Acrylic rubbery polymer, method for producing acrylic rubbery polymer, thermoplastic resin composition and molded article
A graft copolymer using an acrylic rubbery polymer with controlled solubility and swelling properties addresses the balance of impact resistance, surface smoothness, and color development in thermoplastic resin compositions, enhancing their performance for outdoor use.
Patent Information
- Application Number
- JP2023054617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Existing thermoplastic resin compositions, such as ABS and ASA, lack an optimal balance of impact resistance, surface smoothness, and color development, particularly when exposed to outdoor conditions.
A graft copolymer is developed using an acrylic rubbery polymer with specific solubility and swelling characteristics in solvents like butyl benzoate and acetone, combined with a vinyl copolymer, to achieve a thermoplastic resin composition with improved impact resistance, surface smoothness, and color development.
The composition exhibits enhanced impact resistance, surface smoothness, and color development, making it suitable for outdoor applications.
Abstract
Description
[Technical field]
[0001] The present invention relates to an acrylic rubber polymer, and a thermoplastic resin composition containing a graft copolymer and a vinyl copolymer using the same. [Background technology]
[0002] ABS resin, which is made by polymerizing diene rubber polymers, aromatic vinyl monomers, vinyl cyanide monomers, methacrylic acid ester monomers, etc., has excellent impact resistance, moldability, and appearance, and is widely used in various applications such as office equipment, home appliances, and general goods. However, ABS resin has many chemically unstable double bonds in the main chain of the polymer, so it is easily deteriorated by ultraviolet rays and has poor weather resistance, making it difficult to use outdoors. For this reason, a method of using saturated rubber polymers that do not have double bonds in the main chain has been proposed, and ASA resins using acrylic rubber are well known as a representative example and are widely used mainly for vehicle applications.
[0003] Patent Document 1 proposes a resin composition in which an organic silicone oil is added to a composition using a specific acrylic rubber and / or silicone rubber as a method for improving impact resistance, color development, weather resistance, rigidity, heat resistance and processability.
[0004] Patent Document 2 proposes an acrylic rubber-reinforced copolymer resin obtained by polymerizing vinyl monomers containing an aromatic vinyl compound and a vinyl cyanide compound in the presence of an acrylic rubber polymer obtained by emulsion polymerization using an emulsifier containing an alkylsulfonate and a rosinate, as a method for improving vibration welding, hot plate welding properties, and lamp brightness after vapor deposition.
[0005] Patent Document 3 proposes a thermoplastic resin composition using a total of four types of copolymers, including two types of graft copolymers having specific structures and two types of copolymers having specific structures, as a method for improving the balance of impact resistance, heat resistance, surface smoothness, weather resistance, and color development.
[0006] Patent Document 4 proposes a thermoplastic resin composition using a graft copolymer (B) made of a rubbery polymer (A) containing a (meth)acrylic acid ester having a specific crosslinking degree and particle size, a crosslinking agent, and a specific hydrophobic substance, a graft copolymer (E) made of a rubbery polymer (C) having a specific particle size, and another thermoplastic resin (E), as a method for improving impact properties, low-temperature impact resistance, color development, gloss, molded appearance, weather resistance, and the molding speed dependency of molded appearance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2001-031830 A [Patent Document 2] JP 2006-131677 A [Patent Document 3] JP 2016-003284 A [Patent Document 4] JP 2019-137751 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, all of these techniques have been insufficient in terms of the balance between impact resistance, surface smoothness, and color development in the thermoplastic resin composition.
[0009] The present invention aims to solve the problems in the conventional art described above, that is, to provide a thermoplastic resin composition having good impact resistance, surface smoothness and color developability. [Means for solving the problem]
[0010] Means for Solving the Problems The present inventors have conducted extensive research in order to achieve the above object, and have discovered that by preparing a graft copolymer using an acrylic rubber polymer that satisfies specific conditions, a thermoplastic resin composition having good impact resistance, surface smoothness and color development properties can be obtained in a thermoplastic resin composition in which a graft copolymer containing an acrylic rubber polymer is dispersed in a vinyl copolymer, thereby arriving at the present invention.
[0011] That is, one aspect of the present invention is as follows. [1] An acrylic rubber polymer (A) obtained by copolymerizing an acrylic acid ester monomer (a) and a polyfunctional monomer (b), An acrylic rubber-based polymer (A) comprising a component (I) that is insoluble in butyl benzoate when immersed in butyl benzoate for 18 hours, the swelling degree of the butyl benzoate-insoluble component (I) being defined by the following formula (1) being (d1), and further comprising a component (II) that dissolves in acetone when immersed in acetone for 18 hours, the acrylic rubber-based polymer (A) being characterized in that (d1) and (d2) satisfy the following formulas (2) and (3), where (d1) and (d2) are the proportion of the acetone-soluble component (II) when the acrylic rubber-based polymer (A) is taken as 100% by mass. (d1)=(x) / (y) (1) ((x): weight of (A) swollen with butyl benzoate, (y): weight of (A) after drying) 15<(d1)<25 (2) 3.0≦(d2(mass%))≦8.0 (3) [2] The acrylic rubber polymer (A) according to [1], characterized in that it contains a component (III) that is insoluble in acetone when immersed in acetone for 18 hours, and the swelling degrees (d1) and (d3) of the butyl benzoate insoluble component (I) satisfy the following formula (5), where the swelling degree of the acetone-insoluble component (III) in the acrylic rubber polymer (A) defined by the following formula (4) is (d3): (d3)=(z) / (w) (4) ((z): weight of (A) swollen with acetone, (w): weight of (A) after drying) 1.6≦(d1 / d3)≦2.5 (5) [3] The acrylic rubber polymer (A) contains a component (IV) that dissolves in butyl benzoate when immersed in butyl benzoate for 18 hours, and the acrylic rubber polymer (A) is taken as 100% by mass, and the content ratio (d4) of the butyl benzoate soluble component (IV) is 4 to 12% by mass relative to 100% by mass of the acrylic rubber polymer (A), and the difference (d4-d2) between the content ratio (d4) and the content ratio (d2) of the acetone soluble component (II) when the acrylic rubber polymer (A) is taken as 100% by mass is 5% by mass or less. [1] or [2] The acrylic rubber polymer (A) according to the present invention. [4] The thermoplastic resin composition according to any one of [1] to [3], characterized in that the acetone-soluble portion (II) in the acrylic rubber polymer (A) has a weight average molecular weight (M1 (g / mol)) in terms of styrene of 30,000≦(M1)≦60,000. [5] A method for producing an acrylic rubber polymer (A), comprising emulsion-polymerizing 97 to 99.5 mass% of an acrylic acid ester monomer (a) and 0.5 to 3 mass% of a polyfunctional monomer (b) in the presence of at least one emulsifier (d) selected from the group consisting of a sulfate ester emulsifier having an ethylene oxide added structure in its molecular structure and having only one anionic functional group, and a sulfosuccinic acid emulsifier having an ethylene oxide added structure in its molecular structure and having two anionic functional groups, and a carboxylic acid emulsifier (e) having only one anionic functional group. [6] The method for producing the acrylic rubber polymer (A) according to [5], wherein the emulsifier (d) contains a polyoxyethylene alkyl ether sulfate or a polyoxyethylene alkyl sulfosuccinate. [7] The method for producing the acrylic rubber polymer (A) according to [5] or [6], wherein the carboxylic acid emulsifier (e) contains a disproportionated rosin acid salt. [8] The method for producing an acrylic rubber polymer (A) according to any one of [5] to [7], characterized in that the ratio of the amount of the emulsifier (d) to the amount of the carboxylic acid emulsifier (e) used (amount of (d) used / amount of (e) used) is 0.1 to 0.4. [9] A method for producing a graft copolymer (B) obtained by graft polymerizing a monomer mixture (c) containing an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of the acrylic rubber polymer (A) according to any one of [1] to [4].
[10] A thermoplastic resin composition comprising a graft copolymer (B) obtained by graft polymerization of a monomer mixture (c) containing an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of the acrylic rubber polymer (A) according to any one of [1] to [4], and a vinyl copolymer (C).
[11] A molded article obtained by molding the thermoplastic resin composition according to
[10] . Effect of the Invention
[0012] The thermoplastic resin composition containing a graft copolymer using the acrylic rubber polymer of the present invention and a vinyl copolymer can have good impact resistance, surface smoothness and color development when molded. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The acrylic rubber polymer of the present invention is obtained by copolymerizing an acrylic acid ester monomer (a) and a polyfunctional monomer (b) described below.
[0014] The acrylic ester monomer (a) constituting the acrylic rubber polymer (A) is preferably one having an alkyl group having 1 to 10 carbon atoms, such as methyl acrylate, ethyl acrylate, n-butyl acrylate, t-butyl acrylate, and octyl acrylate. Two or more of these may be used. Among these, n-butyl acrylate is preferred.
