, placing it between the sample stage and a rotor with a diameter of 20mm, rotating the rotor, and applying a specified shear rate while switching the application of a magnetic field. The gap between the sample stage and the rotor is 0.5mm.

[0096] The upper limit of the shear stress does not have to be particularly set, but it is preferably 50,000 Pa or less from the viewpoint of ensuring a sufficient reduction in the shear stress when the magnetic field is removed and a sufficient range of change in stress.

[0097] 1.3.Examples of applications of magnetorheological fluids Applications of the magnetorheological fluid 1 include various apparatuses and devices that utilize the difference in stress when the application of a magnetic field is switched. Examples of such apparatuses and devices include vibration control devices such as linear dampers, rotary dampers, and shock absorbers, braking devices such as brakes, power transmission devices such as clutches, muscle parts and end effectors of robots, valves for controlling the flow rate of liquids, tactile presentation devices, audio devices, robot hands for medical and welfare purposes, nursing hands, personal mobility devices, and the like.

[0098] 1.4. Manufacturing method of magnetorheological fluid In the method for producing the magnetorheological fluid 1, first, the raw materials of the magnetorheological fluid 1 described above are mixed and stirred. Examples of the stirring method include stirring with a spatula, a vortex mixer, a high shear mixer, and a low frequency acoustic resonance mixer. Among these, examples of high shear mixers include the L5 series manufactured by Silverson. Examples of low frequency acoustic resonance mixers include LabRAM2 manufactured by Resodyne.

[0099] The stirring time is appropriately set depending on the stirring method, but is preferably 5 minutes to 4 hours. The stirring temperature is appropriately set depending on the stirring method, but is preferably 15°C to 70°C.

[0100] 2. Advantages of the above embodiment As described above, the magnetic metal particle 2 according to the embodiment is a magnetic metal particle used in the magnetorheological fluid 1, is made of an Fe-based alloy material, and has a flat shape with two main surfaces 212 that are reversed to each other and a side surface 214 connecting the main surfaces 212. The area of ​​the main surfaces 212 is S1 [μm 2 ], and the area of ​​the side surface 214 when it is maximum when observed from a direction parallel to the main surface 212 is S0 [μm 2 ], the area ratio S1 / S0 is 4 or more.

[0101] According to this configuration, it is possible to obtain the magnetic metal particles 2 that have high corrosion resistance and that can be used to produce a magnetorheological fluid 1 with a high excitation shear stress. In addition, the dispersion stability of the magnetic metal particles 2 can be improved.

[0102] In addition, the area ratio S1 [μm 2 ] / S0[μm 2 ] is preferably 10 or more and 1000 or less.

[0103] This provides the magnetic metal particles 2 that can be used to produce a magnetorheological fluid 1 with a particularly high excitation shear stress.

[0104] Moreover, the Fe-based alloy material preferably contains Fe as a main component and at least one selected from the group consisting of Si, Cr, B, C, Ni, Mn and Cu.

[0105] Such an Fe-based alloy material has high saturation magnetization and high corrosion resistance, and therefore, by using such an Fe-based alloy material, it is possible to obtain magnetic metal particles 2 capable of producing a magnetorheological fluid 1 having particularly high corrosion resistance and particularly high excitation shear stress.

[0106] Moreover, the Fe-based alloy material is preferably an amorphous alloy material or a microcrystalline alloy material.

[0107] These materials contribute to sufficiently lowering the coercive force of the magnetic metal particles 2 and enhancing the redispersibility of the magnetic metal particles 2. In addition, since these materials have higher toughness and strength than, for example, metal oxides, they can effectively suppress wear and breakage. As a result, it is possible to realize a magnetorheological fluid 1 with a particularly stable range of viscosity change. Furthermore, since these materials have no crystal grain boundaries or the crystal grain boundaries are very small, corrosion originating from the crystal grain boundaries is unlikely to occur. Therefore, by using these alloy materials, it is possible to particularly enhance the corrosion resistance of the magnetic metal particles 2.

[0108] Furthermore, the magnetic metal particles 2 preferably have a saturation magnetization of 100 emu / g or more and 250 emu / g or less.

[0109] This configuration can improve the magnetic field response of the magnetic metal particles 2. It can also further increase the excitation shear stress of the magnetorheological fluid 1 and further expand the range of viscosity change. Furthermore, it can be made easier to select the constituent material of the magnetic metal particles 2.

