Polyester-based resin composition and molding

A polyester resin composition with a viscosity modifier comprising a chain extension component and carrier resin enhances melt viscosity and strength, addressing the issues of recycling and transparency in polyester resin products.

JP2024142456APending Publication Date: 2024-10-11KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023054598
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Polyester resins experience a decrease in melt viscosity and strength upon recycling, and the addition of chain extenders can cause whitening and reduce transparency in molded products if not properly controlled.

Method used

A polyester resin composition is formulated by blending a crystalline polyester resin with a viscosity modifier containing a chain extension component and a carrier resin, where the chain extension component is a polymer with reactive functional groups and another copolymerizable vinyl compound, and the carrier resin improves granulation and dispersibility, with specific weight ratios and molecular weights to enhance melt viscosity and suppress whitening.

Benefits of technology

The composition maintains improved melt viscosity and strength while preventing whitening, ensuring high transparency and effective recycling of polyester resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142456000001
    Figure 2024142456000001
Patent Text Reader

Abstract

To provide a polyester-based resin composition which suppresses whitening while being blended with a chain extender.SOLUTION: A polyester-based resin composition contains a crystalline polyester-based resin (A), a viscosity modifier (B) containing a chain extender component (b1) and a carrier resin (b2), and an amorphous polyester-based resin (C). The chain extender component (b1) is a polymer containing a vinyl-based compound having a reactive functional group, and other copolymerizable vinyl-based compound as constituent monomers, and the carrier resin (b2) is a polymer containing a vinyl-based compound having a reactive functional group as a constituent monomer. In the viscosity modifier (B), a content of the chain extender component (b1) is 50 to 90 wt.%, a content of the carrier resin (b2) is 10 to 50 wt.%, and a content of the amorphous polyester-based resin (C) is 5 to 40 wt.% in the total of the crystalline polyester-based resin (A) and the amorphous polyester-based resin (C).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing a polyester resin, and a molded article thereof. [Background technology]

[0002] Thermoplastic polyester resins such as polyethylene terephthalate are excellent in transparency, mechanical properties, gas barrier properties, heat resistance, solvent resistance, economy, recyclability, etc., and are used in various molding applications such as bottles.

[0003] In recent years, with the growing interest in resource reuse and global environmental protection, recycling is becoming more and more common in various fields. In the case of polyester resins, efforts to recover waste materials once used and reuse them as recycled polyester resins have been attracting attention. However, polyester-based resins have a problem in that their melt viscosity decreases each time they are recycled, resulting in a decrease in strength.

[0004] One known method for improving the melt viscosity of a polyester resin is to add a chain extender to the polyester resin. For example, Patent Document 1 discloses, as a viscosity improver for polyester resins, a viscosity improver that contains a chain extender containing a reactive monomer such as glycidyl methacrylate, and a carrier resin. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2021 / 159009 Summary of the Invention [Problem to be solved by the invention]

[0006] By using a chain extender as described in Patent Document 1, the melt viscosity of the polyester resin can be improved. However, it has been found that when a chain extender is added, if the amount added is large or the heating temperature during molding is high, the polyester resin may whiten, and the transparency of the molded product may be impaired.

[0007] In view of the above-mentioned circumstances, an object of the present invention is to provide a polyester resin composition which contains a chain extender and yet suppresses whitening. [Means for solving the problem]

[0008] The present inventors have found that by blending a viscosity modifier (B) containing a specific chain extension component and a specific carrier resin with a crystalline polyester resin (A), and by blending a specific amount of an amorphous polyester resin (C), it is possible to provide a polyester resin composition that contains a chain extender but suppresses whitening, and have arrived at the present invention.

[0009] That is, the present invention relates to a crystalline polyester resin (A), A viscosity modifier (B) containing a chain extending component (b1) and a carrier resin (b2) that covers the (b1); and Contains an amorphous polyester resin (C), The chain extension component (b1) is a polymer containing, as constituent monomers, a vinyl compound having a reactive functional group and another copolymerizable vinyl compound, The carrier resin (b2) is a polymer containing a vinyl compound having a reactive functional group as a constituent monomer, In the viscosity improver (B), the content of the chain extension component (b1) is 50 to 90% by weight, and the content of the carrier resin (b2) is 10 to 50% by weight, The polyester resin composition has a content of the amorphous polyester resin (C) of 5 to 40% by weight based on the total weight of the crystalline polyester resin (A) and the amorphous polyester resin (C). Effect of the Invention

[0010] According to the present invention, it is possible to provide a polyester resin composition which contains a chain extender but which is inhibited from whitening. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail. The polyester resin composition according to this embodiment contains at least a crystalline polyester resin (A), a viscosity modifier (B), and an amorphous polyester resin (C).

[0012] <Crystalline polyester resin (A)> The crystalline polyester resin (A) refers to a thermoplastic polyester resin which can have crystalline portions in which the polymer molecules are regularly aligned when in a non-molten state. The polyester resin may be an aromatic polyester having a structure in which an aromatic dicarboxylic acid or an ester derivative thereof is linked to a diol component such as an aliphatic diol or an alicyclic diol by an ester reaction. The polyester resin may be obtained by polycondensing the above-mentioned components by a known method.

[0013] The aromatic dicarboxylic acid is not particularly limited, and examples thereof include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 3,3'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-diphenylisopropylidenedicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 2,5-anthracenedicarboxylic acid, 2,6-anthracenedicarboxylic acid, 4,4'-p-terphenylenedicarboxylic acid, and 2,5-pyridinedicarboxylic acid. Only one type of aromatic dicarboxylic acid may be used, or two or more types may be used in combination.

[0014] The aliphatic diol is not particularly limited, and examples thereof include ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 2-methyl-1,3-propanediol, diethylene glycol, triethylene glycol, etc. The alicyclic diol includes, for example, 1,4-cyclohexanedimethanol, etc. As the diol component, only one type may be used, or two or more types may be used in combination.

[0015] The polyester resin may have a structural component derived from a tri- or higher functional monomer, such as glycerin, trimethylolpropane, pentaerythritol, trimellitic acid, or pyromellitic acid.

