Method for producing styrenic resin composition and method for producing foamable styrenic resin particle

By directly supplying styrene resin, carbon, and additives to a multi-screw extruder, the method produces expandable styrenic resin particles with enhanced heat insulation and reduced costs, addressing the inefficiencies of masterbatch-based processes.

JP2024142436APending Publication Date: 2024-10-11KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054573
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for producing expandable styrenic resin particles require a masterbatch process, which increases manufacturing costs and may not achieve optimal heat insulation performance.

Method used

A method involving the direct supply of styrene resin, carbon, brominated flame retardant, and stabilizer to a multi-screw extruder, with specific weight ratios and processing conditions, to produce a styrenic resin composition without a masterbatch, ensuring good carbon dispersion and high heat insulation performance.

Benefits of technology

The method achieves excellent heat insulation performance in styrenic resin foam molded products with reduced manufacturing costs by eliminating the need for a masterbatch and enhancing carbon dispersion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a method for producing a styrenic resin composition which enables production of a styrenic resin foam molding with excellent heat insulation performance and can improve costs than conventional methods.SOLUTION: A method for producing a styrenic resin composition includes a step A of supplying a styrenic resin, carbon, a bromine-based flame retardant and a stabilizer to a multiaxial extruder, and melting and kneading the materials, wherein the carbon, the bromine-based flame retardant and the stabilizer are supplied to the multiaxial extruder in powder states, and a ratio of carbon / (bromine-based flame retardant+stabilizer) which is a weight ratio of the carbon to the total amount of the bromine-based flame retardant and the stabilizer is 1.4 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a styrene-based resin composition and a method for producing expandable styrene-based resin particles. [Background technology]

[0002] Styrene-based resin foams are well-balanced foams having light weight, heat insulating properties, and cushioning properties, and have been widely used as heat insulating materials for food containers, cooler boxes, cushioning materials, and housing, etc.

[0003] In particular, in recent years, in relation to various problems such as global warming, there has been a trend toward energy saving by improving the thermal insulation of buildings such as houses, and it is expected that the demand for styrene-based resin foamed molded products obtained using expandable styrene-based resin particles will increase. For this reason, various studies have been conducted on the weight reduction and improvement of thermal insulation properties of the styrene-based resin foamed products by increasing the expansion ratio.

[0004] For example, Patent Document 1 discloses expandable styrene-based resin particles comprising a styrene-based resin composition containing graphite and a foaming agent, the graphite content being 2 to 10% by weight based on 100% by weight of the styrene-based resin composition, and the number of bubbles present within a range of a radius of 300 μm from the center point of a perpendicular bisecting plane relative to the major axis diameter in the expandable styrene-based resin particles being 550 or less per square millimeter. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-090707 A Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Document 1 discloses that the expandable styrene resin particles disclosed in the patent document 1 can suppress shrinkage immediately after pre-expansion even when expanded at a high expansion ratio, and can obtain a styrene resin foamed molded article having both a high expansion ratio and high thermal insulation. Patent Document 1 discloses a production method for expandable polystyrene resin particles, which includes a step of producing a master batch containing a styrene resin and graphite.

[0007] Means for Solving the Problems The present inventors have conducted extensive research into a method by which a styrene-based resin foam molded article having excellent heat insulating properties can be obtained and at a lower cost than conventional methods. As a result, they have found a method for producing a styrene-based resin composition in which specific materials are supplied to a multi-screw extruder in specific conditions and in specific amounts, thereby completing the present invention. [Means for solving the problem]

[0008] An example aspect of this embodiment is described as follows.

[0009] [1] A process includes a step A of supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture; The carbon, the brominated flame retardant, and the stabilizer are fed in powder form to a multi-screw extruder; A method for producing a styrene-based resin composition, wherein a weight ratio of the carbon to the total amount of the brominated flame retardant and the stabilizer, that is, carbon / (brominated flame retardant+stabilizer), is 1.4 or less. [2] The multi-screw extruder is a twin-screw extruder, The method for producing a styrene-based resin composition according to [1], wherein the Q / N of the twin-screw extruder is within the range of the following formula: Q / N ≦ 8.0×10 -6 ×D 3 (In the above formula, Q is the twin-screw extruder extrusion rate (kg / hr), N is the screw rotation speed (rpm), and D is the twin-screw extruder barrel inner diameter (mm).) [3] The method for producing a styrene-based resin composition according to [1] or [2], wherein the carbon is at least one selected from the group consisting of graphite, graphene, carbon black, carbon nanotubes, activated carbon, and expanded graphite. [4] A process A includes supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture; The carbon, the brominated flame retardant, and the stabilizer are fed in powder form to a multi-screw extruder; A method for producing expandable styrene-based resin particles, wherein a weight ratio of the carbon to the total amount of the brominated flame retardant and the stabilizer, carbon / (brominated flame retardant+stabilizer), is 1.4 or less. [5] The multi-screw extruder is a twin-screw extruder, The method for producing expandable styrene-based resin particles according to [4], wherein the Q / N of the twin-screw extruder is within the range of the following formula: Q / N ≦ 8.0×10 -6 ×D 3 (In the above formula, Q is the twin-screw extruder extrusion rate (kg / hr), N is the screw rotation speed (rpm), and D is the twin-screw extruder barrel inner diameter (mm).) [6] The method for producing expandable styrene-based resin particles according to [4] or [5], wherein the carbon is at least one selected from the group consisting of graphite, graphene, carbon black, carbon nanotubes, activated carbon, and expanded graphite. [7] A method for producing expandable styrene-based resin particles according to any one of [4] to [6], comprising: step B of further adding a blowing agent to the styrene-based resin composition obtained in step A to obtain an expandable styrene-based resin composition; and step C of granulating the expandable styrene-based resin composition to obtain expandable styrene-based resin particles. [8] A method for producing expandable styrene-based resin particles according to any one of [4] to [6], comprising: a step D of granulating the styrene-based resin composition obtained in the step A to obtain styrene-based resin particles; and a step E of impregnating the styrene-based resin particles with a blowing agent to obtain expandable styrene-based resin particles. [9] A method for producing pre-expanded styrene-based resin particles, comprising expanding the expandable styrene-based resin particles obtained by the method for producing expandable styrene-based resin particles according to any one of [4] to [8].

[10] A method for producing a styrene-based resin foamed molded article, comprising molding the styrene-based resin pre-expanded particles obtained by the method for producing the styrene-based resin pre-expanded particles described in [9]. Effect of the Invention

[0010] In the manufacturing method of the present disclosure, carbon can be well dispersed in the styrene-based resin composition without including an additional step such as preparing a masterbatch. By using the styrene-based resin composition, expandable styrene-based resin composition, or expandable styrene-based resin particles obtained by the manufacturing method of the present disclosure, it is possible to obtain a styrene-based resin foamed molded article having excellent heat insulating performance. In addition, there is no need to prepare a masterbatch, and the manufacturing cost is improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The method for producing a styrene-based resin composition according to this embodiment includes a step A of supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture, the carbon, the bromine-based flame retardant, and the stabilizer are supplied to the multi-screw extruder in powder form, and the weight ratio of the carbon to the total amount of the bromine-based flame retardant and the stabilizer, carbon / (bromine-based flame retardant+stabilizer), is 1.4 or less. The method for producing an expandable styrene-based resin particle according to this embodiment includes a step A of supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture, the carbon, the bromine-based flame retardant, and the stabilizer are supplied to the multi-screw extruder in powder form, and the weight ratio of the carbon to the total amount of the bromine-based flame retardant and the stabilizer, carbon / (bromine-based flame retardant+stabilizer), is 1.4 or less.