[0110] The average particle size of the magnetic metal particles 2 is preferably not less than 1 μm and not more than 450 μm.

[0111] With this configuration, it is possible to further increase the excitation shear stress of the magnetorheological fluid 1. It is also possible to suppress the aggregation and sedimentation of the magnetic metal particles 2 when no magnetic field is applied. Furthermore, it is possible to suppress the magnetic field response of the magnetorheological fluid 1 from decreasing.

[0112] Furthermore, when the length of the major axis of the main surface 212 is d1 and the length of the minor axis of the main surface 212 is d2, the average aspect ratio d1 / d2 of the main surface 212 is preferably 1.5 or more and 30.0 or less.

[0113] This configuration can particularly increase the excitation shear stress of the magnetorheological fluid 1. In other words, when the average aspect ratio of the main surface 212 is within the above range, the chain-like clusters CL are formed along the major axis, which increases the contact area between the magnetic metal particles 2. As a result, the bonding force between the magnetic metal particles 2 in the clusters CL can be further increased.

[0114] The magnetorheological fluid 1 according to the embodiment includes the magnetic metal particles 2 according to the embodiment and a dispersion medium 4 for dispersing the magnetic metal particles 2.

[0115] According to this configuration, a magnetorheological fluid 1 having high corrosion resistance and high excitation shear stress can be obtained.

[0116] Moreover, the magnetorheological fluid 1 according to the embodiment preferably has a shear stress of 20,000 Pa or more when measured at a shear rate of 333 [ / s] with a magnetic field of 0.8 T applied.

[0117] The magnetorheological fluid 1 having such an excitation shear stress contributes to improving the performance of various devices when used in various devices that utilize changes in stress to perform various functions.

[0118] While the magnetic metal particles and magnetorheological fluid of the present invention have been described above based on the preferred embodiments, the present invention is not limited thereto.

[0119] For example, the magnetic metal particles and magnetorheological fluid of the present invention may be those to which any optional configuration has been added to the above-described embodiments. EXAMPLES

[0120] Next, specific examples of the present invention will be described. 3. Preparation of Magnetorheological Fluid 3.1 Example 1 First, an alloy powder having a predetermined composition was prepared by water atomization. Next, the prepared alloy powder was subjected to flattening processing using a ball mill. As a result, flat magnetic metal particles were obtained.

[0121] Next, the obtained magnetic metal particles and additives were dispersed in a dispersion medium to prepare a magnetorheological fluid. The composition of the magnetorheological fluid is shown in Tables 1 and 2. As additives, clay powder, which is a solid particle, and a liquid organomolybdenum compound were used. As a dispersion medium, a mixture of poly-α-olefin base oil and dioctyl sebacate (dioctyl sebacate) was used.

[0122] The content of magnetic metal particles in the magnetorheological fluid was 85% by mass, the content of solid particles was 2.0% by mass, and the content of organic molybdenum compound was 3.0% by mass.

[0123] 3.2. Examples 2 to 7 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 2.

[0124] 3.3. Example 8 A magnetic rheological fluid was obtained in the same manner as in Example 1, except that the magnetic metal particles used had a particle body made of the above-mentioned alloy powder, an oxide film formed on the surface thereof, and a surface coating film formed on the surface thereof, and the composition of the magnetic rheological fluid was as shown in Tables 1 and 2. The Stöber method was used to form the oxide film. The average thickness of the oxide film is as shown in Table 2. The surface modification film was a film composed of a compound derived from a silane coupling agent (SC), and methyltrimethoxysilane was used as the silane coupling agent.

[0125] 3.4. Example 9 A magnetorheological fluid was obtained in the same manner as in Example 8, except that magnetic metal particles without an oxide film were used and the composition of the magnetorheological fluid was as shown in Tables 1 and 2.

[0126] 3.5. Example 10 A magnetorheological fluid was obtained in the same manner as in Example 8, except that magnetic metal particles without a surface modification film were used and the composition of the magnetorheological fluid was as shown in Tables 1 and 2.

[0127] 3.6. Examples 11 to 14 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 2. Crystalline alloy 2 (SUS630) is an alloy mainly composed of Fe, containing predetermined amounts of Cr, Ni, Cu and Nb, and small amounts (1.0 mass % or less) of Si and Mn.