[0015] The polyfunctional monomer (b) constituting the acrylic rubber polymer (A) is not particularly limited as long as it has two or more functional groups, and examples of the functional group include groups having a carbon-carbon double bond such as an allyl group and a (meth)acryloyl group. Examples of the polyfunctional monomer (b) include allyl compounds such as allyl acrylate, allyl methacrylate, diallyl maleate, triallyl cyanurate, and triallyl isocyanurate, and di(meth)acrylic acid ester compounds such as divinylbenzene, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, and propylene glycol dimethacrylate. Two or more of these may be used. Among these, allyl methacrylate is preferred.
[0016] The acrylic rubber polymer (A) in the present invention is obtained by copolymerizing 97 to 99.5% by mass of the acrylic acid ester monomer (a) and 0.5 to 3% by mass of the polyfunctional monomer (b) with respect to the total of 100% by mass of the acrylic acid ester monomer (a) and the polyfunctional monomer (b). When the acrylic acid ester monomer (a) is less than 97% by mass and the polyfunctional monomer (b) is more than 3% by mass, the degree of crosslinking of the acrylic rubber polymer (A) described later increases and the swelling degree of the butyl benzoate insoluble matter (I) decreases. As a result, the acrylic rubber polymer (A) hardens, and when stress is applied, the stress is concentrated in the part with a small molecular weight between crosslink points, and the molecular chain breaks, resulting in a decrease in the impact resistance of the molded product. It is preferable that the acrylic acid ester monomer (a) is 98% by mass or more and the polyfunctional monomer (b) is 2% by mass or less, and it is more preferable that the acrylic acid ester monomer (a) is more than 98.5% by mass and the polyfunctional monomer (b) is less than 1.5% by mass.
[0017] When the acrylic acid ester monomer (a) is more than 99.5% by mass and the polyfunctional monomer (b) is less than 0.5% by mass, the swelling degree of the butyl benzoate insoluble matter (I) described later increases, and the acetone soluble matter (II) increases. As a result, the particles of the graft copolymer (B) tend to have an aggregated structure, and the non-crosslinked molecular chains are eluted into the thermoplastic resin composition, resulting in a decrease in surface smoothness. The acrylic acid ester monomer (a) is preferably 99.6% by mass or less, more preferably 99.2% by mass or less. The polyfunctional monomer (b) is preferably 0.6% by mass or more, more preferably 0.8% by mass or more.
[0018] In the present invention, the volume average particle size of the acrylic rubber polymer (A) is not particularly limited, but from the viewpoint of impact resistance and surface smoothness when a thermoplastic resin composition containing a graft copolymer using the acrylic rubber polymer (A) and a vinyl copolymer is molded, it is preferably in the range of 0.05 to 1 μm.
[0019] The volume average particle size of the acrylic rubber polymer (A) can be adjusted to a desired range by, for example, the amounts of water, emulsifier, and polymerization initiator used in the polymerization. It may also be adjusted to a desired range by enlarging the particle size by adding an aqueous solution of an acid such as acetic acid, phosphoric acid, or sulfuric acid, or an acid group-containing latex. Here, the acid group-containing latex is a latex made of an unsaturated acid monomer and an unsaturated carboxylic acid alkyl ester monomer.
[0020] The volume average particle size of the acrylic rubber polymer (A) can be measured by dispersing the acrylic rubber polymer (A) latex in water and using a laser scattering diffraction particle size distribution measuring device.
[0021] The acrylic rubber polymer (A) of the present invention must have an appropriate crosslinking in order to obtain excellent impact resistance, surface smoothness and color development when a thermoplastic resin composition containing a graft copolymer and a vinyl copolymer using the acrylic rubber polymer (A) is molded. In the present invention, the degree of crosslinking of the acrylic rubber polymer (A) is expressed by the swelling degree in two types of solvents with different solubilities of the acrylic rubber polymer (A) and the content ratio of the soluble matter in each solvent. In the present invention, butyl benzoate and acetone are used as solvents to express the appropriate degree of crosslinking of the rubber polymer.
[0022] The acrylic rubber polymer (A) of the present invention contains a component (I) that is not dissolved in butyl benzoate when immersed in butyl benzoate for 18 hours, and the swelling degree (d1) of the butyl benzoate insoluble component (I) is 15 to 25 times. If the swelling degree (d1) of the butyl benzoate insoluble component (I) is 15 times or more, the impact resistance of the thermoplastic resin composition can be maintained while the surface smoothness can be further improved, and if it is 25 times or less, the impact resistance can be further improved while the color development and surface smoothness of the thermoplastic resin composition are maintained.
[0023] The swelling degree (d1) of the butyl benzoate insoluble portion (I) of the acrylic rubber polymer (A) can be determined by the following method. First, in the case of the acrylic rubber polymer (A) latex, the latex and a 10% by mass concentration aqueous calcium chloride solution are added to methanol, and then the solid of the acrylic rubber polymer (A) is obtained by dehydrating and washing. The obtained solid of the acrylic rubber polymer (A) is vacuum dried at 80°C for 3 hours, and then a predetermined amount is impregnated with butyl benzoate for 18 hours, and the weight (x) of the swollen sample of the butyl benzoate insoluble portion (I) is measured. Since the boiling point of butyl benzoate is high at about 250°C, the swollen sample is impregnated with acetone for more than 1 hour, and this operation is repeated three times while exchanging the acetone, thereby replacing the butyl benzoate with acetone. Next, the sample is vacuum dried at 80°C for 3 hours, and the weight (y) of the dried sample of the butyl benzoate insoluble portion (I) is measured. The degree of swelling (d1) is calculated from the weight of the swollen sample (x) and the weight of the sample after drying (y) according to the following formula (1). The swelling degree of the butyl benzoate insoluble fraction (I) (d1) = (x) / (y) (1).
[0024] It is generally known that the affinity between a solvent and a polymer is higher when the distance (HSP distance) between the three-dimensional vectors of the Hansen Solubility Parameters (HSP values) of the solvent and polymer is closer, and the higher the affinity, the more the polymer dissolves. In cases where the polymer is not dissolved due to the constraints of crosslinking, such as rubber, it tends to swell, and if a solvent with extremely high affinity is used, there is a possibility that the parts with less crosslinking will dissolve. In the present invention, the swelling degree in various solvents was tested for the purpose of evaluating an acrylic rubber polymer (A) that is convenient for providing both impact resistance, surface smoothness, and color development properties of a thermoplastic resin composition, and butyl benzoate was found to be a suitable solvent.
[0025] Butyl benzoate has a very high affinity for the acrylic rubber polymer (A) of the present invention, and can penetrate into parts of the acrylic rubber polymer (A) with a high degree of crosslinking. Therefore, the swelling degree (d1) of the butyl benzoate-insoluble matter (I) in the acrylic rubber polymer (A) is very sensitive to the degree of crosslinking.
[0026] On the other hand, in commonly used solvents such as toluene and 2-butanone (methyl ethyl ketone), although there were some numerical differences in the swelling degree of the acrylic rubber polymer (A) in the solvent, no systematic ranking was observed in the physical properties such as impact resistance, surface smoothness and color development of the thermoplastic resin composition. Therefore, it can be said that the swelling degree (d1) of the butyl benzoate insoluble matter (I) of the acrylic rubber polymer (A) is very useful for evaluating the acrylic rubber polymer (A) which is convenient for combining the impact resistance, surface smoothness and color development of the thermoplastic resin composition containing the acrylic rubber polymer (A).
[0027] The acrylic rubber polymer (A) of the present invention contains a component (II) that dissolves in acetone when immersed in acetone for 18 hours, and the content ratio (d2 (mass%)) of the acetone-soluble component (II) when the acrylic rubber polymer (A) is 100 mass% is 3.0 to 8.0 mass%. The acetone-soluble component (II) in the acrylic rubber polymer (A) mainly contains a linear polymer of an acrylic acid ester monomer that is not crosslinked, and this linear polymer dissolves when compounded as a thermoplastic resin composition, which causes the surface smoothness of the thermoplastic resin composition to be impaired. Therefore, if the content ratio (d2) of the acetone-soluble component (II) is 8.0 mass% or less with respect to 100 mass% of the acrylic rubber polymer (A), the surface smoothness can be further improved while maintaining the impact resistance of the thermoplastic resin composition, and if it is 3.0 mass% or more, the impact resistance can be further improved while maintaining the color development and surface smoothness when the thermoplastic resin composition is molded.
[0028] The content (d2) of the acetone soluble matter (II) in the acrylic rubber polymer (A) can be determined by the following method. First, in the case of the acrylic rubber polymer (A) latex, the latex and a 10% by mass calcium chloride aqueous solution are added to methanol, and then the acrylic rubber polymer (A) solid is obtained by dehydration and washing. The obtained solid acrylic rubber polymer (A) is vacuum dried at 80°C for 3 hours, and then a predetermined amount is impregnated in acetone for 18 hours. Next, the acetone insoluble matter is vacuum dried at 80°C for 3 hours, and the weight (n1) of the sample after drying is measured. The content (d2) of the acetone soluble matter (II) is calculated from the weight (m1) of the sample and the weight (n1) of the sample after drying according to the following formula. Acetone soluble matter (II) content (d2.%) = (([m1] - [n1]) / [m1]) × 100.