[0012] (styrene resin) The styrene-based resin may be a styrene homopolymer or a styrene copolymer. As the styrene copolymer, a styrene copolymer obtained by copolymerizing styrene with another monomer copolymerizable with styrene or a derivative thereof can be used. As the styrene-based resin, one type may be used alone, or two or more types may be used. However, in the present embodiment, the styrene-based resin generally excludes a brominated styrene-butadiene copolymer described later.

[0013] Examples of other monomers copolymerizable with styrene or derivatives thereof (hereinafter, sometimes referred to as "other monomers or derivatives thereof") include styrene derivatives such as methylstyrene, dimethylstyrene, ethylstyrene, diethylstyrene, isopropylstyrene, bromostyrene, dibromostyrene, tribromostyrene, chlorostyrene, dichlorostyrene, and trichlorostyrene; polyfunctional vinyl compounds such as divinylbenzene; methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, and butyl acrylate. and (meth)acrylic acid ester compounds such as butyl methacrylate; vinyl cyanide compounds such as (meth)acrylonitrile; diene compounds or derivatives thereof such as butadiene; unsaturated carboxylic acid anhydrides such as maleic anhydride and itaconic anhydride; N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-butylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(2-chlorophenyl)maleimide, N-(4-bromophenyl)maleimide, and N-(1-naphthyl)maleimide. The other monomers or derivatives thereof may be used alone or in combination of two or more.

[0014] The styrene-based resin may be blended with a homopolymer or a copolymer of another monomer or a derivative thereof, as long as the effect of the present invention is not impaired.

[0015] From the viewpoint of impact absorption and heat resistance, the styrene resin may be blended with, for example, diene rubber reinforced polystyrene, acrylic rubber reinforced polystyrene, and / or polyphenylene ether resin.

[0016] The styrene-based resin preferably contains at least one selected from a styrene homopolymer, a styrene-acrylonitrile copolymer, and a styrene-butyl acrylate copolymer, and more preferably contains a styrene homopolymer, because the styrene-based resin is relatively inexpensive, can be foam-molded with low-pressure steam or the like without using a special method, and has an excellent balance of heat insulation, flame retardancy, and cushioning properties.

[0017] The melt flow rate (hereinafter, referred to as "MFR") of the styrene resin is preferably 1 to 15 g / 10 min. When the MFR is in this range, it is easy to obtain expandable styrene resin particles, pre-expanded styrene resin particles, and styrene resin foam molded articles having excellent expandability (high expansion ratio, high air ratio) and surface beauty. The obtained styrene resin foam molded articles have a good balance of mechanical strength such as compressive strength, bending strength, or bending deflection, and properties such as toughness. The MFR is more preferably in the range of 2 to 10 g / 10 min. The MFR in the present invention is a value measured in accordance with JIS K7210.

[0018] In addition, as long as the effects of the present invention are not impaired, other resins may be used in combination with the styrene-based resin as the main component, such as homopolymers of the above-mentioned other monomers or their derivatives, copolymers thereof, polyolefin-based resins, polyester-based resins, polycarbonate-based resins, acrylic-based resins, etc.

[0019] (carbon) The carbon acts as a radiation heat transfer inhibitor in this embodiment. By using carbon together with a styrene resin, a styrene resin foam molded article having high thermal insulation properties can be obtained. In this disclosure, the radiation heat transfer inhibitor refers to a substance having the property of reflecting, scattering, or absorbing light in the near infrared or infrared region.

[0020] The carbon is preferably at least one selected from the group consisting of graphite, graphene, carbon black, carbon nanotubes, activated carbon, and expanded graphite. The carbon may be used alone or in combination of two or more. Among carbons, graphite is preferred because of its high radiation heat transfer suppression effect relative to cost. Examples of graphite include flake graphite, earthen graphite, spherical graphite, and artificial graphite, and among these, flake graphite is preferred because it exhibits a high radiation heat transfer suppression effect. In the present disclosure, the term "flake" also includes scaly, thin, or plate-like graphite. The graphite may be used alone or in combination of two or more.

[0021] The graphite has an average particle size of preferably 0.5 to 9.0 μm, more preferably 2.5 to 9.0 μm, and even more preferably 2.5 to 6.0 μm. In the present disclosure, the average particle size of graphite refers to the particle size (D50) (volume average particle size by laser diffraction scattering method) at which the cumulative volume of the total particle volume is 50% when particle size distribution is measured and analyzed by a laser diffraction scattering method based on the Mie theory in accordance with ISO13320:2009 and JIS Z8825-1.

[0022] The larger the average particle diameter of graphite, the lower the manufacturing cost. In particular, graphite with an average particle diameter of 2.5 μm or more is very inexpensive and can reduce costs because the manufacturing cost, including the cost of crushing, is low. If the average particle diameter is 9.0 μm or less, the cell membrane is less likely to break when producing pre-expanded particles and styrene-based resin foamed molded products from the expandable styrene-based resin particles, which tends to facilitate high expansion, increase ease of molding, and increase the compressive strength of the styrene-based resin foamed molded products.

[0023] Furthermore, if the average particle size of the graphite is 6.0 μm or less, the surface appearance of the molded article is excellent and a lower thermal conductivity, that is, a higher heat insulation property can be obtained.

[0024] In the present invention, the carbon content is not particularly limited, but is preferably 0.1 to 20% by weight, and more preferably 2 to 10% by weight, based on 100% by weight of the styrene-based resin composition.

[0025] The use of graphite as carbon is preferable from the viewpoint of the balance between the thermal conductivity reducing effect and the dispersibility of graphite in the styrene resin composition. The amount of graphite is preferably 2% by weight or more and 10% by weight or less in 100% by weight of the styrene resin composition. When the graphite content is 2% by weight or more, the thermal conductivity reducing effect tends to be sufficient, and when the graphite content is 10% by weight or less, when the pre-expanded particles and the styrene resin foamed molded body are produced from the graphite and the styrene resin, the cell membrane is less likely to break, so that high expansion is easy and the control of the expansion ratio tends to be easy. Furthermore, the graphite content is more preferably 3% by weight or more and 8% by weight or less. When the graphite content is 3% by weight or more, the thermal conductivity is lowered, that is, higher heat insulation can be obtained. When the graphite content is 8% by weight or less, the foamability and the surface beauty of the molded body are good.