[0016] The crystalline nature of a crystalline polyester resin can usually be confirmed by the presence of a clear endothermic peak in differential scanning calorimetry (DSC). Specifically, a clear endothermic peak refers to a peak whose half-width is, for example, within 15° when measured at a heating rate of 10°C / min in differential scanning calorimetry (DSC).

[0017] Specific examples of the crystalline polyester resin (A) are not particularly limited, but include, for example, polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, polybutylene naphthalate, poly-1,4-cyclohexylene dimethylene terephthalate, polyethylene-1,2-bis(phenoxy)ethane-4,4'-dicarboxylate, polyethylene isophthalate / terephthalate, polybutylene terephthalate / isophthalate, polybutylene terephthalate / decane dicarboxylate, polycyclohexane dimethylene terephthalate / isophthalate, polyester / polyether, etc. From the viewpoint of moldability and mechanical properties, polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, polybutylene naphthalate, poly-1,4-cyclohexylene dimethylene terephthalate, polyester / polyether are preferred, and polyethylene terephthalate and polybutylene terephthalate are particularly preferred.

[0018] The crystalline polyester resin (A) may be a recycled product. The melt viscosity of recycled crystalline polyester resin (A) is likely to be lower than that of unused resin. Therefore, it is very important to add a viscosity improver (B) to improve the melt viscosity. Here, the recycled polyester resin refers to a polyester resin that is formed by reusing a polyester resin composition or molded body that was once manufactured and then consumed and discarded, or a waste polyester resin discharged during the manufacturing process of a polyester resin or molded body, etc. The recycled product in this application also includes a mixture in which a recycled polyester resin is mixed with an unused, fresh polyester resin.

[0019] <Viscosity improver (B)> The polyester resin composition according to the present embodiment includes a viscosity modifier (B) containing a chain extension component (b1). By blending the viscosity modifier (B), the melt viscosity of the polyester resin composition can be improved, and the strength of a molded article made of the composition can be increased. The viscosity modifier (B) has excellent granulation properties during production, so it is preferable that the viscosity modifier (B) further includes a carrier resin (b2) that covers the chain extension component (b1).

[0020] (Chain extension component (b1)) The chain extension component (b1) is composed of a copolymer containing, as constituent monomers, a vinyl compound having a reactive functional group and another vinyl compound which is copolymerizable with the vinyl compound.

[0021] The chain extension component (b1) has a reactive functional group derived from the vinyl compound having the reactive functional group. When the crystalline polyester resin (A) and the viscosity modifier (B) are mixed by melt kneading or the like, the reactive functional group of the chain extension component (b1) can react with the terminal functional group (hydroxyl group or carboxyl group) of the crystalline polyester resin (A). This reaction can extend the molecular chain of the crystalline polyester resin (A). It is presumed that this mechanism improves the melt viscosity of the polyester resin composition and improves the strength of the molded product.

[0022] The reactive functional group is preferably a functional group that reacts with the terminal functional group of the crystalline polyester resin (A) to bond. Examples of such reactive functional groups include epoxy groups, hydroxyl groups, carboxyl groups, isocyanate groups, acid anhydride groups, and acyl chloride groups. Since it has good reactivity with the terminal functional group, the epoxy group is particularly preferred as the reactive functional group.

[0023] The vinyl compound having a reactive functional group is preferably a (meth)acrylic monomer having a reactive functional group. Examples of the (meth)acrylic monomer having a reactive functional group include a (meth)acrylic acid alkyl ester monomer having an alkyl group having 1 to 22 carbon atoms and a reactive functional group bonded to the alkyl group.

[0024] Specific examples of the (meth)acrylic monomer having an epoxy group as a reactive functional group include glycidyl acrylate and glycidyl methacrylate.

[0025] Specific examples of the (meth)acrylic monomer having a hydroxyl group as a reactive functional group include hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate.

[0026] Specific examples of the (meth)acrylic monomer having a carboxyl group as a reactive functional group include acrylic acid and methacrylic acid. The vinyl-based compound having a reactive functional group may be used alone or in combination of two or more kinds.

[0027] The content of the vinyl-based compound having a reactive functional group in the chain extension component (b1) can be appropriately set from the viewpoint of the effect of improving the melt viscosity, productivity, etc., but is preferably 5% by weight or more and 45% by weight or less, based on 100% by weight of the chain extension component (b1). The lower limit is more preferably 7% by weight or more, and even more preferably 10% by weight or more. When the lower limit is within the above range, the effect of improving the melt viscosity can be good. In addition, since the production of the chain extension component (b1) can be relatively easy, the upper limit of the content is more preferably 40% by weight or less, and even more preferably 30% by weight or less.

[0028] From the viewpoint of productivity, the chain extension component (b1) contains, as a constituent monomer, other vinyl compounds copolymerizable with the vinyl compounds having reactive functional groups. Examples of such other copolymerizable vinyl compounds include (meth)acrylic acid ester monomers, vinyl cyanide compounds, vinyl acetate, aromatic vinyl compounds, etc. These may be used alone or in combination of two or more.

[0029] The (meth)acrylic acid ester monomer is not particularly limited, and examples thereof include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 22 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; and (meth)acrylic acid esters having an alkyl group having 1 to 22 carbon atoms and an alkoxy group bonded to the alkyl group.

[0030] The number of carbon atoms in the alkyl group in the (meth)acrylic acid ester monomer is not particularly limited, but from the viewpoint of polymerizability, it is preferably 22 or less. Moreover, from the viewpoint of compatibility with the crystalline polyester resin (A), the number of carbon atoms in the alkyl group in the (meth)acrylic acid ester is more preferably 12 or less, and further preferably 8 or less. In particular, (meth)acrylic acid alkyl esters having an alkyl group with 1 to 4 carbon atoms are preferred, and methyl methacrylate and / or butyl acrylate are particularly preferred.

[0031] Examples of the vinyl cyanide compound include acrylonitrile and methacrylonitrile.