[0029] The acrylic rubber polymer (A) of the present invention contains a component (III) that is not dissolved in acetone when immersed in acetone for 18 hours, and the ratio (d1 / d3) of the swelling degree (d1) of the butyl benzoate insoluble component (I) in the acrylic rubber polymer (A) to the swelling degree (d3) of the acetone insoluble component (III) in the acrylic rubber polymer (A) is preferably 1.6 to 2.5. If this ratio (d1 / d3) is 1.6 or more, the surface smoothness and coloring property when the thermoplastic resin composition is molded can be further improved while maintaining the impact resistance of the thermoplastic resin composition. On the other hand, if this ratio (d1 / d3) is 2.5 or less, the impact resistance can be further improved while maintaining the surface smoothness and coloring property of the thermoplastic resin composition.
[0030] The swelling degree (d1) of the butyl benzoate insoluble matter (I) in the acrylic rubber polymer (A) varies greatly depending on the degree of crosslinking, as described above. On the other hand, since acetone has a large HSP distance with respect to the acrylic rubber polymer (A), acetone penetrates only into the less crosslinked parts of the acrylic rubber polymer (A). Therefore, the swelling degree (d3) of the acetone insoluble matter (III) in the acrylic rubber polymer (A) indicates the proportion of parts with a low degree of crosslinking. The parts with a low degree of crosslinking are soft and therefore advantageous for impact resistance, but the graft copolymer (B) described later is likely to form an aggregated structure in the thermoplastic resin composition, and the presence of such coarse particles impairs surface smoothness and color development.
[0031] For this reason, the ratio (d1 / d3) of the swelling degree (d1) of the butyl benzoate insoluble matter (I) in the acrylic rubber polymer (A) to the swelling degree (d3) of the acetone insoluble matter (III) in the acrylic rubber polymer (A) is a parameter that indicates the balance between the highly crosslinked and less crosslinked parts of the acrylic rubber polymer (A), and by controlling this parameter within a certain range, the thermoplastic resin composition can achieve high levels of impact resistance, surface smoothness and color development.
[0032] The swelling degree (d3) of the acetone insoluble portion (III) of the acrylic rubber polymer (A) can be determined by the following method. First, in the case of the acrylic rubber polymer (A) latex, the latex and a 10% by mass concentration aqueous calcium chloride solution are added to methanol, and then the solid of the acrylic rubber polymer (A) is obtained by dehydration and washing. The obtained solid of the acrylic rubber polymer (A) is vacuum dried at 80°C for 3 hours, and then a predetermined amount is impregnated with acetone for 18 hours, and the weight (z) of the sample in which the acetone insoluble portion (III) has swollen is measured. Next, after vacuum drying at 80°C for 3 hours, the weight (w) of the sample after drying of the acetone insoluble portion (III) is measured. The swelling degree (d3) is calculated from the weight (z) of the swollen sample and the weight (w) of the sample after drying according to the following formula. The degree of swelling of the acetone insoluble fraction (III) ((d3) / times) = (z) / (w).
[0033] The acrylic rubber-based polymer (A) of the present invention contains a component (IV) that dissolves in butyl benzoate when immersed in butyl benzoate for 18 hours, and when the content ratio of the butyl benzoate-soluble component (IV) when the acrylic rubber-based polymer (A) is taken as 100% by mass is taken as (d4 (mass%)), the content ratio (d4) is 4 to 12 mass% relative to 100% by mass of the acrylic rubber-based polymer (A), and the difference (d4-d2) between the content ratio (d2) of the acetone-soluble component (II) in the acrylic rubber-based polymer (A) when the acrylic rubber-based polymer (A) is taken as 100% by mass is preferably 5 mass% or less relative to 100% by mass of the acrylic rubber-based polymer (A).
[0034] As described above, butyl benzoate has a very high affinity for the acrylic rubber polymer (A) of the present invention, so the content (d4) of the butyl benzoate soluble matter (IV) includes a portion of the low-crosslinked acrylic rubber polymer (A) in addition to the linear polymer of the non-crosslinked acrylic ester monomer. Since the acetone soluble matter (II) in the acrylic rubber polymer (A) is mainly the linear polymer of the non-crosslinked acrylic ester monomer, (d4-d2) indicates the content of a portion of the low-crosslinked acrylic rubber polymer (A).
[0035] Some of the acrylic rubber-based polymers (A) with a low degree of crosslinking are soft rubbers, which are advantageous in terms of impact resistance, but the graft copolymer (B) described later is likely to form an aggregated structure in the thermoplastic resin composition, and the presence of such coarse particles impairs surface smoothness and color development. If the content ratio (d4) of the soluble matter (IV) of butyl benzoate is 4% by mass or more relative to 100% by mass of the acrylic rubber-based polymer (A), the impact resistance of the thermoplastic resin composition can be further improved while maintaining the surface smoothness, and if it is 12% by mass or less, the surface smoothness of the thermoplastic resin composition can be further improved while maintaining the impact resistance.
[0036] The content (d4) of the butyl benzoate soluble matter (IV) in the acrylic rubber polymer (A) can be determined by the following method. First, in the case of the acrylic rubber polymer (A) latex, the latex and a 10% by mass concentration aqueous calcium chloride solution are added to methanol, and then the solid of the acrylic rubber polymer (A) is obtained by dehydration and washing. The obtained solid of the acrylic rubber polymer (A) is vacuum dried at 80°C for 3 hours, and then a predetermined amount (m2) is impregnated with butyl benzoate for 18 hours. Since the boiling point of butyl benzoate is high at about 250°C, the sample in which the butyl benzoate insoluble matter has swollen is impregnated with acetone for more than 1 hour. This operation is repeated three times while exchanging the acetone, so that the butyl benzoate is replaced with acetone. Next, the sample is vacuum dried at 80°C for 3 hours, and the weight (n2) of the sample after drying of the butyl benzoate insoluble matter is measured. The content (d4) of the butyl benzoate soluble matter (IV) is calculated from the weight (m2) of the sample and the weight (n2) of the sample after drying according to the following formula. Content ratio of butyl benzoate soluble content (IV) ((d2) / %) = (([m2]-[n2]) / [m2]) x 100.
[0037] The styrene-equivalent weight average molecular weight (M1 (g / mol)) of the acetone-soluble portion (II) in the acrylic rubber polymer (A) is preferably 30,000 to 60,000. The acetone-soluble portion (II) in the acrylic rubber polymer (A) mainly contains a straight-chain polymer of an acrylic acid ester monomer that is not crosslinked, and indirectly represents the molecular chain length constituting the acrylic rubber polymer (A). Therefore, if the styrene-equivalent weight average molecular weight (M1) of the acetone-soluble portion (II) in the acrylic rubber polymer (A) is 30,000 or more, the impact resistance can be further improved while maintaining the surface smoothness of the thermoplastic resin composition. In addition, as described above, this straight-chain polymer is a factor that impairs the surface smoothness of the thermoplastic resin composition, and this is remarkable when the straight-chain polymer is a long chain. Therefore, if the styrene-equivalent weight average molecular weight (M1) of the acetone-soluble portion (II) in the acrylic rubber polymer (A) is 60,000 or less, the impact resistance of the thermoplastic resin composition can be further improved while maintaining the impact resistance.
[0038] Here, the weight average molecular weight (M1) of the acetone soluble portion (II) in the acrylic rubber polymer (A) in terms of styrene can be determined by dissolving about 0.02 g of the acetone soluble portion (II) in the acrylic rubber polymer (A) obtained by the above-mentioned method in about 8 g of tetrahydrofuran to prepare a solution of about 0.2 mass%, and converting the GPC chromatogram measured using this solution to polystyrene as a standard substance. The GPC measurement can be performed under the following conditions. Measurement equipment: Waters2695 Column temperature: 40℃ Detector: RI2414 (differential refractometer) Carrier eluent flow rate: 0.3 ml / min (solvent: tetrahydrofuran) Column: TSKgel SuperHZM-M (6.0 mm I.D. x 15 cm), TSKgel SuperHZM-N (6.0 mm I.D. x 15 cm) in series (both manufactured by Tosoh Corporation).
[0039] As a polymerization method for the acrylic rubber polymer (A), an emulsion polymerization method is preferred from the viewpoint of adjusting the degree of crosslinking of the acrylic rubber polymer (A) and, in turn, the swelling degree (d1) of the butyl benzoate insoluble matter (I) to a desired range by the equilibrium between the monomer oil droplets, the aqueous phase, and the polymer particles.
[0040] The initiator used in the polymerization is not particularly limited, and peroxides, azo compounds, persulfates, etc. may be used.
[0041] Specific examples of peroxides include benzoyl peroxide, cumene hydroperoxide, dicumyl peroxide, diisopropylbenzene hydroperoxide, t-butyl hydroperoxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butyl isopropyl carbonate, di-t-butyl peroxide, t-butyl peroctate, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and t-butylperoxy-2-ethylhexanoate.