[0026] The expandable styrene-based resin particles of the present disclosure preferably have a carbon content of 2 to 10% by weight based on 100% by weight of the expandable styrene-based resin particles. Even when graphite is contained as one embodiment of the expandable styrene-based resin particles of the present disclosure, the graphite content is preferably 2% by weight or more and 10% by weight or less in the resin composition of the expandable styrene-based resin particles, and the above more preferred ranges are similarly applicable.

[0027] (Brominated flame retardants) The bromine-based flame retardant is not particularly limited, and any flame retardant containing bromine as a constituent atom that has been conventionally used for styrene-based resin foam molded articles can be used. Examples of the brominated flame retardant include brominated bisphenol compounds such as 2,2-bis[4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl]propane (also known as tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether)) and 2,2-bis[4-(2,3-dibromopropoxy)-3,5-dibromophenyl]propane (also known as tetrabromobisphenol A-bis(2,3-dibromopropyl ether)), tetrabromocyclooctane, tris(2,3-dibromopropyl)isocyanurate, brominated styrene-butadiene block copolymers, brominated random styrene-butadiene copolymers, and brominated styrene-butadiene graft copolymers. As the brominated flame retardant, for example, the heat-stable brominated copolymer disclosed in JP-A-2009-516019 may be used. The brominated flame retardant may be used alone or in combination of two or more kinds.

[0028] The amount of the bromine-based flame retardant used can be determined based on the amount of bromine (bromine content) constituting the bromine-based flame retardant. For example, the amount of the bromine-based flame retardant contained in a styrene-based resin composition or the like can be determined by the product of the amount of the bromine-based flame retardant contained in the composition (% by weight) and the bromine content of the bromine-based flame retardant (% by weight). The bromine-based flame retardant is preferably 0.8% by weight or more and 8.0% by weight or less in 100% by weight of the styrene-based resin composition, because it is easy to control the expansion ratio to the desired value, and from the viewpoint of the balance of flame retardancy when carbon is added, etc. When the bromine content is 0.8% by weight or more, the effect of imparting flame retardancy tends to be large, and when it is 8.0% by weight or less, the strength of the obtained styrene-based resin foam molding is easily increased. The bromine content in the styrene-based resin composition or the expandable styrene-based resin particles is more preferably 1.0 to 7.0% by weight.

[0029] (Stabilizer) The stabilizer is not particularly limited, but it is preferable to use a heat stabilizer that can suppress the deterioration of flame retardancy due to the decomposition of the bromine-based flame retardant and the deterioration of the styrene-based resin. The stabilizers can be used in appropriate combinations depending on the type of styrene-based resin used, the type and content of carbon, the type and content of the bromine-based flame retardant, the type and content of the foaming agent described below, and the like.

[0030] The heat stabilizer is preferably a hindered amine compound, a phosphorus-based compound, a phenol-based stabilizer, or an epoxy compound, because it can arbitrarily control the weight loss temperature in the thermogravimetric analysis of the mixture containing the bromine-based flame retardant. The heat stabilizer can be used alone or in combination of two or more. An example of the hindered amine compound is tetrakis(2,2,6,6-tetramethylpiperidyloxycarbonyl)butane, and an example of the phosphorus-based compound is bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite.

[0031] In the present invention, the content of the stabilizer is not particularly limited, but is preferably 0.01 to 5% by weight, and more preferably 0.03 to 3% by weight, based on 100% by weight of the styrene-based resin composition. In addition, in the present invention, the content of the stabilizer is not particularly limited, but is preferably 99:1 to 80:20, and more preferably 95:5 to 90:10, in terms of the weight ratio of bromine in the bromine-based flame retardant to the stabilizer.

[0032] (foaming agent) In the present disclosure, a foaming agent may be further added to the styrene resin composition to form an expandable styrene resin composition. The expandable styrene resin composition can be molded into expandable styrene resin particles or in-mold foamed molded products described later, or extruded foamed products. The foaming agent is not particularly limited, but from the viewpoint of a good balance between expandability and product life and easy high expansion ratio when actually used, a hydrocarbon having 3 to 6 carbon atoms is preferable, and a hydrocarbon having 4 to 5 carbon atoms is more preferable. When the carbon number of the foaming agent is 3 or more, the volatility is low and the foaming agent is less likely to dissipate when the foaming agent is made into expandable styrene resin particles, so that the foaming agent remains sufficiently in the foaming process when actually used, and it is possible to obtain sufficient foaming power, and it is easy to increase the expansion ratio, which is preferable. In addition, when the carbon number is 6 or less, the boiling point of the foaming agent is not too high, so that it is easy to obtain sufficient foaming power by heating during pre-expansion, and there is a tendency that high expansion is easy. Examples of the hydrocarbon having 3 to 6 carbon atoms include hydrocarbons such as propane, normal butane, isobutane, normal pentane, isopentane, neopentane, cyclopentane, normal hexane, and cyclohexane. These may be used alone or in combination of two or more. From the perspective of the balance between the ease of increasing the expansion ratio and the product life, it is particularly preferable that the blowing agent contains at least one selected from the group consisting of isobutane, normal butane, isopentane, and normal pentane. It is particularly preferable that the blowing agent contains at least one selected from the group consisting of normal pentane, isopentane, and isobutane, and it is even more preferable that the blowing agent contains normal pentane, isopentane, and isobutane.

[0033] The amount of the foaming agent added is preferably 2 to 10 parts by weight, more preferably 4 to 10 parts by weight, relative to 100 parts by weight of the styrene resin composition. In the above range, when the expandable styrene resin particles are obtained, the balance between the expansion speed and the expansion power is better, and the expansion ratio can be more stably increased. When the amount of the foaming agent added is 4 parts by weight or more, the expansion power required for expansion is sufficient, so that high expansion is easy, and there is a tendency that it is easy to produce a styrene resin foam molded product with a high expansion ratio of 50 times or more. In addition, when the amount of the foaming agent is 10 parts by weight or less, the flame retardant performance is good, and the production time (molding cycle) when producing a styrene resin foam molded product is shortened, so that the production cost tends to be low. In addition, the amount of the foaming agent added is more preferably 4.5 to 9 parts by weight, more preferably 5 to 8.5 parts by weight, relative to 100 parts by weight of the styrene resin composition.

[0034] (Other additives) The styrene-based resin composition and the expandable styrene-based resin composition according to the present invention may contain, as necessary, other additives, for example, one or more other additives selected from the group consisting of a radical generator, a processing aid, a light resistance stabilizer, a nucleating agent, a foaming aid, an antistatic agent, and a colorant such as a pigment, within a range that does not impair the effects of the present invention.

[0035] When a radical generator is contained, high flame retardant performance can be achieved by using the radical generator in combination with a brominated flame retardant.

[0036] The radical generators can be used in appropriate combination depending on the type of styrene-based resin, the type and content of carbon, the type and content of bromine-based flame retardant, the type and content of foaming agent, and the like.

[0037] Examples of the radical generator include cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, 2,3-dimethyl-2,3-diphenylbutane, and poly-1,4-diisopropylbenzene.

[0038] Examples of the processing aid include sodium stearate, magnesium stearate, calcium stearate, zinc stearate, barium stearate, and liquid paraffin.