[0032] The aromatic vinyl compound is not particularly limited, but examples thereof include styrene, vinyltoluene, α-methylstyrene, 4-methylstyrene, 3-methylstyrene, 4-methoxystyrene, 4-ethylstyrene, 4-ethoxystyrene, 3,4-dimethylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chloro-3-methylstyrene, 3-(tert-butyl)styrene, 2,4-dichlorostyrene, 2,6-dichlorostyrene, and 1-vinylnaphthalene.

[0033] As the other copolymerizable vinyl compounds, it is preferable to use aromatic vinyl monomers, more preferably aromatic vinyl monomers having 8 to 10 carbon atoms, and particularly preferably styrene, because the transparency of the polyester resin composition is good.

[0034] According to a particularly preferred embodiment, the chain extension component (b1) preferably contains an epoxy group-containing (meth)acrylic acid ester monomer as the vinyl compound having a reactive functional group, and an aromatic vinyl compound and / or a (meth)acrylic acid ester monomer as the other copolymerizable vinyl compound.More preferably, the chain extension component (b1) preferably contains an epoxy group-containing (meth)acrylic acid ester monomer as the vinyl compound having a reactive functional group, and an aromatic vinyl compound as the other copolymerizable vinyl compound.

[0035] The chain extension component (b1) preferably has 2 or more and 10 or less reactive functional groups on average per polymer molecule of the chain extension component (b1). The lower limit may be 3 or more. The upper limit may be any of 10 or less, 8 or less, 7 or less, 6 or less, and 5 or less. When the number of reactive functional groups in the chain extension component (b1) is within the above range, gelation does not occur and the melt viscosity of the polyester resin composition can be suitably improved without impairing mechanical properties, heat resistance, rheological properties, etc.

[0036] From the viewpoint of the balance between the thermal stability and productivity of the chain extension component (b1) and the improvement of the melt viscosity of the polyester resin, the number average molecular weight of the chain extension component (b1) is preferably within the range of 2,000 to 10,000 in terms of polystyrene equivalent molecular weight measured by gel permeation chromatography (GPC). The lower limit of the number average molecular weight of the chain extension component (b1) is more preferably 3,000 or more, even more preferably 4,000 or more, and even more preferably 5,000 or more. The upper limit is more preferably 9,000 or less, and even more preferably 8,000 or less. In order to achieve such a number average molecular weight, it is preferable to use a chain transfer agent during polymerization to produce the chain extension component (b1).

[0037] The chain extension component (b1) is preferably a non-rubber polymer. A non-rubber polymer refers to a polymer that does not have a crosslinked structure between molecular chains of the polymer. When the chain extension component (b1) is a non-rubber polymer, the reaction between the reactive functional group of the chain extension component (b1) and the terminal functional group of the crystalline polyester resin (A) proceeds more efficiently, and the melt viscosity of the polyester resin composition is easily improved.

[0038] (Carrier resin (b2)) The carrier resin (b2) is a component that improves the granulation property during the production of the viscosity modifier (B). When the chain extension component (b1) is powdered alone, it becomes a fine powder and may be difficult to handle. Therefore, in order to obtain a powder of an appropriate particle size that is easy to handle, it is desirable to produce the carrier resin (b2) together with the chain extension component (b1) and isolate both of them. Furthermore, the presence of the carrier resin (b2) improves the dispersibility of the viscosity modifier (B) in the polyester resin composition, and the reaction between the crystalline polyester resin (A) and the chain extension component (b1) proceeds efficiently, making it possible to further improve the melt viscosity of the polyester resin composition.

[0039] The carrier resin (b2) is composed of a vinyl polymer and contains at least a vinyl compound having a reactive functional group as a monomer constituting the polymer, which can improve the dispersibility of the viscosity modifier (B) in the polyester resin composition, reduce the haze of a molded product (e.g., a sheet or film) composed of the polyester resin composition, and make the surface smooth.

[0040] Specific examples of the vinyl-based compound having a reactive functional group contained in the carrier resin (b2) are the same as those described above for the chain extension component (b1). Among them, it is preferable to use an epoxy group-containing (meth)acrylic acid ester monomer. The vinyl-based compound having a reactive functional group contained in the chain extension component (b1) and the vinyl-based compound having a reactive functional group contained in the carrier resin (b2) may be the same compound or different compounds.

[0041] The content of the vinyl-based compound having a reactive functional group in the carrier resin (b2) can be appropriately set from the viewpoints of improving the granulation property during the production of the viscosity modifier (B) and improving the dispersibility of the viscosity modifier (B) in the polyester resin composition, but it is preferable that the content is less than the content of the vinyl-based compound having a reactive functional group in the chain extension component (b1). Specifically, the content of the vinyl-based compound having a reactive functional group in the carrier resin (b2) is preferably 2.5% by weight or more and 10% by weight or less, based on 100% by weight of the carrier resin (b2). The lower limit is more preferably 3% by weight or more, even more preferably 4% by weight or more, and even more preferably 5% by weight or more. The upper limit of the content is more preferably 8% by weight or less, even more preferably 7% by weight or less, and even more preferably 6% by weight or less.

[0042] From the viewpoint of productivity, the carrier resin (b2) preferably contains, as a constituent monomer, a vinyl compound having a reactive functional group and other vinyl compounds copolymerizable with the compound. It is preferable to select the monomer constituting the carrier resin (b2) so as to have high compatibility with the crystalline polyester resin (A) according to the type of the crystalline polyester resin (A) used.

[0043] Other vinyl compounds constituting the carrier resin (b2) include (meth)acrylic acid ester monomers, vinyl cyanide compounds, vinyl acetate, aromatic vinyl compounds, etc. Specific examples of these are the same as those described above for the chain extension component (b1). Among these, it is preferable to use aromatic vinyl compounds and / or (meth)acrylic acid ester monomers. These may be used alone or in combination of two or more.

[0044] When an aromatic vinyl compound is used as another vinyl compound constituting the carrier resin (b2), the content of the aromatic vinyl compound in the carrier resin (b2) is preferably 10% by weight or more and 95% by weight or less, based on 100% by weight of the carrier resin (b2). The lower limit is more preferably 30% by weight or more, even more preferably 50% by weight or more, and even more preferably 60% by weight or more. The upper limit is more preferably 90% by weight or less, and even more preferably 80% by weight or less.