[0042] Specific examples of azo compounds include azobisisobutyronitrile, azobis(2,4-dimethylvaleronitrile, 2-phenylazo-2,4-dimethyl-4-methoxyvaleronitrile, 2-cyano-2-propylazoformamide, 1,1'-azobiscyclohexane-1-carbonitrile, azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl 2,2'-azobisisobutyrate, 1-t-butylazo-2-cyanobutane, and 2-t-butylazo-2-cyano-4-methoxy-4-methylpentane.
[0043] Specific examples of persulfates include potassium persulfate, sodium persulfate, and ammonium persulfate.
[0044] Two or more of the initiators may be used. In the emulsion polymerization method, potassium persulfate, cumene hydroperoxide, etc. are preferably used. Also, a redox initiator can be used.
[0045] The emulsifier used in the emulsion polymerization method for the acrylic rubber polymer (A) is preferably at least one emulsifier (d) selected from the group consisting of sulfate ester emulsifiers having only one anionic functional group and sulfosuccinic acid emulsifiers having two anionic functional groups, and a carboxylic acid emulsifier (e) having only one anionic functional group, since this combination will give an acrylic rubber polymer (A) having the appropriate degree of crosslinking described above.
[0046] When two or more kinds of emulsifiers are used in emulsion polymerization, they are mixed together and participate in the emulsification of micelles or polymer particles. Therefore, the polymerization rate (ease of polymerization control), volume average particle size, and degree of crosslinking are significantly different from the case where only one kind is used alone. For example, when emulsifier (d) is used alone, the polymerization rate is fast and polymerization control is difficult, and the degree of crosslinking is high and the rubber hardens, so that the thermoplastic resin composition cannot exhibit impact resistance, whereas when carboxylic acid-based emulsifier (e) is used alone, the polymerization rate is slow and the degree of crosslinking is low and the rubber is soft, so that the graft copolymer (B) described later is likely to have an aggregated structure in the thermoplastic resin composition, and the presence of such coarse particles impairs the surface smoothness and color development. By using two or more types of emulsifiers in combination, the swelling degree (d1) of the butyl benzoate insoluble matter (I) and the content (d2) of the acetone soluble matter (II) of the acrylic rubber polymer (A) can be adjusted to the desired range, making it possible to provide a thermoplastic resin composition with high levels of impact resistance, surface smoothness, and color development.
[0047] In the present invention, the emulsifier (d) is one or more selected from the group consisting of sulfate ester emulsifiers having only one anionic functional group and sulfosuccinic acid emulsifiers having two anionic functional groups. Here, the anionic functional group refers to a structure that ionizes to become an anion, and in the case of sulfate ester emulsifiers or sulfosuccinic acid emulsifiers, the acid metal salt structures of sulfate, carboxylate, and sulfonate correspond to this. The strength of the emulsifying ability of the emulsifier varies depending on the type and number of anionic functional groups, and the acidity is carboxy group < sulfo group < sulfate group. From the viewpoint of controlling the emulsification state to adjust the swelling degree (d1) of the butyl benzoate insoluble matter (I) of the acrylic rubber polymer (A) and the content ratio (d2) of the acetone soluble matter (II) to the desired range, it is preferable that the sulfate ester emulsifier has one anionic functional group and the sulfosuccinic acid emulsifier has two anionic functional groups.
[0048] Specific examples of sulfate emulsifiers having only one anionic functional group include polyoxyethylene alkyl ether sulfates, polyoxyethylene alkyl phenyl ether sulfates, etc. The salts referred to here include alkali metal salts such as ammonium salts, sodium salts, lithium salts, and potassium salts.
[0049] A specific example of a sulfosuccinic acid-based agent having two anionic functional groups is polyoxyethylene alkyl sulfosuccinate. Examples of the salts include alkali metal salts such as ammonium salts, sodium salts, lithium salts, and potassium salts.
[0050] The emulsifier (d) of the present invention has a structure in which ethylene oxide is added to the molecular structure. Since the structure is highly hydrophilic, an anionic emulsifier having the structure does not produce water-insoluble precipitates due to alkaline earth metal ions such as calcium and magnesium. Since the emulsifier (d) does not produce water-insoluble precipitates due to alkaline earth metal ions such as calcium and magnesium, even when the graft copolymer (B) latex described below is coagulated using a salt of calcium or magnesium, the emulsifier (d) does not remain in the recovered graft copolymer (B), and the surface smoothness and color development can be further improved while maintaining impact resistance.
[0051] In the present invention, the carboxylic acid emulsifier (e) has only one anionic functional group, that is, the carboxylic acid emulsifier (e) has only one carboxylate metal salt structure.
[0052] Specific examples of carboxylic acid emulsifiers having only one anionic functional group include caprylate, caprate, laurate, myristic acid salt, palmitate, stearate, oleate, linoleate, linolenate, disproportionated rosinate, and behenate. From the viewpoint of controlling the emulsification state based on the balance between hydrophobic groups and hydrophilic groups, and adjusting each parameter such as the ratio (d1 / d3) of the swelling degree (d1) of the butyl benzoate insoluble component (I) in the acrylic rubber polymer (A) to the swelling degree (d3) of the acetone insoluble component (III) in the acrylic rubber polymer (A) and the weight average molecular weight (M1) of the acetone soluble component (II) in the styrene equivalent in the acrylic rubber polymer (A) to a desired range, disproportionated rosinate is most preferred. Examples of the salts referred to here include alkali metal salts such as ammonium salts, sodium salts, lithium salts, and potassium salts.
[0053] In the present invention, the weight ratio of the emulsifier (d) and the carboxylic acid emulsifier (e) used in the entire polymerization of the acrylic rubber polymer (A) (weight of (d) used / weight of (e) used) calculated as solid content is preferably 0.1 to 0.4, more preferably 0.11 to 0.35, and most preferably 0.12 to 0.30.
[0054] When the value of the weight of emulsifier (d) used / the weight of carboxylic acid emulsifier (e) used is large, i.e., when the weight of emulsifier (d) used is relatively large compared to the weight of carboxylic acid emulsifier (e) used, the properties approach those of emulsifier (d) alone, so that the polymerization rate is fast, the degree of crosslinking is high, and the rubber hardens, resulting in poor impact resistance. If the weight ratio of emulsifier (d) to carboxylic acid emulsifier (e) used in the entire polymerization of acrylic rubber polymer (A) (weight of (d) used / weight of (e) used) is 0.4 or less, the impact resistance of the thermoplastic resin composition can be maintained while the surface smoothness can be further improved.
[0055] On the other hand, when the value of the weight of emulsifier (d) used / the weight of carboxylic acid emulsifier (e) used is small, that is, when the weight of carboxylic acid emulsifier (e) used is relatively large compared to the weight of emulsifier (d), the properties approach those of the carboxylic acid emulsifier (e) alone, resulting in a slow polymerization rate, a low degree of crosslinking, and a soft rubber, resulting in poor surface smoothness and color development. If the weight ratio of emulsifier (d) to carboxylic acid emulsifier (e) used in the entire polymerization of acrylic rubber polymer (A) (weight of (d) used / weight of (e) used) is 0.1 or more, the impact resistance can be further improved while maintaining the surface smoothness of the thermoplastic resin composition.
[0056] The acrylic rubber polymer (A) of the present invention exhibits excellent properties when it is made into a thermoplastic resin composition containing a graft copolymer (B) obtained by graft polymerizing a monomer mixture (c) containing an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of the acrylic rubber polymer (A) and a vinyl copolymer (C) described below. The thermoplastic resin composition of the present invention can improve the impact resistance when the thermoplastic resin composition is molded by containing the graft copolymer (B) using the acrylic rubber polymer of the present invention. In addition, the surface smoothness and color development can be improved when the thermoplastic resin composition is molded by containing the vinyl copolymer (C).
[0057] Here, the graft copolymer (B) is a general term for the polymers produced in the process of obtaining the graft copolymer (B), and includes the polymer produced by graft polymerization onto the acrylic rubber polymer as well as the polymer component produced without being graft polymerized onto the acrylic rubber polymer. The monomer mixture (c) may further contain other copolymerizable monomers as described below.
[0058] The amount of the acrylic rubber polymer (A) used in the graft copolymer (B) is preferably 20% by mass or more and 80% by mass or less based on the total amount of the acrylic rubber polymer (A) and the monomer mixture (c). If the amount of the acrylic rubber polymer (A) used is 20% by mass or more, the impact resistance can be further improved. The amount of the acrylic rubber polymer (A) is more preferably 35% by mass or more. On the other hand, if the amount of the acrylic rubber polymer (A) used is 80% by mass or less, the impact resistance, surface smoothness and color development when the thermoplastic resin composition is molded can be further improved, and 60% by mass or less is more preferable.