[0039] Examples of the light resistance stabilizer include phenol-based antioxidants, nitrogen-based stabilizers, sulfur-based stabilizers, benzotriazoles, etc. Note that the light resistance stabilizer may also act as a heat stabilizer, such as a hindered amine compound, a phosphorus-based compound, a phenol-based stabilizer, or an epoxy compound, but in the present disclosure, those that belong to both light resistance stabilizers and heat stabilizers are considered to be heat stabilizers.

[0040] Examples of the nucleating agent include inorganic compounds such as silica, calcium silicate, wollastonite, kaolin, clay, mica, zinc oxide, calcium carbonate, sodium hydrogen carbonate, and talc; polymer compounds such as methyl methacrylate copolymers and ethylene-vinyl acetate copolymer resins; olefin waxes such as polyethylene wax; and fatty acid bisamides such as methylene bisstearamide, ethylene bisstearamide, hexamethylene bispalmitic amide, and ethylene bisoleic amide.

[0041] As the foaming assistant, a solvent having a boiling point of 200° C. or less under atmospheric pressure can be desirably used. Examples of the foaming assistant include aromatic hydrocarbons such as styrene, toluene, ethylbenzene, and xylene, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, and acetates such as ethyl acetate and butyl acetate.

[0042] As the antistatic agent and colorant, those used in various resin compositions can be used without any particular limitation.

[0043] These other additives may be used alone or in combination of two or more.

[0044] (Method of producing styrene-based resin composition) The method for producing a styrene-based resin composition according to the present embodiment includes a step A in which a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer are supplied to a multi-screw extruder and melt-kneaded. A styrene-based resin composition is obtained by the step A. The method for producing expandable styrene-based resin particles according to the present embodiment includes the step A, in other words, the method for producing a styrene-based resin composition, as a part thereof.

[0045] In step A, the carbon, the brominated flame retardant, and the stabilizer are supplied to the multi-screw extruder in powder form. As the powder, each of the carbon powder, the brominated flame retardant powder, and the stabilizer powder may be supplied to the multi-screw extruder, or the carbon powder and the powder of a mixture of the brominated flame retardant and the stabilizer may be supplied to the multi-screw extruder. That is, in step A, a master batch such as a master batch prepared by pre-kneading carbon and a styrene resin, a master batch prepared by pre-kneading a brominated flame retardant and a styrene resin, a master batch prepared by pre-kneading a stabilizer and a styrene resin, and a master batch prepared by pre-kneading a brominated flame retardant, a stabilizer, and a styrene resin is not supplied to the multi-screw extruder. Therefore, the manufacturing method of this embodiment can obtain a styrene resin composition that can provide a styrene resin foam molded product with excellent manufacturing cost and excellent heat insulation performance.

[0046] In step A, the weight ratio of the carbon to the total amount of the brominated flame retardant and the stabilizer, that is, carbon / (brominated flame retardant+stabilizer), is 1.4 or less. In general, in order to fully exert the radiation heat transfer suppression effect of graphite, it is necessary to disperse the graphite well in the resin composition. As a method for dispersing the graphite well, a styrene resin and graphite have been kneaded in advance under load using a kneading device equipped with an agitator such as a Banbury mixer, and used in the form of a master batch. Although a styrene resin foam molded product having excellent heat insulating performance can be obtained by the conventional method, a process for producing a styrene resin foam molded product requires a process for producing a master batch containing a styrene resin and graphite. According to the study by the present inventors, by supplying the carbon, the brominated flame retardant, and the stabilizer in powder form to a multi-screw extruder and setting the weight ratio of the carbon to the total amount of the brominated flame retardant and the stabilizer within the above range, a styrene-based resin composition capable of producing a styrene-based resin foamed molded article having excellent heat insulating performance can be obtained without using a master batch. The weight ratio is preferably 1.2 or less, more preferably 1.0 or less, and particularly preferably 0.9 or less. There is no particular restriction on the lower limit of the weight ratio, but it is, for example, 0.1 or more, preferably 0.2 or more, more preferably 0.3 or more, and particularly preferably 0.4 or more.

[0047] In step A, when the multi-screw extruder is a twin-screw extruder, it is preferable that Q / N in the twin-screw extruder is in the range of the following formula. Q / N ≦ 8.0×10 -6 ×D 3 (In the above formula, Q is the twin-screw extruder extrusion rate (kg / hr), N is the screw rotation speed (rpm), and D is the twin-screw extruder barrel inner diameter (mm).)

[0048] By ensuring that the Q / N ratio in the twin-screw extruder is within the above-mentioned specific range, the dispersion state of carbon in the styrene-based resin becomes good, which in turn tends to make it possible to obtain a highly expandable styrene-based resin foamed molding having high thermal insulation performance at low cost, which is preferable.

[0049] The multi-screw extruder used in the present invention can be a known multi-screw extruder. Examples of multi-screw extruders include twin-screw extruders and four-screw extruders. From the viewpoints of kneading properties and productivity, twin-screw extruders are preferred, and co-rotating intermeshing twin-screw extruders are more preferred. Among kneading equipment that can continuously obtain a styrene-based resin composition, single-screw extruders tend to have poor carbon dispersibility compared to multi-screw extruders. In addition, kneaders such as batch mixers and kneaders tend to have excellent carbon dispersibility compared to continuous extruders, but tend to have poor productivity. For the above reasons, a multi-screw extruder is used as the method for producing a styrene-based resin composition of this embodiment, preferably a twin-screw extruder, and more preferably a continuous twin-screw extruder.

[0050] (Conditions in the melt-kneading process) Regarding the conditions of the melt-kneading step of the styrene resin and carbon in a multi-screw extruder in the production process of the styrene resin composition, a description will be given of the case where the multi-screw extruder is a twin-screw extruder.

[0051] (Q / N) The Q / N ratio in the twin-screw extruder was 8.0×10 in both process A and process B described below. -6 ×D 3 The lower the Q / N, the better the carbon dispersion state tends to be, and as a result, it is possible to obtain a styrene-based resin composition or an expandable styrene-based resin composition that can give a styrene-based resin foamed molded article having high thermal insulation performance. -6 ×D 3 If the amount exceeds 6.5×10, the dispersion of carbon in the styrene resin becomes insufficient, and the heat insulating performance tends to deteriorate. -6 ×D 3 The following is the result.

[0052] Q / N indicates the value obtained by dividing the extrusion rate per unit time (kg / hr) of the twin-screw extruder by the screw rotation speed (rpm) of the twin-screw extruder, and D indicates the barrel inner diameter (mm) of the twin-screw extruder. In general, the extrusion rate is roughly determined by the barrel inner diameter of the twin-screw extruder, and the larger D, the larger the extrusion rate that can be processed. As a result of intensive research by the present inventors, in the present invention, it was found that a highly dispersed state of carbon can be realized by controlling Q / N within a certain range regardless of the value of D, i.e., regardless of the extruder size and production scale, and as a result, a styrene-based resin composition that can give a styrene-based resin foam having high thermal insulation performance can be easily obtained.