[0128] 3.7. Comparative Examples 1 to 7 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 2.

[0129] 3.8. Examples 15 to 24 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 3. In Examples 20-22, at least one of an oxide film and a surface coating film was provided in the same manner as in Examples 8-10.

[0130] 3.9. Comparative Examples 8 to 10 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 3.

[0131] 4. Evaluation results of magnetorheological fluid The magnetorheological fluids of each of the examples and comparative examples were evaluated as follows.

[0132] 4.1.Evaluation of corrosion resistance 1 mL of the magnetorheological fluid of each Example and Comparative Example was placed in a glass container with an inner diameter of 6 mm. The magnetorheological fluid in the glass container was left in air at a temperature of 60°C and a relative humidity of 90% for 28 days. The magnetorheological fluid was then washed with hexane, and some of the magnetic metal particles were extracted by magnetic separation.

[0133] Next, the magnetic metal particles were visually observed to confirm the presence or absence of rust. The confirmation results were evaluated in accordance with the following evaluation criteria. The evaluation results are shown in Tables 2 and 3.

[0134] A: No rust was observed. B: Rust was observed (less than 1.5% of the surface area of ​​the magnetic metal particles) C: Rust was observed (1.5% or more but less than 20% of the surface area of ​​the magnetic metal particles) D: Rust was observed (20% or more of the surface area of ​​the magnetic metal particles)

[0135] Next, the magnetorheological fluid containing the magnetic metal particles that were not extracted by the above magnetic separation was left in the above environment for a total of 100 days. After that, the magnetorheological fluid was washed with hexane, and the magnetic metal particles were extracted by magnetic separation.

[0136] Next, the magnetic metal particles were visually observed to confirm the presence or absence of rust. The confirmation results were then evaluated in accordance with the above-mentioned evaluation criteria. The evaluation results are shown in Tables 2 and 3.

[0137] 4.2.Evaluation of excitation shear stress A magnetic field of 0.8 T was applied to the magnetorheological fluids of each Example and Comparative Example, and the excitation shear stress was measured under this condition. The shear rate during measurement was 333 [ / s], and the temperature of the magnetorheological fluid was 25°C.

[0138] For the measurement, a rheometer MCR102 manufactured by Anton Paar was used. In addition, a magnetic field application attachment MRD70 manufactured by Anton Paar was used as a device for applying a magnetic field during the measurement.

[0139] Then, 200 μL of the magnetorheological fluid was sandwiched between the sample stage of the device and a rotor with a diameter of 20 mm, and the rotor was rotated, and the excitation shear stress was measured with the above shear rate and the above magnetic field applied. The gap between the sample stage and the rotor was set to 0.5 mm. The measurement results were evaluated against the following evaluation criteria. The evaluation results are shown in Tables 2 and 3 as "excitation shear stress before corrosion resistance test."

[0140] A: The excitation shear stress is 25,000 Pa or more. B: Excitation shear stress is 20,000 Pa or more and less than 25,000 Pa C: Excitation shear stress is 15,000 Pa or more but less than 20,000 Pa D: Excitation shear stress is less than 15,000 Pa

[0141] Next, the excitation shear stress of the magnetorheological fluids that had been subjected to the 28-day corrosion resistance test in 4.1 was measured in the same manner as above. The measurement results were then evaluated in accordance with the above evaluation criteria. The evaluation results are shown in Tables 2 and 3 as "excitation shear stress after corrosion resistance test."

[0142] 4.3. Evaluation of dispersion stability The dispersion stability of the magnetorheological fluids of each of the Examples and Comparative Examples was evaluated by the following method.

[0143] First, 1 mL of magnetorheological fluid was placed in a 1.5 mL centrifuge tube. The temperature at the time of measurement was 25°C and the relative humidity was 50%. The magnetorheological fluid had been left in this temperature and humidity environment for 24 hours in advance.

[0144] Next, the centrifuge tube was placed in a stirrer and the magnetorheological fluid was stirred. A Taitec E-36 microtube stirrer was used for the stirring. The stirring conditions were horizontal eccentric shaking, a shaking speed of 2500 r / min, and a shaking time of 10 minutes.