[0059] Examples of aromatic vinyl monomers contained in the monomer mixture (c) include styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, o-methylstyrene, vinyltoluene, and t-butylstyrene. The monomer mixture (c) may contain two or more aromatic vinyl monomers. Among these, styrene is preferred.
[0060] Examples of the vinyl cyanide monomer contained in the monomer mixture (c) include acrylonitrile, methacrylonitrile, ethacrylonitrile, etc. Two or more of these may be used. Among these, acrylonitrile is preferred.
[0061] The other copolymerizable monomer contained in the monomer mixture (c) is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include unsaturated carboxylic acid alkyl ester monomers, unsaturated fatty acids, acrylamide monomers, maleimide monomers, etc. Two or more of these may be used.
[0062] Examples of the unsaturated carboxylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, chloromethyl (meth)acrylate, etc. Two or more of these may be used.
[0063] Examples of unsaturated fatty acids include itaconic acid, maleic acid, fumaric acid, butenoic acid, acrylic acid, methacrylic acid, etc. Two or more of these may be used.
[0064] Examples of the acrylamide monomer include acrylamide, methacrylamide, N-methylacrylamide, etc. Two or more of these may be used.
[0065] Examples of the maleimide monomer include N-methylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-hexylmaleimide, N-octylmaleimide, N-dodecylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, etc. Two or more of these may be used.
[0066] The mixing ratio of the monomer mixture (c) is preferably in the range of 60 to 80 mass% of aromatic vinyl monomers, 20 to 40 mass% of vinyl cyanide monomers, and 0 to 20 mass% of other copolymerizable monomers, based on a total amount of 100 mass% of the monomer mixture (c).
[0067] As the polymerization method of the graft copolymer (B), any method such as emulsion polymerization, suspension polymerization, continuous bulk polymerization, and solution continuous polymerization can be used, and two or more of these may be combined. Among these, emulsion polymerization or bulk polymerization is preferred. Emulsion polymerization is most preferred because it is easy to control the temperature during polymerization.
[0068] The emulsifier used in the emulsion polymerization method of the graft copolymer (B) is not particularly limited, and various surfactants can be used. As the surfactant, anionic surfactants such as carboxylate type, sulfate ester salt type, sulfonate type, and sulfosuccinate type are preferably used. Two or more of these may be used.
[0069] Specific examples of anionic surfactants include caprylates, caprates, laurates, myristic acid salts, palmitates, stearates, oleates, linoleates, linolenates, disproportionated rosinates, behenates, castor oil sulfates, lauryl alcohol sulfates, dodecylbenzenesulfonates, alkylnaphthalenesulfonates, alkyldiphenyletherdisulfonates, naphthalenesulfonate condensates, polyoxyethylene alkylether sulfates, polyoxyethylene alkylphenylether sulfates, dialkylsulfosuccinates, polyoxyethylene alkylsulfosuccinates, etc. Examples of the salts mentioned here include alkali metal salts such as ammonium salts, sodium salts, lithium salts, and potassium salts.
[0070] As the polymerization initiator used in the polymerization of the graft copolymer (B), those exemplified as the initiator used in the polymerization of the acrylic rubber polymer (A) can be mentioned.
[0071] A chain transfer agent can also be used for the purpose of adjusting the polymerization degree and graft rate of the graft copolymer (B). Specific examples of the chain transfer agent include mercaptans such as n-octyl mercaptan, t-dodecyl mercaptan, n-dodecyl mercaptan, n-tetradecyl mercaptan, and n-octadecyl mercaptan, and terpenes such as terpinolene. Two or more of these may be used. Among these, n-octyl mercaptan and t-dodecyl mercaptan are preferably used.
[0072] From the viewpoint of adjusting the graft ratio of the graft copolymer (B) to the above-mentioned preferred range, it is preferable to use 0.05 to 0.5 parts by mass of a chain transfer agent, 0.5 to 5 parts by mass of an emulsifier, and 0.1 to 0.5 parts by mass of an initiator in the polymerization of the graft copolymer (B) relative to a total of 100 parts by mass of the acrylic rubber polymer (A) and the monomer mixture (c).
[0073] The graft copolymer (B) can be recovered by adding a coagulant to the graft copolymer (B) latex produced by emulsion polymerization. An acid or a water-soluble salt is used as the coagulant. Specific examples of the coagulant include acids such as sulfuric acid, hydrochloric acid, phosphoric acid, and acetic acid, and water-soluble salts such as calcium chloride, magnesium chloride, barium chloride, aluminum chloride, magnesium sulfate, aluminum sulfate, ammonium aluminum sulfate, potassium aluminum sulfate, and sodium aluminum sulfate. Two or more of these may be used. When coagulation is performed with an acid, a method of recovering the graft copolymer (B) after neutralizing the acid with an alkali can also be used.
[0074] The vinyl copolymer (C) used in the present invention is obtained by copolymerizing at least an aromatic vinyl monomer and a vinyl cyanide monomer, and may be further copolymerized with a monomer copolymerizable therewith, if necessary.
[0075] Specific examples of aromatic vinyl monomers include styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, o-methylstyrene, t-butylstyrene, etc. Two or more of these may be used. Among these, styrene is preferred.
[0076] The content of the aromatic vinyl monomer in the total amount of monomers constituting the vinyl copolymer (C) is preferably 60 to 80 mass%. If the aromatic vinyl monomer is 60 mass% or more, the flowability of the thermoplastic resin composition can be further improved. On the other hand, if the aromatic vinyl monomer is 80 mass% or less, the impact resistance of the molded article can be further improved.
[0077] Specific examples of vinyl cyanide monomers include acrylonitrile, methacrylonitrile, ethacrylonitrile, etc. Two or more of these may be used. Among these, acrylonitrile is preferred.
[0078] The content of the vinyl cyanide monomer in the total amount of monomers constituting the vinyl copolymer (C) is preferably 20 to 40% by mass. If the content of the vinyl cyanide monomer is 20% by mass or more, the impact resistance of the molded article can be further improved. On the other hand, if the content of the vinyl cyanide monomer is 40% by mass or less, the color development and color tone of the thermoplastic resin composition can be further improved.
[0079] The copolymerizable other monomer is not particularly limited as long as it does not impair the effects of the present invention, and specific examples thereof include unsaturated carboxylic acid alkyl ester monomers, unsaturated fatty acids, acrylamide monomers, maleimide monomers, etc. Two or more of these may be used. Specific examples of the other monomer include those exemplified as other monomers constituting the monomer mixture (c) used in the graft copolymer (B).
[0080] In the total amount of the monomers constituting the vinyl copolymer (C), 100% by mass, the content of other copolymerizable monomers is preferably 0 to 20% by mass. If the content of other copolymerizable monomers is 20% by mass or less, the balance between the flowability of the thermoplastic resin composition and the impact resistance of the molded article can be further improved.
[0081] The polymerization method for the vinyl copolymer (C) can be any of the suspension polymerization method, emulsion polymerization method, and continuous bulk polymerization method, and two or more of these methods may be combined. Among these, suspension polymerization is the most preferable in terms of ease of polymerization control and ease of post-treatment.
[0082] Examples of the suspension stabilizer used in the suspension polymerization include inorganic suspension stabilizers such as barium sulfate and magnesium hydroxide, and organic suspension stabilizers such as polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, polyacrylamide, and methyl methacrylate / acrylamide copolymers. Two or more of these may be used. Among these, organic suspension stabilizers are preferred in terms of color stability.
[0083] Examples of initiators used in suspension polymerization of the vinyl copolymer (C) include those exemplified as initiators for the graft copolymer (B). In addition, for the purpose of adjusting the degree of polymerization of the vinyl copolymer (C), it is also possible to use chain transfer agents such as mercaptan and terpene exemplified as chain transfer agents used in the graft copolymer (B). In the suspension polymerization, a slurry of the vinyl copolymer (C) is obtained, which is then dehydrated and dried to obtain a bead-like vinyl copolymer (C).
[0084] The thermoplastic resin composition of the present invention is obtained by blending 20 to 60 parts by mass of the graft copolymer (B) and 80 to 40 parts by mass of the vinyl copolymer (B) with respect to 100 parts by mass in total of the graft copolymer (B) and the vinyl copolymer (C). If the blending amount of the graft copolymer (B) is less than 20 parts by mass and the blending amount of the vinyl copolymer (C) exceeds 80 parts by mass, the impact resistance of the molded article decreases. From the viewpoint of further improving the impact resistance of the molded article, it is preferable to blend 30 parts by mass or more of the graft copolymer (B) and 70 parts by mass or less of the vinyl copolymer (C), and it is more preferable to blend 35 parts by mass or more of the graft copolymer (B) and 65 parts by mass or less of the vinyl copolymer (C). On the other hand, if the blending amount of the graft copolymer (B) exceeds 60 parts by mass and the blending amount of the vinyl copolymer (C) is less than 40 parts by mass, the flowability and moldability of the thermoplastic resin composition decrease. It is preferable to blend 60 parts by mass or less of the graft copolymer (B) and 40 parts by mass or more of the vinyl copolymer (C).