[0053] (Method for producing expandable styrene-based resin composition) The method for producing an expandable styrene-based resin composition according to the present embodiment includes step A of supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture, and step B of further adding a blowing agent to the styrene-based resin composition obtained in step A to obtain an expandable styrene-based resin composition. The expandable styrene-based resin composition is obtained by steps A and B. In one embodiment, the method for producing an expandable styrene-based resin particle includes steps A and B, in other words, a method for producing an expandable styrene-based resin composition, as a part of the method.

[0054] Step A can be carried out by the method described in the section on the method for producing a styrene-based resin composition. Step B is a step carried out following step A. Step B is, for example, a step of dissolving and dispersing a foaming agent in a styrene-based resin by the multi-screw extruder or a dispersing facility following the multi-screw extruder, and the method is not particularly limited. Step B can obtain an expandable styrene-based resin composition by further supplying a foaming agent to the styrene-based resin composition in the middle of a multi-screw extruder similar to step A, in other words, downstream of the point where the raw material used in step A is supplied.

[0055] (Method of producing expandable styrene-based resin particles) The method for producing expandable styrene-based resin particles according to the present embodiment includes step A of supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture. Step A can be carried out by the method described in the above section on the method for producing a styrene-based resin composition.

[0056] The method for producing expandable styrene-based resin particles according to this embodiment can be roughly divided into the following aspects 1 and 2. The method for producing expandable styrene-based resin particles of aspect 1 includes, in addition to the step A, a step B of further adding a blowing agent to the styrene-based resin composition obtained in step A to obtain an expandable styrene-based resin composition, and a step C of granulating the expandable styrene-based resin composition to obtain expandable styrene-based resin particles. The method for producing expandable styrene-based resin particles of aspect 2 includes, in addition to the step A, a step D of granulating the styrene-based resin composition obtained in step A to obtain styrene-based resin particles, and a step E of impregnating the styrene-based resin particles with a blowing agent to obtain expandable styrene-based resin particles.

[0057] The method of the step C is not particularly limited as long as it can process the expandable styrene-based resin composition obtained in the step B into particles. For example, the step C includes a step of supplying the expandable styrene-based resin composition to a die having a plurality of small holes attached after the multi-screw extruder, extruding the molten expandable styrene-based resin composition into a cutter chamber filled with pressurized circulating water, cutting the molten expandable styrene-based resin composition with a rotating cutter that contacts the die immediately after extrusion, and cooling and solidifying the composition.

[0058] The method of the step D is not particularly limited as long as it is possible to process the styrene-based resin composition obtained in the step A into particles. The step D can be carried out in the same manner as the above-mentioned step C, except that the expandable styrene-based resin composition is changed to a styrene-based resin composition.

[0059] The method of the step E is not particularly limited as long as it can impregnate the styrene-based resin particles obtained in the step D with a blowing agent. For example, the step E can be a method of suspending the styrene-based resin particles in water and simultaneously supplying the blowing agent to impregnate the styrene-based resin particles with the blowing agent.

[0060] From the viewpoint of simplicity of equipment, the method for producing expandable styrene-based resin particles is preferably embodiment 1.

[0061] (Pre-expanded particles and styrene-based resin foamed molded products) The styrene-based resin composition and the expandable styrene-based resin composition obtained by the above-mentioned manufacturing method can be used as raw materials for expandable styrene-based resin particles. A styrene-based resin foamed molded product can be obtained by using the expandable styrene-based resin particles. In order to obtain a styrene-based resin foamed molded product, the expandable styrene-based resin particles may be pre-expanded and then subjected to in-mold foaming. The pre-expanded particles are also referred to as pre-expanded particles or styrene-based resin pre-expanded particles. That is, the present disclosure includes a method for producing a styrene-based resin pre-expanded particle, which expands the expandable styrene-based resin particles obtained by the above-mentioned manufacturing method for expandable styrene-based resin particles, and a method for producing a styrene-based resin foamed molded product, which molds the styrene-based resin pre-expanded particles obtained by the manufacturing method for the styrene-based resin pre-expanded particles.

[0062] The expandable styrene resin particles can be used for molding after being expanded 10 to 110 times by a conventionally known pre-expanding process, for example, by heated steam to obtain pre-expanded particles, and then cured for a certain period of time as necessary. The obtained pre-expanded particles can be molded (for example, molded in a mold) by steam using a conventionally known molding machine to produce a styrene resin foamed molded article. Depending on the shape of the mold used, a molded article with a complex shape or a block-shaped molded article can be obtained.

[0063] The expandable styrene resin particles can be molded into a styrene resin foamed molded article with a high expansion ratio. The expansion ratio of the foamed molded article is preferably 40 times or more, more preferably 60 times or more, and particularly preferably 80 times or more. The styrene resin composition, expandable styrene resin composition, and expandable styrene resin particles obtained by the above-mentioned production method can achieve low thermal conductivity even when a styrene resin foamed molded article with an expansion ratio of 80 times or more is formed, and the above-mentioned production method is also excellent in terms of production cost because it does not require the preparation of a master batch.

[0064] In this specification, the expansion ratio is expressed as "times" or "cm 3 / g", but these have the same meaning.

[0065] The pre-expanded particles and the styrene-based resin foamed molded article thereof preferably have an average cell diameter of 70 to 300 μm, more preferably 90 to 250 μm, and even more preferably 100 to 200 μm. By having the average cell diameter within the above range, the styrene-based resin foamed molded article has higher heat insulating properties. When the average cell diameter is 70 μm or more, there is a tendency that the expansion ratio can be easily increased, and when the average cell diameter is 300 μm or less, an increase in thermal conductivity, i.e., a deterioration in heat insulating performance, can be avoided.

[0066] (Applications of foamed molded products) The styrene resin composition obtained by the above-mentioned production method, the expandable styrene resin composition, and the foamed molded article molded using the expandable styrene resin particles have excellent surface beauty, high expansion ratio and high closed cell ratio, low thermal conductivity, the increase in thermal conductivity over time is significantly suppressed, and the heat insulation property is high for a long time. Therefore, they are suitable for various applications such as building insulation materials, food container boxes, cold storage boxes, cushioning materials, agricultural and fishery boxes, bathroom insulation materials, and hot water tank insulation materials.

[0067] In addition, the production conditions of the styrene-based resin composition, expandable styrene-based resin composition, and expandable styrene-based resin particles production method of the present disclosure, and the measurement methods of the physical properties of the obtained products can be carried out by appropriately referring to JP 2019-172828 A in addition to the disclosures in this specification. EXAMPLES

[0068] The present embodiment will be described below with reference to examples, but the present disclosure is not limited to these examples.

[0069] The methods for measuring and evaluating the various physical properties in the following Examples and Comparative Examples are as follows.

[0070] (Measurement of average carbon particle size D50 (μm) and laser scattering intensity (%)) (1) Sample solution preparation conditions (a) When the measurement target is expandable styrene resin particles A sample solution was prepared by dissolving and dispersing 500 mg of expandable styrene resin particles (sample) in 20 mL of a toluene solution of 0.1% (w / w) Span 80. Note that Span 80 is a nonionic surfactant.