[0045] As another vinyl-based compound constituting the carrier resin (b2), it is preferable to use a vinyl-based compound that improves the compatibility with the crystalline polyester resin (A). Examples of such vinyl-based compounds include alkyl acrylates. Among them, methyl acrylate, butyl acrylate, and 4-hydroxyethyl acrylate are preferred.

[0046] The content of the acrylic acid alkyl ester in the carrier resin (b2) is preferably 10% by weight or more and 70% by weight or less, based on 100% by weight of the carrier resin (b2). The lower limit is more preferably 15% by weight or more, and even more preferably 20% by weight or more. The upper limit is more preferably 50% by weight or less, even more preferably 40% by weight or less, and even more preferably 30% by weight or less.

[0047] The number average molecular weight of the carrier resin (b2) is not particularly limited, but is preferably larger than the number average molecular weight of the chain extension component (b1) from the viewpoint of improving the granulation property during the production of the viscosity modifier (B). Specifically, the number average molecular weight of the carrier resin (b2) is preferably 100,000 or more in terms of polystyrene equivalent molecular weight measured by gel permeation chromatography (GPC). The upper limit is preferably 150,000 or less. Similarly to the chain-extending component (b1), the carrier resin (b2) is preferably a non-rubber polymer.

[0048] The viscosity improver (B) according to a preferred embodiment may contain a chain extension component (b1) and a carrier resin (b2). The relationship between the two polymers is not particularly limited, but from the viewpoint of improving granulation properties, it is preferable that the chain extension component (b1) constitutes a particle and at least a part of the carrier resin (b2) is located outside the particle. At least a part of the carrier resin (b2) may cover the outer surface of the particle. Also, a part of the carrier resin (b2) may be located outside the particle, and the rest may be impregnated inside the particle.

[0049] Furthermore, it is preferable that the chain extension component (b1) and the carrier resin (b2) are not chemically bonded to each other. In this case, the chain extension component (b1) and the carrier resin (b2) are considered to be present separately from each other in the polyester resin composition obtained by kneading the viscosity modifier (B) with the crystalline polyester resin (A).

[0050] In the viscosity improver (B), the proportion of the chain extender component (b1) is preferably 50 to 90% by weight. The lower limit is more preferably 60% by weight or more, even more preferably 70% by weight or more, and even more preferably 75% by weight or more. The upper limit may be 85% by weight or less.

[0051] In the viscosity improver (B), the proportion of the carrier resin (b2) is preferably 10 to 50% by weight. The lower limit is more preferably 15% by weight or more. The upper limit is more preferably 40% by weight or less, even more preferably 30% by weight or less, and even more preferably 25% by weight or less.

[0052] In the viscosity improver (B), the total proportion of the chain extender component (b1) and the carrier resin (b2) may be, for example, 70 to 100% by weight, and the lower limit may be any of 80% by weight or more, 90% by weight or more, 95% by weight or more, and 99% by weight or more.

[0053] In the polyester resin composition according to the present embodiment, the amount of the viscosity modifier (B) may be appropriately set, but is preferably 0.2 to 10 parts by weight per 100 parts by weight of the total of the crystalline polyester resin (A) and the amorphous polyester resin (C). The lower limit is more preferably 0.5 parts by weight or more, even more preferably 0.7 parts by weight or more, even more preferably 1 part by weight or more, particularly preferably 1.2 parts by weight or more, and most preferably 1.5 parts by weight or more. The upper limit may be any of 8 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, and 2 parts by weight or less.

[0054] (Method of producing viscosity improver (B)) The method for producing the viscosity modifier (B) can be a conventional polymerization method, and is not particularly limited. For example, bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc. can be adopted, but emulsion polymerization is preferred. When producing the chain extension component (b1), it is preferable to carry out polymerization in the presence of a chain transfer agent in order to control the molecular weight. In addition, when producing the chain extension component (b1) and the carrier resin (b2) continuously, first, a latex of the chain extension component (b1) is produced by emulsion polymerization, and then the monomer components for the carrier resin (b2), polymerization initiators, etc. are added to the latex to polymerize the monomer components.

[0055] The chain transfer agent that can be used in the production of the chain extension component (b1) is not particularly limited, and examples thereof include primary mercaptan chain transfer agents such as n-butyl mercaptan, n-octyl mercaptan, n-hexadecyl mercaptan, n-dodecyl mercaptan, and n-tetradecyl mercaptan; secondary mercaptan chain transfer agents such as sec-butyl mercaptan and sec-dodecyl mercaptan; tertiary mercaptan chain transfer agents such as t-dodecyl mercaptan; and mercaptan compounds, 2- Examples of the thioglycolic acid esters include ethylhexyl thioglycolate, ethylene glycol dithioglycolate, trimethylolpropane tris(thioglycolate), and pentaerythritol tetrakis(thioglycolate), thiophenol, tetraethyl thiuram disulfide, pentane phenylethane, acrolein, methacrolein, allyl alcohol, carbon tetrachloride, ethylene bromide, styrene oligomers such as α-methylstyrene dimer, and terpinolene. These may be used alone or in combination of two or more. The amount of the chain transfer agent used may be appropriately set according to the desired number average molecular weight of the chain extension component (b1).