[0145] Next, acceleration was applied to the centrifuge tube so that the product of acceleration and time was 690 km / s. This encouraged the magnetorheological fluid to forcibly disperse. This acceleration was applied by applying a centrifugal acceleration of 293 G for 4 minutes. A microcentrifuge Model 3300 manufactured by Kubota Manufacturing Co., Ltd. was used to apply the centrifugal acceleration.

[0146] Immediately after the application of acceleration was terminated, the thickness of the supernatant layer formed by the application of acceleration was measured. The measurement result was designated as "thickness tA."

[0147] Next, a magnetic field was applied to the centrifuge tube by bringing a magnet with a surface magnetic flux density of 0.25 T into contact with the side and bottom of the centrifuge tube for 20 minutes.

[0148] Next, the centrifuge tube was again set in the stirrer, and the magnetorheological fluid was stirred under the same stirring conditions as above.

[0149] Next, acceleration was again applied to the centrifuge tube so that the product of acceleration and time was 690 km / s.

[0150] Immediately after the application of acceleration was terminated, the thickness of the supernatant layer formed by the application of acceleration was measured again. The measurement result was designated as "thickness tB."

[0151] Next, the fluctuation rate |tA-tB| / tA was calculated from the thicknesses tA and tB. The calculated fluctuation rate was then compared with the following evaluation criteria to evaluate the dispersion stability of the magnetorheological fluid. The evaluation results are shown in Tables 2 and 3. Note that a smaller fluctuation rate indicates higher dispersion stability of the dispersoid in the magnetorheological fluid.

[0152] A: The fluctuation rate is 5% or less. B: The fluctuation rate is more than 5% and less than 7%. C: Fluctuation rate is more than 7% and less than 10% D: The fluctuation rate is more than 10%.

[0153] [Table 1]

[0154] [Table 2]

[0155] [Table 3]

[0156] As is clear from Tables 2 and 3, the magnetorheological fluids of the examples were excellent in both corrosion resistance and excitation shear stress. It was also found that the magnetorheological fluids of the examples could have improved dispersion stability by optimizing the flatness and average aspect ratio.

[0157] Therefore, it was confirmed that the magnetic metal particles according to the present invention make it possible to produce a magnetorheological fluid having high corrosion resistance and high excitation shear stress. [Explanation of symbols]

[0158] 1...magnetorheological fluid, 2...magnetic metal particle, 3...additive, 4...dispersion medium, 5...dispersoid, 21...particle body, 22...oxide film, 23...surface modification film, 212...main surface, 214...side surface, B...magnetic field, CL...cluster, d1...major axis length, d2...minor axis length, t...thickness

Claims

1. A magnetic metal particle for use in a magnetorheological fluid, comprising: It is made of an Fe-based alloy material, The substrate has a flat shape having two main surfaces that are reversed to each other and a side surface connecting the main surfaces, The area of ​​the main surface is S 1 [μm 2 ], and the area of ​​the side surface when it is maximum when observed from a direction parallel to the main surface is S 0 [μm 2 ], the area ratio S 1 / S 0 is 4 or more.

2. The area ratio S 1 [μm 2 ] / S 0 [μm 2 2. The magnetic metal particle according to claim 1, wherein the n-th order number is 10 or more and 1,000 or less.

3. The Fe-based alloy material is Fe is the main component, 3. The magnetic metal particle according to claim 1, which contains at least one element selected from the group consisting of Si, Cr, B, C, Ni, Mn and Cu.

4. The magnetic metal particle according to claim 3 , wherein the Fe-based alloy material is an amorphous alloy material or a microcrystalline alloy material.

5. 3. The magnetic metal particles according to claim 1, having a saturation magnetization of 100 emu / g or more and 250 emu / g or less.

6. 3. The magnetic metal particles according to claim 1, wherein the average particle size is from 1 μm to 450 μm.

7. When the length of the major axis of the main surface is d1 and the length of the minor axis of the main surface is d2, 3. The magnetic metal particle according to claim 1, wherein the average aspect ratio d1 / d2 of the main faces is 1.5 or more and 30.0 or less.

8. The magnetic metal particles according to claim 1 or 2, A dispersion medium for dispersing the magnetic metal particles; A magnetorheological fluid comprising:

9. 9. The magnetorheological fluid according to claim 8, which has a shear stress of 20,000 Pa or more measured at a shear rate of 333 [ / s] in a state where a magnetic field of 0.8 T is applied.