[0071] (b) When the measurement target is carbon before mixing, i.e., the raw material carbon itself A sample solution was prepared by dissolving and dispersing 20 mg of carbon and 480 mg of styrene-based resin (A) in 20 mL of 0.1% (w / w) Span 80 toluene solution.

[0072] The above-mentioned dissolution / dispersion refers to a state in which the resin is dissolved and the carbon is dispersed.

[0073] (2) Ultrasonic irradiation Next, the sample solution was irradiated with ultrasonic waves under the following conditions in an ultrasonic cleaner to relax the aggregation of carbon. Equipment used: Ultrasonic cleaner, model USM, manufactured by AS ONE Corporation Oscillation frequency: 42kHz Irradiation time: 10 minutes Temperature: room temperature

[0074] (3) Particle size measurement conditions Measurement equipment: Malvern Laser Diffraction Particle Size Distribution Analyzer, Mastersizer 3000 Light source: 632.8nm red He-Ne laser and 470nm blue LED Dispersion unit: Wet dispersion unit, Hydro MV The analysis was carried out with the following settings, and the volume distribution was obtained and the D50 particle size of carbon in the sample was calculated by measurement and analysis using a laser diffraction and scattering method based on the Mie theory in accordance with ISO13320:2009 and JIS Z8825-1. Particle type: non-spherical Carbon refractive index: 2.42 Carbon Absorption Rate: 1.0 Dispersion medium: 0.1% (w / w) Span 80 in toluene Refractive index of dispersion medium: 1.49 Agitation speed in dispersion unit: 2500 rpm Analysis model: General purpose, single mode preserving Measurement temperature: room temperature

[0075] (4) Measurement procedure 120 mL of 0.1% (w / w) Span 80 toluene solution was poured into the dispersion unit, stirred at 2500 rpm, and stabilized. The light intensity measured by the central detector when 632.8 nm red He-Ne laser light was irradiated in the measurement cell without the sample solution sample and only the dispersion medium was taken as the transmitted light intensity Lb. Next, 2 mL of the ultrasonically treated sample solution was taken and added to the dispersion unit. The light intensity measured by the central detector when 632.8 nm red He-Ne laser light was irradiated 1 minute after the addition of the sample solution was taken as the transmitted light intensity Ls. At the same time, the particle size (D50) was measured. From the obtained Ls and Lb, the laser scattering intensity Ob of the sample solution was calculated using the following formula.

[0076] Ob = (1-Ls / Lb) x 100 (%)

[0077] The central detector is a detector located in front of and facing the output of the laser light, and the light detected here is a measure of the transmitted light that was not used for scattering. The laser scattering intensity is a measure of the amount of laser light lost when the laser of the analytical device is scattered by the sample.

[0078] (5) Calculation of laser scattering intensity per unit solution concentration of expandable styrene resin particles The laser scattering intensity per unit solution concentration of the expandable styrene-based resin particles was calculated using the following formula.

[0079] Laser scattering intensity per unit solution concentration of expandable styrene resin particles (sample) (% / (mg / ml)) = laser scattering intensity (Ob) / {sample weight (500 mg) / toluene amount (20 mL) × sample injection amount (2 mL) / total toluene amount in dispersion unit (120 mL + 2 mL)} The laser scattering intensity per unit solution concentration is the measured laser scattering intensity divided by the sample concentration in toluene. Because this measurement device requires measurement in solution, the sample concentration in the toluene solution is kept constant, and measurements are obtained for a constant sample amount.

[0080] (6) Calculation of laser scattering intensity per unit weight of carbon in expandable styrene resin particles The laser scattering intensity per unit weight of carbon contained in the expandable styrene-based resin particles (hereinafter abbreviated as "measurement subject") was calculated using the following formula.

[0081] Laser scattering intensity per unit weight of carbon in the measurement target {% / (mg / ml)} / weight% = Laser scattering intensity per unit solution concentration of the measurement target (% / (mg / ml)) / carbon content of the measurement target (weight%)

[0082] The state of dispersion of carbon can be evaluated by using the laser scattering intensity per unit solution concentration of carbon.

[0083] In addition, since the graphite dispersion state in the expandable styrene-based resin particles is determined by the graphite dispersion state in the styrene-based resin composition, the laser scattering intensity per carbon unit solution concentration of the expandable styrene-based resin particles and the laser scattering intensity per carbon unit solution concentration of the styrene-based resin composition (expandable styrene-based resin composition) are substantially identical.

[0084] The higher the laser scattering intensity per unit solution carbon concentration of the expandable styrene-based resin composition, the higher the heat insulating performance of the resulting styrene-based resin foamed molded article.

[0085] (Method for measuring the expansion ratio of pre-expanded particles) A sample of pre-expanded particles was taken in an amount of W (g) as a measurement sample, and this measurement sample was allowed to fall naturally into a measuring cylinder. The measuring cylinder was then struck to determine the apparent volume of the sample, V (cm 3 ) is constant, and its weight (g) and volume (cm 3 ) was measured, and the expansion ratio was calculated based on the following formula. Expansion ratio (cm 3 / g) = volume of measurement sample (V) / weight of measurement sample (W)

[0086] (Calculation of foaming ratio) A sample of 300 mm length × 300 mm width × 25 mm thickness was cut out from the styrene resin foam molded body in the same manner as in the case of the thermal conductivity measurement described later. The weight (g) of the sample was measured, and the length, width, and thickness were measured using a vernier caliper. The volume (cm) of the sample was calculated from each measured dimension. 3 ) was calculated, and the expansion ratio was calculated according to the following formula.

[0087] Expansion ratio (cm 3 / g) = sample volume (cm 3 ) / sample weight (g) Conventionally, the expansion ratio of styrene resin foam moldings is expressed as "times" in cm 3 / g".

[0088] (Measurement of thermal conductivity of styrene-based resin foam molded bodies) It is generally known that the higher the average temperature at which thermal conductivity is measured, the higher the thermal conductivity value, and it is necessary to determine the average temperature at which it is measured in order to compare thermal insulation. In this specification, the standard temperature of 23°C, as defined in JIS A9511:2006R, which is the standard for foamed plastic insulation materials, was adopted. A sample for measuring thermal conductivity was cut out from a styrene-based resin foam molded body, and the sample was left at 70°C for 4 days, and then left at 23°C for 24 hours, after which the thermal conductivity was measured.

[0089] More specifically, a sample measuring 300 mm in length × 300 mm in width × 25 mm in thickness was cut out from the styrene-based resin foam molded product. The sample was left to stand at 70° C. for 4 days and then at 23° C. for 24 hours, after which the thermal conductivity was measured at an average temperature of 23° C. and a temperature difference of 20° C. using a thermal conductivity measuring device (HC-074, manufactured by Eiko Seiki Co., Ltd.) by the heat flow meter method in accordance with JIS A1412-2:1999.

[0090] The raw materials used in the examples and comparative examples are shown below.