[0056] The emulsifier (dispersant) that can be used in emulsion polymerization is not particularly limited, and may be an anionic surfactant, a nonionic surfactant, a cationic surfactant, an amphoteric surfactant, etc. Dispersants such as polyvinyl alcohol, alkyl-substituted cellulose, polyvinylpyrrolidone, and polyacrylic acid derivatives may also be used. Among the above emulsifiers, the anionic surfactant is not particularly limited, and examples thereof include the following compounds: fatty acid soaps such as potassium laurate, potassium coconut fatty acid, potassium myristate, potassium oleate, potassium oleate diethanolamine salt, sodium oleate, potassium palmitate, potassium stearate, sodium stearate, mixed fatty acid soda soap, semi-hardened beef tallow fatty acid soda soap, and castor oil potassium soap; alkoxyl compounds such as sodium dodecyl sulfate, sodium higher alcohol sulfate, triethanolamine dodecyl sulfate, ammonium dodecyl sulfate, sodium polyoxyethylene alkyl ether sulfate, triethanolamine polyoxyethylene alkyl ether sulfate, sodium polyoxyethylene alkyl phenyl ether sulfate, and sodium 2-ethylhexyl sulfate; Kyl sulfate ester salts; sodium alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; sodium dialkyl sulfosuccinates such as sodium di-2-ethylhexyl sulfosuccinate; sodium alkyl naphthalene sulfonates; sodium alkyl diphenyl ether disulfonates; potassium alkyl phosphate salts; phosphate ester salts such as sodium polyoxyethylene lauryl ether phosphate; sodium salts of naphthalene sulfonate formalin condensates; polycarboxylate type polymer anions; sodium acyl (beef tallow) methyl taurate; sodium acyl (coconut) methyl taurate; sodium cocoyl isethionate; sodium α-sulfofatty acid ester salts; sodium amido ether sulfonate; oleyl sarcosine; sodium lauroyl sarcosine; rosin acid soap, etc.

[0057] Furthermore, among the above-mentioned emulsifiers, the nonionic surfactant is not particularly limited, and examples thereof include the following compounds: polyoxyethylene alkyl allyl ethers or polyoxyethylene alkyl ethers, such as polyoxyethylene nonylphenyl ether, polyoxyethylene oleyl ether, and polyoxyethylene lauryl ether; polyoxyethylene sorbitan esters, such as polyoxyethylene sorbitan monolaurate and polyoxyethylene sorbitan monostearate; polyoxyethylene fatty acid esters, such as polyethylene glycol monolaurate, polyethylene glycol monostearate, and polyethylene glycol monooleate; and oxyethylene / oxypropylene block copolymers.

[0058] Furthermore, among the above emulsifiers, the cationic surfactant is not particularly limited, and examples thereof include the following compounds: alkylamine salts such as coconut amine acetate, stearyl amine acetate, octadecyl amine acetate, and tetradecyl amine acetate; and quaternary ammonium salts such as lauryl trimethyl ammonium chloride, stearyl trimethyl ammonium chloride, cetyl trimethyl ammonium chloride, distearyl dimethyl ammonium chloride, alkyl benzyl dimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, and behenyl trimethyl ammonium chloride.

[0059] Among the above emulsifiers, the amphoteric surfactant is not particularly limited, but examples thereof include the following compounds: alkyl betaines such as lauryl betaine, stearyl betaine, and dimethyl lauryl betaine; sodium lauryl diaminoethyl glycine; amido betaine; imidazoline; lauryl carboxymethyl hydroxyethyl imidazolinium betaine, and the like.

[0060] These emulsifiers (dispersants) may be used alone or in combination of two or more kinds.

[0061] When the emulsion polymerization method is employed, known polymerization initiators, such as 2,2'-azobisisobutyronitrile, hydrogen peroxide, potassium persulfate, and ammonium persulfate, can be used as thermal decomposition initiators.

[0062] Also usable are redox initiators using organic peroxides such as t-butyl peroxyisopropyl carbonate, paramenthane hydroperoxide, cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, and t-hexyl peroxide; inorganic peroxides such as hydrogen peroxide, potassium persulfate, and ammonium persulfate, in combination with a reducing agent such as sodium formaldehyde sulfoxylate and glucose, and a transition metal salt such as iron (II) sulfate, if necessary, a chelating agent such as disodium ethylenediaminetetraacetate, if necessary, and a phosphorus-containing compound such as sodium pyrophosphate, if necessary.

[0063] When a redox type initiator is used, polymerization can be carried out even at a low temperature where the peroxide does not substantially decompose thermally, and the polymerization temperature can be set in a wide range, which is preferable. Among them, it is preferable to use an organic peroxide such as cumene hydroperoxide, dicumyl peroxide, or t-butyl hydroperoxide as the redox type initiator. The amount of the initiator used, and the amount of the reducing agent, transition metal salt, chelating agent, etc. used when a redox type initiator is used, can be within a known range. A surfactant can be additionally used, which is also within a known range.

[0064] The solvent used during emulsion polymerization may be any solvent that allows the emulsion polymerization to proceed stably, and for example, water can be suitably used.

[0065] The temperature during emulsion polymerization is not particularly limited as long as the emulsifier is uniformly dissolved in the solvent, but is, for example, 40 to 75°C, preferably 45 to 73°C, and more preferably 49 to 71°C.

[0066] When the viscosity modifier (B) is produced by emulsion polymerization, for example, the viscosity modifier (B) can be coagulated by mixing the latex of the obtained viscosity modifier (B) with an acid such as hydrochloric acid or a divalent or higher metal salt such as calcium chloride, magnesium chloride, magnesium sulfate, aluminum chloride, calcium acetate, etc., and then heat-treated, dehydrated, washed, and dried according to a known method to separate the viscosity modifier (B) from the aqueous medium. The obtained viscosity modifier (B) is preferably washed with water and / or an organic solvent.

[0067] Also, a water-soluble organic solvent such as alcohol (e.g., methanol, ethanol, propanol, etc.) or acetone can be added to the latex of the viscosity modifier (B) to precipitate the viscosity modifier (B), and the viscosity modifier (B) can be separated from the solvent by centrifugation, filtration, etc., and then dried and isolated. Another method includes a method in which an organic solvent having a small water solubility such as methyl ethyl ketone is added to the latex of the viscosity modifier (B) to extract the viscosity modifier (B) in the latex into an organic solvent layer, and after separating the organic solvent layer, the viscosity modifier (B) is mixed with water or the like to precipitate the viscosity modifier (B).

[0068] Also, the latex of the viscosity modifier (B) can be directly powdered by spray drying. The obtained powder is preferably washed with water and / or an organic solvent. Alternatively, calcium chloride, magnesium chloride, magnesium sulfate, aluminum chloride, etc., preferably as a solution such as an aqueous solution, can be added to the obtained powder, and the powder can be re-dried as necessary, to obtain the same effect as the above washing.