[0085] The thermoplastic resin composition of the present invention may further contain a heat-resistant vinyl copolymer (D) obtained by copolymerizing an aromatic vinyl monomer, a vinyl cyanide monomer, and a maleimide monomer, and / or a polycarbonate resin (E), which can improve heat resistance. The polycarbonate resin (E) is more preferred, and can further improve surface impact resistance.
[0086] As the aromatic vinyl monomer constituting the heat-resistant vinyl copolymer, those exemplified as the aromatic vinyl monomer used in the graft copolymer (B) can be mentioned, and styrene is preferably used. As the cyanide vinyl monomer constituting the heat-resistant vinyl copolymer, those exemplified as the vinyl cyanide monomer used in the graft copolymer (B) can be mentioned, and acrylonitrile is preferably used. As the heat-resistant vinyl monomer constituting the heat-resistant vinyl copolymer, those exemplified as the maleimide monomer optionally used in the graft copolymer (B) can be mentioned, and N-phenylmaleimide is preferably used.
[0087] The monomer composition ratio constituting the heat-resistant vinyl copolymer is preferably in the range of 36 to 65 mass% of aromatic vinyl monomer, 0 to 12 mass% of vinyl cyanide monomer, and 35 to 52 mass% of maleimide monomer, based on a total of 100 mass% of aromatic vinyl monomer, vinyl cyanide monomer, and maleimide monomer.
[0088] In the thermoplastic resin composition of the present invention, the blending amount of the heat-resistant vinyl copolymer is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the total of the graft copolymer (B) and the vinyl copolymer (C). On the other hand, the blending amount of the heat-resistant vinyl copolymer is preferably 100 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 85 parts by mass or less.
[0089] The polycarbonate resin used in the present invention is a thermoplastic resin obtained by reacting a divalent or higher phenolic compound with a carbonate diester compound such as phosgene or diphenyl carbonate. As the polycarbonate resin, for example, a polycarbonate resin obtained by an interfacial polycondensation method in which bisphenol A reacts with phosgene, or a polycarbonate resin obtained by a melt polymerization method in which bisphenol A reacts with diphenyl carbonate is preferable.
[0090] In the thermoplastic resin composition of the present invention, the blending amount of the polycarbonate resin is preferably 10 parts by mass or more relative to 100 parts by mass of the total of the graft copolymer (B) and the vinyl-based copolymer (C). By making the blending amount of the polycarbonate resin 10 parts by mass or more, the heat resistance and surface impact resistance are improved. The blending amount of the polycarbonate resin is more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more. On the other hand, the blending amount of the polycarbonate resin is preferably 400 parts by mass or less from the viewpoint of flowability and moldability.
[0091] The thermoplastic resin composition of the present invention may contain, within the scope of not impairing the effects of the present invention, antioxidants such as hindered phenols, sulfur-containing organic compounds, and phosphorus-containing organic compounds, heat stabilizers such as phenols and acrylates, ultraviolet absorbers such as benzotriazoles, benzophenones, and salicylates, various stabilizers such as organic nickel and hindered amine light stabilizers, lubricants such as metal salts of higher fatty acids and higher fatty acid amides, plasticizers such as phthalates and phosphates, drip prevention agents such as polytetrafluoroethylene, antistatic agents, carbon black, titanium oxide, pigments and dyes, and liquids such as water, silicone oil, and liquid paraffin.Fillers may also be added.
[0092] Examples of fillers include those in the form of fibers, plates, powders, and particles, and any of these may be used in the present invention. Specifically, examples of fillers include polyacrylonitrile (PAN)-based or pitch-based carbon fibers, metal fibers such as stainless steel fibers, aluminum fibers, and brass fibers, organic fibers such as aromatic polyamide fibers, gypsum fibers, ceramic fibers, asbestos fibers, zirconia fibers, alumina fibers, silica fibers, titanium oxide fibers, silicon carbide fibers, glass fibers, rock wool, potassium titanate whiskers, barium titanate whiskers, aluminum borate whiskers, and silicon nitride whiskers, as well as powdery, granular, or plate-like fillers such as mica, talc, kaolin, silica, calcium carbonate, glass flakes, glass beads, glass microballoons, clay, molybdenum disulfide, wollastonite, montmorillonite, titanium oxide, zinc oxide, barium sulfate, calcium polyphosphate, and graphite. Two or more of these may be used. Among these, glass fibers are preferably used. The type of glass fiber is not particularly limited as long as it is generally used for reinforcing resins, and examples thereof include chopped strands of long fiber type or short fiber type, milled fiber, etc. The surface of the filler may be treated with any coupling agent (e.g., silane-based coupling agent, titanate-based coupling agent, etc.) or other surface treatment agent. In addition, the filler may be coated or bundled with a thermoplastic resin such as an ethylene / vinyl acetate copolymer or a thermosetting resin such as an epoxy resin, or may be treated with a coupling agent such as aminosilane or epoxysilane.
[0093] The amount of the filler is preferably 0.01 to 100 parts by mass relative to 100 parts by mass of the total of the graft copolymer (B) and the vinyl copolymer (C). By setting the amount of the filler in this range, the rigidity and heat resistance of the molded article are improved. The amount of the filler is more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more. On the other hand, the amount of the filler is more preferably 50 parts by mass or less, and even more preferably 30 parts by mass or less.
[0094] The method for producing the thermoplastic resin composition is not particularly limited, but from the viewpoint of productivity, the graft copolymer (B), the vinyl copolymer (C), and other components as necessary are generally melt-kneaded. When the above-mentioned additives are blended, the blending method is not particularly limited, and various methods can be used.
[0095] The thermoplastic resin composition of the present invention can be molded by known methods such as injection molding, extrusion molding, blow molding, vacuum molding, compression molding, and gas-assisted molding. Although there is no particular limitation, it is preferably molded by injection molding. Injection molding can be performed at a temperature range of preferably 210 to 320°C. The mold temperature during injection molding is preferably 30 to 80°C.
[0096] The transparent styrene-based thermoplastic resin composition of the present invention can be widely used as a molded product of any shape, such as a film, sheet, fiber, cloth, nonwoven fabric, injection molded product, extrusion molded product, vacuum / compressed air molded product, blow molded product, or a composite with other materials. EXAMPLES
[0097] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited to these examples. First, the evaluation method will be described.
[0098] (1) Volume average particle size The resulting rubber polymer latex was diluted and dispersed in an aqueous medium, and the particle size distribution was measured. The conditions for measuring the volume average particle size are shown below. Instrument: Beckman Coulter LS 13 320 Measurement method: Laser scattering diffraction method Measurement time: 90s
[0099] (2) Swelling degree (d1) of the butyl benzoate insoluble matter (I) of the acrylic rubber polymer (A) Acrylic rubber polymer (A) latex and a 10% by mass calcium chloride aqueous solution were added to methanol, and then dehydration and washing were performed to obtain a solid acrylic rubber polymer (A). The obtained solid acrylic rubber polymer (A) was vacuum dried at 80°C for 3 hours, and a predetermined amount was then impregnated with butyl benzoate for 18 hours, and the weight (x) of the sample in which the butyl benzoate insolubles (I) had swollen was measured. Because the boiling point of butyl benzoate is high at approximately 250°C, the operation of impregnating the sample in which the butyl benzoate insolubles (I) had swollen with acetone for more than 1 hour was repeated three times while exchanging the acetone, thereby replacing the butyl benzoate with acetone. Next, after vacuum drying at 80°C for 3 hours, the weight (y) of the sample after drying of the butyl benzoate insolubles (I) was measured. The swelling degree (d1) was calculated from the weight (x) of the swollen sample and the weight (y) of the sample after drying according to the following formula. The swelling degree (d1) of the butyl benzoate insoluble matter (I) = (x) / (y).
[0100] (3) Content of acetone soluble matter (II) in the acrylic rubber polymer (A) (d2, mass%) Acrylic rubber polymer (A) latex and a 10% by mass calcium chloride aqueous solution were added to methanol, and then dehydration and washing were performed to obtain a solid acrylic rubber polymer (A). The obtained solid acrylic rubber polymer (A) was vacuum dried at 80°C for 3 hours, and then a predetermined amount was dissolved in acetone for 18 hours. Next, the acetone insolubles were vacuum dried at 80°C for 3 hours, and the weight (n1) of the sample after drying the acetone insolubles was measured. The content (d2) of the acetone solubles (II) was calculated from the weight (m1) of the sample and the weight (n1) of the sample after drying the acetone insolubles using the following formula. Content of acetone soluble matter (II) (d2, mass%) = (([m1] - [n1]) / [m1]) × 100.