[0091] (styrene resin) (A) Styrene homopolymer [PS Japan Co., Ltd., 680] (carbon) (B) Graphite [flake graphite SGP-40B, manufactured by Marutoyo Foundry Co., Ltd.] (powder) Average particle size D50=5.8μm Laser scattering intensity per unit solution concentration of carbon (graphite) = 3.7%

[0092] (Brominated flame retardants) (C) 2,2-bis[4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl]propane [manufactured by Daiichi Kogyo Seiyaku Co., Ltd., SR-130, bromine content = 66% by weight] (Heat stabilizer) (D1) Tetrakis(2,2,6,6-tetramethylpiperidyloxycarbonyl)butane [ADEKA Corporation LA-57] (D2) Bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite [ADEKA Corporation, PEP-36] (Mixture of brominated flame retardants and stabilizers) (E) The brominated flame retardant (C), stabilizers (D1) and (D2) were mixed in a mixer to obtain a powder mixture (E) of the brominated flame retardant and stabilizers, with the weight ratio (weight %) of each material being (C):(D1):(D2) = 95:2:3 ((C) + (D1) + (D2) = 100% by weight).

[0093] (foaming agent) (F1) Normal pentane [SK Sangyo Co., Ltd.] (F2) Isopentane [SK Sangyo Co., Ltd.] (F3) Isobutane [Mitsui Chemicals, Inc.] (Additives) (G) Ethylenebisstearic acid amide

[0094] (Production Example 1) (Graphite Masterbatch (H)) The raw materials were fed into a Banbury mixer so that the total weight (A+B+G) of 49% by weight of styrene resin (A), 50% by weight of graphite (B), and 1% by weight of ethylene bisstearic acid amide (G) was 100% by weight, and the mixture was mixed at 5 kgf / cm 2 The mixture was kneaded for 20 minutes without heating or cooling under a load of 1000 g for 20 minutes. The resin temperature was measured and found to be 180°C. The strand-shaped resin was fed to a ruder and extruded at 250 kg / hr through a die with small holes attached to the tip. It was cooled and solidified in a water bath at 30°C and then cut to obtain master batch (H). The graphite content in master batch (H) was 50% by weight.

[0095] Example 1 [Preparation of expandable styrene resin particles] Styrene-based resin (A), graphite (B), and a mixture of bromine-based flame retardant and heat stabilizer (E) were fed by feeders to a tandem-type two-stage extruder in which a 40 mm diameter twin-screw extruder (first extruder) and a 90 mm diameter single-screw extruder (second extruder) were connected in series, and melt-kneaded at a set temperature of 190°C and a rotation speed of 167 rpm for the 40 mm diameter extruder. The ratio and amount of raw materials used were (A):(B):(E) = 89.5:4.5:6.0 by weight, and the total feed amount was 55.7 kg / h. From the middle of the 40 mm diameter extruder (first extruder), 4.7 parts by weight of mixed pentane [mixture of 80% by weight of normal pentane (F1) and 20% by weight of isopentane (F2)] was injected per 100 parts by weight of the melt of the resin mixture (styrene resin composition), and 2.3 parts by weight of isobutane (F3) was injected per 100 parts by weight of the styrene resin composition, and a total of 7.0 parts by weight of foaming agent was added, and the total supply amount of the resin mixture and the foaming agent was 60 kg / h. Then, it was supplied to a 90 mm diameter extruder (second extruder) through a continuation pipe set at 200 ° C.

[0096] In the first extruder for preparing the expandable styrene-based resin composition, the total supply amount of the resin mixture and the blowing agent, 60 kg / h, corresponds to the twin-screw extruder extrusion amount (kg / h), so Q / N is about 0.359 (60 / 167), which is 8.0 × 10 -6 ×D 3 is 0.512, and Q / N ≦ 8.0×10 -6 ×D 3 It met the following criteria.

[0097] The molten resin was cooled to a resin temperature of 160°C using a 90 mm diameter extruder (second extruder), and then extruded from a die having 60 small holes with a diameter of 0.65 mm and a land length of 5.0 mm attached to the tip of the second extruder set at 250°C into pressurized circulating water at a temperature of 62°C and a pressure of 1.1 MPa. The extruded molten resin was cut and pelletized using a rotating cutter with six blades that came into contact with the die, and transferred to a centrifugal dehydrator to obtain expandable styrene-based resin particles.

[0098] [Preparation of pre-expanded particles] The obtained expandable styrene resin particles were stored at 15°C for one week or more, and then 0.04 parts by weight of zinc stearate and 0.1 parts by weight of hydroxystearic acid triglyceride, which are external additives, were dry-blended with the expandable styrene resin particles. 250 g of the expandable styrene resin particles containing the external additives were placed in a pre-expander [batch-type pre-expander manufactured by Daikai Kogyo Co., Ltd.], and the pressure inside the can was set to 0.05 kg / cm. 2 ~0.15kg / cm 2 Then, water vapor at 0.10 MPa was introduced into the pre-expander to expand the mixture to an expansion ratio of 80 times, thereby obtaining pre-expanded particles.

[0099] [Preparation of styrene-based resin foam molded products] The obtained pre-expanded particles were cured at 30°C for 24 hours, and then filled into a mold for in-mold molding (length 400mm x width 400mm x thickness 50mm) attached to a polystyrene foam molding machine [KR-57, manufactured by Daisen Kogyo Co., Ltd.], and 0.06 MPa of water vapor was introduced to cause in-mold foaming, and then water was sprayed onto the mold to cool it. The styrene-based resin foam molded body was held in the mold until the pressure of the styrene-based resin foam molded body pressing the mold reached 0.01 MPa (gauge pressure), and then the styrene-based resin foam molded body was taken out to obtain a styrene-based resin foam molded body. The expansion ratio of the obtained styrene-based resin foam molded body was 80 times, and the thermal conductivity after standing at 70°C for 4 days was 29.9 mW / mK.

[0100] The various properties of the produced expandable styrene resin particles, pre-expanded particles and styrene resin foamed molded articles were measured and evaluated by the above-mentioned measuring and evaluating methods.

[0101] Example 2 The same procedure as in Example 1 was carried out except that the weight ratio of the raw materials was changed from (A):(B):(E)=89.5:4.5:6.0 to (A):(B):(E)=86.5:4.5:9.0, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0102] Comparative Example 1 The same procedure as in Example 1 was carried out except that the weight ratio of the raw materials was changed from (A):(B):(E)=89.5:4.5:6.0 to (A):(B):(E)=93.0:4.5:2.5, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0103] Comparative Example 2 The same procedure as in Example 1 was carried out except that the weight ratio of the raw materials was changed from (A):(B):(E)=89.5:4.5:6.0 to (A):(B):(E)=93.5:4.5:2.0, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0104] Comparative Example 3 The same procedure as in Example 1 was carried out except that the weight ratio of the raw materials was changed from (A):(B):(E)=89.5:4.5:6.0 to (A):(B):(E)=94.0:4.5:1.5, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0105] Comparative Example 4 The same procedure as in Example 1 was carried out except that the weight ratio of the raw materials was changed from (A):(B):(E)=89.5:4.5:6.0 to (A):(B):(E)=94.5:4.5:1.0, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0106] (Reference example 1) The styrene resin (A), graphite master batch (H), and mixture of bromine-based flame retardant and heat stabilizer (E) were fed by feeders to a tandem-type two-stage extruder in which a 40 mm diameter twin screw extruder (first extruder) and a 90 mm diameter single screw extruder (second extruder) were connected in series, and melt-kneaded at a set temperature of 190°C and a rotation speed of 167 rpm for the 40 mm diameter extruder. The ratio and amount of raw materials used were (A):(H):(E) = 88.5:9.0:2.5 by weight, and the total feed amount was 55.7 kg / h. From the middle of the 40 mm diameter extruder (first extruder), 4.7 parts by weight of mixed pentane [a mixture of 80% by weight of normal pentane (F1) and 20% by weight of isopentane (F2)] was injected per 100 parts by weight of the melt of the resin mixture (styrene-based resin composition), and 2.3 parts by weight of isobutane (F3) was injected per 100 parts by weight of the styrene-based resin composition, resulting in a total of 7.0 parts by weight of foaming agent being added. Then, the mixture was supplied to a 90 mm diameter extruder (second extruder) through a continuation pipe set at 200°C.