[0069] <Amorphous polyester resin (C)> The polycarbonate resin composition according to the present embodiment contains an amorphous polyester resin (C). The amorphous polyester resin refers to a highly transparent polyester resin that does not substantially have a crystal structure. By blending the amorphous polyester resin (C), it is possible to obtain a highly transparent molded body by suppressing whitening of the molded body caused by blending the viscosity modifier (B) while achieving the viscosity improving effect achieved by blending the viscosity modifier (B).

[0070] The polyester resin may be an aromatic polyester having a structure in which an aromatic dicarboxylic acid or its ester derivative component is linked to a diol component such as an aliphatic diol or an alicyclic diol by an ester reaction. For example, the polyester resin may be one obtained by polycondensing the above-mentioned components by a known method.

[0071] The aromatic dicarboxylic acid is not particularly limited, and examples thereof include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 3,3'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-diphenylisopropylidenedicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 2,5-anthracenedicarboxylic acid, 2,6-anthracenedicarboxylic acid, 4,4'-p-terphenylenedicarboxylic acid, and 2,5-pyridinedicarboxylic acid. Only one type of aromatic dicarboxylic acid may be used, or two or more types may be used in combination.

[0072] The aliphatic diol is not particularly limited, and examples thereof include ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 2-methyl-1,3-propanediol, diethylene glycol, triethylene glycol, etc. The alicyclic diol includes, for example, 1,4-cyclohexanedimethanol, etc. As the diol component, only one type may be used, or two or more types may be used in combination.

[0073] The polyester resin may have a structural component derived from a tri- or higher functional monomer, such as glycerin, trimethylolpropane, pentaerythritol, trimellitic acid, or pyromellitic acid.

[0074] The fact that a polyester resin is amorphous can usually be confirmed by the absence of a clear endothermic peak in differential scanning calorimetry (DSC). Specifically, a clear endothermic peak refers to a peak whose half-width is, for example, within 15° when measured in differential scanning calorimetry (DSC) at a heating rate of 10° C. / min.

[0075] The amorphous polyester resin (C) is preferably a polymer formed by copolymerizing an aromatic dicarboxylic acid or an ester derivative component thereof as a main component, an aliphatic diol, and another dicarboxylic acid or an ester derivative component thereof or a diol that imparts amorphous properties.

[0076] Examples of the dicarboxylic acid that imparts amorphousness include aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, bis(4,4-carboxyphenyl)methane, anthracenedicarboxylic acid, and 4,4'-diphenyl ether carboxylic acid, and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 4,4'-dicyclohexyldicarboxylic acid.

[0077] Examples of the diol that imparts amorphousness include 1,4-cyclohexanedimethanol, propylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, decamethylene glycol, 4,4-dicyclohexylhydroxymethane, 4,4'-dicyclohexylhydroxypropane, bisphenol A ethylene oxide adduct diol, polyethylene oxide glycol, and polypropylene oxide glycol.

[0078] The amorphous polyester resin (C) is particularly preferably glycol-modified polyethylene terephthalate, which refers to a copolymer of terephthalic acid, ethylene glycol, and a glycol component other than ethylene glycol.

[0079] In the polyester resin composition according to the present embodiment, the content of the amorphous polyester resin (C) in the total of the crystalline polyester resin (A) and the amorphous polyester resin (C) is 5 to 40% by weight. If the content of the amorphous polyester resin (C) is less than 5% by weight, it is difficult to suppress whitening of the polyester resin composition. The lower limit is preferably 8% by weight or more, more preferably 10% by weight or more, and even more preferably 15% by weight or more. In addition, if the content of the amorphous polyester resin (C) exceeds 40% by weight, the chemical resistance and abrasion resistance, which are characteristics of the crystalline polyester resin (A), tend to decrease. The upper limit is preferably 35% by weight or less, more preferably 30% by weight or less, and even more preferably 25% by weight or less.

[0080] (Other resins) The polyester resin composition according to the present embodiment may or may not contain a thermoplastic resin other than the polyester resin. When a thermoplastic resin other than the polyester resin is contained, the thermoplastic resin is not particularly limited, and examples thereof include polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyvinyl acetate, polyurethane, polytetrafluoroethylene, ABS resin, AS resin, acrylic resin, polyacetal, polycarbonate, modified polyphenylene ether, polyamide, and cyclic polyolefin. The amount of the other thermoplastic resin is not particularly limited, and may be, for example, 0 to 100 parts by weight relative to 100 parts by weight of the total of the crystalline polyester resin (A) and the amorphous polyester resin (C). The upper limit may be 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, or 1 part by weight or less.

[0081] (Other additives) The polyester resin composition according to the present embodiment may appropriately contain additives that can be blended into general thermoplastic resin compositions. Such additives are not particularly limited, but examples thereof include flame retardants, flame retardant assistants, anti-dripping agents, reinforcing materials, fillers, antioxidants, pigments, dyes, conductivity imparting agents, hydrolysis inhibitors, thickeners, plasticizers, lubricants, UV absorbers, antistatic agents, flow improvers, release agents, compatibilizers, and heat stabilizers.

[0082] (Method of producing resin composition) The method for producing the polyester-based resin composition according to the present embodiment is not particularly limited, and a general method for producing a thermoplastic resin composition can be applied. For example, the raw materials are mixed using a Henschel mixer or a tumbler mixer, and then melt-kneaded to obtain the polyester-based resin composition. For the melt-kneading, a kneader such as a single-screw or twin-screw extruder, a Banbury mixer, a pressure kneader, or a mixing roll can be used. By such melt-kneading, pellets made of the polyester-based resin composition can be produced.

[0083] The polyester resin composition according to the present embodiment can be molded into a predetermined shape to obtain a molded article. The molding method is not particularly limited, and for example, injection molding, extrusion molding, blow molding, calendar molding, inflation molding, rotational molding, press molding, etc. can be used.