[0101] (4) Swelling degree (d3) of the acetone insoluble matter (III) of the acrylic rubber polymer (A) Acrylic rubber polymer (A) latex and a 10% by mass calcium chloride aqueous solution were added to methanol, and then dehydration and washing were performed to obtain a solid acrylic rubber polymer (A). The obtained solid acrylic rubber polymer (A) was vacuum dried at 80°C for 3 hours, and then a predetermined amount was impregnated with acetone for 18 hours, and the weight (z) of the sample in which the acetone insolubles (III) had swollen was measured. Next, the acetone insolubles (III) were vacuum dried at 80°C for 3 hours, and the weight (w) of the sample after drying was measured. The swelling degree (d3) was calculated from the weight (z) of the sample in which the acetone insolubles (III) had swollen and the weight (w) of the sample after drying of the acetone insolubles (III) using the following formula. The swelling degree of the acetone insoluble fraction (III) (d3) = (z) / (w).
[0102] (5) Content of butyl benzoate soluble matter (IV) in the acrylic rubber polymer (A) (d2, mass%) Acrylic rubber polymer (A) latex and a 10% mass percent calcium chloride aqueous solution were added to methanol, and then dehydration and washing were performed to obtain a solid acrylic rubber polymer (A). The obtained solid acrylic rubber polymer (A) was vacuum dried at 80°C for 3 hours, and then a specified amount (m2) was dissolved in butyl benzoate for 18 hours. Since the boiling point of butyl benzoate is high at about 250°C, the sample in which the butyl benzoate insolubles were swollen was immersed in acetone for more than 1 hour, and this operation was repeated three times while exchanging acetone to replace butyl benzoate. Next, after vacuum drying at 80°C for 3 hours, the weight (n2) of the sample after drying was measured. The content (d4) of butyl benzoate solubles (IV) was calculated from the weight (m2) of the sample and the weight (n2) of the sample after drying using the following formula. Content ratio of butyl benzoate soluble content (IV) (d4.% by mass) = (([m2]-[n2]) / [m2]) x 100.
[0103] (6) Toluene swelling degree of toluene-insoluble matter of acrylic rubber polymer (A) Acrylic rubber polymer (A) latex and a 10% by mass calcium chloride aqueous solution were added to methanol, and then dehydration and washing were performed to obtain a solid acrylic rubber polymer (A). The obtained solid acrylic rubber polymer (A) was vacuum dried at 80°C for 3 hours, and then a specified amount was impregnated with toluene for 18 hours, and the weight (x1) of the sample with swollen toluene insolubles was measured. Next, after vacuum drying at 80°C for 3 hours, the weight (y1) of the sample after drying of the toluene insolubles was measured. The swelling degree was calculated from the weight (x1) of the sample with swollen toluene insolubles and the weight (y1) of the sample after drying using the following formula. Toluene swelling degree = (x1) / (y1).
[0104] (7) MEK swelling degree of 2-butanone (MEK) insoluble portion of acrylic rubber polymer (A) Acrylic rubber polymer (A) latex and a 10% by mass calcium chloride aqueous solution were added to methanol, and then dehydration and washing were performed to obtain a solid acrylic rubber polymer (A). The obtained solid acrylic rubber polymer (A) was vacuum dried at 80°C for 3 hours, and then a predetermined amount was impregnated with MEK for 18 hours, and the weight (x2) of the sample with the MEK insolubles swollen was measured. Next, the sample was vacuum dried at 80°C for 3 hours, and the weight (y2) of the sample after drying of the MEK insolubles was measured. The swelling degree was calculated from the weight (x2) of the sample with the MEK insolubles swollen and the weight (y2) of the sample after drying, using the following formula. MEK swelling degree = (x2) / (y2).
[0105] (8) Weight average molecular weight About 0.02 g of the sample was dissolved in about 8 g of tetrahydrofuran, and the content was calculated from the GPC chromatogram measured using a solution of about 0.2% by mass, using polystyrene as the standard substance. The GPC measurement was performed under the following conditions. Equipment:Waters2695 Column temperature: 40℃ Detector: RI2414 (differential refractometer) Carrier eluent flow rate: 0.3 ml / min (solvent: tetrahydrofuran) Column: TSKgel SuperHZM-M (6.0 mm I.D. x 15 cm), TSKgel SuperHZM-N (6.0 mm I.D. x 15 cm) in series (both manufactured by Tosoh Corporation).
[0106] (9) Surface smoothness (glossiness) The resin composition pellets were dried in a hot air dryer at 80°C for 3 hours, and then loaded into an SE-50DU molding machine manufactured by Sumitomo Heavy Industries, Ltd. with a cylinder temperature set at 230°C, and immediately molded into square plate molded products with a thickness of 3 mm. Using a digital variable angle gloss meter UGV-5D manufactured by Suga Test Instruments Co., Ltd., the gloss at 60° was measured for each of the five obtained square plate molded products, and the number average value was calculated.
[0107] (10) Color development (total light transmittance) The resin composition pellets were dried in a hot air dryer at 80°C for 3 hours, and then loaded into an SE-50DU molding machine manufactured by Sumitomo Heavy Industries, Ltd. with a cylinder temperature set at 230°C, and immediately molded into square plate molded products having a thickness of 3 mm. The total light transmittance was measured for each of the five obtained square plate molded products using a direct reading haze meter manufactured by Toyo Seiki Co., Ltd., and the number average value was calculated.
[0108] (11) Impact resistance (Charpy impact strength) The resin composition pellets were dried in a hot air dryer at 80°C for 3 hours, and then loaded into an SE-50DU molding machine manufactured by Sumitomo Heavy Industries, Ltd. with a cylinder temperature set at 230°C, and immediately molded into dumbbell test pieces with a thickness of 4 mm. The Charpy impact strength of each of the seven dumbbell test pieces obtained was measured by a method conforming to ISO179, and the number average value was calculated.
[0109] (12) Fluidity (Melt Flow Rate) The resin composition pellets were dried in a hot air dryer at 80°C for 3 hours, and then the melt flow rate was measured at 220°C and 98N in accordance with ISO1133. (13) Conversion Rate The monomer concentration (Mac) remaining in the acrylic rubber polymer (A) latex was calculated from the results of gas chromatography measured using a solution obtained by diluting the acrylic rubber polymer (A) latex 30 times with acetone. The remaining monomer weight (Ma) was obtained from the remaining monomer concentration in the acrylic rubber polymer (A) latex and the total charge weight used in the polymerization of the acrylic rubber polymer (A) latex. The polymerization rate was calculated from the total monomer weight (Mi) and the remaining monomer weight (Ma) charged in the polymerization of the acrylic rubber polymer (A) latex using the following formula. The gas chromatography measurement was performed under the following conditions. Polymerization rate=1-((Ma) / (Mi))×100 Equipment: Shimadzu GC-2014S Column: PorapakQ Detection temperature: 250℃
[0110] (Production Example 1) Acrylic rubber polymer (A-1) In a reaction vessel equipped with an agitator, 150 parts by mass of pure water, 0.3 parts by mass of sodium polyoxyethylene lauryl ether sulfate aqueous solution (solid content equivalent) as an emulsifier and 1 part by mass of disproportionated potassium rosinate aqueous solution (solid content equivalent) were charged, and the temperature was raised to 60°C. Under stirring, a mixture of 14.9 parts by mass of n-butyl acrylate and 0.1 parts by mass of allyl methacrylate was continuously added over 30 minutes. Next, while raising the temperature to 75°C, 13 parts by mass of 2% by mass potassium persulfate aqueous solution and 1.0 parts by mass of disproportionated potassium rosinate aqueous solution (solid content equivalent) were continuously added over 5 hours. In addition, 2 hours after the start of the addition of the potassium persulfate aqueous solution and the disproportionated potassium rosinate aqueous solution, a mixture of 84.1 parts by mass of n-butyl acrylate and 0.9 parts by mass of allyl methacrylate was added over 2.5 hours, and the mixture was held for another 1 hour after the completion of the addition to obtain an acrylic rubber polymer (A-1) latex with a polymerization rate of 97%.
[0111] Graft copolymer (B-1) In a reaction vessel equipped with an agitator, a mixture of 13.2 parts by mass of pure water, 0.48 parts by mass of anhydrous glucose, 0.26 parts by mass of sodium pyrophosphate and 0.01 parts by mass of ferrous sulfate, a mixture of 0.7 parts by mass of potassium oleate and 6 parts by mass of pure water, 50 parts by mass of acrylic rubber polymer (A-1) (solid content equivalent) and 100 parts by mass of pure water were charged into the reaction vessel, and the temperature was raised to 58 ° C., and a mixture (i) of 36.5 parts by mass of styrene, 13.5 parts by mass of acrylonitrile and 0.24 parts by mass of t-dodecyl mercaptan was continuously added over 4 hours under stirring. 0.5 hours after the start of continuous addition, the temperature in the vessel was raised to 62 ° C., and a mixture of 0.3 parts by mass of cumene hydroperoxide, 2.0 parts by mass of potassium oleate and 12.5 parts by mass of pure water was continuously added in parallel over 5 hours. Subsequently, the temperature was further raised to 65°C when the addition of (i) was completed, and a graft copolymer (B-1) latex was obtained with a polymerization rate of 98%. 100 parts by mass (solid content equivalent) of the obtained latex was poured into 900 parts by mass of 75°C water containing 3 parts by mass of calcium chloride while stirring to coagulate, and then dehydrated and dried to obtain a powdery graft copolymer (B-1).