[0107] The subsequent operations were carried out in the same manner as in Example 1 to obtain expandable styrene-based resin particles, pre-expanded particles, and a styrene-based resin expansion molded article.

[0108] (Reference example 2) The same procedure as in Reference Example 1 was repeated except that the weight ratio of the raw materials was changed from (A):(H):(E)=88.5:9.0:2.5 to (A):(H):(E)=85.5:12.0:2.5, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0109] (Reference example 3) The same procedure as in Reference Example 1 was repeated except that the weight ratio of the raw materials was changed from (A):(H):(E)=88.5:9.0:2.5 to (A):(H):(E)=81.5:16.0:2.5, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0110] (Reference example 4) The same procedure as in Reference Example 1 was repeated except that the weight ratio of the raw materials was changed from (A):(H):(E)=88.5:9.0:2.5 to (A):(H):(E)=77.5:20.0:2.5, and expandable styrene-based resin particles, pre-expanded particles, and styrene-based resin foamed molded products were obtained.

[0111] For each of the Examples, Comparative Examples, and Reference Examples, the amount of graphite (B) used, the amount of the mixture (E) of the bromine-based flame retardant and stabilizer, the weight ratio thereof, the amount of the graphite master batch (H), the laser scattering intensity per unit weight of carbon in the expandable styrene-based resin particles, and the expansion ratio and thermal conductivity of the styrene-based resin foamed molded article are shown in Table 1. In addition, in Table 1, for the Reference Examples in which the graphite master batch (H) was used, the amount of graphite (B) used as the master batch (H) is also shown in parentheses. In addition, in Table 1, "laser scattering intensity per unit weight of carbon in the expandable styrene-based resin particles" is simply referred to as "laser scattering intensity per unit weight of carbon."

[0112] [Table 1]

[0113] From Table 1, it was suggested that the method described in the Examples had a laser scattering intensity per unit weight of carbon in the expandable styrene-based resin particles equivalent or greater than those of Reference Examples 1 to 4, which used a masterbatch, despite the fact that the method did not use a masterbatch, and that carbon was sufficiently dispersed. In other words, it was suggested that the production method of the present disclosure is a method capable of obtaining a styrene-based resin composition, expandable styrene-based resin particles, etc., of quality equivalent to or better than that of conventional methods at a low cost.

[0114] The upper and / or lower limit values ​​of the numerical ranges described in this specification can be arbitrarily combined to define a preferred range. For example, the upper and lower limit values ​​of the numerical ranges can be arbitrarily combined to define a preferred range, the upper limit values ​​of the numerical ranges can be arbitrarily combined to define a preferred range, and the lower limit values ​​of the numerical ranges can be arbitrarily combined to define a preferred range. In addition, in this application, a numerical range expressed using the symbol "~" includes the numerical values ​​described before and after the symbol "~" as the lower and upper limits, respectively.

[0115] Although the present embodiment has been described in detail above, the specific configuration is not limited to this embodiment, and even if there are design changes within the scope that does not deviate from the gist of this disclosure, they are included in this disclosure.

Claims

1. The process includes a step A of supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture, The carbon, the brominated flame retardant, and the stabilizer are fed in powder form to a multi-screw extruder; A method for producing a styrene-based resin composition, wherein a weight ratio of the carbon to the total amount of the brominated flame retardant and the stabilizer, carbon / (brominated flame retardant+stabilizer), is 1.4 or less.

2. The multi-screw extruder is a twin-screw extruder, The method for producing a styrene-based resin composition according to claim 1, wherein the Q / N of the twin-screw extruder is within the range of the following formula: Q / N≦8.0×10 -6 xD 3 (In the above formula, Q represents the twin-screw extruder extrusion rate (kg / hr), N represents the screw rotation speed (rpm), and D represents the twin-screw extruder barrel inner diameter (mm).)

3. The method for producing a styrene-based resin composition according to claim 1, wherein the carbon is at least one selected from the group consisting of graphite, graphene, carbon black, carbon nanotubes, activated carbon, and expanded graphite.

4. The process includes a step A of supplying a styrene-based resin, carbon, a bromine-based flame retardant, and a stabilizer to a multi-screw extruder and melt-kneading the mixture, The carbon, the brominated flame retardant, and the stabilizer are fed in powder form to a multi-screw extruder; A method for producing expandable styrene-based resin particles, wherein a weight ratio of the carbon to the total amount of the brominated flame retardant and the stabilizer, carbon / (brominated flame retardant+stabilizer), is 1.4 or less.

5. The multi-screw extruder is a twin-screw extruder, The method for producing expandable styrene-based resin particles according to claim 4, wherein the Q / N of the twin-screw extruder is within the range of the following formula: Q / N≦8.0×10 -6 xD 3 (In the above formula, Q represents the twin-screw extruder extrusion rate (kg / hr), N represents the screw rotation speed (rpm), and D represents the twin-screw extruder barrel inner diameter (mm).)

6. The method for producing expandable styrene-based resin particles according to claim 4, wherein the carbon is at least one selected from the group consisting of graphite, graphene, carbon black, carbon nanotubes, activated carbon, and expanded graphite.

7. 5. The method for producing expandable styrene-based resin particles according to claim 4, further comprising step B of adding a foaming agent to the styrene-based resin composition obtained in step A to obtain an expandable styrene-based resin composition, and step C of granulating the expandable styrene-based resin composition to obtain expandable styrene-based resin particles.

8. 5. The method for producing expandable styrene-based resin particles according to claim 4, comprising: a step D of granulating the styrene-based resin composition obtained in the step A to obtain styrene-based resin particles; and a step E of impregnating the styrene-based resin particles with a blowing agent to obtain expandable styrene-based resin particles.

9. A method for producing pre-expanded styrene resin particles, comprising expanding the expandable styrene resin particles obtained by the method for producing expandable styrene resin particles according to claim 4.

10. A method for producing a styrene-based resin foamed molded article, comprising molding the styrene-based resin pre-expanded particles obtained by the method for producing the styrene-based resin pre-expanded particles according to claim 9.

Citation Information

Patent Citations