[0084] (Application) The polyester-based resin composition according to this embodiment and its molded article can be used in a wide range of applications including automotive applications such as cylinder head covers, engine covers, intake manifolds, radiator tanks, oil pans, accelerator pedals, canisters, fuel tubes, air brake tubes, exhaust gas tubes, hydrogen injectors, ducts, industrial fasteners, and door mirror stays; electrical and electronic applications such as coil bobbins, connectors, gears, sockets, switches, electric blanket coated wires, optical fiber cable coating materials, power tools, and electric wire ties; hydraulic and pneumatic connectors and tubes, bearings, covers, and housings. Examples of applications include, but are not limited to, mechanical applications such as bearings, pressure resistant hoses, and cable ties; building material applications such as curtain rail parts, aluminum sash corners, door rollers, handrails, curtain rollers, and door handles; sports and leisure applications such as sports shoe soles, ski and snowboard equipment, reels, and diving snorkels; packaging materials and container applications such as shrink wrapping film, food packaging film, alcoholic beverage bottles, and pesticide bottles; everyday applications such as toothbrushes, chair legs and armrests, combs, knives and forks; and medical applications such as medical catheters and pipes, medical packs, and sutures.

[0085] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] Crystalline polyester resin (A), A viscosity modifier (B) containing a chain extending component (b1) and a carrier resin (b2) that covers the (b1); and Contains an amorphous polyester resin (C), The chain extension component (b1) is a polymer containing, as constituent monomers, a vinyl compound having a reactive functional group and another copolymerizable vinyl compound, The carrier resin (b2) is a polymer containing a vinyl compound having a reactive functional group as a constituent monomer, In the viscosity improver (B), the content of the chain extension component (b1) is 50 to 90% by weight, and the content of the carrier resin (b2) is 10 to 50% by weight, A polyester resin composition, wherein the content of the amorphous polyester resin (C) is 5 to 40% by weight based on the total weight of the crystalline polyester resin (A) and the amorphous polyester resin (C). [Item 2] 2. The polyester resin composition according to item 1, wherein the amorphous polyester resin (C) comprises a glycol-modified polyethylene terephthalate. [Item 3] 3. The polyester resin composition according to item 1 or 2, wherein the crystalline polyester resin (A) is a recycled product. [Item 4] 4. The polyester resin composition according to any one of items 1 to 3, wherein the content of the vinyl compound having a reactive functional group contained in the carrier resin (b2) is 2.5 to 10% by weight in the carrier resin (b2). [Item 5] 5. The polyester resin composition according to any one of items 1 to 4, wherein the vinyl compound having a reactive functional group contained in the carrier resin (b2) is an epoxy group-containing (meth)acrylic acid ester monomer. [Item 6] 6. The polyester resin composition according to any one of items 1 to 5, wherein the carrier resin (b2) further contains an aromatic vinyl compound and / or a (meth)acrylic acid ester monomer as a constituent monomer. [Item 7] 7. The polyester resin composition according to any one of items 1 to 6, wherein the chain extension component (b1) has, on average, 2 to 10 reactive functional groups per polymer molecule. [Item 8] 8. The polyester resin composition according to any one of items 1 to 7, wherein the chain extension component (b1) has a number average molecular weight of 2,000 to 10,000. [Item 9] 9. The polyester resin composition according to any one of items 1 to 8, wherein the chain extension component (b1) contains an epoxy group-containing (meth)acrylic acid ester monomer as the vinyl compound having a reactive functional group, and contains an aromatic vinyl compound and / or a (meth)acrylic acid ester monomer as the other copolymerizable vinyl compound. [Item 10] 10. The polyester resin composition according to any one of items 1 to 9, wherein the content of the viscosity modifier (B) is 0.2 to 10 parts by weight per 100 parts by weight of the total of the crystalline polyester resin (A) and the amorphous polyester resin (C). [Item 11] 11. The polyester resin composition according to any one of items 1 to 10, wherein the crystalline polyester resin (A) contains polyethylene terephthalate and / or polybutylene terephthalate. [Item 12] 12. A molded article obtained by molding the polyester resin composition according to any one of items 1 to 11. EXAMPLES

[0086] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0087] (Synthesis Example 1) An example of the synthesis of the viscosity modifier (B) is shown below. First, the following components were added to a reactor: purified water (180 parts by weight), sodium formaldehyde sulfoxylate (1.5 parts by weight), EDTA (0.0075 parts by weight), ferrous sulfate heptahydrate (0.3 parts by weight), and t-butyl hydroperoxide (0.1 parts by weight).Then, the temperature was raised to 75° C. with stirring, and nitrogen was bubbled in for 30 minutes. The following monomer mixture was then added to the reactor over 150 minutes. Monomer mixture: styrene (70 parts by weight), glycidyl methacrylate (10 parts by weight), and n-octyl mercaptan (1.5 parts by weight). In addition, t-butyl hydroperoxide (0.1 parts by weight) was added sequentially to the reactor simultaneously with the addition of the monomer mixture. In addition, sodium formaldehyde sulfoxylate (0.2 parts by weight) and t-butyl hydroperoxide (0.03 parts by weight) were added to the reactor at any time during the addition of the monomer mixture. The mixture was then reacted until the conversion rate reached 90% or more, and then further reacted for 30 minutes. Next, the following monomer mixture was added to the reactor: butyl acrylate (5 parts by weight), glycidyl methacrylate (1 part by weight), and styrene (14 parts by weight). During the addition of the monomer mixture, sodium ethoxy alkylated alkyl phosphate ester (0.2 parts by weight) and t-butyl hydroperoxide (0.03 parts by weight) were added to the reactor at intervals. The reaction was then continued until the conversion reached 98% or more. Finally, a latex having a conversion rate of 98% and a particle size of 1100 angstroms was obtained. The obtained latex contained 80 parts by weight of the chain extension component (b1) and 20 parts by weight of the carrier resin (b2), the number average molecular weight of the chain extension component (b1) was 7,000, and the number average molecular weight of the carrier resin (b2) was 120,000. The average number of epoxy groups per polymer molecule of the chain extension component (b1) was 9. To recover the latex particles as a powder, the latex was added quickly to a 5% calcium chloride aqueous solution while stirring. The temperature was maintained at 70°C with steam. The temperature was then increased to 85°C to dehydrate the mixture. After drying, the powder was sieved through an 18 mesh screen. Viscosity modifier (B) was thus obtained.