[0112] (Production Examples 2 to 12) Acrylic rubber polymer (A-2 to A-12) latexes were obtained in the same manner as in Production Example 1, except that the n-butyl acrylate, allyl methacrylate, emulsifier, and amount of emulsifier used in Production Example 1 were changed as shown in Tables 1 and 2. Graft copolymers (B-2 to B-12) were produced in the same manner as in Production Example 1, except that the acrylic rubber polymer (A-1) was replaced with the acrylic rubber polymer (A-2 to A-12).
[0113] (Production Example 13) A graft copolymer (B-13) was produced in the same manner as in Production Example 1, except that 33.0 parts by mass of styrene and 17.0 parts by mass of acrylonitrile were used during the graft copolymerization.
[0114] (Production Example 14) Graft copolymer (B-14) was produced in the same manner as in Production Example 1, except that in addition to using 40 parts by mass (solid content equivalent) of the acrylic rubber polymer (A-1) during graft copolymerization, 43.8 parts by mass of styrene and 16.2 parts by mass of acrylonitrile were used.
[0115] (Production Examples 15 to 30) Acrylic rubber polymer (A-13 to A-27) latexes were obtained in the same manner as in Production Example 1, except that the n-butyl acrylate, allyl methacrylate, emulsifier, and amount of emulsifier used in Production Example 1 were changed as shown in Tables 3 to 4. Graft copolymers (B-15 to B-30) were produced in the same manner as in Production Example 1, except that the acrylic rubber polymer (A-13 to A-27) was used instead of the acrylic rubber polymer (A-1).
[0116] (Example 31) Vinyl copolymer (C-1) 80 parts by mass of acrylamide, 20 parts by mass of methyl methacrylate, 0.3 parts by mass of potassium persulfate, and 1800 parts by mass of pure water were charged into a reaction vessel, the gas phase in the reaction vessel was replaced with nitrogen gas, and the mixture was kept at 70° C. under stirring. The reaction was continued until the monomers were completely converted into polymers, after which 20 parts by mass of sodium hydroxide and 2000 parts by mass of pure water were added, and the mixture was stirred at 70° C. for 2 hours and then cooled to room temperature to obtain an aqueous solution of a methyl methacrylate-acrylamide binary copolymer to be used as a suspension polymerization medium.
[0117] A solution of 6 parts by mass of the methyl methacrylate-acrylamide binary copolymer aqueous solution dissolved in 165 parts by mass of pure water was placed in a reaction vessel equipped with an agitator and stirred at 90 rpm, and the system was replaced with nitrogen gas. Next, a monomer mixture of 28.9 parts by mass of acrylonitrile, 11.1 parts by mass of styrene, 0.32 parts by mass of azobisisobutyronitrile, and 0.32 parts by mass of t-dodecyl mercaptan was initially added over 30 minutes while stirring the reaction system, and the copolymerization reaction was started at 70 ° C. After the monomer mixture was added, 15 parts by mass of styrene was added using a feed pump one hour later. Then, styrene was added to the reaction system three times, 15 parts by mass each, at 30-minute intervals. After the completion of the addition of all the monomers, the temperature was raised to 100 ° C. over 60 minutes. After reaching this temperature, the temperature was kept at 100 ° C. for 30 minutes, and then cooled, and the polymer was separated, washed, and dried to obtain a bead-shaped vinyl copolymer (C-1).
[0118] (Examples 1 to 16, Comparative Examples 1 to 16) The graft copolymers (B-1 to 30) prepared in the above Production Examples 1 to 30 and the vinyl polymer (C-1) prepared in Production Example 31 were blended in the blending ratios shown in Tables 1 to 4, respectively, and 0.8 parts by mass of ethylene bisstearic acid amide was further added. The resulting mixture was melt-kneaded at an extrusion temperature of 230°C using a 40 mmφ extruder, extruded into a gut shape, and pelletized. The resulting pellets were injection molded at a molding temperature of 230°C and a mold temperature of 60°C to prepare various test pieces for evaluation. The results of evaluating these test pieces by the above-mentioned methods are shown in 1 to 4.
[0119] [Table 1]
[0120] [Table 2]
[0121] [Table 3]
[0122] [Table 4] [Industrial Applicability]
[0123] The thermoplastic resin composition of the present invention can provide a molded article having excellent impact resistance, surface smoothness, and color development. By utilizing such properties, the composition can be suitably used in outdoor equipment and automotive applications that require impact resistance, surface smoothness, and color development.
Claims
1. The acrylic rubber polymer (A) is obtained by copolymerizing an acrylic acid ester monomer (a) and a polyfunctional monomer (b), and contains a component (I) that is insoluble in butyl benzoate when immersed in butyl benzoate for 18 hours, and further contains a component (II) that is soluble in acetone when immersed in acetone for 18 hours, and is characterized in that, when the swelling degree of the butyl benzoate-insoluble component (I) defined by the following formula (1) is (d1), and the content of the acetone-soluble component (II) is (d2 (mass%)) when the acrylic rubber polymer (A) is 100 mass%, (d1) and (d2) satisfy the following formulas (2) and (3). (d1)=(x) / (y) (1) ((x): weight of (A) swollen with butyl benzoate, (y): weight of (A) after drying) 15≦(d1)≦25 (2) 3.0≦(d2 (mass%))≦8.0 (3)
2. The acrylic rubber polymer (A) according to claim 1, characterized in that the acrylic rubber polymer (A) contains a component (III) that is insoluble in acetone when immersed in acetone for 18 hours, and when the swelling degree of the acetone-insoluble component (III) in the acrylic rubber polymer (A) defined by the following formula (4) is (d3), the swelling degrees (d1) and (d3) of the butyl benzoate-insoluble component (I) satisfy the following formula (5): (d3)=(z) / (w) (4) ((z): weight of (A) swollen with acetone, (w): weight of (A) after drying) 1.6≦(d1 / d3)≦2.5 (5)
3. The acrylic rubber-based polymer (A) contains a component (IV) that dissolves in butyl benzoate when immersed in butyl benzoate for 18 hours, and when the content ratio of the butyl benzoate soluble component (IV) when the acrylic rubber-based polymer (A) is 100% by mass, the content ratio (d4 (mass%)) is 4 to 12% by mass relative to 100% by mass of the acrylic rubber-based polymer (A), and the difference (d4-d2) between the content ratio (d4) and the content ratio (d2) of the acetone soluble component (II) when the acrylic rubber-based polymer (A) is 100% by mass is 5% by mass or less.
4. The acrylic rubber polymer (A) according to claim 1, characterized in that the acetone soluble component (II) in the acrylic rubber polymer (A) has a weight average molecular weight (M1 (g / mol)) in terms of styrene of 30,000≦(M1)≦60,000.
5. A method for producing an acrylic rubber polymer (A), comprising emulsion-polymerizing 97 to 99.5% by mass of an acrylic acid ester monomer (a) and 0.5 to 3% by mass of a polyfunctional monomer (b) in the presence of at least one emulsifier (d) selected from the group consisting of a sulfate ester emulsifier having a structure in which ethylene oxide is added to its molecular structure and having only one anionic functional group, and a sulfosuccinic acid emulsifier having a structure in which ethylene oxide is added to its molecular structure and having two anionic functional groups, and a carboxylic acid emulsifier (e) having only one anionic functional group.
6. 6. The method for producing an acrylic rubber polymer (A) according to claim 5, wherein the emulsifier (d) contains a polyoxyethylene alkyl ether sulfate or a polyoxyethylene alkyl sulfosuccinate.
7. The method for producing an acrylic rubber-like polymer (A) according to claim 56, characterized in that the carboxylic acid-based emulsifier (e) contains a disproportionated rosin acid salt.
8. The method for producing an acrylic rubber-based polymer (A) according to claim 5, characterized in that the weight ratio of the emulsifier (d) to the carboxylic acid-based emulsifier (e) (weight of (d) used / weight of (e) used) is 0.1 to 0.
4.
9. A method for producing a graft copolymer (B), comprising graft polymerizing a monomer mixture (c) containing an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of the acrylic rubber polymer (A) according to any one of claims 1 to 4.
10. A thermoplastic resin composition comprising a graft copolymer (B) obtained by graft polymerizing a monomer mixture (c) containing an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of the acrylic rubber polymer (A) according to any one of claims 1 to 4, and a vinyl copolymer (C).
11. A molded article obtained by molding the thermoplastic resin composition according to claim 10.
Citation Information
Patent Citations
Composite resin composition
JP2003020377A
Thermoplastic resin composition
JP2016180096A
Thermoplastic resin composition and molding thereof
JP2019137751A
Thermoplastic resin composition for vehicle lamp housings
WO2011108486A1
Thermoplastic resin composition
WO2015119040A1
Cited By
Thermoplastic resin composition and method of producing the same
WO2026226027A1