[0088] Crystalline polyester resin (A): Polyethylene terephthalate copolymerized with isophthalic acid

[0089] Amorphous polyester resin (C) GN001: 1,4-cyclohexanedimethanol copolymerized polyethylene terephthalate, Eastman Chemical Company SI173: Neopentyl glycol copolymerized polyethylene terephthalate, manufactured by Toyobo

[0090] (Examples 1 to 3, Comparative Example 1) The viscosity improver (B) obtained in Synthesis Example 1 was kneaded and extruded at 270° C. using a single screw extruder (Brabender, 19 mm, L / D=20) to prepare pellets.

[0091] To investigate the crystallization characteristics, a sheet-shaped sample was prepared using a T-die extruder. First, a compound was prepared using the blending ratio in Table 1, and then heated to 270°C using a twin-screw extruder (Leistritz, 35 mm, L / D=17) to produce pellets. Next, the compound was heated to 270°C using a T-die of LABO PLASTOMILL (manufactured by Toyo Seiki Co., Ltd.) to form a film with a thickness of 200 μm. The IV value and crystallization behavior were evaluated using this film.

[0092] (IV value measurement) The measurements were carried out in accordance with JIS K 7367-5.

[0093] (DSC evaluation) The crystallization behavior of the prepared T-die sheet was measured using a DSC7020 (Hitachi High-Tech Science).

[0094] ·Crystallization temperature The crystallization temperature was determined as the temperature at which the crystallization peak rose when measured under the following conditions. Measurement conditions: The temperature was increased from 30°C to 290°C at a rate of 10°C / min.

[0095] Crystallization time The rise time of the crystallization peak measured under the following conditions was taken as the crystallization time. Measurement conditions: The temperature was raised from 30° C. to 290° C. at a rate of 20° C. / min, and after maintaining that temperature for 4 minutes, the temperature was lowered to 125° C. at a rate of 200° C. / min.

[0096] (Bleaching evaluation) The prepared T-die sheet was heated to 135°C, and after reaching 135°C, vacuum molding (mold: 10cm x 10cm x 1cm) was carried out to obtain a molded body. The whitening state of the molded body was visually evaluated according to the following criteria. 〇: Less than 20% of the bottom surface of the vacuum molded body (10cm x 10cm) is whitened △: 20-50% of the bottom surface of the vacuum molded body (10cm x 10cm) is whitened ×: More than 50% of the bottom surface of the vacuum molded product (10cm x 10cm) is whitened

[0097] [Table 1]

[0098] From Table 1, it can be seen that in Examples 1 to 3, in which the crystalline polyester resin (A) is blended with the viscosity modifier (B) and the amorphous polyester resin (C), the crystallization time is delayed and the crystallization temperature is increased, and whitening due to crystallization is suppressed, compared to Comparative Example 1, in which the amorphous polyester resin (C) is not blended.

Claims

1. A crystalline polyester resin (A), A viscosity improver (B) containing a chain extending component (b1) and a carrier resin (b2) that covers the (b1); and Contains an amorphous polyester resin (C), The chain extension component (b1) is a polymer containing, as constituent monomers, a vinyl-based compound having a reactive functional group and another copolymerizable vinyl-based compound, The carrier resin (b2) is a polymer containing a vinyl compound having a reactive functional group as a constituent monomer, In the viscosity modifier (B), the content of the chain extension component (b1) is 50 to 90% by weight, and the content of the carrier resin (b2) is 10 to 50% by weight. The content of the amorphous polyester resin (C) in the polyester resin composition is 5 to 40% by weight based on the total weight of the crystalline polyester resin (A) and the amorphous polyester resin (C).

2. The polyester resin composition according to claim 1 , wherein the amorphous polyester resin (C) comprises a glycol-modified polyethylene terephthalate.

3. The polyester resin composition according to claim 1 or 2, wherein the crystalline polyester resin (A) is a recycled product.

4. 3. The polyester resin composition according to claim 1, wherein the content of the vinyl compound having a reactive functional group contained in the carrier resin (b2) is 2.5 to 10% by weight in the carrier resin (b2).

5. 3. The polyester resin composition according to claim 1, wherein the vinyl compound having a reactive functional group contained in the carrier resin (b2) is an epoxy group-containing (meth)acrylic acid ester monomer.

6. 3. The polyester resin composition according to claim 1, wherein the carrier resin (b2) further contains an aromatic vinyl compound and / or a (meth)acrylic acid ester monomer as a constituent monomer.

7. 3. The polyester resin composition according to claim 1, wherein the chain extension component (b1) has an average of 2 to 10 reactive functional groups per polymer molecule.

8. 3. The polyester resin composition according to claim 1, wherein the chain-extending component (b1) has a number average molecular weight of 2,000 to 10,000.

9. 3. The polyester resin composition according to claim 1, wherein the chain extension component (b1) contains an epoxy group-containing (meth)acrylic acid ester monomer as the vinyl compound having a reactive functional group, and contains an aromatic vinyl compound and / or a (meth)acrylic acid ester monomer as the other copolymerizable vinyl compound.

10. The polyester resin composition according to claim 1 or 2, wherein the content of the viscosity modifier (B) is 0.2 to 10 parts by weight per 100 parts by weight of the total of the crystalline polyester resin (A) and the amorphous polyester resin (C).

11. 3. The polyester resin composition according to claim 1, wherein the crystalline polyester resin (A) comprises polyethylene terephthalate and / or polybutylene terephthalate.

12. A molded article obtained by molding the polyester resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polyester resin composition for odd-shaped extrusion and molded item obtained therefrom

    JP2003238777A

  • Polyester resin composition and mounting film

    JP2005226039A

  • Modifier for polyester resin and molded article produced by using the same

    JP2006124451A

  • Modifier for polyesters to improve melt viscosity

    JP2023512771A

  • Modifiers for polyesters that improve viscosity in melt

    WO2021159009A1